Electrochemical device and electronic apparatus
By adding an appropriate amount of compound of formula I to the lithium-ion battery and controlling the thickness of the surface layer of the silica carbon particles, combining substances A and B in the electrolyte, the volume expansion and impedance growth of lithium-ion batteries under high temperature and high pressure is solved, and the problem of volume expansion and impedance growth of lithium-ion batteries is improved, and Circulation performance.
Patent Information
- Application Number
- CN202411208223.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
The volume expansion and impedance growth of lithium-ion batteries under high temperature and high pressure conditions affect their cycling performance.
By adding an appropriate amount of specific compounds of formula I to the electrolyte and regulating the thickness of the surface layer of the silica carbon particles, the content of substances A and substance B in the electrolyte is coordinated to form a dense and stable surface layer, protecting the negative electrode active material, reducing volume expansion and Impedance growth.
It significantly improves the volume expansion and impedance growth of lithium-ion batteries under high temperature and high pressure, improves the capacity retention rate of 500 cycles, and improves the battery's high-temperature cycling performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art
[0002] Lithium-ion batteries are widely used in portable electronic devices such as mobile phones, laptops, and cameras due to their high energy density, high operating voltage, long cycle life, and environmental friendliness. They are also the preferred power source for future electric and hybrid vehicles. At present, in order to improve the energy density of lithium-ion batteries, high-specific-capacity electrode materials are mainly used or high voltage is provided. Silicon-based materials, as a type of alloyed negative electrode material, can provide an ultra-high specific capacity of up to 4200mAh / g, but the silicon negative electrode will experience drastic volume expansion / contraction during the lithium ion insertion / deinsertion process. The high voltage required to achieve the required energy density will also cause the battery volume expansion and impedance growth as the temperature rises during the application process. Summary of the invention
[0003] In view of this, the present application provides an electrochemical device and an electronic device, which can improve the high temperature and high pressure performance of silicon negative electrode lithium ion batteries by synergistically regulating the thickness of the surface layer of silicon-carbon particles within a suitable range and the presence of the compound of formula I in the electrolyte and its content within a suitable range.
[0004] In the first aspect, the present application provides an electrochemical device and an electronic device, wherein the electrochemical device comprises a negative electrode plate and an electrolyte, wherein the negative electrode plate comprises a negative electrode material layer, wherein the negative electrode material layer comprises silicon-carbon particles, wherein the surface of the silicon-carbon particles comprises a surface layer, and the thickness of the surface layer is X μm. The surface layer is formed by a silicon negative electrode lithium-ion battery during cyclic charge and discharge, and is mainly formed by a chemical reaction of electrolyte components. The electrolyte comprises a compound of formula I:
[0005]
[0006] R is selected from fluorine-substituted or unsubstituted C 2 ~C 6 Alkyl, fluorine-substituted or unsubstituted C 6 ~C 12 Nitrogen-containing heterocyclic group, fluorine-substituted or unsubstituted C 6 ~C 12Aryl. Based on the mass of the electrolyte, the mass percentage of the compound of formula I is a%, 0.5≤a≤20, 1<X / a<10. The present application can improve the high temperature and high pressure performance of the electrochemical device by regulating the electrolyte to contain the compound of formula I, and the type and content of the compound of formula I are within the above range, and the thickness of the surface layer of the silicon-carbon particles is also coordinated to be appropriate, especially the volume expansion of the electrochemical device under 80°C 4.53V conditions and the impedance growth in the 45°C 4.53V cycle, thereby improving the capacity retention rate of the electrochemical device after 500 cycles at 45°C 4.53V. The inventors have found that the electrolyte containing the compound of formula I of the appropriate type and content can promote the formation of a dense and stable surface layer on the surface of the silicon-carbon particles during the formation and circulation process of the silicon negative electrode lithium ion battery, and further coordinately regulate the thickness of the surface layer and the ratio of the content of the compound of formula I within the above range, which is beneficial to protect the negative electrode active material and reduce the volume expansion and impedance growth caused by the reduction and decomposition of the electrolyte on the surface of the negative electrode active material.
[0007] In some embodiments, the compound of Formula I includes at least one of the following compounds:
[0008]
[0009] The above-mentioned type of formula I compound has a better effect in promoting the formation of a dense and stable surface layer on the surface of silicon-carbon particles during the formation and circulation process of silicon negative electrode lithium ion batteries, is more conducive to protecting the negative electrode active materials, and achieves a better effect in improving the high temperature and high pressure performance of silicon negative electrode lithium ion batteries.
[0010] In some embodiments, the electrochemical device satisfies at least one of the following conditions: (1) 2≤a≤10, (2) 5<X<12. By adjusting the content a of the compound of formula I and the thickness X of the surface layer within the above range, the volume expansion of the electrochemical device under high temperature and high pressure can be further reduced and the impedance growth can be suppressed.
[0011] In some embodiments, the average particle size of the silicon-carbon particles is Y μm, 0.1≤Y<1, 18<X / Y<22, 0.04≤Y / a≤0.15. The ratio of the thickness X of the surface layer to the average particle size Y of the silicon-carbon particles and the ratio of the average particle size Y of the silicon-carbon particles to the content a of the compound of formula I are also appropriately regulated, which is beneficial to further improve the volume expansion of silicon negative electrode lithium ion batteries under high temperature and high pressure and inhibit impedance growth, and improve the cycle performance of silicon negative electrode lithium ion batteries at high temperature.
[0012] In some embodiments, the silicon-carbon particles include a carbon skeleton, amorphous silicon dispersed in the carbon skeleton, and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the carbon skeleton material includes at least one of artificial graphite, natural graphite, mesophase carbon microspheres, soft carbon, or hard carbon. In this way, the high energy density of silicon is utilized.
[0013] In some embodiments, the electrolyte includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate is b%, 12≤b≤22, based on the mass of the electrolyte. By further adding fluoroethylene carbonate to the electrolyte, and the content of fluoroethylene carbonate is within the above range of the present application, it is beneficial to cooperate with the compound of formula I to further improve the high temperature cycle performance of the silicon negative electrode lithium ion battery, especially to improve its capacity retention rate after 500 cycles at 45°C and 4.53V.
[0014] In some embodiments, the electrolyte includes substance A, and the substance A includes at least two of diethyl carbonate, propyl propionate, or ethyl propionate and contains at least diethyl carbonate. Based on the mass of the electrolyte, the mass percentage of the substance A is c%, and 10≤c≤30. The electrolyte is regulated to further contain substance A, and the type and content of substance A are appropriate, and the effect of improving the high temperature cycle performance of the silicon negative electrode lithium ion battery is better.
[0015] In some embodiments, the electrolyte further includes substance B, and the substance B includes ethylene carbonate and / or propylene carbonate, and the mass percentage of substance B is d%, 10≤d≤20 based on the mass of the electrolyte. The electrolyte is regulated to further contain substance B, and the type and content of substance B are within the scope of the present application, which can effectively reduce the side reactions of the battery in high-temperature cycles and reduce the consumption of the electrolyte, and further improve the high-temperature cycle performance of silicon negative electrode lithium-ion batteries.
[0016] In some embodiments, 0.5≤c / d≤3. In this case, the effect of improving the high temperature cycle performance of the electrochemical device is better.
[0017] In some embodiments, the electrolyte includes a boron-containing lithium salt and a substance C, wherein the boron-containing lithium salt includes at least one of lithium tetrafluoroborate, lithium difluorooxalatoborate or lithium dioxalatoborate, and the substance C includes vinylene carbonate and / or 1,3-propane sultone. The total mass of the base electrolyte, the mass percentage of the boron-containing lithium salt is 0.1% to 5%, and the mass percentage of the substance C is 0.5wt% to 5wt%. The above-mentioned types and contents of the boron-containing lithium salt and substance C in the electrolyte are regulated, and the boron-containing lithium salt, substance C and the compound of formula I can cooperate synergistically to promote the formation of a suitable surface layer on the surface of the silicon-carbon particles, thereby improving the high temperature and high pressure performance of the silicon negative electrode lithium ion battery.
[0018] In a second aspect, the present application provides an electronic device, which comprises the electrochemical device in any of the above embodiments. Therefore, the electronic device provided by the present application has good high temperature performance.
[0019] The electrochemical device provided in the first aspect of the present application has a smaller volume expansion and a lower impedance growth under high temperature and high pressure. Thus, the electronic device provided in the second aspect of the present application also has a smaller volume expansion and a lower impedance growth under high temperature and high pressure. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0021] It should be noted that in the specific embodiments of the present application, the present application is explained by taking a lithium ion secondary battery as an example of an electrochemical device, but the electrochemical device of the present application is not limited to a lithium ion secondary battery.
[0022] Lithium-ion secondary battery
[0023] The invention comprises a negative electrode plate and an electrolyte, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode material layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode material layer contains silicon carbon particles, and the surface of the silicon carbon particles has a surface layer, and the thickness of the surface layer is X μm, and the electrolyte comprises a compound of formula I:
[0024]
[0025] R is selected from fluorine-substituted or unsubstituted C 2 ~C 6 Alkyl, fluorine-substituted or unsubstituted C 6 ~C 12 Nitrogen-containing heterocyclic group, fluorine-substituted or unsubstituted C 6 ~C 12Aryl. Based on the mass of the electrolyte, the mass percentage of the compound of formula I is a%, 0.5≤a≤20, 1<X / a<10. Preferably, 2≤a≤10, 5<X<12. The present application can improve the high temperature and high pressure performance of the electrochemical device by regulating the electrolyte to contain the compound of formula I, and the type and content of the compound of formula I are within the above range, and the thickness of the surface layer of the silicon-carbon particles is also coordinated to be within a suitable range. Exemplarily, the value of a% can be 0.5%, 0.9%, 2%, 2.2%, 3.5%, 5.4%, 7%, 8.7%, 10%, 10.5%, 11.5%, 13.2%, 15.3%, 16.8%, 17.1%, 18.6%, 20% or a range consisting of any two of the above values. Exemplarily, the value of X can be 5.1, 5.8, 6, 6.4, 7.1, 7.6, 8, 8.4, 8.9, 9.6, 10, 10.5, 11.1, 11.8, or a range consisting of any two of the above values. Exemplarily, the value of X / a can be 1.2, 1.4, 2.2, 2.9, 3, 4.3, 4.6, 5.5, 6.0, 6.9, 7.4, 8.2, 8.9, 9.5, 9.9, or a range consisting of any two of the above values.
[0026] In some embodiments, the compound of Formula I includes at least one of the following compounds:
[0027]
[0028] In some embodiments, the average particle size of the silicon-carbon particles is Y μm, 0.1 ≤ Y < 1, 18 < X / Y < 22, 0.04 ≤ Y / a ≤ 0.15. The ratio of the thickness X of the surface layer to the average particle size Y of the silicon-carbon particles and the ratio of the average particle size Y of the silicon-carbon particles to the content a of the compound of formula I are also in a suitable range, which is conducive to further improving the volume expansion of silicon negative electrode lithium ion batteries under high temperature and high pressure and inhibiting impedance growth, and improving the cycle performance of silicon negative electrode lithium ion batteries under high temperature and high pressure. Exemplarily, the value of Y can be 0.1, 0.17, 0.22, 0.29, 0.36, 0.42, 0.45, 0.58, 0.62, 0.68, 0.75, 0.79, 0.90, 0.99 or a range consisting of any two of the above values. Exemplarily, the value of X / Y can be 18.1, 18.5, 18.8, 19, 19.3, 19.5, 19.8, 20, 20.5, 21, 21.3, 21.5, 21.8, or a range consisting of any two of the above values. Exemplarily, the value of Y / a can be 0.04, 0.05, 0.06, 0.08, 0.1, 0.12, 0.13, 0.15, or a range consisting of any two of the above values.
[0029] In some embodiments, the electrolyte includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate is b%, 12≤b≤22 based on the mass of the electrolyte. Adding fluoroethylene carbonate in the above content range to the electrolyte is beneficial to its synergistic coordination with the compound of formula I, and further improves the high temperature cycle performance of the silicon negative electrode lithium ion battery. Exemplarily, the value of b can be 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22 or a range consisting of any two of the above values.
[0030] In some embodiments, the electrolyte includes substance A, substance A includes at least two of diethyl carbonate, propyl propionate or ethyl propionate and contains at least diethyl carbonate, and the sum of the mass percentages of substance A based on the mass of the electrolyte is c%, 10≤c≤30. The type and content of substance A in the electrolyte are within the scope of the present application, which can further improve the high temperature cycle performance of the lithium-ion battery. Exemplarily, the value of c can be 10, 12, 13, 15, 18, 20, 25, 28, 30 or a range consisting of any two of the above values.
[0031] In some embodiments, the electrolyte includes substance B, substance B includes ethylene carbonate and / or propylene carbonate, and the mass percentage of substance B is d%, 10≤d≤20 based on the mass of the electrolyte. Preferably, 0.5≤c / d≤3. Further adding the above-mentioned type and content of substance B to the electrolyte can effectively reduce the side reactions of the battery during high-temperature cycles and reduce the consumption of the electrolyte, thereby improving the high-temperature cycle performance of silicon negative electrode lithium-ion batteries. Exemplarily, the value of d can be 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or a range consisting of any two of the above values. Exemplarily, the value of c / d can be 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.5, 2.8, 3 or a range consisting of any two of the above values.
[0032] In some embodiments, the electrolyte includes a boron-containing lithium salt and a substance C, the boron-containing lithium salt includes at least one of lithium tetrafluoroborate, lithium difluorooxalatoborate or lithium dioxalatoborate, the substance C includes vinylene carbonate and / or 1,3-propane sultone, based on the total mass of the electrolyte, the mass percentage of the boron-containing lithium salt is 0.1% to 5%, and the mass percentage of the substance C is 0.5wt% to 5wt%. At this time, the boron-containing lithium salt, the substance C and the compound of formula I can cooperate to promote the formation of a suitable surface layer on the surface of the silicon-carbon particles, thereby improving the high temperature and high pressure performance of the silicon negative electrode lithium ion battery.
[0033] The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode current collector is 5 μm to 12 μm. The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, it can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or composite current collector, etc.
[0034] The negative electrode material layer may also include a binder and a thickener. The present application does not particularly limit the types of the binder and the thickener, as long as the purpose of the present application can be achieved. For example, the binder may include but is not limited to at least one of polyvinyl alcohol, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber or acrylic (ester) styrene-butadiene rubber; the thickener may include but is not limited to at least one of sodium carboxymethyl cellulose or lithium carboxymethyl cellulose.
[0035] The negative electrode material layer may also include a conductive agent. The present application does not particularly limit the type of the conductive agent, as long as the purpose of the present application can be achieved. For example, the conductive agent may include, but is not limited to, at least one of conductive carbon black, carbon nanotubes (CNTs), carbon fibers, Ketjen black, graphene, metal materials or conductive polymers. The present application does not particularly limit the mass ratio of the negative electrode active material, conductive agent, binder and thickener in the negative electrode active layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. Optionally, the negative electrode sheet may also include a conductive layer, which is located between the negative electrode current collector and the negative electrode active layer. The present application does not particularly limit the composition of the conductive layer, which may be a conductive layer commonly used in the art. For example, the conductive layer includes a conductive agent and a binder. The present application does not particularly limit the conductive agent and binder in the conductive layer, for example, it may be at least one of the conductive agent and binder in the above-mentioned negative electrode active layer.
[0036] other
[0037] The lithium-ion secondary battery also includes a positive electrode sheet, which includes a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector. The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved, for example, it may include aluminum foil, aluminum alloy foil or a composite current collector (for example, a composite current collector with a metal layer disposed on the surface of a polymer layer).
[0038] The present application has no particular limitation on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 13 μm.
[0039] The positive electrode active material layer includes a positive electrode active material. There is no particular limitation on the positive electrode active material in this application, as long as the object of this application can be achieved. For example, the positive electrode active material may include a composite metal oxide of lithium with one or more selected from the group consisting of cobalt, manganese, and nickel, or a lithium-containing olivine-type phosphate selected from one or more of iron, cobalt, nickel, and manganese. These positive electrode active substances can be used alone or in combination of two or more.
[0040] As such a lithium composite metal oxide, for example, those selected from LiCoO 2 , LiMn 2 O 4 , LiNiO 2 , LiCo 1-x Ni x O 2 (0.01 < x < 1), LiNi x MnyCo z O 2 (x + y + z = 1), Li 2 MnO 3 and a solid solution of LiMO 2 (M is a transition metal such as Co, Ni, Mn, Fe, etc.), LiNi 1 / 2 Mn 3 / 2 O 4 , LiFePO 4 , LiMnPO 4 , and LiMn 1-x Fe x PO 4 (0.01 < x < 1) and more preferably two or more. A part of these composite metal oxides of lithium or lithium-containing olivine-type phosphates can be replaced with other elements, or a part of cobalt, nickel, manganese, and iron can be replaced with one or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W, and Zr, or coated with a compound containing these other elements or a carbon material. There is no particular limitation on the thickness of the positive electrode active material layer in this application, as long as the object of this application can be achieved. For example, the thickness of the positive electrode active material layer is 30 μm to 120 μm.
[0041] The positive electrode active material layer may also include a conductive agent and a binder. The present application does not particularly limit the types of the conductive agent and the binder, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black, carbon nanotubes (CNT), carbon fiber, Ketjen black, graphene, metal materials or conductive polymers. The binder may include but is not limited to at least one of polyacrylic acid, polyacrylate, acrylate polymer, polyvinyl alcohol, polyvinylidene fluoride, polytetrafluoroethylene or vinylidene fluoride-hexafluoropropylene copolymer.
[0042] The present application has no particular restriction on the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode active material layer. Those skilled in the art can select the ratio according to actual needs as long as the purpose of the present application can be achieved.
[0043] The lithium-ion secondary battery also includes a diaphragm, which is used to separate the positive electrode plate and the negative electrode plate, prevent the internal short circuit of the secondary battery, allow the electrolyte ions to pass freely, and do not affect the electrochemical charge and discharge process. The present application has no particular restrictions on the diaphragm, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (for example, polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid; the type of diaphragm may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spun membrane.
[0044] In the present application, the diaphragm may include a substrate and a surface treatment layer. The substrate may be a non-woven fabric or a composite film having a porous structure, and the material of the substrate may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the present application has no particular restrictions on the above-mentioned inorganic particles, for example, it may include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on the above-mentioned binder, for example, it may be at least one of the aforementioned binders. The polymer layer contains a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene).
[0045] The pore size of the diaphragm in the present application is 0.01 μm to 1 μm, and the thickness is 5 μm to 50 μm. In some embodiments, the thickness of the diaphragm is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the diaphragm is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the diaphragm is within the above range, the insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.
[0046] The electrochemical device of the present application also includes a packaging bag for containing a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the art in the electrochemical device, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.
[0047] Lithium-ion secondary batteries can be prepared according to conventional methods in the art. For example, the positive electrode sheet, separator and negative electrode sheet are stacked in order, and the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, to obtain an electrode assembly, or the electrode assembly can be obtained after winding; the electrode assembly is placed in a packaging shell, and the electrolyte is injected and sealed to obtain a secondary battery. The structure of the lithium-ion secondary battery is not particularly limited, and can be applied to coin-type batteries, cylindrical batteries, square batteries, or soft-pack batteries with single-layer or multi-layer separators.
[0048] The purpose of the lithium ion secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the lithium ion battery of the present application can be used for, but not limited to, notebook computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium ion capacitors, etc.
[0049] Hereinafter, examples and comparative examples are given to more specifically illustrate the embodiments of the present application. Unless otherwise stated, the parts, percentages and ratios listed are all based on mass.
[0050] Example 1-1
[0051] (I) Preparation of lithium-ion batteries
[0052] <Preparation of negative electrode sheet>
[0053] Artificial graphite, negative silicon carbon particles with a silicon content of 15%, conductive carbon black, and binder polyacrylic acid PAA are mixed in a mass ratio of 70%: 15%: 5%: 10%, and an appropriate amount of water is added, and kneaded at a solid content of about 55wt% to 70wt%. Add an appropriate amount of water to adjust the viscosity of the slurry to about 4000Pa·s to 6000Pa·s to prepare a negative electrode slurry. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and the copper foil is dried at 85°C for 4 hours to obtain a negative electrode sheet coated with a negative electrode mixture layer on one side. After cold pressing (cold pressing pressure of 20t), cutting and slitting, it is dried under vacuum conditions at 120°C for 12 hours to obtain a negative electrode sheet with a specification of 76.6mm×875mm. Among them, the compaction density of the negative electrode material layer after cold pressing is 1.70g / cm 3 .
[0054] <Preparation of positive electrode sheet>
[0055] The positive electrode active material is lithium cobalt oxide (LiCoO 2 ), conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 97:1.4:1.6, and N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 75wt%. The positive electrode slurry is obtained after being stirred evenly with a vacuum mixer. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 85°C to obtain a positive electrode sheet with a single-sided positive electrode material layer coated with a coating thickness of 110μm. After that, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode material layer coated. After coating, the positive electrode sheet is cold pressed and cut into a specification of 74mm×867mm for standby use. Among them, the compaction density of the positive electrode material layer after cold pressing is 4.15g / cm 3 .
[0056] <Preparation of Electrolyte>
[0057] In an argon atmosphere glove box with a water content of less than 10 ppm, dimethyl carbonate and ethyl methyl carbonate are used as base solvents, lithium hexafluorophosphate and the compound of formula I are added to the base solvents, and mixed evenly to obtain an electrolyte. Wherein, based on the mass of the electrolyte, the mass percentage of lithium hexafluorophosphate is 12.5%, the mass percentage of the compound of formula I is as shown in Table 1, and the rest is the base solvent, and the mass ratio of dimethyl carbonate to ethyl methyl carbonate is 1:1.
[0058] <Diaphragm>
[0059] A polyethylene (PE) porous membrane with a thickness of 5 μm was used.
[0060] <Preparation of lithium-ion batteries>
[0061] The prepared positive electrode sheet, separator, negative electrode sheet and separator are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain an electrode assembly. After welding the pole ear, the electrode assembly is placed in an aluminum plastic film packaging bag, placed in an 85°C vacuum oven for 12 hours to remove moisture, and the prepared electrolyte is injected. After vacuum packaging, standing, formation (0.7C constant current charging to 4.4V, constant voltage charging to 0.025C, standing for 5 minutes and then discharging at 0.5C to 3.0V), shaping, and capacity testing procedures, a lithium-ion battery is obtained.
[0062] Example 1-2 to Example 1-21
[0063] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. For example, the surface layer thickness X in Table 1 can be achieved by adjusting the value of the average particle size Y of the silicon carbon particles, that is, the smaller the value of Y is, the smaller the thickness value of the surface layer is.
[0064] Example 2-1 to Example 2-9
[0065] During the preparation of the electrolyte of Example 1-1, the substances listed in Table 2 were added to the base solvent, with the remainder being the base solvent, and the rest being the same as in Example 1-1.
[0066] Example 3-1 to Example 3-6
[0067] During the preparation of the electrolyte of Example 1-1, the substances listed in Table 3 were added to the base solvent, with the remainder being the base solvent, and the rest being the same as in Example 1-1.
[0068] Embodiment 3-7
[0069] During the preparation of the electrolyte of Example 2-7, the substances listed in Table 3 were further added to the base solvent, with the remainder being the base solvent, and the rest being the same as in Example 2-7.
[0070] Comparative Examples 1 to 5
[0071] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1.
[0072] (II) Test methods
[0073] (1) Negative electrode parameter test
[0074] The lithium-ion batteries prepared in the above-mentioned embodiments and comparative examples were disassembled to obtain negative electrode sheets for subsequent detection and analysis.
[0075] The negative electrode material layer on the negative electrode sheet was scraped off with a scraper, and the powder of the scraped negative electrode material layer was heat-treated at 400° C. for 4 h in a tube furnace under argon protection for subsequent detection and analysis.
[0076] Detection of silicon carbon particle surface layer thickness and average particle size
[0077] The electrochemical device detects relevant parameters of the silicon-carbon particles in a fully discharged state. Specifically, the lithium-ion batteries in the embodiments and comparative examples are disassembled according to the above method to obtain negative electrode sheets.
[0078] The negative electrode sheet was cut into a size of 0.5 cm × 1 cm, and the cut negative electrode sheet was pasted on a 1 cm × 1.5 cm silicon wafer carrier using conductive glue. The cross section of the negative electrode sheet along the thickness direction was processed using argon ion polishing (parameters: 8KV acceleration voltage, 4h treatment) for subsequent observation. Combined with scanning electron microscope SEM, ZEISS SEM (Sigma 02 33) (0.1 30KV) equipment was used in the backscatter mode, at a magnification of 100K, to observe the cross section of the negative electrode sheet obtained by the above treatment along the thickness direction to obtain an SEM image. In the SEM image, all silicon-carbon particles in the field of view were observed, and the longest distance between any two points on the silicon-carbon particles was used as the particle size of the silicon-carbon particles, and the average particle size of the silicon-carbon particles was calculated. Select any silicon-carbon particle, measure the thickness of any 100 points on the edge of the surface layer of the silicon-carbon particle, and calculate the average value to obtain the thickness of the surface layer of the silicon-carbon particle.
[0079] (2) High temperature volume expansion test (80℃ 4.53V)
[0080] The lithium-ion battery was charged to 4.53V at a constant current of 0.2C, and then charged to 0.05C at a constant voltage of 4.53V. After standing for 5 minutes, the initial thickness H0 of the lithium-ion battery was tested.
[0081] The lithium-ion battery was placed in a thermostat at 80° C. and left to stand for 7 hours. The final thickness H′ of the lithium-ion battery was tested. The volume expansion rate = (H′H0) / H0×100%.
[0082] (3) High temperature cycle test (45℃ 4.53V)
[0083] Place the lithium-ion battery in a 45°C constant temperature environment and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature of 45°C. Charge it to 4.53V at a constant current of 1C, charge it to a current of 0.025C at a constant voltage of 4.53V, let it stand for 5 minutes, and discharge it to 3.0V at a constant current of 0.5C. Record the initial discharge capacity as C0 and the initial impedance as I0. Cycle the above charge and discharge steps for 500 cycles, and record the discharge capacity after 500 cycles as C1 and the impedance as I1.
[0084] Cycle capacity retention rate = C1 / C0×100%, impedance growth rate = I1 / I0×100%.
[0085] Table 1
[0086]
[0087]
[0088] Note: “ / ” in the table means there is no related parameter.
[0089] Combined with Table 1, compared with Example 1-1, the ratio (X / a) of the surface layer thickness X of the silicon-carbon particles in Examples 1 to 2 to the content a of the compound of formula I in the electrolyte is not within a suitable range, the content a of the compound of formula I in the electrolyte of Examples 3 to 4 is not within a suitable range, and the electrolyte of Example 5 does not contain the compound of formula I. It can be seen from Table 1 that the high temperature performance of the silicon negative electrode lithium ion batteries corresponding to Examples 1 to 5 is significantly inferior to the high temperature performance of Example 1-1, especially, the volume expansion rate of the silicon negative electrode lithium ion batteries of Examples 1 to 5 at 80°C and 4.53V is above 15.3%, and can reach up to 28.5%, and the cycle impedance growth rate at 45°C and 4.53V is above 90.3%, resulting in a capacity retention rate of only 72.4% at most after 500 cycles at 45°C and 4.53V. The volume expansion rate of the silicon negative electrode lithium ion battery of Example 1-1 at 80°C and 4.53V is only 12.3%, and its cycle impedance growth rate at 45°C is significantly reduced to 85.2%. Under the same conditions, the capacity retention rate after 500 cycles is increased to 75.8%.
[0090] In particular, when the content a of the compound of formula I and the surface layer thickness X of the silicon-carbon particles are further regulated within a preferred range, and the particle size of the silicon-carbon particles is synergistically regulated within a suitable range, the effect of improving the volume expansion and impedance growth of the silicon negative electrode lithium ion battery under high temperature and high pressure is better, that is, it is beneficial to further improve the cycle performance of the silicon negative electrode lithium ion battery under high temperature and high temperature.
[0091] Table 2
[0092]
[0093] It can be seen from Table 2 that when an appropriate amount of fluoroethylene carbonate is further added to the electrolyte of Example 1-1, the cycle performance of the silicon negative electrode lithium ion battery at high temperature can be further improved, especially the capacity retention rate of 500 cycles at 45°C and 4.53V. And when an appropriate amount of substance A and substance B are further added, and the types of substance A and substance B are also within the above range, the effect of improving the cycle performance of the silicon negative electrode lithium ion battery at high temperature is better.
[0094] Table 3
[0095]
[0096] It can be seen from Table 3 that when an appropriate amount of boron-containing lithium salt and substance C are added to the electrolyte of Example 1-1, and the types of boron-containing lithium salt and substance C are also appropriate, the high temperature and high pressure performance of the silicon negative electrode lithium ion battery can also be improved. In particular, when the above types and contents of boron-containing lithium salt and substance C are further added to the electrolyte of Example 2-7, the effect of improving the high temperature and high pressure performance of the silicon negative electrode lithium ion battery is optimal.
[0097] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. An electrochemical device, characterized in that The electrochemical device comprises a negative electrode sheet and an electrolyte; The negative electrode plate comprises a negative electrode material layer, the negative electrode material layer contains silicon carbon particles, the surface of the silicon carbon particles has a surface layer, and the thickness of the surface layer is X μm; The electrolyte comprises a compound of formula I; wherein R is selected from fluorine-substituted or unsubstituted C2-C6 alkyl, fluorine-substituted or unsubstituted C6-C 12 Nitrogen-containing heterocyclic group, fluorine-substituted or unsubstituted C6~C 12 Aryl; Based on the mass of the electrolyte, the mass percentage of the compound of formula I is a%, 0.5≤a≤20, 1<X / a<10.
2. The electrochemical device according to claim 1, characterized in that The compound of formula I includes at least one of the following compounds:
3. The electrochemical device according to claim 1, characterized in that The electrochemical device satisfies at least one of the following conditions: (1)2≤a≤10; (2)5<X<12。 4. The electrochemical device according to any one of claims 1 to 3, characterized in that: The average particle size of the silicon-carbon particles is Y μm, 0.1≤Y<1.
5. The electrochemical device according to any one of claims 1 to 3, characterized in that: The electrolyte includes fluoroethylene carbonate; Based on the mass of the electrolyte, the mass percentage of the fluoroethylene carbonate is b%, and 12≤b≤22.
6. The electrochemical device according to claim 5, characterized in that The electrolyte includes substance A, wherein substance A includes at least two of diethyl carbonate, propyl propionate or ethyl propionate and contains at least diethyl carbonate; Based on the mass of the electrolyte, the mass percentage of the substance A is c%, 10≤c≤30.
7. The electrochemical device according to claim 6, characterized in that The electrolyte further comprises a substance B, wherein the substance B comprises ethylene carbonate and / or propylene carbonate; Based on the mass of the electrolyte, the mass percentage of the substance B is d%, 10≤d≤20.
8. The electrochemical device according to claim 7, characterized in that 0.5≤c / d≤3.
9. The electrochemical device according to any one of claims 1 to 3, characterized in that: The electrolyte includes a boron-containing lithium salt and a substance C; The boron-containing lithium salt includes at least one of lithium tetrafluoroborate, lithium difluorooxalatoborate or lithium dioxalatoborate, and the substance C includes vinylene carbonate and / or 1,3-propane sultone; Based on the total mass of the electrolyte, the mass percentage of the boron-containing lithium salt is 0.1% to 5%, and the mass percentage of the substance C is 0.5wt% to 5wt%.
10. An electronic device, characterized in that: The electronic device comprises the electrochemical device according to any one of claims 1 to 9.
Citation Information
Cited By
Secondary battery and electrochemical device
CN121097214A