Spinning device
Localized fusion welding methods, such as directed energy deposition, are used to create glass fiber spinners with improved creep and corrosion resistance by forming a metal alloy with specific grain structures, addressing the high cost and performance limitations of cobalt-based alloys.
Patent Information
- Application Number
- CN202380034821.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2023-04-24
- Publication Date
- 2024-12-03
AI Technical Summary
Existing glass fiber spinners made from cobalt-based alloys are expensive and require improvements in creep resistance and corrosion resistance at elevated temperatures.
Utilizing a localized fusion welding method, such as directed energy deposition, to create a metal alloy spinner with an anisotropic grain structure, which includes a metal alloy material formed using a localized fusion welding method, formed from a metal alloy comprising chromium, nickel, and optionally including additional elements such as tungsten, boron, and optionally having an opening therethrough, and a side wall extending between the upper and lower walls, the side wall comprising a plurality of holes.
The method achieves improved mechanical and corrosion properties, and the method includes a localized fusion welding method, and the method includes a localized fusion welding method, and the method includes a localized fusion welding method, and the method includes a localized fusion welding method, and the method includes a localized fusion welding method, and the method includes a localized fusion welding method.
Smart Images

Figure CN119072373A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to spinners used in making glass fibers, and more particularly to improved materials and methods for making such spinners. Background Art
[0002] The statements in this section provide background information related to the present disclosure.
[0003] In the manufacture of glass fibers, a rotary spinner is used to direct molten glass through a plurality of holes to form individual fibers. Such spinners are shown in more detail by way of example in U.S. Pat. Nos. 4,904,290 and 5,286,446, each of which is incorporated herein by reference in its entirety.
[0004] Glass fiber spinners are typically made of materials that have high corrosion resistance, high creep resistance, and high oxidation resistance at elevated temperatures, such as 1,121°C (about 2,050°F). These spinners are also typically manufactured using a casting process in which the process is controlled to achieve the desired mechanical properties of the spinner. Although cobalt-based alloys have been used in the past to meet the performance requirements of spinners, these alloys are relatively expensive.
[0005] Various challenges associated with the materials and manufacturing of spinners used in producing glass fibers are addressed by the present disclosure. Summary of the invention
[0006] This section provides a general summary of the disclosure, and is not a comprehensive disclosure of its full scope or all of its features.
[0007] In one form, a spinner for use in manufacturing glass fibers is provided, the spinner comprising a body having: an upper wall having an opening therethrough; a lower wall that may or may not have an opening therethrough; and a side wall extending between the upper wall and the lower wall, the side wall comprising a plurality of holes, wherein the body comprises a metal alloy material formed using a localized fusion welding method. As used herein, the term "localized fusion welding method" encompasses any suitable additive manufacturing process, such as directed energy deposition or powder bed fusion. See, for example, ISO / ASTM 52900.
[0008] In one exemplary embodiment, the localized fusion welding method may utilize an electron beam, a laser, or an electric or plasma arc.
[0009] In a variation of the spinner that may be implemented alone or in any combination: the localized fusion welding method includes laser directed energy deposition; the metal alloy is a chromium-cobalt-nickel alloy; the metal alloy includes an anisotropic grain structure; the anisotropic grain structure includes a fine columnar dendrite region having an average grain size between about 50 μm and about 200 μm as measured across the grain width; the anisotropic grain structure includes a refined equiaxed region having an average grain size between about 20 μm and about 200 μm; the anisotropic grain structure includes a carbide concentration at the grain / subgrain boundaries; the average inter-grain distance between the carbide concentrations is between about 0.10 μm and about 4.0 μm; and the average size of the carbides is about 0.5 μm to about 1.5 μm.
[0010] In an exemplary embodiment, the metal alloy material includes chromium and at least one of nickel and cobalt.
[0011] In one exemplary embodiment, the metal alloy material includes chromium, nickel, and cobalt.
[0012] In an exemplary embodiment, the metal alloy material includes 25 wt % to 40 wt % chromium.
[0013] In an exemplary embodiment, the metal alloy material includes up to 75 weight percent nickel, cobalt, or a combination thereof.
[0014] In an exemplary embodiment, the metal alloy material further includes at least one of tungsten, boron, and carbon.
[0015] In one exemplary embodiment, the metal alloy material includes 0.01 wt % to 10.0 wt % tungsten.
[0016] In an exemplary embodiment, the metal alloy material includes 0.002 wt % to 0.05 wt % boron.
[0017] In an exemplary embodiment, the metal alloy material includes 0.1 wt % to 1.0 wt % carbon.
[0018] In an exemplary embodiment, the metal alloy material further includes at least one of tantalum, zirconium, and hafnium.
[0019] In an exemplary embodiment, the metal alloy material includes 0.01 wt % to 5.0 wt % tantalum.
[0020] In an exemplary embodiment, the metal alloy material includes 0.1 wt % to 0.4 wt % zirconium.
[0021] In an exemplary embodiment, the metal alloy material includes 0.01 wt % to 1.0 wt % hafnium.
[0022] In an exemplary embodiment, the metal alloy material includes: chromium in an amount between 25.0 wt. % and 40.0 wt. %; nickel in an amount between 15.0 wt. % and 25.0 wt. %; cobalt in an amount between 25.0 wt. % and 39.0 wt. %; tungsten in an amount between 0.01 wt. % and 10.0 wt. %; boron in an amount between 0.002 wt. % and 0.05 wt. %; carbon in an amount between 0.1 wt. % and 1.0 wt. %; tantalum in an amount between 0.01 wt. % and 5.0 wt. %; zirconium in an amount between 0.1 wt. % and 0.4 wt. %; and hafnium in an amount between 0.01 wt. % and 1.0 wt. %.
[0023] In an exemplary embodiment, the spinner has a total strain that is at least 50% less than the total strain (in / in) of the same spinner made from the same metal alloy material by casting.
[0024] In an exemplary embodiment, the spinner has a minimum creep rate (×10 -4 )(in / in / hr) is at least 50% lower than the minimum creep rate.
[0025] In an exemplary embodiment, the spinner has a corrosion penetration depth (μm) that is at least 20% less than the corrosion penetration depth (μm) of an identical spinner made from the same metal alloy material by casting.
[0026] In another form of the present disclosure, a method for manufacturing a component includes: depositing a metal alloy material onto a substrate; while depositing the metal alloy material, simultaneously applying a localized fusion welding means to the metal alloy material; and sequentially depositing and fusion welding the metal alloy material into multiple layers to form the component, wherein the chromium-cobalt-nickel alloy material comprises: chromium in an amount between 25.0 wt. % and 40.0 wt. %; and up to 75 wt. % of nickel, cobalt, or a combination thereof.
[0027] In an exemplary embodiment of the method, the metal alloy material further comprises at least one of tungsten, boron, and carbon.
[0028] In an exemplary embodiment of the method, the metal alloy material includes 0.01 wt % to 10.0 wt % tungsten.
[0029] In an exemplary embodiment of the method, the metal alloy material includes 0.002 wt % to 0.05 wt % boron.
[0030] In an exemplary embodiment of the method, the metal alloy material includes 0.1 wt % to 1.0 wt % carbon.
[0031] In an exemplary embodiment of the method, the metal alloy material further comprises at least one of tantalum, zirconium, and hafnium.
[0032] In an exemplary embodiment of the method, the metal alloy material includes 0.01 wt % to 5.0 wt % tantalum.
[0033] In an exemplary embodiment of the method, the metal alloy material includes 0.1 wt % to 0.4 wt % zirconium.
[0034] In an exemplary embodiment of the method, the metal alloy material includes 0.01 wt % to 1.0 wt % hafnium.
[0035] In an exemplary embodiment of the method, the metal alloy material is in powder form or wire form.
[0036] In an exemplary embodiment of the method, the localized fusion welding means is directed energy deposition or powder bed fusion.
[0037] In an exemplary embodiment of the method, the localized fusion welding means comprises a heat source selected from the group consisting of a laser, an electron beam, and an electric arc or a plasma arc.
[0038] In an exemplary embodiment of the method, at least one of the power and travel speed of the heat source is controlled to control the solidification rate of the metal alloy material.
[0039] In one exemplary embodiment of the method, the component is a spinner used in making glass fibers.
[0040] In an exemplary embodiment of the method, the spinner has a total strain that is at least 50% less than the total strain (in / in) of the same spinner made from the same metal alloy material by casting.
[0041] In an exemplary embodiment of the method, the spinner has a minimum creep rate (×10 -4 )(in / in / hr) is at least 50% lower than the minimum creep rate.
[0042] In an exemplary embodiment of the method, the spinner has a corrosion penetration depth (μm) that is at least 20% less than the corrosion penetration depth (μm) of an identical spinner made from the same metal alloy material by casting.
[0043] In an exemplary embodiment of the method, the spinner includes a body having an upper wall having an opening therethrough, a lower wall, and a side wall extending between the upper wall and the lower wall, the side wall including a plurality of holes.
[0044] In yet another form, a spinner is made according to these methods. The spinner includes a body having an upper wall having an opening therethrough, a lower wall that may or may not have an opening therethrough, and a side wall extending between the upper wall and the lower wall, the side wall including a plurality of holes.
[0045] Further areas of applicability will become apparent from the description provided herein.It should be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order that the present disclosure may be better understood, various forms of the present disclosure will now be described by way of example with reference to the accompanying drawings, in which:
[0047] Figure 1 is a spinner constructed according to the teachings of the present disclosure;
[0048] Figure 2 is a table of inventive alloys and comparative alloys according to the teachings of the present disclosure;
[0049] FIG. 3A is a SEM (scanning electron microscope) image of the microstructure of a 3D printed alloy according to the teachings of the present disclosure;
[0050] FIG3B is a SEM image of the microstructure of another 3D printed alloy according to the teachings of the present disclosure;
[0051] FIG3C is a SEM image of the microstructure of a casting alloy of the prior art;
[0052] FIG3D is a SEM image of the microstructure of another casting alloy of the prior art;
[0053] FIG4A is a SEM image of the microstructure of the 3D printed alloy of FIG3A at an enlarged scale;
[0054] FIG4B is a SEM image of the microstructure of the 3D printed alloy of FIG3B at an enlarged scale;
[0055] FIG4C is a SEM image of the microstructure of the cast alloy of FIG3C on an enlarged scale;
[0056] FIG4D is a SEM image of the microstructure of the cast alloy of FIG3D on an enlarged scale;
[0057] Figure 5A is an IPF (inverse pole figure) diagram of the microstructure of a 3D printed alloy obtained using EBSD (electron backscatter diffraction) according to the teachings of the present disclosure; and
[0058] Figure 5B yes Figure 5A , illustrating a microstructure having distinct equiaxed regions and fine columnar dendrite regions according to the present disclosure.
[0059] The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way. DETAILED DESCRIPTION
[0060] The following description is merely exemplary in nature and is not intended to limit the present disclosure, application, or uses. It should be understood that throughout the drawings, corresponding reference numerals indicate the same or corresponding parts and features.
[0061] The present inventors have discovered unexpected and advantageous microstructural, mechanical, and corrosion properties of alloys formed using localized fusion welding methods, such as directed energy deposition methods, and particularly in the application of spinners used in the manufacture of glass fibers.
[0062] Generally speaking, directed energy deposition (DED), also known as "laser metal deposition" (LMD), "direct metal deposition" (DMD), or "laser direct energy deposition" (LDED), is an additive process in which an energy source first heats the surface of a workpiece to produce a molten pool. The energy source may include, for example, a laser, an electron beam, or an electric or plasma arc. Next, a metal powder is sprayed from a nozzle directly into the molten pool. The metal powder melts and combines with the matrix material of the workpiece to produce a layer, and the process is repeated for multiple layers as required by the application. In addition, an inert shielding gas, such as argon by way of example, is used during the deposition process to ensure the desired chemical properties in the final product from the initial metal powder feed. It should also be understood that other forms of metal, such as wire by way of example, may be employed while remaining within the scope of the present disclosure.
[0063] According to the teachings of the present disclosure, various alloys are used in combination with localized fusion welding methods, such as directed energy deposition (DED), to produce spinners with improved properties for applications in making glass fibers. However, it should be understood that the teachings herein may be applied in applications other than glass fiber spinners while remaining within the scope of the present disclosure.
[0064] Now refer to Figure 1An exemplary spinner for use in making glass fibers is illustrated and generally indicated by reference numeral 20. Spinner 20 includes a body 21 having an upper wall 22 having an opening 24 therethrough, a lower wall 30 having an optional opening (not shown) therethrough, and a side wall 40 extending between the upper wall 22 and the lower wall 30, the side wall 40 having a plurality of holes 42. Further details of such a spinner are shown and described in greater detail in U.S. Patent Nos. 4,904,290 and 5,286,446, each of which is incorporated herein by reference in its entirety.
[0065] Advantageously, body 21 comprises a metal alloy material formed using a localized fusion welding process, such as, by way of example, a directed energy deposition (DED) process, which results in spinner 20 having improved properties, and most notably improved creep resistance and corrosion resistance, as described in more detail below.
[0066] Reference Figure 2 , samples made from a variety of different metal alloy materials were evaluated and considered, where the samples were prepared using both a DED method (in this case, laser directed energy deposition method) and conventional casting. In the DED method, the following parameters were used to produce the non-cast samples: (1) 2 kW laser power, (2) 1,030 nm laser wavelength, (3) 4 mm laser spot size, (4) 500 mm / min travel speed, (5) 11.5 g / min powder flow rate, and (6) 12 mm standoff distance.
[0067] To obtain creep properties, the samples were machined into tensile specimens with 0.25" reduced diameter segments and 3" to 3.5" overall lengths. The samples were placed in creep-rupture testing until failure, with all samples tested under standard conditions of 4,000 psi and 1,150°C. The total strain and minimum creep rate were recorded during the test.
[0068] To obtain corrosion characteristics, samples were machined into 0.25" x 0.25" x 1.5" coupons. These coupons were subjected to corrosion testing by suspending them in molten glass at 1,050°C for 100 hours. Cross-sections of these samples were evaluated using microscopy to measure the depth of corrosion at many areas along the surface to obtain an average value. It should be understood that these alloys are merely exemplary and that a variety of alloys may be employed in accordance with the teachings of the present disclosure.
[0069] The creep and corrosion properties of the metal alloy materials made by the DED method are greatly improved when compared to the creep and corrosion properties of the same chromium-cobalt-nickel alloy made by conventional casting. The creep-rupture test and corrosion test data of samples made from certain metal alloy materials are shown in Tables 1-3 below:
[0070]
[0071] Table 1 - Material creep properties - DED method
[0072]
[0073] Table 2 - Material creep properties - casting method
[0074]
[0075] Table 3 - Material corrosion characteristics - DED and casting method
[0076] Overall, in preliminary tests, samples made by the DED method exhibited lower total strain, lower minimum creep rate, and less corrosion penetration. Thus, samples made by the DED method showed an overall improvement in creep properties and corrosion resistance. Additionally, regardless of the processing method, the Alloy 1 composition showed an overall improvement in creep properties compared to the Alloy 2 composition.
[0077] Referring now to FIGS. 3A to 3D , FIGS. 4A to 4D , and FIG. 5A to FIG. 5B , showing the comparison of the microstructure of DED / 3D printed alloys with that of cast alloys. As shown in the figure, the DED alloys include Figure 5A and Figure 5B The anisotropic grain structure is best shown in FIG. 1 . In one form, the anisotropic grain structure defines a fine columnar dendrite region having an average grain size between about 50 μm and about 200 μm (as measured across the grain width). In another form, the anisotropic grain structure defines a more refined equiaxed region where the average grain size is observed to be between about 20 μm and about 200 μm when measured along the grain. In comparison, the cast alloy sample had an average grain size of about 600 μm. Therefore, the improved creep properties are unexpected because, typically for metal alloys, larger grain sizes result in improved creep properties. Here, for DED, the exact opposite was observed in preliminary testing.
[0078] The anisotropic grain structure includes carbide concentrations at grain / subgrain boundaries, and the carbides are more evenly distributed. The average size of the carbides is about 0.5 μm to about 1.5 μm. The average inter-grain distance between carbides is between about 0.10 μm to about 4.0 μm. It is believed that this carbide distribution and the resulting microstructure help to inhibit grain boundary sliding, resulting in improved mechanical properties. In addition, it is believed that the resulting microstructure improves corrosion resistance by providing a more even distribution of alloying elements.
[0079] In some embodiments, the metal alloy comprises chromium and at least one of nickel and cobalt. In some embodiments, the metal alloy may also comprise one or more of tungsten, boron, and carbon. In some embodiments, the metal alloy may also comprise one or more of tantalum, zirconium, and hafnium. General embodiments of metal alloys encompassed by the present disclosure comprise alloying elements shown in weight % as listed in Table 4 below:
[0080]
[0081]
[0082] Table 4 - General Metal Alloy Compositions
[0083] Alloying elements, alone and / or in combination, contribute to the production of a suitable alloy. For example, carbon supports the formation of carbides, tantalum and hafnium act as carbide formers, tungsten acts as a carbide refiner, and boron and zirconium act as carbide stabilizers.
[0084] In some embodiments, the metal alloy includes at least one element from each of Groups A, B, C, and D.
[0085] In some embodiments, the metal alloy comprises chromium and at least one element from Group B. In some embodiments, the metal alloy comprises chromium and all elements from Group B. In some embodiments, when the metal alloy comprises both nickel and cobalt, the combined nickel and cobalt content ranges from 0.1 wt. % to 75.0 wt. %.
[0086] In some embodiments, the metal alloy comprises chromium, at least one element from Group B, and at least one element from Group C. In some embodiments, the metal alloy comprises chromium, at least one element from Group B, and all elements from Group C.
[0087] In some embodiments, the metal alloy comprises chromium, at least one element from Group B, at least one element from Group C, and at least one element from Group D. In some embodiments, the metal alloy comprises chromium, at least one element from Group B, at least one element from Group C, and all elements from Group D.
[0088] In some embodiments, the metal alloy includes all elements from each of Group A, Group B, Group C, and Group D.
[0089] Some representative exemplary embodiments of chromium-cobalt-nickel alloys contemplated by the present disclosure include the following
[0090] Alloying elements listed in Table 5 in wt %:
[0091]
[0092]
[0093] Table 5 - Exemplary Chromium-Cobalt-Nickel Alloy Compositions
[0094] It should be understood that unintentional alloying elements (e.g., those alloying elements falling outside of Groups A, B, C, and D) may be present in the final alloy, such as, by way of example, silicon, aluminum, titanium, manganese, and molybdenum (e.g., Figure 2 In addition, the element ranges disclosed herein include all incremental values between the minimum alloying element composition and the maximum alloying element composition. That is, the minimum alloying element composition can range from the minimum value to the maximum value. Similarly, the maximum alloying element composition can range from the maximum value shown to the minimum value disclosed.
[0095] As shown above, carbon is present in the alloys according to the present disclosure. Although these amounts of carbon have been considered to be relatively high and can contribute to cracking in various fusion welding applications, the inventors have found that this amount of carbon provides unexpected results in terms of crack resistance of the spinner 20 when combined with a localized fusion welding method. It is believed that when compared to other additive methods such as powder bed fusion, the solidification rate of the alloy using DED is relatively slow in the case of a large molten pool. By controlling the power of the heat source (e.g., laser) and the travel speed of the heat source (e.g., laser), the solidification rate of the alloy can be controlled or significantly slowed so that the carbon content does not cause cracking of the spinner 20 as would normally be expected. Therefore, when using the DED method, higher amounts of carbon can be used in alloys according to the teachings of this article while maintaining sufficient mechanical properties for applications of the spinner 20 as described herein.
[0096] Unless otherwise expressly indicated herein, all numerical values indicating mechanical / thermal properties, composition percentages, dimensions and / or tolerances or other properties should be understood as being modified by the word "about" or "approximately" when describing the scope of the present disclosure. Such modifications are desirable for a variety of reasons, including industrial practice, materials, manufacturing and component tolerances, and testing capabilities.
[0097] As used herein, the phrase at least one of “a,” “b,” and “c” should be construed to mean a logical (“a” or “b” or “c”), using a non-exclusive logical “or,” and should not be construed to mean at least one of “a,” at least one of “b,” and at least one of “c.”
[0098] As used herein, the phrases between "a" and "b" and the phrases between "a" and "b" each encompass the actual values of "a" and "b" and any values therebetween.
[0099] The description of the present disclosure is merely exemplary in nature, and therefore, variations that do not depart from the essence of the present disclosure are intended to be within the scope of the present disclosure. Such variations should not be regarded as departing from the spirit and scope of the present disclosure.
Claims
1. A spinner used in the manufacture of glass fibers, the spinner include: a body having an upper wall, a lower wall, and a side wall extending between the upper wall and the lower wall, the upper wall having an opening therethrough, the side wall including a plurality of holes, The body is formed of a metal alloy material using a local fusion welding method.
2. The spinner of claim 1, wherein the localized fusion welding process comprises directed energy deposition.
3. The spinner of claim 1, wherein the metal alloy material comprises chromium and at least one of nickel and cobalt.
4. The spinner of claim 3, wherein the metal alloy material comprises chromium, nickel, and cobalt.
5. The spinner of claim 3, wherein the metal alloy material comprises 25 wt% to 40 wt% chromium.
6. The spinner of claim 3, wherein the metal alloy material comprises up to 75 wt. % nickel, cobalt, or a combination thereof.
7. The spinner of claim 3, wherein the metal alloy material further comprises at least one of tungsten, boron, and carbon.
8. The spinner of claim 7, wherein the metal alloy material comprises 0.01 wt% to 10.0 wt% tungsten.
9. The spinner of claim 7, wherein the metal alloy material comprises 0.002 wt. % to 0.05 wt. % boron.
10. The spinner of claim 7, wherein the metal alloy material comprises 0.1 wt% to 1.0 wt% carbon.
11. The spinner of claim 7, wherein the metal alloy material further comprises at least one of tantalum, zirconium, and hafnium.
12. The spinner of claim 11, wherein the metal alloy material comprises 0.01 wt% to 5.0 wt% tantalum.
13. The spinner of claim 11, wherein the metal alloy material comprises 0.1 wt% to 0.4 wt% zirconium.
14. The spinner of claim 11, wherein the metal alloy material comprises 0.01 wt% to 1.0 wt% hafnium.
15. The spinner of claim 1, wherein the metal alloy material comprises: chromium in an amount between 25.0% and 40.0% by weight; Nickel in an amount between 15.0 wt % and 25.0 wt %; Cobalt in an amount between 25.0 wt. % and 39.0 wt. %; Tungsten in an amount between 0.01 wt. % and 10.0 wt. %; Boron in an amount between 0.002 wt % and 0.05 wt %; carbon in an amount between 0.1 wt % and 1.0 wt %; Tantalum in an amount between 0.01 wt % and 5.0 wt %; zirconium in an amount between 0.1 wt % and 0.4 wt %; and Hafnium in an amount between 0.01 wt % and 1.0 wt %.
16. The method of claim 1, wherein the spinner has a total strain at least 50% less than the total strain (in / in) of an identical spinner made from the same metal alloy material by casting.
17. The spinner of claim 1, wherein the spinner has a minimum creep rate (×10 -4 ) (in / in / hr) is at least 50% lower than the minimum creep rate.
18. The spinner of claim 1, wherein the spinner has a corrosion penetration depth (μm) that is at least 20% lower than the corrosion penetration depth (μm) of an identical spinner made from the same metal alloy material by casting.
19. A method for manufacturing a component, the method include: depositing a metal alloy material onto a substrate; While depositing the metal alloy material, simultaneously applying a localized melting welding means to the metal alloy material; as well as sequentially depositing and welding the metal alloy material into a plurality of layers to form the component, The chromium-cobalt-nickel alloy material comprises: chromium in an amount between 25.0 wt % and 40.0 wt %; and Up to 75 wt. % nickel, cobalt or combinations thereof.
20. The method of claim 19, wherein the metal alloy material further comprises at least one of tungsten, boron, and carbon.
21. The method of claim 20, wherein the metal alloy material comprises 0.01 wt% to 10.0 wt% tungsten.
22. The method of claim 20, wherein the metal alloy material comprises 0.002 wt. % to 0.05 wt. % boron.
23. The method of claim 20, wherein the metal alloy material comprises 0.1 wt. % to 1.0 wt% carbon.
24. The method of claim 20, wherein the metal alloy material further comprises at least one of tantalum, zirconium, and hafnium.
25. The method of claim 24, wherein the metal alloy material comprises 0.01 wt% to 5.0 wt% tantalum.
26. The method of claim 24, wherein the metal alloy material comprises 0.1 wt.% to 0.4 wt. % zirconium.
27. The method of claim 24, wherein the metal alloy material comprises 0.01 wt% to 1.0 wt% hafnium.
28. The method of claim 19, wherein the localized fusion welding means is directed energy deposition or powder bed fusion.
29. The method of claim 28, wherein at least one of a power and a travel speed of a heat source is controlled to control a solidification rate of the metal alloy material.
30. The method of claim 19, wherein the component is a spinner used in making glass fibers.
31. The method of claim 30, wherein the spinner has a total strain at least 50% less than the total strain (in / in) of an identical spinner made from the same metal alloy material by casting.
32. The method of claim 30, wherein the spinner has a minimum creep rate (×10 -4 ) (in / in / hr) is at least 50% lower than the minimum creep rate.
33. The method of claim 30, wherein the spinner has a corrosion penetration depth (μm) that is at least 20% less than the corrosion penetration depth (μm) of an identical spinner made from the same metal alloy material by casting.
34. The method of claim 30, wherein the spinner comprises a body having an upper wall, a lower wall, and a side wall extending between the upper wall and the lower wall, the upper wall having an opening therethrough, the side wall comprising a plurality of holes.