Composite sodium ferrous sulfate positive electrode material as well as preparation method and application thereof
By synthesizing uniform doped metal phase and sodium composite oxides under high temperature hydrothermal method, and by carbon coating technology, the problem of insufficient performance of sodium ferrous sulfate positive electrode material at low sintering temperature is solved, significantly improving sodium ions The diffusion coefficient and electron conductivity improve electrochemical performance.
Patent Information
- Application Number
- CN202411190978.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
When the sintering temperature of the existing sodium ferrous sulfate positive electrode materials are low, the ion diffusion speed is slow, making it difficult to achieve uniform mixing of doped metals and iron and the formation of eutectics, resulting in insufficient material performance.
Synthesize uniform doped metal phase, iron and sodium composite oxides under high temperature hydrothermal conditions, avoid ferrous ions by adding reducing agents, and improve electron conductivity through carbon coating, controlling dopants and phosphate. The ratio is to improve the diffusion coefficient and conductivity of sodium ions.
The performance improvement of the composite sodium ferrous sulfate positive electrode material is achieved, the sodium ion diffusion coefficient and electronic conductivity are improved, the powder resistivity is reduced, and the electrochemical performance is significantly improved.
Smart Images

Figure CN119069672A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium batteries, and in particular to a composite sodium ferrous sulfate positive electrode material and a preparation method and application thereof. Background Art
[0002] As an element in the same main group as lithium, sodium has very similar electrochemical properties and is abundant in reserves, with an abundance of about 2.64% in the earth's crust, and its cost is also lower. Therefore, using sodium to replace lithium to develop sodium-ion batteries has a very broad application prospect, and finding and developing suitable electrode materials has become one of the main tasks of sodium-ion battery research.
[0003] Polyanion sodium battery materials have the characteristics of low cost and excellent cycle performance. People's research on sodium ion battery positive electrode materials also focuses on polyanion materials. Among the many polyanion compounds, SO 4 2- With higher electronegativity and stronger inductive effect, sulfate materials have higher working voltage and thus receive more extensive attention. Since sodium ferrous sulfate has lower sintering temperature and lower energy consumption, the sulfate series polyanions have lower cost among polyanion materials. When sodium ferrous sulfate is used as the positive electrode material for sodium ion batteries, it is lower than LiFePO 4 Positive electrode materials, the battery's charge and discharge platform is higher. However, the low electronic conductivity and sodium ion diffusion coefficient of sodium ferrous sulfate materials limit its practical application.
[0004] In the prior art, the ionic conductivity of the positive electrode material of the polyanion sodium battery is generally improved by doping metal ions, and the electronic conductivity of the material is improved by carbon coating. In the conventional doping method, the doped metal salt and the iron salt are generally mixed and ground first, and then the mixture is sintered. The positive electrode material obtained by the above scheme has poor electrical properties. The reason is that in order to prevent the decomposition of the necessary raw material sulfate, the sintering temperature of the positive electrode material cannot exceed 350°C. However, at the above temperature, the ion diffusion rate is slow, and it is difficult to achieve the formation of a uniform mixed eutectic of the doped metal and iron. Therefore, it is necessary to provide a solution to reduce the decomposition of sulfate and improve the material performance of the composite sodium ferrous sulfate positive electrode material. Summary of the invention
[0005] In view of the technical problems existing in the background technology, the present application provides a composite sodium ferrous sulfate positive electrode material and its preparation method and application, aiming to solve the technical problem of how to reduce sulfate decomposition and improve the material performance of the composite sodium ferrous sulfate positive electrode material.
[0006] In a first aspect, the present invention provides a composite sodium ferrous sulfate positive electrode material, comprising a core, wherein the chemical formula of the core is Na x M y Fez (PO 4 ) k (SO 4 ) (0.4~0.6)x O t , wherein M includes at least one of manganese, vanadium, and titanium, 16≤x≤17, y=1, 4≤z≤5, 2≤k≤2.6, y+z-0.1x-1.5k≤t≤y+z+0.1x-1.5k.
[0007] In the technical solution of the embodiment of the present application, the composite sodium ferrous sulfate positive electrode material improves the ion conductivity by element doping, ensures the sodium ion diffusion coefficient, and has a high degree of sulfate ion retention, and iron and doped metals form a uniform compound, thereby achieving further improvement in the performance of the composite sodium ferrous sulfate positive electrode material.
[0008] In some embodiments, the composite sodium ferrous sulfate positive electrode material also includes a carbon coating layer, which is coated on the surface of the inner core, and the molar ratio of the carbon element in the carbon coating layer to the sodium element in the inner core is greater than or equal to 0.5 and less than or equal to 1.
[0009] In this embodiment, the electronic conductivity of the material is improved by the carbon-coated core-shell structure.
[0010] In some embodiments, the sodium ion diffusion coefficient of the composite sodium ferrous sulfate positive electrode material is 1*10 -10 cm 2 / s-5*10 -10 cm 2 / s; powder resistivity is 15Ω.cm-25Ω.cm.
[0011] In this embodiment, the sodium ion diffusion coefficient is high, the powder resistivity is low, and the obtained composite sodium ferrous sulfate positive electrode material has good electrochemical performance.
[0012] In a second aspect, the present application provides a method for preparing a composite sodium ferrous sulfate positive electrode material, comprising the following steps:
[0013] S1, mixing a ferrous source, a sodium source, a phosphorus source, a dopant, a reducing agent and a first solvent to obtain a first slurry;
[0014] S2, subjecting the first slurry to a hydrothermal reaction, followed by filtering and washing to obtain a washed material;
[0015] S3, mixing the washing material, the sulfate compound, the carbon source and the second solvent to obtain a second slurry;
[0016] S4. Dry and calcine the second slurry, and then crush and remove impurities to obtain a composite sodium ferrous sulfate positive electrode material.
[0017] In the technical solution of the embodiment of the present application, a uniform doped metal phase, iron, and sodium composite oxide precipitate is first synthesized under hydrothermal conditions, and the oxidation of ferrous ions is avoided by adding a reducing agent; after calcination, the carbon source is coated on the surface of the composite sodium ferrous sulfate, which effectively reduces the powder resistivity of the material and improves the electronic conductivity of the material; the preparation method of the composite sodium ferrous sulfate positive electrode material provided by the present application reduces the decomposition of sulfate ions while performing metal element doping and anion doping, thereby increasing the sodium ion diffusion coefficient and improving the performance of the composite sodium ferrous sulfate positive electrode material.
[0018] In some embodiments, in the first slurry, the dopant includes a doping element, and the molar ratio of the doping element to the iron element, the sodium element, and the phosphorus element is 1:(4-5):(16.0-17.0):(2-2.6); the molar ratio of the iron element in the ferrous source to the reducing agent is 1:(0.1-0.3); the solid content of the first slurry is 25%-35%; the molar ratio of the sodium element in the washing material to the carbon source is 1:(0.5-1); the solid content of the second slurry is 20%-30%.
[0019] In this embodiment, by controlling the molar ratio of the doping element, iron element, sodium element, and phosphorus element in the first slurry within this range, uniform mixing and eutectic of iron, sodium, and doped metal can be achieved through hydrothermal reaction, and at the same time, if the ratio is unbalanced, it will be detrimental to achieving the above purpose; by controlling the molar ratio of iron to reducing agent in the first slurry within this range, it is beneficial to avoid oxidation of ferrous iron.
[0020] In some embodiments, the ferrous source includes at least one of ferrous acetate and ferrous phosphate; the sodium source includes at least one of sodium hydroxide, sodium oxide, sodium carbonate, sodium acetate, and sodium phosphate; the phosphorus source includes sodium phosphate; the reducing agent includes sodium phosphite; the dopant includes at least one of a manganese source, a vanadium source, and a titanium source; the carbon source includes at least one of graphene and carbon nanotubes; the sulfate compound includes at least one of sulfuric acid and ammonium sulfate; in the second slurry, the molar ratio of the sodium element in the washing material to the sulfuric acid is 1:(0.3-0.4); the molar ratio of the sodium element in the washing material to the ammonium sulfate is 1:(0.1-0.2).
[0021] In this embodiment, the introduction of manganese source, vanadium source and titanium source as dopants is beneficial to improving ion conductivity.
[0022] In some embodiments, the temperature of the hydrothermal reaction is 200° C.-300° C., the time of the hydrothermal reaction is 12 h-15 h, the pressure of the hydrothermal reaction is 1.5 MPa-2 MPa; and the hydrothermal reaction is carried out under stirring.
[0023] In this embodiment, by controlling the temperature and time of the hydrothermal reaction within this range, the reaction can be completed and excessive energy consumption can be avoided. If the temperature of the hydrothermal reaction is too high, the energy consumption is high and the requirements for equipment are also high. If the temperature of the hydrothermal reaction is low, the reaction cannot be completed. If the time of the hydrothermal reaction is too long, the energy consumption is high and the production efficiency is low. If the time of the hydrothermal reaction is too short, the reaction cannot be completed.
[0024] In some embodiments, in the second slurry, the molar ratio of the sodium element in the washing material to sulfuric acid is 1:(0.3-0.4); the molar ratio of the sodium in the washing material to ammonium sulfate is 1:(0.1-0.2); the molar ratio of the sodium in the washing material to the carbon source is 1:(0.5-1); and the solid content of the second slurry is 20%-30%.
[0025] In this embodiment, by controlling the ratio of sulfate, part of the sulfate can be replaced by oxygen (from metal oxides formed by high-temperature hydrothermal method) and phosphate in the washing material, and while cation doping is performed, anion doping and recombination are also achieved.
[0026] In some embodiments, in the step of drying and calcining the second slurry, the calcination temperature is 300°C-350°C, the calcination time is 4h-8h, the heating rate is 1°C / min-2°C / min, the cooling rate is 2°C / h-4°C / h, and the calcination is carried out under a protective atmosphere.
[0027] In this embodiment, by drying and calcining the second slurry, the carbon source is advantageously coated on the surface of the composite sodium ferrous sulfate as a coating layer without causing decomposition of sulfate.
[0028] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising the composite sodium ferrous sulfate positive electrode material provided in the present application or a composite sodium ferrous sulfate positive electrode material prepared by the preparation method of the composite sodium ferrous sulfate positive electrode material provided in the present application.
[0029] In the technical solution of the embodiment of the present application, the positive electrode plate includes the above-mentioned composite sodium ferrous sulfate positive electrode material, so when applied to a secondary battery, it has more excellent electrical properties in terms of discharge capacity, cycle performance, etc.
[0030] In a fourth aspect, an embodiment of the present application provides a secondary battery, comprising the positive electrode plate provided in the third aspect of the present application.
[0031] In the technical solution of the embodiment of the present application, the secondary battery includes the above-mentioned positive electrode plate, and thus has more excellent advantages in terms of charging capacity, discharging capacity, cycle performance, etc.
[0032] Compared with the prior art, the beneficial effects of the present application include: the composite sodium ferrous sulfate positive electrode material improves the ion conductivity by element doping, ensures the sodium ion diffusion coefficient, and has a high degree of sulfate ion retention, and iron and doped metals form a uniform compound, thereby achieving further improvement in the performance of the composite sodium ferrous sulfate positive electrode material.
[0033] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0035] Figure 1 A process flow chart of a method for preparing a composite sodium ferrous sulfate positive electrode material provided in an embodiment of the present application;
[0036] Figure 2 This is a scanning electron microscope (SEM) result of the washing material obtained in Example 1 of the present application;
[0037] Figure 3 This is a scanning electron microscope (SEM) result of the composite sodium ferrous sulfate positive electrode material obtained in Example 1 of the present application;
[0038] Figure 4 These are the charging curve and discharging curve of the composite sodium ferrous sulfate positive electrode material obtained in Example 1 of the present application at 0.1C rate and 1C rate. DETAILED DESCRIPTION
[0039] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0041] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0042] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0043] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0044] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0045] In the preparation of existing sodium ferrous sulfate positive electrode materials, since sulfate is easily decomposed, the sintering temperature is relatively low, generally below 350°C. At this temperature, the ion diffusion rate is slow, and it is difficult to achieve uniform mixing of doped metals and iron and the formation of a eutectic, resulting in insufficient performance of the final positive electrode material.
[0046] In order to solve the technical problem that it is difficult to achieve uniform mixing of doped metals and iron and the formation of eutectics by conventional doping methods in the prior art, resulting in insufficient performance of the final positive electrode material, the present application provides a composite sodium ferrous sulfate positive electrode material and a preparation method thereof, a positive electrode plate and a secondary battery, wherein the present application first achieves uniform mixing and eutectic of iron, sodium and doped metals under high-temperature hydrothermal conditions, and simultaneously dopes part of phosphate, and then obtains the composite sodium ferrous sulfate positive electrode material by converting anions at high temperature. The composite sodium ferrous sulfate positive electrode material improves the ion conductivity through element doping, ensures the sodium ion diffusion coefficient, and has a high degree of sulfate ion retention, and iron and the doped metal form a uniform compound, thereby achieving further improvement in the performance of the composite sodium ferrous sulfate positive electrode material.
[0047] In a first aspect, the present invention provides a composite sodium ferrous sulfate positive electrode material, comprising a core, wherein the chemical formula of the core is Na x M y Fe z (PO 4 ) k (SO 4 ) (0.4~0.6)x O t , wherein M includes at least one of manganese, vanadium, and titanium sources, 16≤x≤17, y=1, 4≤z≤5, 2≤k≤2.6, y+z-0.1x-1.5k≤t≤y+z+0.1x-1.5k.
[0048] In the technical solution of the embodiment of the present application, the composite sodium ferrous sulfate positive electrode material is doped with M ions to improve the ionic conductivity and ensure the sodium ion diffusion coefficient. In addition, the sulfate ion retention degree is high, and iron and doped metals form a uniform compound, thereby further improving the performance of the polyanion sodium battery positive electrode material with sulfate ions.
[0049] In some embodiments, the composite sodium ferrous sulfate positive electrode material also includes a carbon coating layer, which is coated on the surface of the inner core, and the molar ratio of the carbon element in the carbon coating layer to the sodium element in the inner core is greater than or equal to 0.5 and less than or equal to 1; for example, the molar ratio of the carbon element in the carbon coating layer to the sodium element in the inner core is 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, or any value between 0.5-1.0.
[0050] In some embodiments, the mass fraction of the carbon coating layer in the composite sodium ferrous sulfate positive electrode material is 5% to 10%, for example, it can be 5.5%, 5.8%, 6%, 7%, 7.5%, 8%, 9%, 9.5%, or any value between 5% and 10%.
[0051] In this embodiment, the electronic conductivity of the material is improved by the carbon-coated core-shell structure.
[0052] In some embodiments, the composite sodium ferrous sulfate positive electrode material includes a core and a C coating layer, and the chemical formula of the composite sodium ferrous sulfate positive electrode material is Na x M y Fe z (PO 4 ) k (SO 4 ) (0.4~0.6)x O t / C, wherein M includes at least one of manganese, vanadium and titanium sources, 16≤x≤17, y=1, 4≤z≤5, 2≤k≤2.6, y+z-0.1x-1.5k≤t≤y+z+0.1x-1.5k.
[0053] In some embodiments, the chemical formula of the composite sodium ferrous sulfate positive electrode material is Na 16.6 Mn e4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C、Na 16 MnFe 4 (PO 4 ) 2 (SO 4 ) 6.4 O 3.6 / C、Na 17 MnFe 5 (PO 4 ) 2.6 (SO 4 ) 9.35 O 0.85 / C、Na 16.6 VF e4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C、Na 16.6 TiF e4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 3.05 / C or Na 16.6 Mn e4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C.
[0054] In some embodiments, the sodium ion diffusion coefficient of the composite sodium ferrous sulfate positive electrode material is 1*10 -10 cm 2 / s-5*10 -10 cm 2 / s, for example, the sodium ion diffusion coefficient of the composite sodium ferrous sulfate positive electrode material is 1*10 -10 cm 2 / s, 2*10 -10 cm 2 / s, 2.5*10 -10 cm 2 / s, 3*10 -10 cm 2 / s, 4*10 -10 cm2 / s, 5*10 -10 cm 2 / s or 1*10 -10 cm 2 / s-5*10 -10 cm 2 The powder resistivity of the composite sodium ferrous sulfate positive electrode material is 15Ω.cm-25Ω.cm, for example, the powder resistivity of the composite sodium ferrous sulfate positive electrode material is 15Ω.cm, 18Ω.cm, 20Ω.cm, 22Ω.cm, 25Ω.cm or any value between 15Ω.cm-25Ω.cm.
[0055] In this embodiment, the composite sodium ferrous sulfate positive electrode material has a high sodium ion diffusion coefficient and a low powder resistivity, which is beneficial to improving the electrochemical performance of the battery when applied to a secondary battery.
[0056] Please refer to Figure 1 The present invention provides a method for preparing a composite sodium ferrous sulfate positive electrode material, comprising the following steps:
[0057] S1, mixing a ferrous source, a sodium source, a phosphorus source, a dopant, a reducing agent and a first solvent, and uniformly mixing them into a slurry state to obtain a first slurry;
[0058] S2, subjecting the first slurry to a hydrothermal reaction, followed by filtering and washing to obtain a washed material;
[0059] In steps S1 and S2, a uniform doped metal phase, iron, and sodium composite oxide precipitate are synthesized by using a ferrous source, a sodium source, a phosphorus source, a doping agent, and a reducing agent under hydrothermal conditions, and a reducing agent is added to prevent the ferrous ions from being oxidized; steps S1 and S2 enable each material to form a uniform compound;
[0060] S3, mixing the washing material, the sulfate compound, the carbon source and the second solvent to obtain a second slurry;
[0061] Step S3 is an anion conversion process, the purpose of which is to introduce sulfate into the composite sodium ferrous sulfate positive electrode material; by adding sulfuric acid and ammonium sulfate, not only sulfate can be introduced, but also pH can be adjusted, and ammonium ions and hydrogen ions are easily volatilized and will not cause residues;
[0062] S4, spray drying and calcining the second slurry, and then crushing and removing impurities to obtain a composite sodium ferrous sulfate positive electrode material;
[0063] In step S4, after spray drying, the carbon source and the iron / sodium / doped metal composite oxide can be uniformly mixed, and then after calcination, the carbon source can be coated on the surface of the composite sodium ferrous sulfate, thereby effectively reducing the powder resistivity of the material and improving the electronic conductivity of the material.
[0064] The present application does not limit the type of carbon source, and those skilled in the art may limit it according to actual conditions. For example, the carbon source may be graphene, carbon nanotubes (CNT), etc.
[0065] Further, in some embodiments, in the first slurry, the molar ratio of the doping element, iron element, sodium element, and phosphorus element in the dopant is 1:(4-5):(16.0-17.0):(2-2.6); suitably but not restrictively, the molar ratio of the doping element, iron element, sodium element, and phosphorus element in the dopant is 1:4:16:2; 1:5:17:2.6; 1:4:17:2.3.
[0066] In the technical solution of the embodiment of the present application, by controlling the molar ratio of the doping element, iron element, sodium element and phosphorus element in the first slurry within this range, uniform mixing and eutectic of iron element, sodium element and doping element can be achieved through hydrothermal reaction, while part of the phosphate is doped. If the ratio is unbalanced, it is difficult to achieve this goal.
[0067] Further, in some embodiments, in the first slurry, the molar ratio of the iron element to the reducing agent is 1:(0.1-0.3); for example, the molar ratio of the iron element to the reducing agent is 1:0.1, 1:0.2, 1:0.3.
[0068] In the technical solution of the embodiment of the present application, by controlling the molar ratio of iron to reducing agent in the first slurry within this range, the oxidation of ferrous iron can be avoided. If too much reducing agent is added, the final product will have an unbalanced ratio and a high phosphate content, which will ultimately affect the cycle performance and capacity of the material.
[0069] Further, in some embodiments, the ferrous source includes at least one of ferrous acetate and ferrous phosphate; the sodium source includes at least one of sodium hydroxide, sodium oxide, sodium carbonate, sodium acetate, and sodium phosphate; the phosphorus source includes sodium phosphate; the reducing agent includes sodium phosphite; the doping agent includes at least one of a manganese source, a vanadium source, and a titanium source; the manganese source includes at least one of manganese sulfate, manganese nitrate, and manganese acetate, the vanadium source includes at least one of ammonium metavanadate and sodium metavanadate, and the titanium source includes titanium tetrachloride; the carbon source includes at least one of graphene and carbon nanotubes; the sulfate compound includes at least one of sulfuric acid and ammonium sulfate; it is understandable that a compound having both phosphorus and sodium elements can be used as a phosphorus source and a sodium source at the same time, such as sodium phosphite, and phosphorous acid is also used as a reducing agent. In some embodiments, the sodium source is sodium hydroxide, sodium oxide, and sodium carbonate, which provides an alkaline environment for the reaction while providing a sodium source.
[0070] The present application does not limit the type of dopant, and those skilled in the art can select it according to the actual situation, as long as the ionic conductivity of the positive electrode material can be improved by doping. For example, the dopant can be one or more of a manganese source, a titanium source, and a vanadium source.
[0071] In the technical solution of the embodiment of the present application, by introducing a manganese source as a dopant, the improvement of ionic conductivity can be achieved.
[0072] The present application does not limit the type of manganese source, and those skilled in the art can select it according to actual conditions. For example, the manganese source is manganese acetate.
[0073] Furthermore, in some embodiments, in the first slurry, the dopant is manganese acetate, the ferrous source is ferrous acetate, the sodium source is sodium hydroxide and sodium phosphate, the phosphorus source is sodium phosphate, and the reducing agent is sodium phosphite; the molar ratio of manganese acetate to ferrous acetate is 1:(4-5), the molar ratio of manganese acetate to sodium hydroxide is 1:(8-12), the molar ratio of manganese acetate to sodium phosphite is 1:(0.5-1), and the molar ratio of manganese acetate to sodium phosphate is 1:(1-2).
[0074] Further, in some embodiments, in the first slurry, the dopant is ammonium metavanadate, the ferrous source is ferrous phosphate, the sodium source is sodium carbonate, the phosphorus source is sodium phosphate, and the reducing agent is sodium phosphite; the molar ratio of ammonium metavanadate to ferrous phosphate is 1:(4-5), the molar ratio of ammonium metavanadate to sodium carbonate is 1:(8-12), the molar ratio of ammonium metavanadate to sodium phosphite is 1:(0.5-1), and the molar ratio of ammonium metavanadate to sodium phosphate is 1:(1-2).
[0075] Furthermore, in some embodiments, in the first slurry, the dopant is titanium tetrachloride, the ferrous source is ferrous acetate, the sodium source is sodium carbonate, the phosphorus source is sodium phosphate, and the reducing agent is sodium phosphite; the molar ratio of titanium tetrachloride to ferrous acetate is 1:(4-5), the molar ratio of titanium tetrachloride to sodium carbonate is 1:(8-12), the molar ratio of titanium tetrachloride to sodium phosphite is 1:(0.5-1), and the molar ratio of titanium tetrachloride to sodium phosphate is 1:(1-2).
[0076] Further, in some embodiments, in the first slurry, the solid content (the solid content in the first slurry is the mass fraction of the solid in the first slurry) is 25%-35%, including but not limited to 25%, 27%, 29%, 31%, 33%, 35%, etc., which is not limited in the present application.
[0077] In the technical solution of the embodiment of the present application, if the dosage of the first solvent is too low, it is easy to cause some raw materials to fail to completely dissolve in water and crystallize out. If the dosage of the first solvent is too high, the production efficiency is low. Suitable but non-restrictive, the first solvent is selected from pure water, deionized water, distilled water, etc.
[0078] Further, in some embodiments, the temperature of the hydrothermal reaction is 200°C-300°C, including but not limited to 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, etc., which is not limited in the present application; the time of the hydrothermal reaction is 12h-15h, including but not limited to 12h, 13h, 14h, 15h, etc., which is not limited in the present application; the pressure is 1.5MPa-2MPa, including but not limited to 1.5MPa, 1.6MPa, 1.7MPa, 1.8MPa, 1.9MPa, 2MPa, etc., which is not limited in the present application.
[0079] In the technical solution of the embodiment of the present application, by controlling the temperature and time of the hydrothermal reaction within this range, the reaction can be complete and excessive energy consumption can be avoided. If the temperature of the hydrothermal reaction is too high, the energy consumption is high and the requirements for equipment are also high. If the temperature of the hydrothermal reaction is low, the reaction cannot be complete. If the time of the hydrothermal reaction is too long, the energy consumption is high and the production efficiency is low. If the time of the hydrothermal reaction is too short, the reaction cannot be complete.
[0080] Further, in some embodiments, the hydrothermal reaction is carried out under stirring conditions.
[0081] Furthermore, in some embodiments, during the hydrothermal reaction, the stirring speed is 200r / min-300r / min, including but not limited to 200r / min, 220r / min, 240r / min, 260r / min, 280r / min, 300r / min, etc., which is not limited in the present application.
[0082] Furthermore, in some embodiments, washing is stopped when the conductivity of the washing water becomes ≤500 μS / cm.
[0083] Further, in some embodiments, in the second slurry, the molar ratio of sodium to sulfuric acid in the washing material is 1:(0.3-0.4), including but not limited to 1:0.3, 1:0.32, 1:0.34, 1:0.36, 1:0.38, 1:0.4, etc., which is not limited in the present application; the molar ratio of sodium to ammonium sulfate in the washing material is 1:(0.1-0.2), including but not limited to 1:0.1, 1:0.12, 1:0.14, 1:0.16, 1:0.18, 1:0.2, etc., which is not limited in the present application.
[0084] In the technical solution of the embodiment of the present application, when introducing sulfate, the proportion of sulfate is controlled so that part of the sulfate is replaced by oxygen (from metal oxides formed by high-temperature hydrothermal method) and phosphate, thereby achieving anion doping and recombination while performing cation doping.
[0085] Furthermore, in some embodiments, the molar ratio of sodium to carbon source in the washing material is 1:(0.5-1), including but not limited to 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, etc., which is not limited in the present application.
[0086] Further, in some embodiments, in the second slurry, the solid content (the solid content in the second slurry is the mass fraction of the solid in the second slurry) is 20-30%, including but not limited to 20%, 22%, 24%, 26%, 28%, 30%, etc., which is not limited in the present application.
[0087] In the technical solution of the embodiment of the present application, if the solid content of the second slurry is too high, it is easy to block the material during drying (for example, spray drying); if the solid content of the second slurry is too low, the energy consumption required for drying is too high. In some embodiments, the second solvent used in the second slurry is selected from one of pure water, deionized water or distilled water, and the carbon source is CNT (carbon nanotube).
[0088] In step S4, the second slurry is first dried and calcined; then crushed and impurities are removed to obtain a composite sodium ferrous sulfate positive electrode material.
[0089] In some embodiments, drying is performed by spray drying, and the parameters of spray drying are as follows: the air inlet temperature is 150°C-350°C, including but not limited to 150°C, 200°C, 250°C, 300°C, 350°C, etc., and the present application does not limit this; the air outlet temperature is 70°C-95°C, including but not limited to 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, etc., and the present application does not limit this. During the spray drying process, protective gas is used as the gas source. The particle size of the spray dried material is 3μm-10μm, including but not limited to 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, etc., and the present application does not limit this.
[0090] In some embodiments, the parameters of the calcination process are as follows: the calcination temperature is 300°C-350°C, including but not limited to 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, etc., which is not limited in the present application; the calcination time is 4h-8h, including but not limited to 4h, 5h, 6h, 7h, 8h, etc., which is not limited in the present application; the calcination is carried out under protective gas.
[0091] The present application does not limit the type of protective gas, and those skilled in the art can select it according to actual conditions, for example, it can be nitrogen, argon, etc. During the calcination process, the heating rate is 1°C / min-2°C / min, and the cooling rate is 2°C / h-4°C / h. The material is discharged after cooling to a material temperature of ≤70°C after calcination.
[0092] Crushing and impurity removal include airflow crushing, screening, iron removal, and packaging processes; in some embodiments, during the airflow crushing process, protective gas is used as the gas source for crushing, and the air pressure is 0.5MPa-0.8MPa; the material is crushed to a particle size of 1μm-3μm. Under this condition, the degree of crushing is more sufficient, which is convenient for subsequent screening. In some embodiments, the screening process uses a 100-200 mesh ultrasonic vibrating screen, which is conducive to the uniformity of the particle size obtained. In some embodiments, an electromagnetic iron remover is used for iron removal. In some embodiments, packaging is carried out in a constant temperature and humidity room with a humidity of ≤10% and a temperature of 25±5°C.
[0093] The embodiment of the application provides a positive electrode plate, including the composite sodium ferrous sulfate positive electrode material provided in the present application or the composite sodium ferrous sulfate positive electrode material prepared by the preparation method of the composite sodium ferrous sulfate positive electrode material provided in the present application.
[0094] In the technical solution of the embodiment of the present application, the positive electrode plate includes the above-mentioned composite sodium ferrous sulfate positive electrode material, so when applied to a secondary battery, it has more excellent electrical properties in terms of discharge capacity, cycle performance, etc.
[0095] An embodiment of the present application provides a secondary battery, comprising the positive electrode plate provided in the third aspect of the present application.
[0096] In the technical solution of the embodiment of the present application, the secondary battery includes the above-mentioned positive electrode plate, and thus has more excellent advantages in terms of charging capacity, discharging capacity, cycle performance, etc.
[0097] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0098] 1. Preparation method
[0099] Example 1
[0100] The preparation of the composite sodium ferrous sulfate positive electrode material in this embodiment is as follows:
[0101] (1) manganese acetate, ferrous acetate, sodium hydroxide, sodium phosphite and sodium phosphate are mixed in a molar ratio of 1:4.5:10.5:0.8:1.5, pure water is added to make the solid content 29%, and the mixture is mixed and slurried to obtain a first slurry. In the first slurry, the molar ratio of manganese to iron, sodium and phosphorus is 1:4.5:16.6:2.3, and the molar ratio of iron in ferrous acetate to reducing agent sodium phosphite is 1:0.178.
[0102] (2) The first slurry is added into a high-pressure hydrothermal autoclave, reacted at a temperature of 260° C. for 13 h, a pressure of 1.8 MPa, and a stirring speed of 250 r / min, and then filtered and washed with pure water until the conductivity of the washing water of the first slurry is ≤500 μS / cm, thereby obtaining a washed material.
[0103] (3) sulfuric acid, ammonium sulfate and CNT are added to the washed material, and the molar ratio of sodium in the washed material to the added sulfuric acid, ammonium sulfate and CNT is 1:0.35:0.15:0.7, and then pure water is added and stirred to slurry so that the solid content is 25%, thereby obtaining a second slurry.
[0104] (4) The second slurry is spray-dried with an air inlet temperature of 150°C and an air outlet temperature of 70°C. Protective gas is used as the gas source to obtain a spray-dried material with a particle size of 7 μm. The material is then calcined. During the calcination process, the temperature is increased at a rate of 1.5°C / min to a temperature of 330°C. The calcination time is 7h and the temperature is decreased at a rate of 3°C / h. The material is discharged after the temperature is decreased to a temperature of ≤70°C to obtain a calcined material. The calcined material is subjected to air flow pulverization using 0.7MPa nitrogen as the gas source to pulverize the material until the particle size is 1.7μm. The material is then sieved using a 100-mesh ultrasonic vibrating screen. The material under the sieve is de-ironed using an electromagnetic de-ironing device and then packaged. The packaging is carried out in a constant temperature and humidity room with a humidity of ≤10% and a temperature of 25±5°C to obtain a composite sodium ferrous sulfate positive electrode material.
[0105] The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 16.6 MnFe 4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C, the final carbon content is 7.26%.
[0106] Example 2
[0107] The preparation of the composite sodium ferrous sulfate positive electrode material in this embodiment is as follows:
[0108] (1) Manganese acetate, ferrous acetate, sodium hydroxide, sodium phosphite, and sodium phosphate are mixed in a molar ratio of 1:4:10.4:0.4:1.6, and pure water is added to make the solid content 29%, and the mixture is mixed and slurried to obtain a first slurry. In the first slurry, the molar ratio of the doped metal to iron, sodium, and phosphorus is 1:4:16:2; and the molar ratio of iron to the reducing agent is 1:0.1.
[0109] (2) The first slurry is added into a high-pressure hydrothermal autoclave, reacted at a temperature of 200° C. for 15 h, a pressure of 1.5 MPa, and a stirring speed of 250 r / min, and then filtered and washed with pure water. The washing is stopped when the conductivity of the washing water of the first slurry is ≤500 μS / cm to obtain a washed material.
[0110] (3) adding sulfuric acid, ammonium sulfate and CNT to the washed material, wherein the molar ratio of sodium in the washed material to the added sulfuric acid, ammonium sulfate and CNT is 1:0.3:0.1:0.5, and then adding pure water for stirring and slurrying to make a solid content of 25%, thereby obtaining a second slurry.
[0111] (4) The second slurry is spray-dried, and nitrogen gas with a temperature of 230° C. is used as the gas source for spray drying. The obtained spray-dried material has a particle size of 3 μm, and then calcined. During the calcination process, the calcination temperature is 300° C., the calcination time is 8 hours, the heating rate is 1° C. / min, the cooling rate is 2° C. / h, and the material temperature is cooled to ≤70° C. before discharging. The calcination is carried out under protective gas; during the air flow pulverization process, protective gas is used as the gas source for pulverization, and the gas pressure is 0.5 MPa, and the material is pulverized to a particle size of 1 μm; during the screening process, a 200-mesh ultrasonic vibrating screen is used; during the iron removal process, an electromagnetic iron remover is used for iron removal; the packaging process is carried out in a constant temperature and humidity room, the humidity is ≤10%, and the temperature is 25±5° C., to obtain a composite sodium ferrous sulfate positive electrode material.
[0112] The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 16 MnFe 4 (PO 4 ) 2 (SO 4 ) 6.4 O 3.6 / C, the final carbon content is 5.86%.
[0113] Example 3
[0114] The preparation method of the composite sodium ferrous sulfate positive electrode material in this embodiment is the same as that in Example 1, except that: in the obtained first slurry, the molar ratio of the doped metal to iron, sodium, and phosphorus is 1:5:17:2.6; the molar ratio of iron to the reducing agent is 1:0.3; and the solid content of the first slurry is 35%.
[0115] The temperature of the hydrothermal reaction is 300° C., the time of the hydrothermal reaction is 12 h, and the pressure of the hydrothermal reaction is 2 MPa; the hydrothermal reaction is carried out under stirring conditions.
[0116] In the second slurry, the molar ratio of sodium in the washing material to sulfuric acid is 1:0.35; the molar ratio of sodium in the washing material to ammonium sulfate is 1:0.2; the solid content of the second slurry is 30%; the molar ratio of sodium in the washing material to carbon source CNT is 1:1.
[0117] During the spray drying process, the air inlet temperature is 350°C, the air outlet temperature is 95°C, protective gas is used as the gas source, and the particle size of the spray dried material is 10μm; during the calcination process, the calcination temperature is 350°C, the calcination time is 4h, the heating rate is 2°C / min, the cooling rate is 4°C / h, and the material is discharged after the material temperature is cooled to ≤70°C, and the calcination is carried out under protective gas; during the air flow pulverization process, protective gas is used as the gas source for pulverization, the gas pressure is 0.8MPa, and the material is pulverized to a particle size of 3μm; during the screening process, a 100-mesh ultrasonic vibrating screen is used; during the iron removal process, an electromagnetic iron remover is used for iron removal; the packaging process is carried out in a constant temperature and humidity room, the humidity is ≤10%, and the temperature is 25±5°C.
[0118] The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 17 MnFe 5 (PO 4 ) 2.6 (SO 4 ) 9.35 O 0.85 / C, the final carbon content is 9.78%.
[0119] Example 4
[0120] The preparation method of the composite sodium ferrous sulfate positive electrode material in this embodiment is the same as that in Embodiment 1, except that manganese acetate is replaced by sodium metavanadate.
[0121] The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 16.6 VFe 4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C, the final carbon content is 7.75%.
[0122] Example 5
[0123] The preparation method of the composite sodium ferrous sulfate positive electrode material in this embodiment is the same as that in Embodiment 1, except that manganese acetate is replaced by titanium tetrachloride.
[0124] The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 16.6 TiFe 4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 3.05 / C, the final carbon content is 7.78%.
[0125] Example 6
[0126] The preparation method of the composite sodium ferrous sulfate positive electrode material in this embodiment is the same as that in Example 1, except that the solid content of the first slurry is 25%, the solid content of the second slurry is 20%, and the carbon source is graphene. The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 16.6 MnFe 4.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C, the final carbon content is 7.21%.
[0127] Comparative Example 1
[0128] The preparation of the composite sodium ferrous sulfate positive electrode material is as follows:
[0129] (1) After mixing ferrous acetate, sodium hydroxide, sodium phosphite and sodium phosphate in a molar ratio of 5.5:10.5:0.98:1.32, pure water is added to make the solid content 29%, and the mixture is mixed and slurried to obtain a first slurry. In the first slurry, the molar ratio of iron, sodium and phosphorus is 5.5:16.6:2.3, and the molar ratio of iron in ferrous acetate to the reducing agent sodium phosphite is 1:0.178.
[0130] (2) The first slurry is added into a high-pressure hydrothermal autoclave, reacted at a temperature of 260° C. for 13 h, a pressure of 1.8 MPa, and a stirring speed of 250 r / min, and then filtered and washed with pure water until the conductivity of the washing water of the first slurry is ≤500 μS / cm, thereby obtaining a washed material.
[0131] (3) sulfuric acid, ammonium sulfate and CNT are added to the washed material, and the molar ratio of sodium in the washed material to the added sulfuric acid, ammonium sulfate and CNT is 1:0.35:0.15:0.7, and then pure water is added and stirred to slurry so that the solid content is 25%, thereby obtaining a second slurry.
[0132] (4) The second slurry is spray-dried with an air inlet temperature of 150°C and an air outlet temperature of 70°C. Protective gas is used as the gas source to obtain a spray-dried material with a particle size of 7 μm. The material is then calcined. During the calcination process, the temperature is increased at a rate of 1.5°C / min to a temperature of 330°C. The calcination time is 7h and the temperature is decreased at a rate of 3°C / h. The material is discharged after the temperature is decreased to a temperature of ≤70°C to obtain a calcined material. The calcined material is subjected to air flow pulverization using 0.7MPa nitrogen as the gas source to pulverize the material until the particle size is 1.7μm. The material is then sieved using a 100-mesh ultrasonic vibrating screen. The material under the sieve is de-ironed using an electromagnetic de-ironing device and then packaged. The packaging is carried out in a constant temperature and humidity room with a humidity of ≤10% and a temperature of 25±5°C to obtain a composite sodium ferrous sulfate positive electrode material.
[0133] The chemical formula of the composite sodium ferrous sulfate positive electrode material finally obtained in this embodiment is: Na 16.6 Fe 5.5 (PO 4 ) 2.3 (SO 4 ) 8.3 O 2.05 / C.
[0134] Comparative Example 2
[0135] The preparation method of the composite sodium ferrous sulfate positive electrode material in this embodiment is:
[0136] Manganese acetate, ferrous acetate, sodium hydroxide, sodium phosphite and sodium phosphate are mixed in a molar ratio of 1:4.5:10.5:0.8:1.5 to obtain a mixture, sulfuric acid, ammonium sulfate and CNT are added to the mixture, and the molar ratio of sodium in the mixture to sulfuric acid, ammonium sulfate and CNT is 1:0.35:0.15:0.7, and the mixture is stirred and slurried to make the solid content 25%, and then spray-dried, with an inlet air temperature of 150°C and an outlet air temperature of 70°C, and protective gas is used as a gas source to obtain a spray-dried material with a particle size of 7μm, and then calcined. During the calcination process, the heating rate is 1.5°C / min, the temperature is raised to 330°C, the calcination time is 7h, the cooling rate is 3°C / h, and the material temperature is lowered to ≤70°C before discharging to obtain a calcined material; the calcined material is subjected to air flow pulverization, 0.7MPa nitrogen is used as a gas source for pulverization, and the material is pulverized to a particle size of 1.7μm, and then sieved with a 100-mesh ultrasonic vibration screen, and the screened material is deironed with an electromagnetic deironing device, and then packaged. The packaging is carried out in a constant temperature and humidity room with a humidity of ≤10% and a temperature of 25±5°C to obtain a composite sodium ferrous sulfate positive electrode material.
[0137] 2. Test Method
[0138] 1. Property test of composite sodium ferrous sulfate positive electrode material:
[0139] 1. Perform SEM test on the above reaction materials and composite sodium ferrous sulfate positive electrode material;
[0140] 2. The contents of Na, Fe and S were detected by inductively coupled plasma atomic emission spectrometry;
[0141] 3. The C content is tested by carbon sulfur instrument;
[0142] 4.D10, D50 and D90 are tested by laser particle size analyzer;
[0143] 5. The specific surface area was determined by gas adsorption BET method;
[0144] 6. The powder resistivity is tested by four-probe method with a test pressure of 10MPa;
[0145] 7.PD (compacted density): tested by compacted density meter, test pressure is 3T, pressing time is 30S;
[0146] 8. pH and free sodium element test: The pH value determination method refers to GB / T 9724, General Rules for pH Determination of Chemical Reagents; the free sodium element content is determined by potentiometric titration;
[0147] 9. The moisture content is tested by KF moisture test method;
[0148] 10. The trivalent iron is measured by colorimetry;
[0149] 11. The sodium ion diffusion coefficient is obtained by electrochemical impedance spectroscopy (EIS) test.
[0150] 2. Properties test of secondary batteries
[0151] The composite sodium ferrous sulfate positive electrode materials obtained in the embodiment and the comparative example were respectively prepared into positive electrode sheets and applied to batteries. The battery assembly and testing process was as follows:
[0152] 1. Preparation of positive electrode sheet: In the positive electrode slurry, the mass ratio of composite sodium ferrous sulfate positive electrode material, acetylene black (as a conductive agent), and polyvinylidene fluoride (PVDF, as a binder) is 88:6:6, and the mass is accurate to 0.001g. Aluminum foil is used as the current collector for the positive electrode sheet. The composite sodium ferrous sulfate positive electrode material, acetylene black, PVDF and N-methylpyrrolidone are stirred and slurried to obtain the positive electrode slurry, and the positive electrode slurry is evenly coated on the aluminum foil. After drying in an oven at 100°C, it is cut into electrode sheets with a diameter of 18mm and a thickness of 0.10mm. The electrode sheets are weighed, and the mass is accurate to 0.0001g. The mixing and coating process of the positive electrode slurry is strictly controlled, and the area and thickness of the electrode sheet to be measured remain consistent.
[0153] 2. Battery assembly: In an inert gas glove box with water and oxygen content ≤ 0.0005%, a metal sodium sheet was used as the negative electrode material, a polypropylene microporous film was used as the separator, and 1 mol / L sodium perchlorate (NaClO 4 ) and a sodium ion battery electrolyte composed of a mixed carbonate-based organic solvent [ethylene carbonate (EC) / diethyl carbonate (DEC) / fluoroethylene carbonate (FEC) (the volume ratio of EC, DEC, and FEC is 1:1:0.05)] were assembled and sealed to form a test cell.
[0154] 3. Battery test: The test battery was charged and discharged on a sodium ion battery electrochemical performance tester (Wuhan Blue Electric CT2001A battery test system) at 25°C:
[0155] (a) 0.1C and 1C current charging, charging limit voltage 4.5V;
[0156] (b) 0.1C and 1C rate current discharge, discharge termination voltage 2.0V.
[0157] III. Analysis of test results of various embodiments and comparative examples
[0158] Table 1 Physical and chemical indicators of positive electrode materials obtained in Examples and Comparative Examples
[0159]
[0160]
[0161] Please refer to Figure 2 , the washing material of Example 1 is flaky particles, indicating that the reaction material forms a uniform and stable eutectic material; please refer to Figure 3 ,pass Figure 3 It can be seen that the composite sodium ferrous sulfate positive electrode material prepared in Example 1 is in granular form, indicating that carbon coating has been achieved.
[0162] Please refer to Table 1. It can be seen from the data in Table 1 that the composite sodium ferrous sulfate positive electrode material prepared in Example 1 has a high compaction density, low powder internal resistance, and relatively low pH and free sodium. Compared with Comparative Example 1 in which the Mn element is not introduced, the material obtained in Example 1 of the present application has a high sodium ion diffusion coefficient and a low powder resistivity, indicating that the doping of the Mn element is conducive to the improvement of electrochemical performance; Comparative Example 2 directly obtains the composite sodium ferrous sulfate positive electrode material by mixed calcination. The raw materials do not form a uniform and stable eutectic, but are directly spray-dried and calcined. Compared with Comparative Example 2, the material obtained in Example 1 of the present application has a high sodium ion diffusion coefficient and a significantly low powder resistivity, which is conducive to the improvement of electrochemical performance.
[0163] Table 2 Material performance test results of the embodiments and comparative examples
[0164]
[0165]
[0166] Figure 4 The 0.1C and 1C charge-discharge curves of the composite sodium ferrous sulfate positive electrode material obtained in Example 1 of the present application are shown in Table 2 and Figure 4 It can be seen that compared with Comparative Examples 1 and 2, the composite sodium ferrous sulfate positive electrode material prepared in Examples 1-6 has a high capacity and excellent electrical properties such as rate performance and cycle performance. Compared with the composite sodium ferrous sulfate positive electrode material prepared in the comparative example, the composite sodium ferrous sulfate positive electrode material prepared in the present application has better electrical properties, and the cycle performance is better than that of pure sodium ferrous sulfate and sodium ferrous sulfate prepared by conventional processes.
[0167] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A composite sodium ferrous sulfate positive electrode material, It is characterized in that The composite sodium ferrous sulfate positive electrode material comprises a core, the chemical formula of which is Na x M y Fe z (PO 4 ) k (SO 4 ) (0.4~0.6)x O t , wherein M includes at least one of manganese, vanadium, and titanium, 16≤x≤17, y=1, 4≤z≤5, 2≤k≤2.6, y+z-0.1x-1.5k≤t≤y+z+0.1x-1.5k.
2. The composite sodium ferrous sulfate positive electrode material according to claim 1, It is characterized in that The composite sodium ferrous sulfate positive electrode material also includes a carbon coating layer, which is coated on the surface of the inner core, and the molar ratio of the carbon element in the carbon coating layer to the sodium element in the inner core is greater than or equal to 0.5 and less than or equal to 1.
3. The composite sodium ferrous sulfate positive electrode material according to claim 1, It is characterized in that The sodium ion diffusion coefficient of the composite sodium ferrous sulfate positive electrode material is 1*10 -10 cm 2 / s-5*10 -10 cm 2 / s; the powder resistivity of the composite sodium ferrous sulfate positive electrode material is 15Ω.cm-25Ω.cm.
4. A method for preparing a composite sodium ferrous sulfate positive electrode material, It is characterized in that The following steps are involved: Mixing a ferrous source, a sodium source, a phosphorus source, a dopant, a reducing agent and a first solvent to obtain a first slurry; Performing a hydrothermal reaction on the first slurry, followed by filtering and washing to obtain a washed material; mixing the washing material, the sulfate compound, the carbon source and the second solvent to obtain a second slurry; The second slurry is dried and calcined, and then crushed and impurities are removed to obtain a composite sodium ferrous sulfate positive electrode material.
5. The method for preparing the composite sodium ferrous sulfate positive electrode material according to claim 4, It is characterized in that In the first slurry, the dopant includes a doping element, and the molar ratio of the doping element to the iron element, the sodium element, and the phosphorus element is 1: (4-5): (16.0-17.0): (2-2.6); and / or The molar ratio of the iron element in the ferrous source to the reducing agent is 1:(0.1-0.3); and / or The solid content of the first slurry is 25%-35%; and / or The molar ratio of the sodium element to the carbon source in the washing material is 1:(0.5-1); and / or The solid content of the second slurry is 20%-30%.
6. The method for preparing the composite sodium ferrous sulfate positive electrode material according to claim 4, It is characterized in that The ferrous source comprises at least one of ferrous acetate and ferrous phosphate; and / or The sodium source includes at least one of sodium hydroxide, sodium oxide, sodium carbonate, sodium acetate, and sodium phosphate; and / or The phosphorus source comprises sodium phosphate; and / or The reducing agent comprises sodium phosphite; and / or The dopant comprises at least one of a manganese source, a vanadium source and a titanium source; and / or The carbon source includes at least one of graphene and carbon nanotubes; and / or The sulfate compound comprises at least one of sulfuric acid and ammonium sulfate; and / or In the second slurry, the molar ratio of the sodium element in the washing material to the sulfuric acid is 1:(0.3-0.4); and / or The molar ratio of the sodium element to ammonium sulfate in the washing material is 1:(0.1-0.2).
7. The method for preparing the composite sodium ferrous sulfate positive electrode material according to claim 4, It is characterized in that The temperature of the hydrothermal reaction is 200° C.-300° C., the time of the hydrothermal reaction is 12 h-15 h, and the pressure of the hydrothermal reaction is 1.5 MPa-2 MPa.
8. The method for preparing the composite sodium ferrous sulfate positive electrode material according to claim 4, It is characterized in that In the step of drying and calcining the second slurry, the calcination temperature is 300° C.-350° C., the calcination time is 4 h-8 h, and the calcination is carried out under a protective atmosphere.
9. A positive electrode sheet, It is characterized in that The positive electrode plate comprises the composite sodium ferrous sulfate positive electrode material according to any one of claims 1 to 3 or the composite sodium ferrous sulfate positive electrode material obtained by the preparation method according to any one of claims 4 to 8.
10. A secondary battery, It is characterized in that The secondary battery comprises the positive electrode sheet according to claim 9.
Citation Information
Patent Citations
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery
CN115050957A
Preparation method of sodium ferric sulfate positive electrode material
CN115863570A
Composite sodium ferrous sulfate positive electrode material as well as preparation method and application thereof
CN116995227A
Sulfate sodium ion battery positive electrode material and preparation method thereof
CN117174846A
Positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery
CN117996015A
Cited By
Lithium precipitation mother liquor recovery method, composite sodium ferrous sulfate material, positive pole piece and secondary battery
CN121020660A
Composite sodium iron sulfate positive electrode material, and preparation method therefor and use thereof
EP4836054A1