Phosphate composite positive active material and preparation method thereof, positive pole piece, battery monomer, battery and electric device
The graphite oxide is peeled off by a high-speed dispersion homogenizer and formed graphene oxide. Combined with high-efficiency grinding treatment, an amorphous carbon cladding layer is constructed, which solves the problem of poor electronic conductivity of the phosphate positive electrode active material and improves the capacity and electrochemical performance of the battery. .
Patent Information
- Application Number
- CN202310637376.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The electronic conductivity of phosphate positive electrode active materials is poor, resulting in poor battery capacity and electrochemical performance, and it is difficult to achieve complete coverage of graphene's high cost and poor interface binding force.
The graphite oxide is peeled off into graphene oxide by a high-speed dispersion homogenizer, and an amorphous carbon cladding layer is formed with the phosphate positive electrode active material precursor in high-efficiency grinding treatment to build a continuous conductive network.
It reduces the cost of raw materials and energy consumption, improves the electronic conductivity and ionic conductivity of phosphate composite cathode active materials, and improves the capacity and electrochemical performance of the battery, such as cycling performance and rate performance.
Smart Images

Figure BDA0004262409500000201 
Figure HDA0004262409510000011 
Figure HDA0004262409510000012
Abstract
Description
Technical Field
[0001] The present application relates to a phosphate composite positive electrode active material and a preparation method thereof, a positive electrode sheet, a battery cell, a battery and an electrical device. Background Art
[0002] In recent years, batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. Positive electrode active material is one of the key factors affecting the electrochemical performance of batteries. Phosphate positive electrode active material has become one of the most concerned positive electrode active materials due to its advantages such as rich raw material sources. However, the electronic conductivity of phosphate positive electrode active materials is poor. At present, the electronic conductivity of phosphate positive electrode active materials is mainly improved by coating phosphate positive electrode active materials with graphene. However, the raw material cost of graphene is high, and the interface bonding force between graphene and phosphate positive electrode active material particles is poor, so it is difficult to achieve complete coating, which affects the capacity of the battery and the electrochemical performance of the battery. The above statement is only used to provide background technical information related to the present application, and does not necessarily constitute the prior art. Summary of the invention
[0003] The present application provides a phosphate composite positive electrode active material and a preparation method thereof, a positive electrode plate, a battery cell, a battery and an electrical device, which can reduce the raw material cost, energy consumption cost and time cost of the phosphate composite positive electrode active material, and can also improve the capacity and electrochemical performance of the phosphate composite positive electrode active material.
[0004] In a first aspect, the present application provides a method for preparing a phosphate composite positive electrode active material, comprising the following steps: providing a first mixed solution comprising graphite oxide and a metal salt for preparing a phosphate positive electrode active material, wherein the solvent in the first mixed solution comprises water; subjecting the first mixed solution to a first exfoliation reaction at a first shear rate of more than 6000 r / min, so that the graphite oxide is exfoliated into graphene oxide, to obtain a second mixed solution; maintaining the first shear rate, adding a precipitant or an aqueous solution of the precipitant to the second mixed solution for a second precipitation reaction, to obtain a third mixed solution, wherein the precipitant comprises one or more of oxalic acid and a water-soluble oxalate; The third mixed liquid is washed and dried to obtain a mixture of a phosphate positive electrode active material precursor and graphene oxide; the mixture of the phosphate positive electrode active material precursor and graphene oxide is ground with a lithium source, a phosphorus source, a carbon source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent to obtain a slurry, and then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material, wherein the phosphate composite positive electrode active material includes a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
[0005] The preparation method of the phosphate composite positive electrode active material provided by the present application uses low-cost graphite oxide as a raw material, thereby reducing the raw material cost in production, and also reducing energy consumption cost and time cost. The preparation method of the phosphate composite positive electrode active material provided by the present application also has the advantages of simple process and high production efficiency, and thus is also easy to carry out industrial large-scale production.
[0006] The preparation method of the phosphate composite positive electrode active material provided in the present application can obtain a phosphate composite positive electrode active material with a single crystal phase, high purity, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. In addition, the obtained phosphate composite positive electrode active material can form a continuous conductive network. Therefore, the phosphate composite positive electrode active material obtained by the preparation method provided in the present application has high electronic conductivity and high ionic conductivity, which is conducive to promoting the efficient transmission of electrons, and is also conducive to shortening the transmission path of ions, thereby helping to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0007] In any embodiment, the first stripping reaction is performed in a high-speed dispersing homogenizer.
[0008] In any embodiment, the first shearing speed is 6000-15000 r / min, and can be optionally 6000-10000 r / min.
[0009] In any embodiment, the time of the first stripping reaction is 30-150 minutes, and can be 60-120 minutes.
[0010] In any embodiment, the number of layers of the graphene oxide is 1-6, and can be optionally 3-5.
[0011] The number of graphene oxide layers can be adjusted by adjusting the first shear rate and the time of the first peeling reaction. The greater the first shear rate and the longer the time of the first peeling reaction, the fewer the number of graphene oxide layers obtained by peeling from graphite oxide. Therefore, the preparation method provided in the embodiment of the present application can also achieve the regulation of the number of graphene oxide layers.
[0012] In any embodiment, the mass ratio of the graphite oxide to the metal salt for preparing the phosphate positive electrode active material is 0.03:1-0.08:1.
[0013] In any embodiment, the concentration of the metal salt for preparing the phosphate positive electrode active material in the first mixed solution is 0.5-2 mol / L.
[0014] In any embodiment, the metal salt used to prepare the phosphate positive electrode active material includes a water-soluble divalent metal salt. Optionally, the water-soluble divalent metal salt includes one or more of sulfate, nitrate, hydrochloride and acetate.
[0015] In any embodiment, the divalent metal element includes Mn element and / or Fe element and optionally M element, and the M element represents the doping element of the Mn position and / or Fe position of the phosphate composite positive electrode active material, and optionally includes one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr.
[0016] In any embodiment, the second precipitation reaction time is 10-60 min.
[0017] In any embodiment, the molar ratio of the precipitant to the metal salt used to prepare the phosphate positive electrode active material is 1:1-3:1. Adjusting the amount of the precipitant helps to improve the conversion efficiency of metal ions and reduce the difference in precipitation rates of different metal ions in the reaction system, thereby facilitating the uniform coprecipitation of metal ions, and further facilitating the ratio of each metal element in the prepared phosphate composite positive electrode active material to the ratio of each metal element in the raw material to have a high consistency. Adjusting the amount of the precipitant also helps to make the coprecipitation reaction more complete, thereby reducing the metal ion content in the reaction waste liquid, reducing the difficulty of the waste liquid treatment process and reducing environmental pollution; in addition, it also helps to improve the purity of the obtained phosphate positive electrode active material precursor and reduce the impurity content.
[0018] In any embodiment, the precipitating agent includes one or more of oxalic acid, sodium oxalate, potassium oxalate and ammonium oxalate.
[0019] In any embodiment, the concentration of the aqueous solution of the precipitant is 0.5-2 mol / L.
[0020] In any embodiment, the step of providing a first mixed solution containing graphite oxide and a metal salt for preparing a phosphate positive electrode active material comprises the following steps: under a protective gas atmosphere, adding graphite oxide to water, and then adding the metal salt for preparing a phosphate positive electrode active material, and dispersing them evenly to obtain the first mixed solution.
[0021] In any embodiment, the shielding gas includes nitrogen, an inert gas, or a combination thereof.
[0022] In any embodiment, the first solvent includes one or more of an alcohol solvent and water, and may optionally include one or more of ethanol and water.
[0023] In any embodiment, the grinding process comprises a high energy ball milling process or a sand milling process.
[0024] In any embodiment, the grinding process has a rotation speed of 1000-2500 r / min.
[0025] In any embodiment, the grinding treatment time is 1-5h.
[0026] In any embodiment, the sintering process includes a pre-sintering process and a high-temperature sintering process;
[0027] In any embodiment, the temperature of the pre-sintering process is 350-550°C, and can be 400-500°C.
[0028] In any embodiment, the pre-sintering treatment time is 2-12 hours, and can be 3-10 hours.
[0029] In any embodiment, the temperature of the high temperature sintering treatment is 600-800°C, and can be optionally 650-750°C.
[0030] In any embodiment, the high temperature sintering treatment time is 5-24 hours, and can be optionally 8-12 hours.
[0031] In any embodiment, the pre-sintering process is performed under a protective gas atmosphere.
[0032] In any embodiment, the high temperature sintering process is performed under a protective gas atmosphere.
[0033] In any embodiment, the step of grinding the phosphate positive electrode active material precursor and the graphene oxide mixture with a lithium source, a phosphorus source, a carbon source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent to obtain a slurry, and then spray-drying, granulating, and sintering to obtain a phosphate composite positive electrode active material includes the following steps: grinding the phosphate positive electrode active material precursor and the graphene oxide mixture with a lithium source, a phosphorus source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent for a first time to obtain a first slurry; spray-drying and granulating the first slurry to obtain a powder, and then pre-sintering to obtain a pre-sintered powder; grinding the pre-sintered powder with the carbon source in the presence of a first solvent for a second time to obtain a second slurry; spray-drying and granulating the second slurry to obtain a powder, and then high-temperature sintering and optionally crushing to obtain the phosphate composite positive electrode active material.
[0034] Thereby, the obtained phosphate composite positive electrode active material can form a continuous conductive network, which is beneficial to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0035] In any embodiment, the rotation speed of the first grinding process is 1500-2500r / min.
[0036] In any embodiment, the first grinding process is performed for 1-5 hours.
[0037] In any embodiment, the rotation speed of the second grinding process is 1000-2500r / min.
[0038] In any embodiment, the second grinding process is performed for 1-3 hours.
[0039] In any embodiment, the Li-site doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo, and W.
[0040] In any embodiment, the P-site doping element includes one or more elements selected from the group consisting of B, S, Si and N.
[0041] In any embodiment, the O-site doping element includes one or more elements selected from the group consisting of S, F, Cl and Br.
[0042] In any embodiment, the lithium source includes one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium nitrate and lithium acetate.
[0043] In any embodiment, the phosphorus source includes one or more of phosphoric acid, monoammonium hydrogen phosphate, and diammonium hydrogen phosphate.
[0044] In any embodiment, the carbon source includes one or more of sucrose, glucose, polyvinyl alcohol, polyethylene glycol, phenolic resin, citric acid and cyclodextrin.
[0045] In any embodiment, the Li-site doping element source includes one or more of sulfates, nitrates, hydrochlorides and acetates of the Li-site doping element.
[0046] In any embodiment, the P-site doping element source includes one or more of sulfates, borates, nitrates and silicates of the P-site doping element.
[0047] In any embodiment, the O-site doping element source includes one or more of a simple substance and an ammonium salt of the O-site doping element.
[0048] The second aspect of the present application provides a phosphate composite positive electrode active material prepared by the method of the first aspect of the present application, wherein the phosphate composite positive electrode active material comprises a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
[0049] The phosphate composite positive electrode active material provided in the present application has the characteristics of single crystal phase, high purity, regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. In addition, the phosphate composite positive electrode active material also has a continuous conductive network and a shortened ion transmission path, which is beneficial to promote the efficient transmission of electrons and ions, and further helps to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0050] In any embodiment, the volume distribution particle size Dv50 of the phosphate composite positive electrode active material satisfies 0.5 μm≤Dv50≤3 μm.
[0051] In any embodiment, the volume distribution particle sizes Dv90 and Dv50 of the phosphate composite positive electrode active material satisfy 1<Dv90 / Dv50≤1.5.
[0052] In any embodiment, the powder resistivity of the phosphate composite positive electrode active material is 1-100 Ω·cm.
[0053] In any embodiment, the molecular formula of the phosphate positive electrode active material is Li a N b Fe x Mn y M 1-x-y P 1-m Q mO 4- n R n , M represents a doping element at the Mn position and / or the Fe position, optionally including one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr; N represents a doping element at the Li position, optionally including one or more elements of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a doping element at the P position, optionally including one or more elements of B, S, Si and N; R represents an O position doping element, optionally including one or more elements of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1; 0≤x≤1; 0≤y≤1; 0≤1-xy<1; 0≤m≤0.1; 0≤n≤0.1.
[0054] In any embodiment, 0.001≤x≤0.999, 0.001≤y≤0.999, and 0≤1-xy≤0.10.
[0055] In any embodiment, 0.199≤x≤0.500, 0.499≤y≤0.800, and 0<1-xy≤0.10.
[0056] The third aspect of the present application provides a positive electrode plate, including a positive electrode collector and a positive electrode film layer arranged on at least one surface of the positive electrode collector, wherein the positive electrode film layer includes a phosphate composite positive electrode active material prepared by the method of the first aspect of the present application or the phosphate composite positive electrode active material of the second aspect of the present application.
[0057] A fourth aspect of the present application provides a battery cell, comprising the positive electrode sheet according to the third aspect of the present application.
[0058] A fifth aspect of the present application provides a battery, comprising the battery cell of the fourth aspect of the present application.
[0059] A sixth aspect of the present application provides an electrical device, which includes the battery of the fifth aspect of the present application.
[0060] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some implementation methods of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0062] Figure 1It is a schematic diagram of the structure of a battery cell provided in some embodiments of the present application.
[0063] Figure 2 It is a schematic diagram of an exploded view of a battery cell provided in some embodiments of the present application.
[0064] Figure 3 It is a schematic diagram of the structure of the battery module provided in some embodiments of the present application.
[0065] Figure 4 It is a schematic diagram of the structure of the battery pack provided in some embodiments of the present application.
[0066] Figure 5 yes Figure 4 An exploded diagram of the battery pack is shown.
[0067] Figure 6 It is a schematic diagram of an electrical device provided in some embodiments of the present application.
[0068] Figure 7 (a) shows the Mn prepared in Example 1 0.6 Fe 0.4 Scanning electron microscope (SEM) image of a mixture of C2O4·2H2O and graphene oxide. Figure 7 (b) shows the Mn prepared in Comparative Example 1 0.6 Fe 0.4 Scanning electron microscope (SEM) image of C2O4·2H2O.
[0069] Figure 8 (a) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Example 1, Figure 8 (b) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Comparative Example 1.
[0070] Fig. 9 The capacity-voltage curves of button cells prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1.
[0071] Fig.10 The rate curves of button cells prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1.
[0072] In the drawings, the drawings may not be drawn according to the actual scale. The reference numerals are as follows: 1, battery pack; 2, upper box; 3, lower box; 4, battery module; 5, battery cell; 51, housing; 52, electrode assembly; 53, cover plate. DETAILED DESCRIPTION
[0073] Hereinafter, the phosphate composite positive electrode active material and its preparation method, positive electrode sheet, battery cell, battery and electric device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0074] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0075] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.
[0076] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.
[0077] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0078] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0079] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0080] If not otherwise specified, in this application, the terms "first", "second", "third", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.
[0081] In the present application, the terms "plurality" and "multiple" refer to two or more.
[0082] Unless otherwise specified, the terms used in this application have the commonly understood meanings that are commonly understood by those skilled in the art.
[0083] Unless otherwise specified, the values of the parameters mentioned in this application can be measured by various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise specified, the test temperature of each parameter is 25°C.
[0084] Poor electronic conductivity is an important factor that restricts the large-scale application of phosphate positive electrode active materials. At present, the main method is to directly mix phosphate positive electrode active materials with commercially available graphene, and prepare coated phosphate composite positive electrode active materials through a complex hydrothermal method or high-temperature solid phase method to improve the electronic conductivity of the core of the phosphate positive electrode active material. However, the price of commercially available graphene is relatively high, resulting in a high raw material cost for phosphate composite positive electrode active materials, which is not conducive to its promotion and application; at the same time, the interface bonding force between graphene and the core of phosphate positive electrode active materials is also poor, making it difficult to achieve complete coating and form a continuous conductive network, which results in the electronic conductivity of the phosphate composite positive electrode active material failing to achieve the expected effect, thereby affecting the capacity of the battery and the electrochemical performance of the battery.
[0085] In addition, graphene-coated phosphate composite positive electrode active materials are mainly prepared by high-temperature solid phase method, for example, physical grinding and mixing of lithium source, manganese source, iron source, doping element source and graphene by high-energy ball milling. Limited by the particle size of each raw material, it is difficult to mix manganese and iron elements at the atomic level, and the doping elements are not easy to enter the interior of the phosphate crystal, which affects the electrochemical performance of the prepared phosphate composite positive electrode active material. At the same time, the content of each metal element in the prepared phosphate composite positive electrode active material is also greatly deviated from the metal ratio in the raw material, resulting in poor batch consistency of the product.
[0086] In view of this, the inventors have improved the preparation process of phosphate composite positive electrode active materials.
[0087] The embodiment of the present application provides a method for preparing a phosphate composite positive electrode active material, comprising the following steps: providing a first mixed solution comprising graphite oxide and a metal salt for preparing a phosphate positive electrode active material, wherein the solvent in the first mixed solution comprises water; subjecting the first mixed solution to a first exfoliation reaction at a first shear rate of more than 6000 r / min, so that the graphite oxide is exfoliated into graphene oxide, to obtain a second mixed solution; maintaining the first shear rate, adding a precipitant or an aqueous solution of the precipitant to the second mixed solution for a second precipitation reaction, to obtain a third mixed solution, wherein the precipitant comprises one or more of oxalic acid and a water-soluble oxalate; The third mixed liquid is washed and dried to obtain a mixture of a phosphate positive electrode active material precursor and graphene oxide; the phosphate positive electrode active material precursor and the graphene oxide mixture are ground with a lithium source, a phosphorus source, a carbon source, an optional Li-site doping element source, an optional P-site doping element source, and an optional O-site doping element source in the presence of a first solvent to obtain a slurry, and then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material, wherein the phosphate composite positive electrode active material includes a phosphate positive electrode active material, amorphous carbon coated with the phosphate positive electrode active material, and reduced graphene oxide coated with the amorphous carbon.
[0088] The first peeling reaction is carried out in a high-speed dispersing homogenizer.
[0089] The high-speed dispersing homogenizer has a unique stator and rotor structure, which can generate super strong shear force and can also circulate materials to complete online dispersing, emulsifying, homogenizing and mixing processes.
[0090] When preparing phosphate composite positive electrode active materials, the high-speed rotation of the high-speed dispersing homogenizer can be used to suck the first mixed solution into its working chamber, and its strong centrifugal force can be used to throw the material radially into the narrow and precise gap between the rotor and the stator. At this time, the material will be fully dispersed and crushed under the effects of strong liquid phase shear, liquid layer friction and tearing collision, and then ejected at high speed through the stator slot, and then the flow direction is changed under the resistance of the material itself and the container wall. At the same time, under the action of the upper and lower axial suction forces generated in the rotor area, two strong upper and lower turbulent flows are formed. In this way, after multiple cycles, graphite oxide (usually in block form) can be stripped into graphene oxide, and the metal ions in the first mixed solution can also be tightly adsorbed on the graphene oxide. Conventional agitators can only play a simple dispersing role even at high stirring speeds, and they cannot strip graphite oxide into graphene oxide.
[0091] The surface of the graphene oxide stripped from graphite oxide has oxygen-containing functional groups (such as hydroxyl, carboxyl, etc.), which can produce electrostatic adsorption with metal ions with positive charge, so that metal salts can be closely adsorbed on the surface of graphene oxide. After adding a precipitant, the nucleus can grow and attach in situ on the surface of graphene oxide, and the phosphate positive active material precursor wrapped by graphene oxide can also be formed under the strong dispersion and crushing of the high-speed dispersion homogenizer. In addition, under the high-speed shearing effect of the high-speed dispersion homogenizer, the initial concentration of the reaction system can be instantly increased after adding a precipitant, and the metal salt and the precipitant are directly coprecipitated, which is conducive to faster nucleation rather than particle growth, and then it is conducive to preparing a phosphate positive active material precursor of small particle size; In addition, it is also conducive to each metal element to be uniformly coprecipitated, and then the phosphate positive active material precursor obtained can also be made to have a regular morphology, a narrow particle size distribution, uniform element distribution and high batch consistency.
[0092] When the obtained phosphate positive electrode active material precursor and graphene oxide mixture are further ground with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent, the carbon source can be filled between the phosphate positive electrode active material particles, and an amorphous carbon coating layer grown in situ is formed on the surface of the phosphate positive electrode active material. The amorphous carbon coating layer can enhance the interface interaction between the graphene coating layer and the phosphate positive electrode active material, and can also form a continuous conductive network with the outer graphene coating layer. The continuous conductive network can interconnect the phosphate positive electrode active material particles in the positive electrode film layer, and can reduce the aggregation of the phosphate positive electrode active material particles, so that the prepared phosphate composite positive electrode active material has high electronic conductivity, which is conducive to the efficient transmission of electrons, and is also conducive to improving the cycle performance and rate performance of the battery.
[0093] The phosphate positive electrode active material precursor obtained by the preparation method provided in the embodiment of the present application has the advantages of regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. When it is used as a raw material to continue to prepare a phosphate composite positive electrode active material, the grinding time (such as high-energy ball milling or sand milling) can be reduced, thereby reducing the energy consumption cost and time cost in production; it is also easy to achieve uniform mixing of multiple elements (such as Mn elements, Fe elements, doping elements, etc.), and the ratio of each metal element in the prepared phosphate composite positive electrode active material is highly consistent with the ratio of each metal element in the raw material, thereby also making the prepared phosphate composite positive electrode active material have high batch consistency and good electrochemical performance.
[0094] Therefore, the preparation method of the phosphate composite positive active material provided in the embodiment of the present application adopts low-cost graphite oxide as a raw material, thereby reducing the raw material cost in production, and also reducing the energy cost and time cost. The preparation method of the phosphate composite positive active material provided in the embodiment of the present application also has the advantages of simple process and high production efficiency, and thus is easy to carry out industrial large-scale production.
[0095] The preparation method of the phosphate composite positive electrode active material provided in the embodiment of the present application can obtain a phosphate composite positive electrode active material with a single crystal phase, high purity, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. In addition, the obtained phosphate composite positive electrode active material can form a continuous conductive network. Therefore, the phosphate composite positive electrode active material obtained by the preparation method provided in the embodiment of the present application has high electronic conductivity and high ionic conductivity, which is conducive to promoting the efficient transmission of electrons, and is also conducive to shortening the transmission path of ions, thereby helping to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0096] The first shearing speed can be 6000r / min, 7000r / min, 8000r / min, 9000r / min, 10000r / min, 11000r / min, 12000r / min, 13000r / min, 14000r / min, 15000r / min, or any range thereof. Optionally, in some embodiments, the first shearing speed is 6000-15000r / min, optionally 6000-10000r / min.
[0097] In some embodiments, the first stripping reaction time may be 30-150 min, and optionally 60-120 min.
[0098] In some embodiments, the number of graphene oxide layers may be 1-6, and may be 3-5.
[0099] The number of graphene oxide layers can be adjusted by adjusting the first shear rate and the time of the first peeling reaction. The greater the first shear rate and the longer the time of the first peeling reaction, the fewer the number of graphene oxide layers obtained by peeling from graphite oxide. Therefore, the preparation method provided in the embodiment of the present application can also achieve the regulation of the number of graphene oxide layers.
[0100] In some embodiments, the mass ratio of graphite oxide to the metal salt used to prepare the phosphate positive active material may be 0.03:1-0.08:1.
[0101] In some embodiments, the concentration of the metal salt used to prepare the phosphate positive electrode active material in the first mixed solution may be 0.5-2 mol / L. The concentration of the metal salt refers to the total concentration of all metal salts used to prepare the phosphate positive electrode active material in the first mixed solution. For example, the metal salt includes ferrous sulfate and manganese sulfate, and the concentration of the metal salt refers to the total concentration of ferrous sulfate and manganese sulfate.
[0102] In some embodiments, the metal salt used to prepare the phosphate positive active material includes a water-soluble divalent metal salt. Alternatively, the water-soluble divalent metal salt may include one or more of a sulfate, a nitrate, a hydrochloride, and an acetate of a divalent metal.
[0103] In some embodiments, the divalent metal element may include Mn element and / or Fe element and optionally M element, where M element represents the doping element of the Mn position and / or Fe position of the phosphate composite positive electrode active material, optionally including one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr.
[0104] The phosphate positive electrode active material precursor refers to the product of the precipitation reaction between the metal salt used to prepare the phosphate positive electrode active material and the precipitant. In some embodiments, the phosphate positive electrode active material precursor may include manganese iron oxalate and the like.
[0105] In some embodiments, the step of providing a first mixed solution containing graphite oxide and a metal salt for preparing a phosphate positive electrode active material comprises the following steps: under a protective gas atmosphere, adding graphite oxide to water, and then adding the metal salt for preparing a phosphate positive electrode active material, and dispersing them evenly to obtain a first mixed solution.
[0106] In some embodiments, the shielding gas may include nitrogen, an inert gas, or a combination thereof.
[0107] In some embodiments, the second precipitation reaction time can be 10-60 min.
[0108] In some embodiments, the molar ratio of the precipitant to the metal salt used to prepare the phosphate positive electrode active material can be 1:1-3:1. By adjusting the amount of precipitant, it is helpful to improve the conversion efficiency of metal ions and reduce the difference in precipitation rates of different metal ions in the reaction system, thereby facilitating the uniform coprecipitation of metal ions, and further facilitating the ratio of each metal element in the prepared phosphate composite positive electrode active material to the ratio of each metal element in the raw material to have a high consistency. By adjusting the amount of precipitant, it is also helpful to make the coprecipitation reaction more complete, thereby reducing the metal ion content in the reaction waste liquid, reducing the difficulty of the waste liquid treatment process and reducing environmental pollution; in addition, it is also helpful to improve the purity of the obtained phosphate positive electrode active material precursor and reduce the impurity content.
[0109] In some embodiments, the precipitating agent may include one or more of oxalic acid, sodium oxalate, potassium oxalate, and ammonium oxalate.
[0110] The precipitant can be added to the second mixed solution in the form of an aqueous solution of the precipitant. In some embodiments, the concentration of the aqueous solution of the precipitant can be 0.5-2 mol / L.
[0111] In some embodiments, when washing the third mixed liquid, the washing liquid may include ethanol, water, or a mixture of the two, and the number of washing times may be one or more, which is not limited in the embodiments of the present application.
[0112] The washed material may be dried using a known drying process. In some embodiments, a vacuum drying process may be used. Optionally, the drying temperature may be below 100°C.
[0113] The grinding process may adopt a suitable grinding method known in the art. In some embodiments, the grinding process may include high-energy ball milling or sand milling, which is not limited in the embodiments of the present application.
[0114] In some embodiments, the grinding process may be performed at a rotation speed of 1000-2500 r / min.
[0115] In some embodiments, the grinding process may last for 1-5 hours.
[0116] In some embodiments, the sintering process may include a pre-sintering process and a high temperature sintering process.
[0117] In some embodiments, the temperature of the pre-sintering process may be 350°C-550°C, optionally 400°C-500°C.
[0118] In some embodiments, the pre-sintering treatment time may be 2-12 hours, and optionally 3-10 hours.
[0119] In some embodiments, the pre-sintering process may be performed under a protective gas atmosphere.
[0120] In some embodiments, the temperature of the high temperature sintering process may be 600°C-800°C, and optionally 650°C-750°C.
[0121] In some embodiments, the high temperature sintering treatment time may be 5-24 hours, and optionally 8-12 hours.
[0122] In some embodiments, the high temperature sintering process may be performed under a protective gas atmosphere.
[0123] In some embodiments, the pre-sintering process and the high temperature sintering process may be performed in a tube furnace.
[0124] In some embodiments, the shielding gas may include nitrogen, an inert gas, or a combination thereof.
[0125] In some embodiments, the phosphate positive electrode active material precursor and the graphene oxide mixture are ground with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source under the condition of a first solvent to obtain a slurry, and then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material. The steps include the following steps: the phosphate positive electrode active material precursor and the graphene oxide mixture are ground with a lithium source, a phosphorus source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source under the condition of a first solvent to obtain a first slurry; the first slurry is spray-dried and granulated to obtain a powder, and then pre-sintered to obtain a pre-sintered powder; the pre-sintered powder and the carbon source are ground for a second time under the condition of a first solvent to obtain a second slurry; the second slurry is spray-dried and granulated to obtain a powder, and then high-temperature sintering and optional crushing are performed to obtain a phosphate composite positive electrode active material. Optionally, the crushing can be air flow crushing.
[0126] Thereby, the obtained phosphate composite positive electrode active material can form a continuous conductive network, which is beneficial to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0127] In some embodiments, the rotation speed of the first grinding process can be 1500-2500 r / min.
[0128] In some embodiments, the first grinding process may last for 1-5 hours.
[0129] In some embodiments, the rotation speed of the second grinding process can be 1000-2500 r / min.
[0130] In some embodiments, the second grinding process may last for 1-3 hours.
[0131] In some embodiments, the first solvent may include one or more of an alcohol solvent and water, and may optionally include one or more of ethanol and water.
[0132] In some embodiments, the lithium source may be a lithium-containing compound known in the art that can be used to prepare phosphate positive electrode active materials. For example, the lithium source may include one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, lithium hydrogen phosphate, lithium nitrate, and lithium acetate.
[0133] In some embodiments, the phosphorus source may be a phosphorus-containing compound known in the art for preparing a phosphate positive active material. For example, the phosphorus source may include one or more of phosphoric acid, ammonium monohydrogen phosphate, and ammonium dihydrogen phosphate.
[0134] In some embodiments, the carbon source may include one or more of an organic carbon source and an inorganic carbon source. For example, the carbon source may include one or more of sucrose, glucose, polyvinyl alcohol, polyethylene glycol, phenolic resin, citric acid, and cyclodextrin.
[0135] In some embodiments, the Li-site doping element may include one or more elements of Zn, Al, Na, K, Mg, Nb, Mo, and W.
[0136] In some embodiments, the Li-site doping element source may include one or more of a sulfate, a nitrate, a hydrochloride, and an acetate of the Li-site doping element.
[0137] In some embodiments, the P-site doping element may include one or more elements of B, S, Si, and N.
[0138] In some embodiments, the P-site doping element source may include one or more of sulfates, borates, nitrates, and silicates of the P-site doping element.
[0139] In some embodiments, the O-site doping element may include one or more elements of S, F, Cl, and Br.
[0140] In some embodiments, the O-site doping element source may include one or more of a simple substance and an ammonium salt of the O-site doping element.
[0141] In the preparation method of the phosphate composite positive electrode active material provided in the present application, the amount of each raw material added can conform to the stoichiometric ratio of the target phosphate composite positive electrode active material. In some embodiments, the amount of lithium source added can be slightly excessive, for example, it can be 100%-110% of the theoretical mass of the lithium source, and the theoretical mass of the lithium source refers to the mass of the lithium source calculated according to the stoichiometric ratio of the phosphate composite positive electrode active material.
[0142] In the preparation method of the phosphate composite positive electrode active material provided in the present application, unless otherwise specified, all raw materials and instruments used can be directly purchased. Each raw material may contain crystalline water or may not contain crystalline water.
[0143] The present application also provides a phosphate composite positive electrode active material obtained by the above preparation method. The phosphate composite positive electrode active material includes a phosphate positive electrode active material, amorphous carbon coated with the phosphate positive electrode active material, and reduced graphene oxide coated with the amorphous carbon.
[0144] The phosphate composite positive electrode active material provided in the embodiments of the present application has the characteristics of single crystal phase, high purity, regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency. In addition, the phosphate composite positive electrode active material also has a continuous conductive network and a shortened ion transmission path, which is beneficial to promote the efficient transmission of electrons and ions, and further helps to improve the capacity and electrochemical performance of the battery, such as cycle performance and rate performance.
[0145] In some embodiments, the volume distribution particle size Dv50 of the phosphate composite positive active material satisfies 0.5 μm≤Dv50≤3 μm.
[0146] In some embodiments, the volume distribution particle sizes Dv90 and Dv50 of the phosphate composite positive active material satisfy 1<Dv90 / Dv50≤1.5.
[0147] In some embodiments, the powder resistivity of the phosphate composite positive electrode active material may be 1-100 Ω·cm.
[0148] In some embodiments, the phosphate positive electrode active material has the formula Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n , M represents a doping element at the Mn position and / or the Fe position, optionally including one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr; N represents a doping element at the Li position, optionally including one or more elements of Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a doping element at the P position, optionally including one or more elements of B, S, Si and N; R represents an O position doping element, optionally including one or more elements of S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1; 0≤x≤1; 0≤y≤1; 0≤1-xy<1; 0≤m≤0.1; 0≤n≤0.1.
[0149] In some embodiments, 0.001≤x≤0.999, 0.001≤y≤0.999, 0≤1-xy≤0.10. Alternatively, 0.199≤x≤0.500, 0.499≤y≤0.800, 0<1-xy≤0.10.
[0150] The embodiment of the present application also provides a positive electrode plate.
[0151] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0152] The positive electrode film layer includes the above-mentioned phosphate composite positive electrode active material or the phosphate composite positive electrode active material obtained by the above-mentioned preparation method. Of course, the positive electrode film layer may also include other positive electrode active materials, for example, it may also include lithium transition metal oxides and the like. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. The modified compound may be a doping modification and / or surface coating modification of the positive electrode active material.
[0153] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0154] In some embodiments, the positive electrode film layer may further include a positive electrode binder. The present application has no particular restrictions on the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin.
[0155] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0156] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, the optional positive electrode conductive agent, the optional positive electrode binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.
[0157] The embodiment of the present application also provides a battery.
[0158] The battery mentioned in the embodiments of the present application may be a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module or a battery pack.
[0159] A battery cell is the smallest unit of a battery, which can independently realize the functions of charging and discharging. The battery cell can be cylindrical, rectangular or in other shapes, etc., which is not limited in the present application. Figure 1 The battery cell 5 is a rectangular parallelepiped structure as an example.
[0160] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed connection through a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a case and battery cells, and the battery cells or battery modules are accommodated in the case. In some embodiments, the case may serve as part of the chassis structure of the vehicle. For example, part of the case may become at least a part of the floor of the vehicle, or part of the case may become at least a part of the crossbeam and longitudinal beam of the vehicle.
[0161] In some embodiments, the battery may be an energy storage device, which includes an energy storage container, an energy storage cabinet, and the like.
[0162] The battery cells mentioned in the embodiments of the present application include lithium-ion primary battery cells, lithium-ion secondary battery cells, lithium metal battery cells, negative electrode-free lithium metal battery cells, etc., which are not limited in the embodiments of the present application.
[0163] The battery cell includes an electrode assembly. The electrode assembly may be a winding structure or a laminated structure, which is not limited in the present application.
[0164] The battery cell also includes an outer package, which can be used to encapsulate the electrode assembly and the electrolyte. The outer package can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS).
[0165] In some embodiments, Figure 2As shown, the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The electrode assembly 52 is encapsulated in the receiving cavity. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, which can be adjusted according to demand.
[0166] In some embodiments, battery cells may be assembled into a battery module. The battery module may contain multiple battery cells, and the specific number may be adjusted according to the application and capacity of the battery module. Figure 3 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 3 As shown, in the battery module 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.
[0167] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.
[0168] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0169] Figure 4 and Figure 5 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 4 and Figure 5 As shown, the battery pack 1 may include a box body and a plurality of battery modules 4 disposed in the box body. The box body includes an upper box body 2 and a lower box body 3, and the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the box body in any manner.
[0170] The battery cell includes the above-mentioned positive electrode sheet and negative electrode sheet. The structure and composition of the negative electrode sheet can be selected according to the type of the battery cell, and the embodiment of the present application is not limited to this.
[0171] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0172] The negative electrode active material may adopt materials known in the art. As an example, the negative electrode active material may include, but is not limited to, one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials may also be used.
[0173] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent. As an example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0174] In some embodiments, the negative electrode film layer may further include a negative electrode binder. The present application has no particular restrictions on the type of negative electrode binder. As an example, the negative electrode binder may include styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS). One or more.
[0175] In some embodiments, the negative electrode film layer may further include other additives. As an example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.
[0176] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0177] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional negative electrode conductive agent, optional negative electrode binder, other optional auxiliary agents, etc. in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.
[0178] The negative electrode plate does not exclude other additional functional layers besides the negative electrode film layer. For example, in some embodiments, the negative electrode plate may also include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode plate may also include a protective layer covering the surface of the negative electrode film layer.
[0179] In some embodiments, the negative electrode plate may include a negative electrode current collector and a metal layer disposed on at least one surface of the negative electrode current collector, and the metal layer may include one or more of lithium single substance and lithium alloy.
[0180] The lithium alloy may be an alloy formed by metallic lithium and other metallic elements or non-metallic elements. As an example, the other metallic elements in the lithium alloy may include one or more of tin, zinc, aluminum, magnesium, silver, gold, gallium, indium, and platinum, and the non-metallic elements in the lithium alloy may include one or more of boron, carbon, and silicon.
[0181] In some embodiments, the negative electrode plate may further include a negative electrode current collector but not a metal layer, thereby forming a negative electrode metal-free battery cell.
[0182] In some embodiments, the negative electrode plate may also be directly made of a sheet (or foil) of lithium or a lithium alloy.
[0183] [Electrolytes]
[0184] The electrolyte plays a role in conducting active ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can include one or more of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte).
[0185] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0186] As an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0187] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the solvent may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE) One or more.
[0188] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature power performance.
[0189] [Isolation film]
[0190] Battery cells using electrolytes and some battery cells using solid electrolytes also include a separator. The separator is arranged between the positive electrode and the negative electrode, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The present application has no particular restrictions on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.
[0191] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different.
[0192] The preparation method of battery cells is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the above-mentioned electrolyte is injected after drying. After vacuum packaging, standing, formation, shaping and other processes, a battery cell is obtained. Multiple battery cells can also be further connected in series, in parallel or in mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.
[0193] Electrical devices
[0194] The embodiment of the present application also provides an electrical device, which includes the battery of the present application. The battery can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.
[0195] The electrical device can select a specific type of battery, such as a battery cell, a battery module or a battery pack, according to its usage requirements.
[0196] Figure 6 Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module can be used as a power source.
[0197] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a battery cell may be used as a power source.
[0198] Example
[0199] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present application will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0200] Example 1
[0201] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by ferrous sulfate and manganese sulfate, with a molar ratio of Mn:Fe of 6:4, to prepare a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0202] The first mixed solution was sheared and exfoliated by a high-speed homogenizer, the rotation speed (shear rate) was 8000r / min, and the exfoliation reaction time was 120min, to prepare a second mixed solution, in which the graphite oxide was exfoliated into graphene oxide. Maintaining the rotation speed of 8000r / min, the precipitant oxalic acid aqueous solution was added to the second mixed solution to form an instantaneous supersaturated suspension, the molar ratio of the precipitant oxalic acid to the metal salt was 1:2, and the precipitation reaction time was 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation, and then the slurry was placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0203] Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1, and then an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C and nitrogen atmosphere for 5h, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and 6wt% sucrose (based on the total weight of the pre-sintered powder) is weighed and placed in a sand mill, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, LiMn coated phosphate positive electrode active material 0.6 Fe 0.4 Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0204] Example 2
[0205] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by ferrous sulfate and manganese sulfate, with a molar ratio of Mn:Fe of 6:4, to prepare a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0206] The first mixed solution was sheared and exfoliated by a high-speed homogenizer, the rotation speed (shear rate) was 10000r / min, and the exfoliation reaction time was 60min, to prepare a second mixed solution, in which the graphite oxide was exfoliated into graphene oxide. Maintaining the rotation speed of 10000r / min, the precipitant oxalic acid aqueous solution was added to the second mixed solution to form an instantaneous supersaturated suspension, the molar ratio of the precipitant oxalic acid to the metal salt was 1:2, and the precipitation reaction time was 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation, and then the slurry was placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0207] Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1, and then an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C and nitrogen atmosphere for 5h, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and 6wt% sucrose (based on the total weight of the pre-sintered powder) is weighed and placed in a sand mill, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, LiMn coated phosphate positive electrode active material 0.6 Fe 0.4Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0208] Example 3
[0209] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by ferrous sulfate and manganese sulfate, with a molar ratio of Mn:Fe of 7:3, to prepare a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0210] The first mixed solution was sheared and exfoliated by a high-speed homogenizer at a rotation speed (shear rate) of 6000 r / min and an exfoliation reaction time of 120 min to prepare a second mixed solution in which graphite oxide was exfoliated into graphene oxide. The precipitant ammonium oxalate aqueous solution was added to the second mixed solution at a rotation speed of 6000 r / min to form an instantaneous supersaturated suspension. The molar ratio of the precipitant ammonium oxalate to the metal salt was 1:2, and the precipitation reaction time was 20 min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80 ° C for drying to obtain Mn 0.7 Fe 0.3 C2O4·2H2O and graphene oxide mixture, in which graphene oxide encapsulates Mn 0.7 Fe 0.3 C2O4·2H2O.
[0211] Mn 0.7 Fe 0.3 C2O4·2H2O and graphene oxide mixture, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.7:0.3:1, and then an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C and nitrogen atmosphere for 5h, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and 6wt% PVA (based on the total weight of the pre-sintered powder) is weighed and placed in a sand mill, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.7 Fe0.3 PO4, LiMn coated phosphate positive electrode active material 0.7 Fe 0.3 Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0212] Example 4
[0213] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by ferrous sulfate and manganese sulfate, with a molar ratio of Mn:Fe of 6:4, to prepare a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0214] The first mixed solution was sheared and exfoliated by a high-speed homogenizer at a rotation speed (shear rate) of 8000 r / min and an exfoliation reaction time of 120 min to prepare a second mixed solution in which graphite oxide was exfoliated into graphene oxide. The precipitant ammonium oxalate aqueous solution was added to the second mixed solution at a rotation speed of 8000 r / min to form an instantaneous supersaturated suspension. The molar ratio of the precipitant ammonium oxalate to the metal salt was 1:2, and the precipitation reaction time was 20 min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation. The slurry was then placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0215] Mn 0.6 Fe 0.4C2O4·2H2O and graphene oxide mixture, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1, and then an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C and nitrogen atmosphere for 5h, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and 3wt% PVA and 3% glucose (based on the total weight of the pre-sintered powder) are weighed and placed in a sand mill, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder was placed in a tube furnace and sintered at 720°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, LiMn coated phosphate positive electrode active material 0.6 Fe 0.4 Amorphous carbon of PO4 and reduced graphene oxide coated with amorphous carbon.
[0216] Comparative Example 1
[0217] Under nitrogen protection, ferrous sulfate and manganese sulfate were added to an appropriate amount of deionized water at a Mn:Fe molar ratio of 6:4 to prepare a 1 mol / L mixed metal salt solution, which was then dispersed and dissolved using an agitator at a rotation speed of 600 r / min to prepare a mixed solution.
[0218] Under the condition of stirring speed of 600r / min, the precipitant oxalic acid aqueous solution was added to the mixed solution to form an instantaneous supersaturated suspension, the molar ratio of the precipitant oxalic acid to the metal salt was 1:2, and the precipitation reaction time was 20min until the reaction was complete. The obtained mixed solution was washed with deionized water and ethanol for multiple times and the slurry was collected by centrifugation, and then the slurry was placed in a vacuum oven at 80℃ for drying to obtain Mn 0.6 Fe 0.4 C2O4·2H2O.
[0219] Mn 0.6 Fe 0.4C2O4·2H2O, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1, and then an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C and nitrogen atmosphere for 5h, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and 11wt% sucrose (based on the total weight of the pre-sintered powder) is weighed and placed in a sand mill, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, LiMn coated phosphate positive electrode active material 0.6 Fe 0.4 Amorphous carbon of PO4.
[0220] Comparative Example 2
[0221] Under nitrogen protection, graphite oxide was added to an appropriate amount of deionized water, followed by ferrous sulfate and manganese sulfate, with a molar ratio of Mn:Fe of 6:4, to prepare a first mixed solution with a metal salt concentration of 1 mol / L. The mass ratio of graphite oxide to metal salt was 0.05:1.
[0222] The first mixed solution was sheared and exfoliated by a high-speed homogenizer, the rotation speed (shear rate) was 8000r / min, and the exfoliation reaction time was 120min, to prepare a second mixed solution, in which the graphite oxide was exfoliated into graphene oxide. Maintaining the rotation speed of 8000r / min, the precipitant oxalic acid aqueous solution was added to the second mixed solution to form an instantaneous supersaturated suspension, the molar ratio of the precipitant oxalic acid to the metal salt was 1:2, and the precipitation reaction time was 20min to obtain a third mixed solution. The obtained third mixed solution was washed with deionized water and ethanol several times and the slurry was collected by centrifugation, and then the slurry was placed in a vacuum oven at 80°C for drying to obtain Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, in which graphene oxide encapsulates Mn 0.6 Fe 0.4 C2O4·2H2O.
[0223] Mn 0.6 Fe 0.4 C2O4·2H2O and graphene oxide mixture, Li2CO3 and NH4H2PO4 are weighed in a molar ratio of Li:Mn:Fe:P=1.02:0.6:0.4:1, and then an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 400°C and nitrogen atmosphere for 5h, and naturally cooled to room temperature to obtain a pre-sintered powder. The obtained pre-sintered powder is placed in a sand mill, an appropriate amount of deionized water is added as a solvent, and sand milled at a speed of 2500r / min for 2h to obtain a slurry. The obtained slurry is transferred to a spray drying device for spray drying and granulation to obtain a powder, and the drying temperature is set to 210°C. The obtained powder is placed in a tube furnace and sintered at 700°C in a nitrogen atmosphere for 10 hours, cooled naturally to room temperature, and pulverized by air flow to obtain a phosphate composite positive electrode active material. The phosphate composite positive electrode active material includes a phosphate positive electrode active material LiMn 0.6 Fe 0.4 PO4, LiMn coated phosphate positive electrode active material 0.6 Fe 0.4 PO4 reduction of graphene oxide.
[0224] Test Section
[0225] (1) Powder resistivity test
[0226] Use a powder resistivity tester, such as Yuanneng Technology's PRCD1100, to test the powder resistivity of phosphate composite cathode active materials. Take a certain amount of phosphate composite cathode active material powder and put it in a special mold, then put the mold on the compaction density instrument, set the pressure to 4MPa, and read the corresponding powder resistivity after applying pressure.
[0227] (2) Volume distribution particle size Dv50 test
[0228] Use a laser particle size analyzer, such as Malvern Master Size 3000, to test the volume distribution particle size of the phosphate composite positive electrode active material. Dv50 refers to the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 50%. The test basis can refer to GB / T 19077-2016.
[0229] (3) Metal element content test
[0230] The contents of manganese and iron in the phosphate composite positive electrode active material are tested by ICP-OES using an inductively coupled plasma optical emission spectrometer, such as Plasma 3000, and their molar ratios are calculated.
[0231] (4) Test of average number of graphene layers
[0232] The number of graphene layers is determined using an atomic force microscope, such as Multimode 8. The thickness of a single layer of graphene is usually between 0.4 nm and 0.7 nm. The morphology of graphene is observed by atomic force microscopy, and the number of graphene layers can be estimated based on the height curve.
[0233] (5) Preparation and testing of button cells
[0234] The phosphate composite positive electrode active material prepared in the above embodiments and comparative examples, polyvinylidene fluoride (PVDF), and conductive carbon were added to a certain amount of N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5, stirred in a drying room to form a slurry, coated on an aluminum foil, dried, and cold pressed to form a positive electrode sheet. A lithium sheet was used as the negative electrode, and assembled into a button battery in a button box with the positive electrode sheet prepared above. The concentration of the electrolyte was 1 mol / L, the lithium salt was LiPF6, and the solvent was a mixed system of ethylene carbonate (EC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) in a volume ratio of 1:1:1.
[0235] At 25°C, the button cell prepared above was charged to 4.3V at a constant current of 0.1C, then charged at a constant voltage at 4.3V to a current ≤ 0.05C, and left to stand for 2 minutes. The charging capacity at this time was recorded as C0; then the button cell was discharged to 2.0V at a constant current of 0.1C. The discharge capacity at this time was the initial discharge capacity, recorded as D0. The discharge specific capacity of the button cell (mAh / g) = D0 / m, where m represents the mass of the phosphate composite positive electrode active material.
[0236] At 25°C, charge each button cell prepared above to 4.3V at 1C constant current, then charge at 4.3V at constant voltage to a current ≤ 0.05C, let stand for 2 minutes, record the charge capacity at this time, which is the charge capacity of the first cycle; then discharge the button cell to 2.0V at 1C constant current, record the discharge capacity at this time, which is the discharge capacity of the first cycle. Perform cyclic charge and discharge tests on the button cell according to the above method, and record the discharge capacity after each cycle. The capacity retention rate of the button cell after 200 cycles = discharge capacity after 200 cycles / discharge capacity of the first cycle.
[0237] At 25°C, the button batteries prepared above were charged to 4.3V at constant currents of 0.1C, 0.5C, 1C, 2C, 5C and 10C, respectively, and then charged at constant voltage at 4.3V to a current ≤0.05C and allowed to stand for 2 min; then the button batteries were discharged to 2.0V at constant currents of 0.1C, 0.5C, 1C, 2C, 5C and 10C, respectively, and the discharge capacities of the button batteries at different charge and discharge rates (0.1C, 0.5C, 1C, 2C, 5C and 10C) were recorded.
[0238] The above test results are shown in Table 1.
[0239] Table 1
[0240]
[0241] Figure 7 (a) shows the Mn prepared in Example 1 0.6 Fe 0.4 Scanning electron microscope (SEM) image of a mixture of C2O4·2H2O and graphene oxide. Figure 7 (b) shows the Mn prepared in Comparative Example 1 0.6 Fe 0.4 Scanning electron microscope (SEM) image of C2O4·2H2O. Figure 7 It can be seen that the phosphate positive electrode active material precursor obtained by the preparation method provided in the embodiment of the present application has the characteristics of regular morphology, small particle size, narrow particle size distribution, and can also be well wrapped by graphene oxide.
[0242] Figure 8 (a) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Example 1, Figure 8 (b) shows a scanning electron microscope (SEM) image of the phosphate composite positive electrode active material prepared in Comparative Example 1. Figure 8 It can be seen that the phosphate composite positive electrode active material obtained by the preparation method provided in the embodiment of the present application can form a continuous conductive network.
[0243] Fig. 9 The capacity-voltage curves of button cells prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1. Fig.10 The rate curves of button cells prepared from the phosphate composite positive electrode active materials of Example 1 and Comparative Example 1 are shown. Fig. 9 , Fig.10As can be seen from the test results in Table 1, the preparation method provided in the embodiments of the present application can not only reduce the cost of raw materials, but also make the obtained phosphate composite positive electrode active material have the characteristics of regular morphology, small particle size, narrow particle size distribution, uniform element distribution and high batch consistency, and can also form a continuous conductive network and shorten the ion transmission path, which is conducive to promoting the efficient transmission of electrons and ions, and thus can make the battery have high discharge specific capacity, good rate performance and good cycle stability.
[0244] In Comparative Example 2, no carbon source was added during the preparation of the phosphate composite positive electrode active material. At this time, a continuous conductive network could not be constructed in the phosphate composite positive electrode active material, resulting in the prepared phosphate composite positive electrode active material having high powder resistivity and poor electron transmission capacity, thereby affecting the rate performance of the battery. In addition, it would also affect the cycle stability of the battery.
[0245] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing a phosphate composite positive electrode active material, comprising the following steps: Providing a first mixed solution comprising graphite oxide and a metal salt for preparing a phosphate positive electrode active material, wherein the solvent in the first mixed solution comprises water; The first mixed solution is subjected to a first exfoliation reaction at a first shear rate of more than 6000 r / min, so that the graphite oxide is exfoliated into graphene oxide, thereby obtaining a second mixed solution; Maintaining the first shear rate, adding a precipitant or an aqueous solution of the precipitant to the second mixed solution to perform a second precipitation reaction to obtain a third mixed solution, wherein the precipitant includes one or more of oxalic acid and a water-soluble oxalate; Washing and drying the third mixed solution to obtain a mixture of a phosphate positive electrode active material precursor and graphene oxide; The phosphate positive electrode active material precursor and graphene oxide mixture are ground with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a slurry, and then spray-dried, granulated, and sintered to obtain a phosphate composite positive electrode active material. in, The phosphate composite positive electrode active material comprises a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
2. The method according to claim 1, wherein: The first stripping reaction is carried out in a high-speed dispersing homogenizer; and / or, The first shearing speed is 6000-15000 r / min, and can be 6000-10000 r / min; and / or, The first stripping reaction time is 30-150 minutes, and can be 60-120 minutes; and / or, The number of layers of the graphene oxide is 1-6, and can be 3-5.
3. The method according to claim 1 or 2, wherein: The mass ratio of the graphite oxide to the metal salt used to prepare the phosphate positive electrode active material is 0.03:1-0.08:1; and / or, The concentration of the metal salt used to prepare the phosphate positive electrode active material in the first mixed solution is 0.5-2 mol / L; and / or, The metal salt used to prepare the phosphate positive electrode active material includes a water-soluble divalent metal salt. Optionally, the water-soluble divalent metal salt includes one or more of sulfate, nitrate, hydrochloride and acetate.
4. The method according to claim 3, wherein: The divalent metal element includes Mn element and / or Fe element and optionally M element, wherein M element represents the doping element of Mn position and / or Fe position of the phosphate composite positive electrode active material, and optionally includes one or more elements of Ni, Co, Mg, Zn, Ca, Ti, V and Cr.
5. The method according to any one of claims 1 to 4, wherein: The second precipitation reaction time is 10-60 min; and / or, The molar ratio of the precipitant to the metal salt used to prepare the phosphate positive electrode active material is 1:1-3:1; and / or, The precipitant comprises one or more of oxalic acid, sodium oxalate, potassium oxalate and ammonium oxalate; and / or, The concentration of the aqueous solution of the precipitant is 0.5-2 mol / L.
6. The method according to any one of claims 1 to 5, wherein: The step of providing a first mixed solution containing graphite oxide and a metal salt for preparing a phosphate positive electrode active material comprises the following steps: Under a protective gas atmosphere, adding graphite oxide to water, then adding a metal salt for preparing a phosphate positive electrode active material, and dispersing the mixture evenly to obtain the first mixed solution; Optionally, the protective gas includes nitrogen, an inert gas or a combination thereof.
7. The method according to any one of claims 1 to 6, wherein: The first solvent includes one or more of an alcohol solvent and water, and may optionally include one or more of ethanol and water; and / or, The grinding process includes high-energy ball milling or sand milling; and / or, The grinding process has a rotation speed of 1000-2500 r / min; and / or, The grinding time is 1-5h.
8. The method according to any one of claims 1 to 7, wherein: The sintering process includes a pre-sintering process and a high-temperature sintering process; Optionally, the pre-sintering temperature is 350-550° C., optionally 400-500° C.; and / or, Optionally, the pre-sintering treatment time is 2-12 hours, optionally 3-10 hours; and / or, Optionally, the temperature of the high temperature sintering treatment is 600-800° C., optionally 650-750° C.; and / or, Optionally, the high temperature sintering treatment time is 5-24 hours, optionally 8-12 hours; and / or, Optionally, the pre-sintering process is performed under a protective gas atmosphere; and / or, Optionally, the high-temperature sintering treatment is performed under a protective gas atmosphere.
9. The method according to claim 8, wherein: The steps of grinding the mixture of the phosphate positive electrode active material precursor and graphene oxide with a lithium source, a phosphorus source, a carbon source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a slurry, and then spray drying, granulating, and sintering to obtain a phosphate composite positive electrode active material include the following steps: The phosphate positive electrode active material precursor and the graphene oxide mixture are subjected to a first grinding treatment with a lithium source, a phosphorus source, an optional Li-position doping element source, an optional P-position doping element source, and an optional O-position doping element source in the presence of a first solvent to obtain a first slurry; The first slurry is spray-dried and granulated to obtain powder, and then pre-sintered to obtain pre-sintered powder; Grinding the pre-sintered powder and the carbon source for a second time in the presence of a first solvent to obtain a second slurry; The second slurry is spray-dried and granulated to obtain powder, which is then subjected to high-temperature sintering treatment and optionally crushing treatment to obtain the phosphate composite positive electrode active material.
10. The method according to claim 9, wherein: The rotation speed of the first grinding process is 1500-2500r / min; and / or, The first grinding treatment lasts for 1-5 hours; and / or, The rotation speed of the second grinding process is 1000-2500r / min; and / or, The second grinding process lasts for 1-3 hours.
11. The method according to any one of claims 1 to 10, wherein: The Li-site doping element includes one or more elements selected from the group consisting of Zn, Al, Na, K, Mg, Nb, Mo and W; and / or, The P-site doping element includes one or more elements selected from B, S, Si and N; and / or, The O-site doping element includes one or more elements selected from the group consisting of S, F, Cl and Br.
12. The method according to any one of claims 1 to 11, wherein: The lithium source includes one or more of lithium hydroxide, lithium carbonate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, lithium nitrate and lithium acetate; and / or, The phosphorus source includes one or more of phosphoric acid, ammonium monohydrogen phosphate and ammonium dihydrogen phosphate; and / or, The carbon source comprises one or more of sucrose, glucose, polyvinyl alcohol, polyethylene glycol, phenolic resin, citric acid and cyclodextrin; and / or, The Li-doping element source includes one or more of sulfate, nitrate, hydrochloride and acetate of the Li-doping element; and / or, The P-site doping element source includes one or more of sulfates, borates, nitrates and silicates of the P-site doping element; and / or, The O-site doping element source includes one or more of a simple substance and an ammonium salt of the O-site doping element.
13. A phosphate composite positive electrode active material prepared by the method according to any one of claims 1 to 12, wherein the phosphate composite positive electrode active material comprises a phosphate positive electrode active material, amorphous carbon coating the phosphate positive electrode active material, and reduced graphene oxide coating the amorphous carbon.
14. The phosphate composite positive electrode active material according to claim 13, wherein: The volume distribution particle size Dv50 of the phosphate composite positive electrode active material satisfies 0.5 μm≤Dv50≤3 μm; and / or, The volume distribution particle sizes Dv90 and Dv50 of the phosphate composite positive electrode active material satisfy 1<Dv90 / Dv50≤1.5; and / or, The powder resistivity of the phosphate composite positive electrode active material is 1-100Ω·cm.
15. The phosphate composite positive electrode active material according to claim 13 or 14, wherein: The molecular formula of the phosphate positive electrode active material is Li a N b Fe x Mn y M 1-x-y P 1-m Q m O 4-n R n , M represents a doping element at the Mn position and / or the Fe position, and may optionally include one or more elements selected from the group consisting of Ni, Co, Mg, Zn, Ca, Ti, V and Cr; N represents a Li-site doping element, optionally including one or more elements selected from Zn, Al, Na, K, Mg, Nb, Mo and W; Q represents a P-site doping element, which may optionally include one or more elements selected from B, S, Si and N; R represents an O-position doping element, which may optionally include one or more elements selected from S, F, Cl and Br; 0.9≤a≤1.1; 0≤b≤0.1; 0≤x≤1; 0≤y≤1; 0≤1-xy<1; 0≤m≤0.1; 0≤n≤0.
1.
16. The phosphate composite positive electrode active material according to claim 15, wherein: 0.001≤x≤0.999, 0.001≤y≤0.999, 0≤1-xy≤0.10; Optionally, 0.199≤x≤0.500, 0.499≤y≤0.800, 0<1-xy≤0.
10.
17. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein: The positive electrode film layer comprises a phosphate composite positive electrode active material prepared by the method according to any one of claims 1 to 12 or a phosphate composite positive electrode active material according to any one of claims 13 to 16.
18. A battery cell comprising the positive electrode sheet according to claim 17.
19. A battery comprising the battery cell according to claim 18.
20. An electrical device comprising the battery according to claim 19.
Citation Information
Patent Citations
Preparation method of graphene modified LiMnxFe1-xPO4 / C composite material
CN104993133A
Phosphate-graphene composite positive electrode material, preparation method thereof and lithium ion battery
CN115692673A
Composite phosphate positive electrode material and preparation method thereof
CN115939335A
Boron-doped reduced graphene oxide coated lithium manganese iron phosphate composite material and preparation method thereof