Current collector and preparation method thereof, and negative-electrode-free lithium metal battery

By designing the current collector of the porous sponge-like structure in lithium metal batteries, the lithium-philicity and pore size change in the thickness direction, the dead lithium and dendrites caused by uneven lithium deposition are solved, and the cycle life and safety of the battery are improved performance.

CN119069712AActive Publication Date: 2024-12-03BYD CO LTD

Patent Information

Application Number
CN202310638327.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

In existing lithium metal batteries, lithium is prone to uneven deposition in the current collector, resulting in the generation of dead lithium and lithium dendrites, resulting in low cycle life, safety hazards and short circuits.

Method used

Design a current collector with a porous sponge-like structure, whose lithium-philicity and pore size vary in the thickness direction, and is formed by corrosion solution along the thickness direction of the alloy foil, ensuring preferential deposition of lithium ions at the bottom and avoiding dendrites growth .

Benefits of technology

It improves the cycle life and safety performance of lithium metal batteries, reduces the growth of lithium dendrites, significantly improves electrochemical activity and conductivity, and promotes the commercial application of negative electrode-free lithium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069712A_ABST
    Figure CN119069712A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrochemistry, and discloses a current collector, a preparation method thereof and a negative-electrode-free lithium metal battery. The current collector has a porous spongy body structure; in the thickness direction of the current collector, the lithium affinity of the current collector is gradually increased from one surface of the current collector to the other opposite surface of the current collector, and the hole diameters of holes of the current collector are gradually reduced. The free moving alkali metal ions can be preferentially deposited at the bottom due to the affinity gradient, so that a bottom-to-top growth mode is ensured; the gradient of the aperture can realize the change of actual deposition kinetics from slow to fast in the vertical direction, so that internal small holes guide compact deposition of lithium ions, and large holes in the surface still keep relatively fast ion transmission. When the current collector is used as a negative-electrode-free battery, a deposition space can be provided for lithium ions in the cycle process, dendritic crystal growth is limited, the cycle life is prolonged, and the safety performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrochemical technology, and in particular to a gradient current collector and a preparation method thereof, and a negative electrode-free lithium metal battery. Background Art

[0002] Lithium metal batteries have ultra-high energy density and are expected to be used in many fields such as consumer electronics and power batteries in the future. However, using lithium foil directly as the negative electrode during its use will bring high costs and certain safety hazards during the manufacturing process. Therefore, if only the current collector is used as the negative electrode material to make a negative electrode-free lithium metal battery, not only can a higher energy density be obtained in theory, but the cost can also be significantly reduced.

[0003] CN107293754A discloses a method for preparing a porous copper current collector for a negative electrode of a lithium metal battery. A Cu-X alloy sheet is used as a substrate, and acids of different concentrations are used as a medium to etch porous copper current collectors of different pore sizes by electrochemical methods. When the current collector is used as a lithium battery current collector, since the upper layer has the best lithium ion concentration and electronic conductivity, metallic lithium will be preferentially deposited in the porous area of ​​the surface, which is easy to block the pores and form lithium dendrites, resulting in "dead lithium" and safety hazards.

[0004] CN110112367A discloses a three-dimensional composite metal lithium negative electrode and a preparation method, wherein the three-dimensional composite metal lithium negative electrode comprises a conductor with a three-dimensional porous structure and metal lithium, and the metal lithium is embedded and filled in the three-dimensional porous structure of the conductor. However, the reserved lithium-philic zinc element is evenly distributed in the entire porous framework. Due to the good electronic ion conductivity, the metal lithium will still be preferentially deposited in the surface porous area, which will not only fail to alleviate the violent volume expansion during lithium deposition, but also easily cause the generation of lithium dendrites.

[0005] CN110993954A discloses a negative electrode current collector for a lithium metal secondary battery and a preparation method thereof, wherein the current collector is composed of three layers of ZnO / graphene / carbon nanotubes, and the ZnO content gradually decreases from the bottom layer to the top layer, and accordingly, the lithium affinity gradually weakens from the bottom layer to the top layer; the skeleton of the current collector is a highly conductive porous sheet structure. Designing a gradient structure of lithium affinity can induce lithium metal to preferentially deposit at the bottom of the porous current collector, thereby effectively alleviating the problem of volume expansion and uneven deposition of metallic lithium. However, during long-term circulation, the lithium metal at the bottom is prone to disordered growth, resulting in dendrites, resulting in lower pore utilization.

[0006] Therefore, it is necessary to study a gradient current collector to solve the problem in the prior art that lithium is easily unevenly deposited in the current collector to produce dead lithium and even lithium dendrites, which leads to low cycle life, short circuit and thermal runaway, and even safety hazards. Summary of the invention

[0007] The purpose of the present invention is to overcome the problem in the prior art that lithium is easily unevenly deposited in the current collector to produce dead lithium and even lithium dendrites, and to provide a current collector having a porous sponge-like structure, and the lithium affinity and pore size change in a dual gradient along the thickness direction of the current collector.

[0008] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a current collector, which contains a lithium-philic metal element and an inert metal element; wherein the current collector has a porous sponge-like structure; and in the thickness direction of the current collector, from one side of the current collector to the other opposite side, the lithium-philicity of the current collector gradually increases, and the pore size of the pores of the current collector gradually decreases.

[0009] A second aspect of the present invention provides a method for preparing a current collector, comprising the following steps:

[0010] (1) using a corrosive solution to corrode and penetrate from one side of the alloy foil to the other side along the thickness direction of the alloy foil to obtain a corroded alloy foil;

[0011] (2) washing and drying the corroded alloy foil in water to obtain the current collector;

[0012] The alloy foil contains a lithium-philic metal element and an inert metal element.

[0013] The third aspect of the present invention provides a negative electrode-free lithium metal battery, characterized in that the negative electrode-free lithium metal battery comprises a lithium-embedded positive electrode material, a positive electrode current collector, a separator, an electrolyte and the current collector described in the first aspect or the current collector prepared by the method described in the second aspect.

[0014] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects:

[0015] (1) The current collector proposed in the present invention has a dual gradient change in lithium affinity and pore size from one side of the current collector to the other side in the thickness direction of the current collector, wherein the lithium affinity gradient of the current collector increases and the pore size gradient of the pores of the current collector decreases. The gradient of lithium affinity can make the freely moving lithium ions deposit preferentially at the bottom, ensuring a bottom-up growth mode; the gradient of pore size can realize the change of actual deposition dynamics from slow to fast in the vertical direction, so that the small pores inside guide the dense deposition of lithium ions while the large pores on the surface still maintain faster ion transport.

[0016] (2) The current collector proposed in the present invention has a porous sponge-like structure, which, on the one hand, is conducive to the effective infiltration of the electrolyte in the entire battery, improves the ion / electron conductivity and ensures the electrochemical consistency inside the battery; on the other hand, it can significantly increase the electrochemically active specific surface area, reduce the actual current density of lithium during the deposition process, and alleviate the growth of lithium dendrites.

[0017] (3) The current collector proposed in the present invention is applied to a negative electrode-free lithium metal battery. The chemical energy released by alloying between lithium metal and lithium-philic metal and the strong capillary action of nanopores promote the effective deposition of lithium ions.

[0018] (4) The current collector proposed in the present invention is applied to a negative electrode-free lithium metal battery, which can provide deposition space for lithium ions and limit dendrite growth during the cycle process, thereby improving the cycle life and safety performance and promoting the commercial application of negative electrode-free batteries.

[0019] (5) The preparation method of the current collector proposed in the present invention has excellent self-supporting performance and can meet the needs of large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the current collector structure with a, b, and c surfaces selected at equal intervals;

[0021] Figure 2 is a SEM image of a nanoporous structure of a current collector in a specific embodiment of the present invention;

[0022] Figure 3 is a schematic diagram of the current collector structure;

[0023] Figure 4 It is a schematic diagram of a negative electrode-free lithium metal battery;

[0024] Figure 5 is a SEM image of the current collector prepared in Example 1. DETAILED DESCRIPTION

[0025] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0026] A first aspect of the present invention provides a current collector, which comprises a lithium-philic metal element and an inert metal element; wherein the current collector has a porous sponge-like structure; and in the thickness direction of the current collector, from one side of the current collector to the other opposite side, the lithium-philicity of the current collector gradually increases, and the pore size of the pores of the current collector gradually decreases.

[0027] In the present invention, in order to illustrate the structure of the current collector, with respect to "in the thickness direction of the current collector, from one side of the current collector to the other opposite side", "one side of the current collector" is defined as side A, and "the other opposite side" that is opposite to side A is defined as side B.

[0028] The inventors found in their research that the lithium affinity of the current collector gradually increases from the A side to the B side of the current collector, and the pore size of the pores of the current collector gradually decreases.

[0029] like Figure 1 As shown. Define the content of lithium-philic elements on the A surface as x A , the aperture size is y A , the content of lithium-philic elements on the B surface is x B , the aperture size is y B From surface A to surface B, take surfaces a, b, and c at equal distances along the thickness direction of the current collector, where the content of the lithium-philic element on surface a is x a , the aperture size is y a ; The content of lithium-philic elements on the b surface is x b , the aperture size is y b ; The content of the lithiophilic element on the c-plane is x c , the aperture size is y c Then x A 、x a 、x b 、x c and x B Satisfy x A <x a <x b <x c <x B ;y A ,y a ,y b ,y c and B Satisfy A >y a >y b >y c >y B .

[0030] Furthermore, the size of the A-surface ligament is defined as z A , the size of the B-side ligament is z B, from surface A to surface B, take surfaces a, b, and c at equal distances along the thickness direction of the current collector, where the ligament size of surface a is z a ; b face ligament size is z b ; The size of the c-face ligament is z c .z A 、z a 、z b 、z c and z B Satisfy z A >z a >z b >z c >z B .

[0031] In the present invention, the affinity gradient can make the freely moving lithium ions deposit preferentially at the bottom, ensuring a bottom-up growth mode; the pore size gradient can realize the change of the actual deposition dynamics from slow to fast in the vertical direction, so that the small pores inside guide the dense deposition of lithium ions while the large pores on the surface still maintain faster ion transport.

[0032] According to the present invention, the porosity of the current collector is 30%-80%, preferably 40-60wt%. When the porosity of the current collector is less than 30%, the internal space of the current collector will be small, and the pores cannot completely accommodate the lithium released from the positive electrode during charging, which is likely to cause the generation of dendrites and reduce the cycle life. When the porosity of the current collector is greater than 80%, the internal space of the current collector will be too large, the strength of the current collector will be reduced, and the battery cycle life will be affected.

[0033] In the present invention, the porosity test method is the mercury intrusion method. Take a current collector with a mass of 1g, ensure that the sample (current collector) is dry, put it into a mercury intrusion instrument for testing, the pressure used is 200MPa, and each sample (current collector) is tested 3 times, and the average value is taken. Among them, mercury does not wet general solids. In order to make mercury enter the pore, external pressure needs to be applied. The greater the external pressure, the smaller the radius of the pore that mercury can enter. The corresponding pore size and pore volume can be known by measuring the amount of mercury entering the pore under different external pressures.

[0034] In the present invention, under preferred conditions, the porosity of the current collector can reach 40-60wt%. Compared with the porosity of 5%-95% of the current collector disclosed in the prior art, the current collector of the present invention has a porosity greater than 40%, which can not only ensure that the lithium released from the positive electrode is fully accommodated during the charging process, but also promote the rapid diffusion of the electrolyte, reduce polarization, and improve the rate performance; increase the specific surface area, reduce the actual current density, slow down the growth of lithium dendrites, and improve the cycle life. On the other hand, the porosity of the current collector of the present invention is less than 60%, which can ensure that it has better self-support after corrosion, so that the battery has good stability during production and use.

[0035] According to the present invention, the thickness of the current collector is 10-100 μm, preferably 20-50 μm. When the thickness is greater than 100 μm, the battery size will be further increased, thereby reducing the energy density of the battery; when the thickness is less than 10 μm, the internal pores of the current collector cannot completely accommodate the lithium released from the positive electrode during charging, resulting in a reduced cycle life. In addition, if the negative electrode current collector is too thin, it will affect the mechanical strength and stability of the material, and may cause the battery to deform or be damaged during operation. And if the negative electrode current collector is too thin, the internal resistance of the battery will increase, causing the battery to be damaged with a short service life.

[0036] In the present invention, in order to ensure that the negative electrode can fully accommodate the lithium deposited by the positive electrode during the charging process, the porosity β and thickness d of the current collector and the surface capacity C and capacity-thickness constant k of the positive electrode need to satisfy the following formula:

[0037]

[0038] k = 4.84 × 10 -4 cm 3 / mAh.

[0039] The physical meaning of k is the volume occupied by dense lithium deposition per unit capacity. The calculation process is as follows: The theoretical gram capacity of lithium is 3860 mAh / g, and the theoretical density of lithium is 0.534 g / cm 3 , the k value is 1 / (m*p).

[0040] In the present invention, the positive electrode surface capacity C ranges from 1 to 5 mAh / cm 2 , preferably 2-4 mAh / cm 2 .

[0041] In the present invention, if this formula is not satisfied, the lithium deposited from the positive electrode during the charging process will exceed the maximum lithium content that the pores of the negative electrode current collector itself can accommodate, causing lithium to be deposited on the surface of the current collector, which is likely to cause the growth of lithium dendrites and cause severe volume expansion during long-term cycling, thereby reducing the cycle life of the battery.

[0042] According to the present invention, the porous sponge-like structure comprises ligaments and pores.

[0043] In the present invention, the ligament is a skeleton formed by the enrichment of inert metal elements; the pore is a hole formed by the dissolution or precipitation of lithium-philic metal elements in the corroded solution.

[0044] According to the present invention, preferably, the ligaments are interconnected and the holes are interconnected to form a unique double-continuous distribution structure, which is beneficial to the effective infiltration of the electrolyte in the entire battery, improves the ion / electronic conductivity and ensures the electrochemical consistency inside the battery.

[0045] In the present invention, the ligament has tortuosity, and the rich tortuosity of the ligament can significantly increase the electrochemical active specific surface area, reduce the actual current density of lithium during the deposition process, and alleviate the growth of lithium dendrites.

[0046] In the present invention, the holes have tortuosity, which can effectively increase the storage of electrolyte, facilitate the infiltration of electrolyte in the entire battery, improve ion and electron conductivity and ensure the electrochemical consistency inside the battery. At the same time, a large amount of internal space can accommodate lithium precipitated during charging.

[0047] According to the present invention, preferably, the average size of the ligaments gradually decreases from one side of the current collector to the other opposite side;

[0048] According to the present invention, the average size of the ligaments gradually decreases from 0.1-10 μm to 10-200 nm from one side of the current collector to the other side opposite thereto.

[0049] In the present invention, the average size of the ligament decreases gradually from one side of the current collector to the other side, so that the bottom specific surface area is larger, the actual exchange current density during the charging process is reduced, and it is conducive to denser deposition of lithium at the bottom, thereby improving the internal space utilization.

[0050] In the present invention, the average size of the ligament can be obtained by combining SEM with statistics using the graphic processing software Image J.

[0051] According to the present invention, the lithiophilic metal element includes one or more of lithium, sodium, magnesium, aluminum, manganese, iron, zinc, tin, antimony, and bismuth;

[0052] And / or, the inert metal element includes one or more of gold, silver, platinum, titanium, chromium, copper, nickel, and cobalt.

[0053] According to the present invention, the content of the lithium-philic metal element gradually increases from 0.2-10wt% to 20-70wt% from one side of the current collector to the other side opposite to the current collector;

[0054] Preferably, the content of the lithiophilic metal element gradually increases from 1-8 wt % to 30-40 wt %.

[0055] In the present invention, the gradient of lithium affinity from one side of the current collector to the other side can significantly reduce the kinetic barrier for the electrochemical reaction of the bottom lithium ions, so that the freely moving lithium ions are preferentially deposited at the bottom, ensuring a bottom-up growth mode, thereby avoiding the generation of dendrites and improving the safety performance of the battery. At the same time, in the long-term deposition / stripping process, it can also disperse lithium nucleation and induce uniform and dense lithium deposition, slow down dead lithium, and improve the battery cycle life. In addition, the gradient content change brought about by single-sided corrosion allows the bottom to maintain the higher mechanical properties of the original alloy foil, improving the processability of the current collector during film making and assembly and the stability during long-term circulation.

[0056] In the present invention, the surface element testing method is to take a square sample with a side length of 5mm×5mm after corrosion, ensure that the sample is flat and dry, and use X-ray photoelectron spectroscopy (XPS) to quantitatively analyze the elements on the surface. Each sample is tested three times and the average value is taken. XPS irradiates the sample surface with X-rays to measure the energy distribution of the excited photoelectrons to obtain the required information. It has a high recognition ability for the chemical characteristics of the sample surface and has good sensitivity to the chemical state of the elements. It can detect all elements on the periodic table except hydrogen and helium.

[0057] According to the present invention, the pore size gradually decreases from 0.1-100 μm to 1-500 nm from one side of the current collector to the other side opposite thereto;

[0058] Preferably, the pore size gradually decreases from 0.1-10 μm to 10-200 nm.

[0059] In the present invention, the pore size gradient can achieve a change in the actual deposition kinetics from slow to fast in the vertical direction, so that the small pores inside guide the dense deposition of alkali metals while the large pores on the surface still maintain faster ion transport.

[0060] The pore size distribution of the current collector in one embodiment of the present invention is as follows: Figure 2 shown.

[0061] A second aspect of the present invention provides a method for preparing a current collector, comprising the following steps:

[0062] (1) using a corrosive solution to corrode and penetrate from one side of the alloy foil to the other side along the thickness direction of the alloy foil to obtain a corroded alloy foil;

[0063] (2) washing and drying the corroded alloy foil in water to obtain the current collector;

[0064] The alloy foil contains a lithium-philic metal element and an inert metal element.

[0065] In the present invention, the alloy foil is fixedly suspended above the surface of the corrosive solution, and the corrosive solution gradually corrodes and penetrates the alloy foil under the action of capillaries. In the process of the corrosive solution gradually penetrating the alloy foil, the lithium-philic metal elements are partially etched to form holes, and the inert metal elements form ligaments. The holes and the ligaments are a dynamic evolution process, gradually forming a stable and uniform porous sponge-like structure with good mechanical properties. Among them, the side of the alloy foil that is in direct contact with the corrosive solution is the A side, and the other side opposite to the A side along the thickness direction of the current collector is the B side. The holes formed by the A side that is in direct contact with the corrosive solution are larger; the holes formed by the B side that is not in direct contact with the corrosive solution are smaller. Therefore, from the A side to the B side along the thickness direction, the pore size gradient decreases. At the same time, the A side that is in direct contact with the corrosive solution is etched more completely, so that the content of lithium-philic metal elements is lower; the B side that is not in direct contact with the corrosive solution is etched less, so that the content of lithium-philic metal elements is higher. Therefore, from the A side to the B side along the thickness direction, the lithium-philic gradient increases. The structural schematic diagram of the current collector is shown as follows Figure 3 shown.

[0066] In the present invention, preferably, the alloy foil is brass foil.

[0067] In the present invention, the step of cleaning the alloy foil is included before step (1), and the cleaning method is selected from any one of solvent ultrasonic cleaning, airflow cleaning, laser cleaning, ultra-high pressure water cleaning, sandblasting cleaning, and nano-aerosol cleaning, preferably solvent ultrasonic cleaning.

[0068] Among them, air flow cleaning uses air flow to flush the surface to remove surface dust and impurities; laser cleaning uses laser beams to remove surface dirt and impurities; ultra-high pressure water cleaning uses ultra-high pressure water to clean the surface to remove dirt and impurities attached to the surface; sandblasting cleaning uses high-pressure gas to spray sand particles onto the surface for flushing to remove surface dirt and oxide layers; nano aerosol cleaning uses nano aerosol spray to clean and disinfect the surface, which can remove tiny dust, bacteria and other pollutants.

[0069] In the present invention, the solvent of the solvent ultrasonic cleaning is selected from at least one of ethanol, methanol, acetone and deionized water, preferably ethanol; the solvent ultrasonic cleaning conditions include: temperature of 10-60°C and time of 5-30 minutes. After the solvent ultrasonic cleaning, the sample is dried for use. The purpose of the solvent ultrasonic cleaning is to remove oxides and impurities on the surface of the alloy foil.

[0070] According to the present invention, the alloy foil contains a lithiophilic metal element and an inert metal element, and the electrode potential difference between the lithiophilic metal element and the inert metal element is greater than 0.5V.

[0071] In the present invention, when the electrode potential difference between the lithium-philic metal element and the inert metal element is greater than 0.5 V, the metal elements with relatively active electrochemical properties in the alloy foil can be selectively dissolved into the corrosive solution under the action of the corrosive solution, leaving the inert metal elements, and the remaining components form a porous sponge-like structure.

[0072] In the present invention, the lithiophilic metal element is selected from at least one of lithium, sodium, magnesium, aluminum, manganese, iron, zinc, tin, antimony, and bismuth; the inert metal element is selected from at least one of gold, silver, platinum, titanium, chromium, copper, nickel, and cobalt.

[0073] According to the present invention, the content of the lithium-philic metal element in the alloy foil is 20-80wt%, preferably 40-60wt%.

[0074] In the present invention, the lithium-philic metal element is partially corroded to form holes, and the hole formed on the A surface in direct contact with the corrosive solution is larger; the hole formed on the B surface not in direct contact with the corrosive solution is smaller. Therefore, the pore size gradient decreases from the A surface to the B surface along the thickness direction. At the same time, the A surface in direct contact with the corrosive solution is etched more completely, so that the content of the lithium-philic metal element is lower; the B surface not in direct contact with the corrosive solution is etched less, so that the content of the lithium-philic metal element is higher. Therefore, the lithium-philic gradient increases from the A surface to the B surface along the thickness direction. On the other hand, the inert metal element is not etched by the corrosive solution, and is mainly used to form a three-dimensional skeleton that is interconnected, playing the role of electronic conduction and supporting carrier.

[0075] According to the present invention, the infiltration method in step (1) is selected from at least one of chemical dealloying, electrochemical dealloying, liquid metal dealloying, vapor phase evaporation dealloying, and radio frequency plasma assisted dealloying.

[0076] According to the present invention, preferably, the infiltration method is selected as a chemical dealloying method.

[0077] According to the present invention, preferably, the chemical dealloying method is selected as a single-side etching method.

[0078] In the present invention, a single-sided etching method is adopted, and only one side of the alloy foil is contacted with the liquid surface of the etching solution, and the alloy foil should be avoided from being moved to prevent the alloy foil from sinking into the etching solution. During the etching process, due to the difference in electrochemical behavior between different components in the alloy foil, the lithium-philic metal elements in the alloy foil can be selectively dissolved by the etching solution to form holes, and the undissolved alloy elements will be reorganized into a bicontinuous structure different from the initial alloy composition to form ligaments.

[0079] According to the present invention, the reaction conditions of the single-side etching method include: etching temperature of 50-200° C., etching time of 8-120 h;

[0080] Preferably, the etching temperature is 80-120° C. and the etching time is 24-48 h.

[0081] In the present invention, if the etching reaction temperature is too low, the corrosion time is long, which affects the production efficiency; if the etching reaction temperature is high, the energy consumption is increased, and the etching reaction speed is also faster, causing the A-hole structure to collapse easily, resulting in poor mechanical strength of the current collector.

[0082] In the present invention, if the etching reaction time is too short, it will result in fewer and smaller holes on the A surface, a thicker dense layer on the B surface that has not been etched, and a lower overall porosity, which is not conducive to accommodating lithium deposition and alleviating severe volume expansion during the cycle; if the etching reaction time is too long, it will increase energy consumption, the A surface will be larger and the B surface will be easily corroded, resulting in poor overall mechanical strength of the current collector and easy breakage.

[0083] According to the present invention, it is characterized in that the etching solution comprises ammonium chloride and an acid solution, and the acid solution is selected from one or more of perchloric acid, sulfuric acid, nitric acid, hydrochloric acid, hydrofluoric acid, phosphoric acid, formic acid, and acetic acid;

[0084] Preferably, the corrosive solution is a mixture of hydrochloric acid and ammonium chloride;

[0085] Preferably, the molar ratio of hydrochloric acid to ammonium chloride is 1:(3-6).

[0086] The third aspect of the present invention provides a negative electrode-free lithium metal battery, wherein the negative electrode-free lithium metal battery comprises a lithium-intercalated positive electrode material, a positive electrode current collector, a separator, an electrolyte, and the current collector described in the first aspect or the current collector prepared by the method described in the second aspect. A schematic diagram of a negative electrode-free lithium metal battery is shown in FIG. Figure 4 As shown, the A side of the current collector is arranged close to the diaphragm, and the B side is arranged away from the diaphragm.

[0087] The current collector provided by the present invention is used as a negative electrode-free battery, which can provide deposition space for lithium ions and limit dendrite growth during the cycle process, thereby improving the cycle life and safety performance and promoting the commercial application of negative electrode-free batteries.

[0088] In the present invention, the lithium-intercalated positive electrode material is selected from LiAl 0.05 Co 0.15 Ni 0.80 O2、LiNi 0.80 Co 0.10 Mn 0.10 O2、LiNi 0.90 Co 0.05 Mn 0.05 O2、LiNi 0.60 Co 0.20 Mn 0.20O2, LiCoO2, LiMn2O4, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, LiNi 0.5 Mn 1.5 At least one of O4, Li3V3(PO4)3, lithium sulfide, lithium-intercalated V2O5, lithium-intercalated MnO2, lithium-intercalated TiS2 and lithium-intercalated FeS2.

[0089] In the present invention, the electrolyte includes a lithium salt and a solvent, the lithium salt is selected from one or more of LiPF6, LiFB4, LiTFSI, LiDFOB, LiBOB, LiFSI, LiClO4, and LiAsF6, and the solvent is at least one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), ethylene glycol dimethyl ether (DME), 1,3-dioxolane (DOL), and triacetaldehyde (TTE).

[0090] In the present invention, the material of the positive electrode current collector is not particularly limited.

[0091] In the present invention, the material of the separator is not particularly limited.

[0092] The present invention will be described in detail below by way of examples. In the following examples,

[0093] (1) Average size of pores and ligaments: measured by SEM combined with image processing software Image J.

[0094] (2) Content of lithiophilic metal elements and inert metal elements: measured by quantitative analysis using X-ray photoelectron spectroscopy (XPS). The specific method is: take a square sample with a side length of 5 mm × 5 mm, use X-ray photoelectron spectroscopy (XPS) to quantitatively analyze the elements on the surface, repeat the test 3 times for each sample, and take the average value.

[0095] (3) Porosity: measured by mercury intrusion method. The specific method is: take a sample with a mass of 1g and put it into a mercury intrusion instrument for testing. The test pressure is 200MPa. Each sample is tested three times and the average value is taken.

[0096] Example 1

[0097] (1) selecting a brass foil having a Zn content of 38 wt % and a thickness of 30 μm, and continuously ultrasonically cleaning the brass foil with ethanol and deionized water to remove impurities on the surface of the brass foil, and then vacuum drying the brass foil for later use;

[0098] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 24 hours;

[0099] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-1 with a lithium affinity / pore dual gradient, and its porosity is 50%.

[0100] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. Figure 5 As shown, the surface is the aforementioned A surface, the bottom is the aforementioned B surface, (a) is the SEM image of the A surface; (b) is the partial enlarged image of (a); (c) is the SEM image of the B surface; (d) is the partial enlarged image of (c). The Zn content of the A surface is 6.8wt% as tested by XPS. By SEM combined with ImageJ software, the pore size is 2.0μm, the average size of the ligament is 1.5μm, and the optical photo shows a more obvious pure copper color. In contrast, the Zn content of the B surface is 34wt%, the pore size is 50nm, the average size of the ligament is 50nm, and the optical photo shows a more obvious brass color.

[0101] Example 2

[0102] (1) Select a brass foil with a Zn content of 38 wt % and a thickness of 20 μm, clean the brass foil with ethanol and deionized water by continuous ultrasonic cleaning to remove impurities on the surface, and then vacuum dry the brass foil for later use;

[0103] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 16 hours;

[0104] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-2 with a double gradient of lithium affinity and pores, and its porosity is 45%.

[0105] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 8.1wt% as tested by XPS, and the pore size is 1.1μm and the average size of the ligament is 1.2μm through SEM combined with ImageJ software. In contrast, the Zn content of surface B is 36wt%, the pore size is 10nm, and the average size of the ligament is 10nm.

[0106] Example 3

[0107] (1) Select a brass foil with a Zn content of 38 wt % and a thickness of 50 μm, clean the brass foil with ethanol and deionized water by continuous ultrasonic cleaning to remove impurities on the surface, and then vacuum dry the brass foil for later use;

[0108] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 48 hours;

[0109] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-3 with a double gradient of lithium affinity and pores, and the porosity is 60%.

[0110] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 1.2wt% as tested by XPS, and the pore size is 8μm and the average size of the ligament is 8.9μm through SEM combined with ImageJ software. In contrast, the Zn content of surface B is 29wt%, the pore size is 160nm, and the average size of the ligament is 189nm.

[0111] Example 4

[0112] (1) selecting a brass foil having a Zn content of 38 wt % and a thickness of 30 μm, and continuously ultrasonically cleaning the brass foil with ethanol and deionized water to remove impurities on the surface of the brass foil, and then vacuum drying the brass foil for later use;

[0113] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 28 hours;

[0114] (3) The etched alloy foil was placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-4 with a lithium affinity / pore dual gradient, and its porosity was 55%.

[0115] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 2wt% as tested by XPS, and the pore size is 1.8μm and the average size of the ligament is 1.9μm by SEM combined with ImageJ software. In contrast, the Zn content of surface B is 32wt%, the pore size is 70nm, and the average size of the ligament is 80nm.

[0116] Example 5

[0117] (1) selecting a brass foil having a Zn content of 38 wt % and a thickness of 30 μm, and continuously ultrasonically cleaning the brass foil with ethanol and deionized water to remove impurities on the surface of the brass foil, and then vacuum drying the brass foil for later use;

[0118] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 20 hours;

[0119] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-5 with a lithium affinity / pore dual gradient, and its porosity is 45%.

[0120] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 10wt% as tested by XPS, and the pore size is 1.2μm and the average size of the ligament is 1.4μm by SEM combined with ImageJ software. In contrast, the Zn content of surface B is 36wt%, the pore size is 30nm, and the average size of the ligament is 37nm.

[0121] Example 6

[0122] (1) selecting a brass foil having a Zn content of 38 wt % and a thickness of 30 μm, and continuously ultrasonically cleaning the brass foil with ethanol and deionized water to remove impurities on the surface of the brass foil, and then vacuum drying the brass foil for later use;

[0123] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 16 hours;

[0124] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-6 with a lithium affinity / pore dual gradient, and its porosity is 40%.

[0125] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 13wt% as tested by XPS, and the pore size is 0.8μm and the average size of the ligament is 0.85μm by SEM combined with ImageJ software. In contrast, the Zn content of surface B is 38wt%, the pore size is 10nm, and the average size of the ligament is 11nm.

[0126] Example 7

[0127] (1) Select a brass foil with a Zn content of 60 wt % and a thickness of 50 μm, clean the brass foil with ethanol and deionized water by continuous ultrasonic cleaning to remove impurities on the surface, and then vacuum dry it for later use;

[0128] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 100°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 52 hours;

[0129] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-7 with a lithium affinity / pore dual gradient, and its porosity is 75%.

[0130] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 0.5wt% as tested by XPS, and the pore size is 21μm and the average size of the ligament is 18μm by SEM combined with ImageJ software. In contrast, the Zn content of surface B is 23wt%, the pore size is 300nm, and the average size of the ligament is 240nm.

[0131] Comparative Example 1

[0132] A commercial pure copper foil with a thickness of 10 μm was selected, and the copper foil was continuously ultrasonically cleaned with ethanol and deionized water to remove impurities on the surface, and then vacuum dried for use.

[0133] Comparative Example 2

[0134] (1) selecting a brass foil having a Zn content of 38 wt % and a thickness of 30 μm, and continuously ultrasonically cleaning the brass foil with ethanol and deionized water to remove impurities on the surface of the brass foil, and then vacuum drying the brass foil for later use;

[0135] (2) The clean brass foil is completely immersed in a mixed solution of ammonium chloride and hydrochloric acid at 120°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 48 hours;

[0136] (3) The etched alloy foil was washed in deionized water for multiple times and vacuum dried to obtain a current collector Cu-2 with a porosity of 60%.

[0137] The surface in direct contact with the etching liquid is recorded as surface A, and the surface not in direct contact with the etching liquid is recorded as surface B. The Zn content of surface A is 0wt% as tested by XPS, and the pore size is 2.5μm and the average size of the ligament is 2.8μm through SEM combined with ImageJ software. In contrast, the Zn content of surface B is 0wt%, the pore size is 2.5μm, and the average size of the ligament is 3.5μm.

[0138] Comparative Example 3

[0139] (1) selecting a brass foil having a Zn content of 38 wt % and a thickness of 30 μm, and continuously ultrasonically cleaning the brass foil with ethanol and deionized water to remove impurities on the surface of the brass foil, and then vacuum drying the brass foil for later use;

[0140] (2) The clean brass foil is suspended in a mixed solution of ammonium chloride and hydrochloric acid at 80°C, where the concentration ratio of the two is 5:1, so that the brass foil is slowly and continuously dealloyed on one side. During the entire corrosion process, movement should be avoided as much as possible to prevent the alloy foil from sinking into the corrosion solution. The electrode is removed after 24 hours;

[0141] (3) The etched alloy foil is placed in deionized water for multiple cleanings and vacuum dried to obtain a nanoporous brass foil NPCuZn-F with a lithium affinity / pore dual gradient, and its porosity is 50%.

[0142] Among them, the surface in direct contact with the corrosive liquid is recorded as surface B, and the surface not in direct contact with the corrosive liquid is recorded as surface A. The Zn content of surface A is 34wt% as tested by XPS, and the pore size is 50nm and the average size of the ligament is 50nm through SEM combined with ImageJ software. In contrast, the Zn content of surface B is 6.8wt%, the pore size is 1.5μm, and the average size of the ligament is 1.5μm. From surface A to surface B, the pore size gradient increases, and the affinity gradient decreases.

[0143] Test Example 1

[0144] The current collectors prepared in the above Examples 1-6 and Comparative Examples 1-3 were assembled into negative electrode-free lithium metal batteries according to the following steps to test the electrochemical properties of the current collectors.

[0145] Step 1: Preparation of positive electrode

[0146] Ternary LiNi 0.80 Co 0.10 Mn 0.10O2 was used as the positive electrode active material. The positive electrode active material was uniformly mixed with carbon black and PVDF binder in NMP at a ratio of 8:1:1 using a vacuum mixer to prepare a uniform slurry. The stirring speed was 1000 rpm for 12 hours. The obtained slurry was then coated on the current collector aluminum sheet and then dried at 80°C to remove the NMP solvent. The positive electrode sheet was obtained after being pressed by a roller press. The surface capacity C of the positive electrode was 3 mAh / cm 2 , and then cut it into pieces with a diameter of 15mm to assemble button batteries.

[0147] Step 2: Assembly of anode-free lithium metal battery

[0148] The current collector NPCuZn 1-7 or NPCu1-3 obtained in the above embodiments and comparative examples is directly used as the negative electrode and assembled in a button battery. From top to bottom, they are respectively the positive electrode, electrolyte, separator, electrolyte and negative electrode, wherein the A side of the current collector faces the positive electrode, the electrolyte is 4MLiFSI of ethylene glycol dimethyl ether (DME), and after sufficient infiltration, they are packaged to obtain batteries S1-S7 and DS1-DS3, respectively.

[0149] Step 3: Electrochemical cycle test:

[0150] Take 3 batteries S1-S6 and DS1-DS3 respectively, and charge them to 4.3V at 0.2C constant current and constant voltage on the secondary battery performance test device, with a cut-off current of 0.05C; after standing for 5 minutes, discharge them to 3V at 0.5C, which is 1 cycle. Repeat this step, and when the battery capacity in grams is less than 80% of the initial capacity during the cycle, the cycle is terminated. The number of cycles is the cycle life of the battery, and the average value is taken for each group. This parameter and the data of the average initial discharge capacity of the battery, as well as the change rate of the negative electrode thickness before and after the battery cycle are shown in Table 1 (Data of the average initial discharge capacity in grams of the battery and the change rate of the negative electrode thickness before and after the battery cycle).

[0151] Table 1

[0152]

[0153]

[0154] Test Example 2

[0155] Batteries S1-S7 and DS1-DS3 were used for the first lithium deposition, and the experiment was repeated twice. They were charged to 4.3 V at a current density of 0.2 C.

[0156] The specific steps of sample preparation and observation are as follows:

[0157] (1) Disassemble the button cell after the first charge in a glove box filled with argon gas (water oxygen value < 0.1 ppm);

[0158] (2) Take out the negative electrode sheet, wash it repeatedly with DME (ethylene glycol dimethyl ether) solution three times, let it stand for 8 hours and then dry it naturally;

[0159] (3) Use ceramic scissors to cut a square electrode with a side length of 2 mm × 2 mm and place it on a sample table covered with conductive glue;

[0160] (4) The sample stage was placed in a vacuum transfer box and taken out of the glove box. The deposition position and morphology of lithium were observed by SEM. The experimental results are shown in Table 2.

[0161] Table 2 Battery lithium deposition location table

[0162] Serial number Battery Morphology Example 1 S1 No obvious lithium deposition on the surface Example 2 S2 No obvious lithium deposition on the surface Example 3 S3 No obvious lithium deposition on the surface Example 4 S4 No obvious lithium deposition on the surface Example 5 S5 No obvious lithium deposition on the surface Example 6 S6 No obvious lithium deposition on the surface Example 6 S7 No obvious lithium deposition on the surface Comparative Example 1 DS1 There is a large amount of lithium deposition on the surface, and there are dendritic lithium Comparative Example 2 DS2 There is a small amount of loose lithium deposition on the surface Comparative Example 3 DS3 There is a large amount of lithium deposition on the surface, and there are dendritic lithium

[0163] It can be concluded from Table 1 and Table 2 that although the comparative examples have a gram capacity substantially equivalent to that of the examples in the initial stage, the lithium metal in comparative examples 1-3 can only be deposited on the surface of the current collector or loosely deposited in the internal pores, resulting in rapid capacity decay and a large expansion of the negative electrode thickness at the end of the cycle. The batteries provided in Examples 1-7 of the present application include the current collector provided in the present application, so that the batteries have the advantages of high charge and discharge capacity, not prone to the generation of lithium dendrites, high safety performance, and long cycle life.

[0164] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A current collector, characterized in that: The current collector comprises a lithium-philic metal element and an inert metal element; wherein the current collector has a porous sponge-like structure; and in the thickness direction of the current collector, from one side of the current collector to the other opposite side, the lithium-philicity of the current collector gradually increases, and the pore size of the pores of the current collector gradually decreases.

2. The current collector according to claim 1, characterized in that: The porosity of the current collector is 30%-80%, preferably 40-60wt%.

3. The current collector according to claim 1 or 2, characterized in that: The thickness of the current collector is 10-100 μm, preferably 20-50 μm.

4. The current collector according to any one of claims 1 to 3, characterized in that: The porous sponge-like structure includes ligaments and holes; Preferably, the ligaments are connected to each other, and the holes are interconnected; Preferably, the average size of the ligaments gradually decreases from one side of the current collector to the other opposite side; Preferably, from one side of the current collector to the other side thereof, the average size of the ligaments gradually decreases from 0.1-10 μm to 10-200 nm.

5. The current collector according to any one of claims 1 to 4, characterized in that: The lithiophilic metal element includes one or more of lithium, sodium, magnesium, aluminum, manganese, iron, zinc, tin, antimony, and bismuth; And / or, the inert metal element includes one or more of gold, silver, platinum, titanium, chromium, copper, nickel, and cobalt.

6. The current collector according to any one of claims 1 to 5, characterized in that: From one side of the current collector to the other side thereof, the content of the lithium-philic metal element gradually increases from 0.2-10 wt % to 20-70 wt %; Preferably, the content of the lithiophilic metal element gradually increases from 1-8 wt % to 30-40 wt %.

7. The current collector according to any one of claims 1 to 6, characterized in that: From one side of the current collector to the other side opposite to the current collector, the pore size gradually decreases from 0.1-100 μm to 1-500 nm; Preferably, the pore size gradually decreases from 0.1-10 μm to 10-200 nm.

8. A method for preparing a current collector, characterized in that: The following steps are involved: (1) using a corrosive solution to corrode and penetrate from one side of the alloy foil to the other side along the thickness direction of the alloy foil to obtain a corroded alloy foil; (2) washing and drying the corroded alloy foil in water to obtain the current collector; The alloy foil contains a lithium-philic metal element and an inert metal element.

9. The method according to claim 8, characterized in that The electrode potential difference between the lithiophilic metal element and the inert metal element is greater than 0.5 V; Preferably, the lithiophilic metal element includes one or more of lithium, sodium, magnesium, aluminum, manganese, iron, zinc, tin, antimony, and bismuth; Preferably, the inert metal element includes one or more of gold, silver, platinum, titanium, chromium, copper, nickel and cobalt.

10. The method according to claim 9, characterized in that The content of the lithium-philic metal element in the alloy foil is 20-80wt%, preferably 40-60wt%.

11. The method according to any one of claims 8 to 9, characterized in that: The infiltration method in step (1) is selected from at least one of chemical dealloying, electrochemical dealloying, liquid metal dealloying, vapor evaporation dealloying, and radio frequency plasma assisted dealloying; Preferably, the infiltration method is selected as a chemical dealloying method; Preferably, the chemical dealloying method is selected as a single-side etching method.

12. The method according to claim 11, characterized in that The reaction conditions of the single-sided etching method include: etching temperature of 50-200° C., etching time of 8-120 h; Preferably, the etching temperature is 80-120° C. and the etching time is 24-48 h.

13. The method according to any one of claims 8 to 12, characterized in that:The corrosive solution comprises ammonium chloride and an acid solution, wherein the acid solution is selected from one or more of perchloric acid, sulfuric acid, nitric acid, hydrochloric acid, hydrofluoric acid, phosphoric acid, formic acid, and acetic acid; Preferably, the corrosive solution is a mixture of hydrochloric acid and ammonium chloride; Preferably, the molar ratio of hydrochloric acid to ammonium chloride is 1:(3-6).

14. A negative electrode-free lithium metal battery, characterized in that: The negative electrode-free lithium metal battery comprises a lithium-embedded positive electrode material, a positive electrode current collector, a separator, an electrolyte, and a current collector according to any one of claims 1 to 7 or a current collector prepared by the method according to any one of claims 8 to 13.

Citation Information

Patent Citations

  • Aluminum alloy surface treatment agent and aluminum alloy surface treatment method

    CN105112978A

  • Negative pole plate for sodium ion battery

    CN107316975A

  • Porous aluminum current collector capable of suppressing sodium dendritic crystal

    CN108417843A

  • Negative electrode for lithium metal battery, and lithium metal battery comprising same

    CN110462902A

  • Lithium metal secondary battery anode current collector and preparation method thereof

    CN110993954A

Cited By

  • Negative current collector and preparation method thereof, negative-electrode-free lithium metal battery and power utilization device

    CN120809828A