Resin composition, method for producing same, and cured product of resin composition

By controlling the reaction of the polymaleimide resin with 1,2,4-trimethylbenzene in an organic solvent, the side reaction problem in its manufacturing was solved, and a resin combination with small dispersion and excellent dielectric properties was obtained. used to improve the performance of printed circuit boards and semiconductor materials.

CN119072518APending Publication Date: 2024-12-03RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035613.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-05
Filing Date
2023-10-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Polymaleimide resins are prone to side reactions during the manufacturing process, resulting in high dispersion and making it difficult to obtain excellent dielectric properties.

Method used

By using 1,2,4-trimethylbenzene as a solvent in an organic solvent, the reaction conditions of tetracarboxylic dianhydride and polyamine are controlled, side reactions are suppressed, and a polymaleimide resin with low dispersion is obtained, and Reacting with maleic anhydride to form a resin composition with excellent dielectric properties.

Benefits of technology

The side reaction of the polymaleimide resin is effectively suppressed, and a resin composition with low dispersion and excellent dielectric properties and its cured products are obtained, which are suitable for printed circuit boards and semiconductor materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005095835120000021
    Figure BDA0005095835120000021
  • Figure BDA0005095835120000031
    Figure BDA0005095835120000031
  • Figure BDA0005095835120000061
    Figure BDA0005095835120000061
Patent Text Reader

Abstract

Disclosed is a method for producing a resin composition. This method for producing a resin composition comprises: a step for obtaining a polyimide resin by reacting a tetracarboxylic acid dianhydride and a polyamine in an organic solvent; and reacting maleic anhydride with the polyimide resin to obtain a resin composition containing the polymaleimide resin and the organic solvent. The polyamine comprises a dimer diamine. The organic solvent contains 1, 2, 4-trimethylbenzene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a method for producing the same, and a cured product of the resin composition. Background Art

[0002] Printed wiring boards and multilayer wiring boards using the same are used in mobile communication devices such as mobile phones and smart phones, and their base station devices; network-related electronic devices such as servers / routers; and large computers.

[0003] In recent years, high-frequency electrical signals have been used in these products for high-speed transmission / processing of large amounts of information. However, high-frequency signals are very susceptible to attenuation, so in order to suppress transmission loss, insulating materials with excellent dielectric properties are required as insulating materials used in the above-mentioned printed wiring boards and multilayer wiring boards.

[0004] As such insulating materials, epoxy resin compositions disclosed in Patent Documents 1 to 3 are known in the past. Patent Document 1 discloses that an epoxy resin composition containing an epoxy resin, an active ester compound, and a triazine-containing cresol novolac resin is effective for reducing dielectric loss tangent. Furthermore, Patent Documents 2 and 3 disclose that a resin composition containing an epoxy resin and an active ester compound as essential components can form a cured product with a low dielectric loss tangent, and is useful as an insulating material.

[0005] On the other hand, Patent Document 4 reports that a resin film composed of a resin composition containing a polymaleimide resin having a long-chain alkyl group and a curing agent as a non-epoxy insulating material has excellent dielectric properties (low relative dielectric constant and low dielectric loss tangent).

[0006] Previous technical literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2011-132507

[0009] Patent Document 2: Japanese Patent Application Publication No. 2015-101626

[0010] Patent Document 3: Japanese Patent Application Publication No. 2017-210527

[0011] Patent Document 4: Japanese Patent Application Publication No. 2018-201024 Summary of the invention

[0012] Technical issues to be solved by the invention

[0013] Polymaleimide resin is usually prepared by reacting tetracarboxylic dianhydride and polyamine to obtain polyimide resin, and then reacting the obtained polyimide resin with maleic anhydride. However, the present inventors have studied polymaleimide resin in particular and found that it is difficult to obtain a polymaleimide resin with a small dispersion due to side reactions.

[0014] Therefore, a main object of the present invention is to provide a method for producing a resin composition capable of suppressing side reactions in the production of a polymaleimide resin.

[0015] Means for solving technical problems

[0016] The inventors of the present invention have conducted in-depth research to solve the above-mentioned problems, and as a result, have found that the use of 1,2,4-trimethylbenzene can suppress side reactions and easily obtain a polymaleimide resin with a small degree of dispersion, thereby completing the invention of the present invention. According to the research of the inventors, it has also been found that the polymaleimide resin obtained in this way has a tendency to be easily dissolved in 1,2,4-trimethylbenzene.

[0017] The present invention provides a method for producing the resin composition described in [1] to [4], the resin composition described in [5] and [6], and a cured product of the resin composition described in [7].

[0018] [1] A method for producing a resin composition, comprising the steps of: reacting tetracarboxylic dianhydride and polyamine in an organic solvent to obtain a polyimide resin; and reacting maleic anhydride with the polyimide resin to obtain a resin composition containing the polymaleimide resin and the organic solvent, wherein the polyamine contains dimer diamine and the organic solvent contains 1,2,4-trimethylbenzene.

[0019] [2] The method for producing a resin composition according to [1], wherein

[0020] The dimer diamine is at least one selected from the group consisting of a compound represented by the following general formula (1) and a compound represented by the following general formula (2).

[0021]

[0022]

[0023] [In formulas (1) and (2), m, n, p, and q each independently represent an integer greater than 1. Among them, m and n are integers satisfying the condition of m+n=6 to 17, and p and q are integers satisfying the condition of p+q=8 to 19. The bond represented by the dotted line represents a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by the dotted line is a carbon-carbon double bond, formulas (1) and (2) are structures obtained by subtracting 1 from the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond from the number represented by formulas (1) and (2).]

[0024] [3] The method for producing a resin composition according to [1] or [2], wherein:

[0025] The blending amount of the dimer diamine is 20 mol% or more based on the total amount of the polyamine.

[0026] [4] The method for producing a resin composition according to any one of [1] to [3], wherein

[0027] The weight average molecular weight of the polymaleimide resin is 3,000 to 40,000.

[0028] [5] A resin composition comprising a polymaleimide resin which is a reaction product of tetracarboxylic dianhydride, a polyamine, and maleic anhydride; and an organic solvent, wherein the polyamine comprises a dimer diamine; and the organic solvent comprises 1,2,4-trimethylbenzene.

[0029] [6] The resin composition according to [5], further comprising a polymerization initiator, wherein the polymerization initiator comprises a thermal polymerization initiator or a photopolymerization initiator.

[0030] [7] A cured product, which is a cured product of the resin composition according to [5] or [6].

[0031] Effects of the Invention

[0032] According to the present invention, there is provided a method for producing a resin composition capable of suppressing side reactions in the production of a polymaleimide resin, and also according to the present invention, there is provided a resin composition obtained by the production method and a cured product thereof. DETAILED DESCRIPTION

[0033] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.

[0034] In this specification, the numerical range represented by "~" indicates a range including the numerical values ​​recorded before and after "~" as the minimum value and the maximum value, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of any stage can also be replaced by the upper limit or lower limit of the numerical range of other stages. Moreover, in the numerical range recorded in this specification, the upper limit or lower limit of its numerical range can be replaced by the value shown in the embodiment. Moreover, the upper limit and lower limit recorded individually can be combined arbitrarily. In the expression of the numerical range "A~B" and the like, the numerical values ​​A and B at both ends are included in the numerical range as the lower limit and the upper limit, respectively. In this specification, for example, the description of "more than 10" refers to "10" and "a numerical value exceeding 10", and this is used as a reference even if the numerical values ​​are different. Moreover, for example, the description of "less than 10" refers to "10" and "a numerical value less than 10", and this is used as a reference even if the numerical values ​​are different.

[0035] In the present specification, the "polymaleimide resin" refers to a polyfunctional maleimide resin having two or more maleimide groups.

[0036] In this specification, "polyamine" refers to a polyfunctional amine having two or more amino groups.

[0037] In this specification, "(meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl" and "(meth)acrylic acid". In addition, "A or B" may include either A or B, or both.

[0038] Unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more. The amount of each component in the method for producing the composition, the content of each component in the composition, etc., when there are multiple substances corresponding to each component, refer to the total amount of the multiple substances unless otherwise specified.

[0039] [Method for producing resin composition]

[0040] The method for producing the resin composition of the present embodiment includes the following steps: a step of reacting tetracarboxylic dianhydride (hereinafter, sometimes referred to as "(a1) component", etc.) and polyamine (hereinafter, sometimes referred to as "(a2) component", etc.) in an organic solvent (hereinafter, sometimes referred to as "(B) component", etc.) to obtain a polyimide resin (hereinafter, sometimes referred to as "first step", etc.); and a step of reacting maleic anhydride (hereinafter, sometimes referred to as "(a3) component", etc.) with a polyimide resin to obtain a resin composition containing a polymaleimide resin (hereinafter, sometimes referred to as "(A) component", etc.) and (B) component (hereinafter, sometimes referred to as "second step", etc.). The first step may be a step of performing an imidization reaction of the components (a1) and (a2), and the second step may be a step of performing a maleimidization reaction of the reaction product of the components (a1) and (a2) with the component (a3). (A) Component can also be called a reaction product of (a1) component, (a2) component, and (a3) ​​component.

[0041] <1st step>

[0042] This step is a step of obtaining a polyimide resin by reacting the components (a1) and (a2) in the component (B).

[0043] Examples of the component (a1) include pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione, 4,4'-oxydiphthalic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3' , 4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenyl ketone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidene diphenyloxy) diphthalic anhydride, 1,2,3,4-butanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride , bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, bis(1,3-dioxo-1,3-dihydroxyisobenzofuran-5-carboxylic acid)1,4-phenylene, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 4,4'-(ethynyl-1,2-diyl)diphthalic anhydride, 5-(2,5-dioxotetrahydrofuran)-3-methyl-3-cyclohexene-1,2- dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, 3,4'-oxydiphthalic anhydride, 3,4'-diphthalic anhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic acid-5,5',6,6'-dianhydride, etc.

[0044] From the viewpoint of excellent dielectric properties or high Tg (glass transition point), the component (a1) may contain an anhydride selected from the group consisting of pyromellitic anhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-c]furan-1,3-dione, 3,3',4,4'-biphenyltetracarboxylic anhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic anhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride, 5-(2,5-dioxotetrahydrofuran)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3 , 4,3',4'-tetracarboxylic dianhydride, 3,4'-diphthalic anhydride, and 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic acid-5,5',6,6'-dianhydride. It may also contain at least one selected from the group consisting of pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione, 3,3',4,4'-biphenyltetracarboxylic anhydride, and 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride. It may also contain pyromellitic dianhydride.

[0045] The component (a2) may contain a diamine (hereinafter, sometimes referred to as "component (a2-1)" etc.). The component (a2) may contain a triamine (hereinafter, sometimes referred to as "component (a2-2)" etc.) in addition to the component (a2-1).

[0046] Examples of the component (a2-1) include dimer diamine, 1,3-diaminopropane, norbornane diamine, 4,4-methylenedianiline, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene. , 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, 4,4'-(hexafluoroisopropylidene)diphenylamine, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.02,6]decane, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), 1,1-bis( 4-aminophenyl)cyclohexane, 2,7-diaminofluorene, 4,4'-ethylenediphenylamine, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2-ethyl-6-methylaniline), 2,2-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]methane, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, [4-(3-aminophenoxy)phenyl]ketone, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethylbiphenyl-4,4'-diamine, (4,4'-diamino)diphenyl ether, (3,3'-diamino)diphenyl ether, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, 2,2'-dimethylbiphenyl-4,4'-diamine, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, and the like.

[0047] The component (a2) may contain a dimer diamine as the component (a2-1). Here, the dimer diamine is, for example, a compound derived from a dimer acid which is a dimer of an unsaturated fatty acid such as oleic acid. The dimer diamine may be any known dimer diamine without particular limitation, but may be, for example, at least one selected from the group consisting of a compound represented by the following general formula (1) and a compound represented by the following general formula (2).

[0048]

[0049]

[0050] In formula (1) and formula (2), m, n, p, and q each independently represent an integer greater than 1, and may be an integer from 1 to 12. Among them, m and n are integers satisfying the condition of m+n=6 to 17, p and q are integers satisfying the condition of p+q=8 to 19, and the bond represented by the dotted line represents a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by the dotted line is a carbon-carbon double bond, formula (1) and formula (2) are structures obtained by subtracting 1 from the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond from the number represented by formula (1) and formula (2).

[0051] From the viewpoint of heat resistance, high Tg, dielectric properties, etc., the dimer diamine may be a compound represented by the general formula (1) or a compound represented by the following formula (3).

[0052]

[0053] Examples of commercially available dimer diamines include PRIAMINE 1075 and PRIAMINE 1074 (both manufactured by Croda Japan KK, and containing a mixture of a compound represented by the general formula (1) and a compound represented by the general formula (2)).

[0054] The blending amount of the component (a2-1) may be 20 to 100 mol %, 40 to 100 mol %, 60 to 100 mol %, or 80 to 100 mol %, based on the total amount of the component (a2).

[0055] The amount of the dimer diamine may be 20 mol% or more, 40 mol% or more, or 60 mol% or more, or 95 mol% or less, 90 mol% or less, or 80 mol% or less, based on the total amount of the component (a2). If the content of the dimer diamine is within this range, the dielectric properties of the cured product of the obtained resin composition tend to be more excellent.

[0056] Examples of the component (2-2) include tris(2-aminomethyl)amine, tris(2-aminoethyl)amine, tris(2-aminopropyl)amine, 2-(aminomethyl)-2-methyl-1,3-propylenediamine, trimertriamine, 3,4,4'-triaminodiphenyl ether, 1,2,4-triaminobenzene, 1,3,5-triaminobenzene, 1,2,3-triaminobenzene, 1,3,5-triazine-2,4,6-triamine, 2,4,6-triaminopyrimidine, 1,3,5-tris(4-aminophenyl)benzene, and 1,3,5-tris(4-aminophenoxy)benzene. Among these, the component (a2) may contain an aliphatic triamine as the component (a2-2) from the viewpoint of solubility of the component (A) in an organic solvent, and may contain tris(2-aminomethyl)amine or tris(2-aminoethyl)amine as the component (a2-2) from the viewpoint of increasing Tg.

[0057] The blending amount of the component (a2-2) may be 0 to 80 mol%, 0 to 60 mol%, 0 to 40 mol%, or 0 to 20 mol%, based on the total amount of the component (a2).

[0058] By using dimer diamine as component (a2), there is a tendency that the dielectric properties of the cured product of the obtained resin composition are more excellent. On the other hand, when only dimer diamine is used as component (a2), the Tg of the cured product of the resin composition is sometimes reduced. In contrast, by using diamines other than triamines or dimer diamines simultaneously, the Tg of the cured product can be increased while the dielectric properties of the cured product are maintained.

[0059] In the method for manufacturing a resin composition, the molecular weight of the component (A) finally obtained can be controlled by the mixing ratio of the component (a1) and the component (a2). The mixing amount of the component (a1) can be 0.30 to 0.95 mol, or 0.40 to 0.85 mol or 0.50 to 0.80 mol relative to 1.0 mol of the component (a2). If the mixing amount of the component (a1) is less than 0.95 mol, there is a tendency to increase the maleimide groups that can be introduced by the reaction, and there is a tendency to obtain an easily cured component (A) when heated with a thermal polymerization initiator or irradiated with active energy rays. In addition, if the ratio of the component (a1) is above 0.30, the low molecular weight component can be reduced, and there is a tendency to easily obtain a component (A) with good heat resistance.

[0060] The (B) component contains 1,2,4-trimethylbenzene (1,2,4-trimethylbenzene, boiling point: 169°C) (hereinafter, sometimes referred to as "(b1) component", etc.). The (b1) component tends to be easily dissolved in the (a3) ​​component used in the second step. According to the research of the present inventors, it was found that there is a tendency that the (A) component with a small dispersion degree is easily obtained by suppressing the side reaction by using the (b1) component. According to further research by the present inventors, it was also found that the (A) component obtained in this way tends to be easily dissolved in the (b1) component.

[0061] The amount of the component (a3) ​​dissolved in the component (b1) at 25°C may be, for example, 10 g or more relative to 100 g of the component (b1). If the amount of the component (a3) ​​dissolved in the component (b1) is 10 g or more relative to 100 g of the component (b1), side reactions are suppressed and the component (A) with a small degree of dispersion is easily obtained. The amount of the component (a3) ​​dissolved in the component (b1) at 25°C may be measured, for example, by the method described in the examples below.

[0062] In order to dissolve the (a1) component by esterification in the imidization reaction in the first step, the (B) component may contain alcohols (hereinafter, sometimes referred to as "(b2) component", etc.). As long as the (b2) component is a known alcohol, it can be used without particular limitation. As the (b2) component, for example, methanol, ethanol, 1-propanol, isopropanol, 1-butanol, benzyl alcohol, etc. can be cited. Among these, methanol or ethanol can be contained from the viewpoint of the ease of separation during the imide ring closure. Here, the ease of hydrolysis of the ester generally depends on the number of carbon atoms (boiling point) of the alcohol. The lower the boiling point of the alcohol, the higher the ability to separate, and it has a tendency to easily separate during the imide ring closure. By using the (b2) component, the dehydration ring-closure reaction in the first step can be further promoted, and the reaction can be carried out uniformly, and the (A) component with high molecular weight and small dispersion can be effectively manufactured.

[0063] The usage of (b2) component is not particularly limited, but from the viewpoint of promoting the dehydration ring-closure reaction in the first step and more fully obtaining the effect of making the reaction uniform, it can be more than 2 mol relative to 1 mol of (a1) component, or 2 to 16 mol. In addition, when (b2) component is used simultaneously with (b1) component, from the same viewpoint as above, based on the total amount of (B) component, the usage of (b2) component can be 0.1 to 40% by mass, or 5 to 25% by mass. In other words, when (b2) component is used simultaneously with (b1) component, based on the total amount of (B) component, the usage of (b1) component can be 60 to 99.9% by mass, or 75 to 95% by mass.

[0064] The amount of component (B) used is not particularly limited as long as it is an amount that can dissolve the synthesized component (A), but from the viewpoint of optimizing the viscosity and promoting the dehydration ring-closure reaction, it can be an amount that allows the total concentration of components other than component (B) in the reaction solution formed by mixing component (a1), component (a2), component (B), etc. to be 10 to 70% by mass, or it can be an amount that allows the total concentration to be 20 to 60% by mass.

[0065] In the first step, first, the components (a1) and (a2) are subjected to a re-addition reaction in the component (B) at a temperature of about 60 to 120° C. (preferably 70 to 90° C.) for usually about 0.1 to 2 hours (preferably 0.1 to 1.0 hours). Then, the obtained re-addition product is further subjected to an imidization reaction, i.e., a dehydration ring-closure reaction, at a temperature of about 80 to 250° C. (preferably 100 to 200° C.) for about 0.5 to 30 hours (preferably 0.5 to 10 hours). That is, by conducting a dehydration ring-closure reaction, a polyimide resin as an intermediate can be obtained. The re-addition reaction and the imidization reaction can be carried out under any condition of atmospheric pressure (normal pressure), reduced pressure, or pressurized pressure. The pressure conditions of the re-addition reaction and the imidization reaction can be, for example, normal pressure (0.00 MPa) to reduced pressure (-0.04 MPa). Furthermore, if necessary, the component (b2) and the generated water may be removed and a re-addition reaction and an imidization reaction may be performed.

[0066] <Step 2>

[0067] This step is a step of reacting the component (a3) ​​(maleic anhydride) with the polyimide resin to obtain a resin composition containing the components (A) and (B).

[0068] The component (a3) ​​is added in order to react with the polyimide resin in the second reaction step after the polyimide resin as an intermediate is synthesized in the first reaction step. The amount of the component (a3) ​​added can be 1.0 to 3.0 mol, or 1.3 to 2.0 mol relative to 1 mol of the amino group of the polyimide resin. If the amount of the component (a3) ​​added is 1.0 mol or more relative to 1 mol of the amino group of the polyimide resin, the side reaction can be further suppressed, and there is a tendency to improve the heat resistance of the obtained component (A). If the amount of the component (a3) ​​added is 3.0 mol or less relative to 1 mol of the amino group of the polyimide resin, there is a tendency to make it easier to purify the component (A).

[0069] In addition, the amino group (mol) of the polyimide resin can be calculated according to the following formula (X), for example, when the component (a2) is composed of the component (a2-1) (divalent diamine).

[0070] Amino group of polyimide resin (mol) = mole number of component (a2) × 2 - mole number of component (a1) × 2 (X)

[0071] When adding (a3) ​​component to polyimide resin, the addition rate of (a3) ​​component can be 0.25 mol / min or more relative to 1 mol of amino group of polyimide resin, or can be 0.3 mol / min or more, 0.5 mol / min or more, 0.7 mol / min or more, 1.0 mol / min or more, 1.2 mol / min or more, 1.5 mol / min or more, 1.7 mol / min or more, 2.0 mol / min or more, 2.2 mol / min or more, or 2.5 mol / min or more. If the addition rate of (a3) ​​component is sufficiently fast when adding to polyimide resin, the side reaction is suppressed, and there is a tendency to easily obtain (A) component with small dispersion. The addition rate of (a3) ​​component can be, for example, 9.0 mol / min or less, 8.0 mol / min or less, 7.0 mol / min or less, 6.0 mol / min or less, or 5.0 mol / min or less relative to 1 mol of amino group of polyimide resin. When adding the component (a3) ​​to the polyimide resin, the addition rate of the component (a3) ​​may be, for example, 1 mol or more (eg, 1.5 mol) of the component (a3) ​​per 1 mol of amino groups in the polyimide resin.

[0072] In the second step, component (a3) ​​is added to the polyimide resin obtained in the first step, and the polyimide resin and component (a3) ​​are subjected to a maleimide reaction, i.e., a dehydration ring-closure reaction, at a temperature of about 60 to 250° C. (preferably 80 to 200° C.) for about 0.5 to 30 hours (preferably 0.5 to 10 hours), thereby obtaining a resin composition containing component (A) and component (B) as the target. The maleimide reaction can be carried out under any of atmospheric pressure (normal pressure), reduced pressure, or pressurized conditions. The pressure conditions of the maleimide reaction can be, for example, normal pressure (0.00 MPa) to reduced pressure (-0.04 MPa). In addition, as needed, component (b2) and the generated water can be removed and the maleimide reaction can be carried out.

[0073] In the first step and the second step, various known reaction catalysts and dehydrating agents can be used. Examples of the reaction catalyst include aliphatic tertiary amines such as triethylamine, aromatic tertiary amines such as dimethylaniline, heterocyclic tertiary amines such as pyridine, picoline, and isoquinoline, methanesulfonic acid, p-toluenesulfonic acid monohydrate, and organic acids such as trifluoromethanesulfonic acid. Examples of the dehydrating agent include aliphatic acid anhydrides such as acetic anhydride, and aromatic acid anhydrides such as benzoic anhydride.

[0074] The obtained resin composition can be purified by various known methods. By purifying the obtained resin composition, the purity of the (A) component in the resin composition can be improved. As an example of the purification of the resin composition, for example, a method using a separatory funnel can be cited. In this method, first, the resin composition and water are placed in a separatory funnel, and the mixed solution in the separatory funnel is shaken. Then, the water layer and the organic layer are separated, and the organic layer is recovered, thereby being able to remove the (b2) component while improving the purity of the (A) component.

[0075] In this manner, a resin composition containing the components (A) and (B) which are reaction products of the components (a1), (a2), and (a3) ​​can be obtained.

[0076] Hereinafter, an example of the component (A) obtained by the above-mentioned manufacturing method is described. The component (A) may be, for example, a polymaleimide resin represented by the following general formula (4) or a polymaleimide resin represented by the following general formula (5). In one embodiment, the polymaleimide resin represented by the general formula (4) and the polymaleimide resin represented by the general formula (5) may be a bismaleimide resin.

[0077]

[0078] In formula (4), R A represents a tetravalent organic group. B represents a divalent organic group which may have a maleimide group. A Represents an integer from 0 to 100. A When it is greater than 1, there are multiple R A They can be the same or different. There are multiple R B They may be the same or different from each other. A It can be an integer from 1 to 30.

[0079] R A It may be a tetravalent organic group having a substituted or unsubstituted aliphatic hydrocarbon group, a substituted or unsubstituted heteroaliphatic hydrocarbon group, a substituted or unsubstituted aromatic hydrocarbon group, or a substituted or unsubstituted heteroaromatic hydrocarbon group. The aliphatic hydrocarbon group may be an alicyclic hydrocarbon group. The tetravalent organic group may be an organic group having 4 to 30 carbon atoms. 1The tetravalent organic group represented by may include, for example, a group formed by removing four hydrogen atoms from aromatic hydrocarbons (aryl groups) such as benzene, naphthalene, perylene, and biphenyl; compounds having an aromatic hydrocarbon group such as diphenyl ether, diphenyl sulfone, diphenyl propane, diphenyl hexafluoropropane, and benzophenone; heteroaromatic hydrocarbons such as pyrrole, furan, thiophene, oxazole, thiazole, pyridine, pyrimidine, quinoline, coumarin, indole, benzofuran, acridine, phenoxazine, and carbazole; compounds having a heteroaromatic hydrocarbon group such as dipyridine disulfide; aliphatic hydrocarbons (alkanes) such as butane, cyclobutane, and cyclopentane; and heteroaliphatic hydrocarbons such as piperidine, piperazine, morpholine, and pyrrolidine. The compound having an aromatic hydrocarbon group may be a group formed by removing four hydrogen atoms from an aromatic hydrocarbon. From the viewpoint of improving the heat resistance of the obtained bismaleimide resin and easy availability, R 1 The tetravalent organic group represented may be a group obtained by removing four hydrogen atoms from an aromatic hydrocarbon, or may be a group obtained by removing four hydrogen atoms from benzene or biphenyl.

[0080] R B It may be a divalent organic group having a substituted or unsubstituted aliphatic hydrocarbon group, a substituted or unsubstituted heteroaliphatic hydrocarbon group, a substituted or unsubstituted aromatic hydrocarbon group, or a substituted or unsubstituted heteroaromatic hydrocarbon group. Here, the divalent organic group may be an organic group having 4 to 100 carbon atoms, or an organic group having 4 to 60 carbon atoms. B It is a residue of the component (a2) (polyamine such as diamine and triamine). The residue of the component (a2) may include a residue of a dimer diamine.

[0081] When the polymaleimide resin represented by the general formula (4) is a bismaleimide resin having two maleimide groups, R B When the polymaleimide resin represented by the general formula (4) is a polymaleimide resin having three or more maleimide groups, R B At least a part of the hydrogen atoms of the divalent organic group is substituted with a maleimide group, and is a divalent organic group having a maleimide group.

[0082]

[0083] In formula (5), R B and n A The meaning is the same as above R B and n A have the same meaning.

[0084] From the viewpoint of solubility in solvent and heat resistance, the weight average molecular weight (Mw) of component (A) may be 3000 to 40000, 6000 to 25000 or 9000 to 20000. If the Mw of component (A) is 40000 or less, the solubility in component (B) tends to be good. If the Mw of component (A) is 3000 or more, the effect of improving heat resistance tends to be fully obtained.

[0085] From the viewpoint of solubility in solvents and heat resistance, the number average molecular weight (Mn) of component (A) may be 1000 to 12000, 2000 to 8000, or 4000 to 6000. If the Mn of component (A) is 12000 or less, the solubility in component (B) tends to be good. If the Mn of component (A) is 1000 or more, the effect of improving heat resistance tends to be sufficiently obtained.

[0086] In this specification, Mw and Mn of the component (A) refer to polystyrene-equivalent values ​​using a calibration curve based on standard polystyrene in gel permeation chromatography (GPC).

[0087] The dispersity (Mw / Mn) of the (A) component may be, for example, less than 3.5, or less than 3.3, less than 3.2, less than 3.1, less than 3.0, less than 2.9, less than 2.8, less than 2.7, less than 2.6, or less than 2.5. According to the method for manufacturing the resin composition of the present embodiment, the side reaction can be suppressed, so there is a tendency that the dispersity of the (A) component becomes smaller. In addition, if the dispersity of the (A) component is less than 3.5, there is a tendency that the solubility of the (B) component in the (B) component becomes good. The dispersity of the (A) component may be, for example, more than 1.0, more than 1.5, or more than 2.0.

[0088] The component (A) can be cured by heating and / or irradiation with active energy rays.

[0089] The component (A) is cured by heating at a temperature of usually about 150 to 250° C. (preferably 180 to 220° C.) for usually about 0.1 to 3 hours (preferably 0.1 to 1.5 hours).

[0090] When the component (A) is cured by irradiation with active energy rays, examples of the active energy rays include visible light, ultraviolet rays, X-rays, electron beams, and the like. Since inexpensive devices can be used for the active energy rays, ultraviolet rays may be used. When ultraviolet rays are used, light sources include ultrahigh pressure, high pressure, medium pressure, or low pressure mercury lamps; metal halide lamps; xenon lamps; electrodeless discharge lamps; carbon arc lamps, and the like. The irradiation with active energy rays may be from several seconds to several minutes.

[0091] [Resin composition]

[0092] The resin composition of the present embodiment contains component (A) and component (B) which are reaction products of component (a1), component (a2), and component (a3). The resin composition can be obtained by the above-mentioned manufacturing method. In addition, the resin composition can also be obtained by separating component (A) from the resin composition obtained by the above-mentioned manufacturing method, and mixing the separated component (A) and component (B).

[0093] The content of the component (A) in the resin composition may be 10 to 70% by mass, or 20 to 60% by mass, based on the total amount of the resin composition. The content of the component (A) can be adjusted by increasing or decreasing the amount of the component (B) (mainly the component (b1)).

[0094] In the resin composition, the main component of the component (B) may be the component (b1). The content of the component (b1) may be 70% by mass or more, 80% by mass or more, 90% by mass or more, or 95% by mass or more based on the total amount of the component (B).

[0095] The resin composition may further contain a polymerization initiator (hereinafter, sometimes referred to as "component (C)" etc.). Component (C) may contain a thermal polymerization initiator (hereinafter, sometimes referred to as "component (c1)" etc.) or a photopolymerization initiator (hereinafter, sometimes referred to as "component (c2)" etc.).

[0096] Examples of the component (c1) include organic peroxides, imidazole compounds, phosphine compounds, and phosphonium salt compounds. Among these, the component (c1) may be an organic peroxide or an imidazole compound from the viewpoint of functioning as a polymerization initiator and excellent dielectric properties.

[0097] Examples of the organic peroxide include methyl ethyl ketone peroxide, methyl cyclohexanone peroxide, methyl acetoacetate peroxide, acetylacetone peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(4,4-dimethylperoxy)cyclohexane, -tert-butylperoxycyclohexyl) propane, 1,1-bis(tert-butylperoxy)cyclododecane, n-butyl-4,4-bis(tert-butylperoxy)valerate, 2,2-bis(tert-butylperoxy)butane, 1,1-bis(tert-butylperoxy)-2-methylcyclohexane, tert-butyl hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, tert-hexyl hydroperoxide, diisophenylpropyl peroxide (Dicumyl peroxide), 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, α,α'-bis(tert-butylperoxy)diisopropylbenzene, tert-butylisophenylpropyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane-3, isobutyryl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, cinnamic acid peroxide, m-toluoyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, α,α'-bis(neodecanoyl) peroxy) diisopropylbenzene, isophenylpropyl peroxyneodecanoate, 1,1,3,3,-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoyl peroxy)hexane, 1,1,3,3-tetramethylbutyl Peroxy-2-ethylhexanoate, 1-cyclohexyl-1-methylethyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxymaleic acid, tert-butyl peroxylaurate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, tert-butylperoxyacetate, tert-hexylperoxybenzoate, tert-butylperoxy-m-toluoylbenzoate, tert-butylperoxybenzoate, bis(tert-butylperoxy)isophthalate (Isophthalate), tert-butylperoxyallylmonocarbonate, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, etc. Among these, the organic peroxide may be diisophenylpropyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, or α,α'-bis(tert-butylperoxy)diisopropylbenzene. ,

[0098] Examples of the imidazole compound include 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2,4-dimethylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-vinyl-2-methylimidazole, 1-propyl-2-methylimidazole, 2-isopropylimidazole, 1-cyanomethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, and 1-cyanoethyl-2-phenylimidazole. Among these, the imidazole compound may be 1-cyanoethyl-2-phenylimidazole or 2-ethyl-4-methylimidazole.

[0099] As the phosphine compound, for example, primary phosphine, secondary phosphine, tertiary phosphine, etc. can be mentioned. As the primary phosphine, alkyl phosphine such as ethyl phosphine and propyl phosphine can be mentioned; phenyl phosphine, etc. can be mentioned. As the secondary phosphine, dialkyl phosphine such as dimethyl phosphine and diethyl phosphine can be mentioned; diphenyl phosphine, methyl phenyl phosphine; ethyl phenyl phosphine, etc. can be mentioned. As the tertiary phosphine, trialkyl phosphine such as trimethyl phosphine, triethyl phosphine, tributyl phosphine, trioctyl phosphine can be mentioned; tricyclohexyl phosphine; triphenyl phosphine; alkyl diphenyl phosphine; dialkyl phenyl phosphine; tribenzyl phosphine; tritolyl phosphine; tri-p-phenylphenyl phosphine; tri(2,6-dimethoxyphenyl)phosphine; tri-4-methylphenyl phosphine; tri-4-methoxyphenyl phosphine; tri-2-cyanoethyl phosphine, etc. can be mentioned. The phosphine compound can be a tertiary phosphine group.

[0100] Examples of the phosphonium salt compound include compounds having tetraphenylphosphonium salts, alkyltriphenylphosphonium salts, tetraalkylphosphonium salts, etc. Examples of the phosphonium salt compound include tetraphenylphosphonium-thiocyanate, tetraphenylphosphonium-tetra-p-methylphenyl borate, butyltriphenylphosphonium-thiocyanate, tetraphenylphosphonium-phthalic acid, tetrabutylphosphonium-1,2-cyclohexyldicarboxylic acid, tetrabutylphosphonium-1,2-cyclohexyldicarboxylic acid, tetrabutylphosphonium-lauric acid, etc.

[0101] Examples of the component (c2) include acetophenone, 2,2-dimethoxyacetophenone, p-dimethylaminoacetophenone, Michler's ketone, diphenylethylene, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, diphenylethylene dimethyl ketal, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{ 4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane-1-one, 2-methyl-1-(4-methylphenylthio)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyl oxime), ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime), 2,4-dimethylthioxanthone, and the like.

[0102] Among these, from the viewpoint of being able to form fine patterns using a reduced projection exposure machine (stepper, light source wavelength: 365 nm, 436 nm) used as standard in the manufacturing process of semiconductor protective films, etc., the component (c2) may be a photopolymerization initiator that efficiently generates free radicals at an exposure wavelength of 310 to 436 nm (more preferably 365 nm). From the viewpoint of reactivity, the component (c2) may be a compound having an oxime structure or a thioxanthone structure.

[0103] Examples of the compound having an oxime structure or a thioxanthone structure, i.e., component (c2), include 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(0-benzoyloxime) (manufactured by BASF JAPAN LTD., IRGACURE OXE-01), ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyloxime) (manufactured by BASF JAPAN LTD., IRGACURE OXE-02) having an oxime structure; and 2,4-dimethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., DETX-S) having a thioxanthone structure.

[0104] The content of the component (C) is not particularly limited, and may be 0.1 to 10 parts by mass, 0.5 to 5 parts by mass, or 0.7 to 3 parts by mass based on 100 parts by mass of the total amount of the component (A).

[0105] The resin composition may further contain other components other than component (A), component (B), and component (C). As other components, for example, additives such as release agents, flame retardants, ion traps, antioxidants, tackifiers, low stress agents, colorants, coupling agents, inorganic fillers, etc.; resins other than component (A) such as epoxy resins, acrylate compounds, vinyl compounds, benzoxazine compounds, bismaleimide compounds, etc. The content of other components is not particularly limited as long as it is within the range that does not impair the effect of the present invention, but it can be 0.1 to 30 parts by mass relative to 100 parts by mass of the total amount of component (A).

[0106] [Cured product of resin composition]

[0107] The cured product of the resin composition of the present embodiment can be obtained by curing the above-mentioned resin composition. More specifically, the cured product of the resin composition can be obtained by a method including the following steps: applying the resin composition on a substrate to obtain a coating film (coating); volatilizing the organic solvent from the coating film to obtain a dry film (dried product); and curing the dry film by heating and / or irradiation with active energy rays to obtain a cured film (cured product). The cured product of the resin composition of the present embodiment has a tendency to have a relatively small surface roughness.

[0108] The substrate may be an organic substrate or an inorganic substrate. As an organic substrate, for example, polyimide; polyimide-silicon dioxide mixture; polyamide; polyethylene (PE); polypropylene (PP); polyethylene terephthalate (PET); polyethylene naphthalate (PEN); polymethyl methacrylate resin (PMMA); polystyrene resin (PSt); polycarbonate resin (PC); acrylonitrile-butadiene-styrene resin (ABS); polyethylene terephthalate; aromatic polyester resin (liquid crystal polymer, Vexter (manufactured by KURARAY CO., LTD.), etc.) films obtained from phenolic acid, phthalic acid, hydroxynaphthoic acid, etc. and parahydroxybenzoic acid can be used. As an inorganic substrate, for example, glass; metals such as iron, aluminum, 42 alloy, copper; ITO; silicon; silicon carbide substrates, etc. can be cited. The thickness of the substrate can be appropriately set according to the purpose. When an organic substrate is used as the substrate, the thickness of the organic substrate can be, for example, 1 to 250 μm.

[0109] Examples of methods for applying the resin composition on a substrate include methods using a knife coater, roll coater, applicator, comma coater, die coater, etc. The thickness of the cured film (cured product) can be adjusted by adjusting the amount of the resin composition applied.

[0110] The heating conditions for volatilizing the organic solvent from the coating film can be appropriately set according to the organic solvent used, etc. The heating conditions may be, for example, a heating temperature of 40 to 150° C. and a heating time of 0.1 to 30 minutes.

[0111] The heating conditions or the irradiation conditions of the active energy rays for curing the dried film may be the same as the heating conditions or the irradiation conditions of the active energy rays for curing the above-mentioned component (A).

[0112] The shape of the cured film (cured product) of the resin composition is not particularly limited. When used for bonding a substrate, the film thickness of the cured film (cured product) can be set to a sheet shape of generally about 1 to 200 μm (preferably about 3 to 100 μm). The film thickness of the cured film (cured product) of the resin composition can be appropriately adjusted according to the application.

[0113] [Adhesive sheet]

[0114] The adhesive sheet of this embodiment comprises a substrate (first substrate) and a dry film formed by volatilizing an organic solvent from the above-mentioned resin composition. The substrate (first substrate) may be the same as the substrate exemplified in the cured product of the resin composition. The thickness of the dry film may be, for example, 1 to 200 μm, or 3 to 100 μm.

[0115] [Laminated body]

[0116] The laminate of the present embodiment can be obtained by further thermocompression bonding a substrate (second substrate) to the adhesive surface (surface of the dry film) of the above-mentioned adhesive sheet. The substrate (second substrate) can be the same as the substrate exemplified in the cured product of the resin composition. The laminate of the present embodiment can be cured under heating conditions or irradiation conditions of active energy rays for curing the above-mentioned dry film.

[0117] [Printed circuit boards and printed wiring boards]

[0118] The printed substrate of the present embodiment can use the above-mentioned adhesive sheet or use the above-mentioned laminate. The printed substrate of the present embodiment can be obtained, for example, by further laminating the adhesive surface (the surface of the dry film) of the above-mentioned adhesive sheet on the inorganic substrate surface of the above-mentioned laminate. The printed substrate can be a polyimide film used as an organic substrate and a metal foil (especially copper foil) used as an inorganic substrate. By using such a printed substrate, the metal surface of the printed substrate can be soft-etched to form a circuit, and a printed circuit board can be obtained by further laminating the above-mentioned adhesive sheet on the circuit and performing hot pressing.

[0119] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples.

[0120] [Manufacturing of resin composition]

[0121] (Example 1-1)

[0122] Into a 1L flask container equipped with a cooler, a nitrogen inlet pipe, a thermocouple, a stirrer, and a vacuum pump, 54.68 parts by mass of pyromellitic dianhydride (manufactured by Daicel Corporation), 432.92 parts by mass of 1,2,4-trimethylbenzene (manufactured by Toyo Gosei Co., Ltd.), and 94.78 parts by mass of Solmix A-11 (product name, manufactured by JAPAN ALCOHOL TRADING COMPANY LIMITED, an alcoholic solvent with ethanol as the main component) were added. After the addition, the temperature was raised to 80°C and kept for 0.5 hours, and 179.46 parts by mass of dimer diamine (product name: PRIAMINE1075, manufactured by Croda Japan KK) was added dropwise. After the addition, the temperature was kept at 80°C for 0.5 hours, and then 6.42 parts by mass of a methanesulfonic acid aqueous solution (70% aqueous solution, product name: Lutropur MSA, manufactured by BASF) was added. Thereafter, the pressure in the reaction vessel was reduced from atmospheric pressure to 0.03MPa (-0.03MPa), the alcohol solvent in the reaction solution was removed and the temperature was raised to 160°C. After heating, a dehydration ring-closure reaction was carried out at 160°C for 2 hours, water and alcohol solvent in the reaction solution were removed, and a solution of a polyimide resin containing an intermediate was obtained. Then, atmospheric pressure was reached in the reaction vessel, the solution containing the obtained polyimide resin was cooled to 130°C, and 24.58 parts by mass of maleic anhydride (manufactured by FUSO CHEMICAL CO., LTD.) was added at an addition rate of 2.9mol / min relative to 1mol of amino groups of the polyimide resin. Thereafter, the pressure in the reaction vessel was reduced from atmospheric pressure to 0.03MPa (-0.03MPa), and the temperature was raised to 160°C. After heating, a dehydration ring-closure reaction was carried out at 160°C for 4 hours, water in the reaction solution was removed, and a solution containing a polymaleimide resin was obtained.

[0123] The solution containing the obtained polymaleimide resin is added to a separatory funnel, 1200 parts by mass of pure water is added, the separatory funnel is shaken, and it is allowed to stand. After standing, the organic layer and the aqueous layer are separated, and only the organic layer is recovered. The recovered organic layer is put into a 1L glass container equipped with a cooler, a nitrogen inlet pipe, a thermocouple, a stirrer, and a vacuum pump, and the temperature is raised to 88-93°C and water is removed. Then, the temperature is raised to 100°C, and the solvent is partially removed for 0.5 hours under a state of reducing the pressure by 0.1MPa from the atmospheric pressure, and a resin composition of Example 1-1 containing a polymaleimide resin (A-1) and an organic solvent is obtained.

[0124] (Example 1-2)

[0125] A resin composition of Example 1-2 containing a polymaleimide resin (A-2) and an organic solvent was obtained in the same manner as in Example 1-1 except that the addition rate of maleic anhydride was changed to 0.5 mol / min relative to 1 mol of amino groups of the polyimide resin.

[0126] (Example 1-3)

[0127] The resin composition of Example 1-3 containing a polymaleimide resin (A-3) and an organic solvent was obtained in the same manner as in Example 1-1, except that pyromellitic dianhydride was changed to 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-C]furan-1,3-dione (product name: TDA-100, manufactured by New Japan Chemical Co., Ltd.), the amount of each component was changed as shown in Table 1, and the addition rate of maleic anhydride was changed to 0.5 mol / min relative to 1 mol of amino group of the polyimide resin.

[0128] (Comparative Example 1-1)

[0129] A resin composition of Comparative Example 1-1 containing a polymaleimide resin (a-1) and an organic solvent was obtained in the same manner as in Example 1-1, except that 1,2,4-trimethylbenzene was replaced with 1,2,3,4-tetrahydronaphthalene (tetrahydronaphthalene, manufactured by FUJIFILM Wako Pure Chemical Corporation) and the pressure conditions in the reaction container were changed to those shown in Table 1.

[0130] (Comparative Example 1-2)

[0131] The production of the resin composition was investigated in the same manner as in Example 1-1 except that 1,2,4-trimethylbenzene was replaced with cyclohexanone (manufactured by FUJIFILM Wako Pure Chemical Corporation) and the pressure conditions in the reaction vessel were changed to those shown in Table 1. However, cyclohexanone participated in the reaction and a polymaleimide resin could not be obtained.

[0132] [Evaluation of organic solvents]

[0133] The organic solvents (1,2,4-trimethylbenzene, tetralin, and cyclohexanone) used in Examples and Comparative Examples were evaluated as follows.

[0134] <Amount of Maleic Anhydride Dissolved in Organic Solvent>

[0135] To a 20 mL spiral tube, 2 g of maleic anhydride, 10 g of each of 1,2,4-trimethylbenzene (Example 1-1 to Example 1-3), tetralin (Comparative Example 1-1), and cyclohexanone (Comparative Example 1-2) used in the examples and comparative examples were added, and mixed at a rotation speed of 70 revolutions / min at room temperature (25°C) for 4 hours using a mixing rotor. After mixing, the mixture was allowed to stand for more than 1 hour, and then 20 mg of the supernatant and 0.6 mL of deuterated chloroform were injected into an NMR tube to prepare a sample. A nuclear magnetic resonance apparatus (manufactured by Bruker Japan) was used to measure the sample at a frequency of 400 MHz and an integration number of 16 times. 1 H-NMR, based on the peak integration ratio of maleic anhydride and the organic solvent, the amount of maleic anhydride dissolved in 100 g of the organic solvent was calculated. The case where the amount of maleic anhydride dissolved relative to 100 g of the organic solvent was 10 g or more was regarded as excellent in the amount of maleic anhydride dissolved in the organic solvent and was evaluated as "A", and the case where it was less than 10 g was evaluated as "C".

[0136] [Evaluation of resin composition]

[0137] The following evaluations were performed on the resin compositions of Examples and Comparative Examples.

[0138] <Ratio of non-volatile matter (NV)>

[0139] 0.75 g ± 0.25 g of the resin composition was weighed in a metal petri dish using a precision balance. The mixture was then dried at 150° C. for 0.5 hours using a hot air dryer, and the ratio of the nonvolatile component (NV) was calculated using the following formula. The results are shown in Table 1.

[0140] NV (mass %) = {(W3-W1) / W2} × 100

[0141] W1: Mass of the empty metal petri dish (g)

[0142] W2: Mass of the resin composition before drying (g)

[0143] W3: Total mass of the dried resin composition and the metal petri dish (g)

[0144] <Weight average molecular weight (Mw), number average molecular weight (Mn), and dispersion degree (Mw / Mn)>

[0145] The Mw and Mn of the polymaleimide resin were measured by GPC (gel permeation chromatography). A 50 μL sample was injected into a column heated to 30°C (GL-R420×1 root, GL-R430×1 root, GL-R440×1 root (all made by Hitachi High-Tech Fielding Corporation)). The sample was dissolved in tetrahydrofuran (THF) in a manner such that the concentration of the polymaleimide resin became 3% by mass. THF was used as a developing solvent and the flow rate was 1.6 mL / min. The Mw and Mn of the polymaleimide resin were converted according to the elution time using a molecular weight / elution time curve made using standard polystyrene (made by TOSOH CORPORATION). And, based on these, Mw / Mn was obtained. The results are shown in Table 1.

[0146]

[0147] As shown in Table 1, it is judged that in the manufacture of the resin composition of Example 1-1 to Example 1-3 using 1,2,4-trimethylbenzene, the obtained polymaleimide resin has a smaller dispersion than the resin composition of the comparative example in which the organic solvent of 1,2,4-trimethylbenzene is not used. As the reason why the dispersion of the polymaleimide resin is larger in the manufacture of the resin composition of Comparative Example 1-1, it can be inferred that it is because the dissolution amount of maleic anhydride in tetralin is low and the side reaction is carried out to form a high molecular weight. As described above, it is confirmed that the manufacturing method of the resin composition of the present invention can suppress the side reaction.

[0148] [Preparation of resin composition]

[0149] (Example 2-1)

[0150] The resin composition of Example 2-1 was prepared by adding 0.55 parts by mass of DCP (diisophenylpropyl peroxide, product name: PERCUMYL D, manufactured by NOF CORPORATION) to 100 parts by mass of the resin composition of Example 1-1 (polymaleimide resin (A-2): 55.1 parts by mass, organic solvent (mainly 1,2,4-trimethylbenzene): 44.9 parts by mass).

[0151] [Adhesive sheet production]

[0152] An adhesive sheet was prepared using the resin composition of Example 2-1. The adhesive sheet was prepared by applying the resin composition onto FILMBYNA (registered trademark) (PET film, manufactured by FUJIMORI KOGYO CO., LTD., product name: NS14, film thickness 75 μm) using an applicator so that the thickness after drying was 100 μm, and drying was performed at 130° C. for 15 minutes using a dryer to obtain an adhesive sheet of Example 2-1 having a film and a dry film disposed on the film.

[0153] Then, the PET film of the adhesive sheet was peeled off, and copper foil (product name: 3EC-M2S-VLP, manufactured by MITSUI MINING & SMELTING C0., LTD.) was laminated on both sides of the dry film, and laminated using a vacuum laminator at 75°C, 30 seconds, and -100 kPa to obtain a first laminate of a structure of copper foil / dry film / copper foil. The first laminate obtained was cured at 200°C for 1 hour using a dryer. After curing, the copper foil was removed by etching with an ammonium persulfate aqueous solution, and dried at 110°C for 30 minutes to obtain the cured films of Example 2-1.

[0154] [Evaluation of Cured Film]

[0155] <Determination of Elastic Modulus>

[0156] Using the cured film, a test piece with a sample size of 20 mm × 10 mm was prepared. Using this test piece, a dynamic viscoelasticity measuring device (product name: DMS6100, manufactured by Seiko Instruments Inc.) was used to measure the elastic modulus at 20°C under the conditions of a frequency of 1 Hz, a measuring temperature of -40°C to 220°C, and a heating rate of 10°C / min. The results are shown in Table 2.

[0157] <5% Weight Reduction Temperature>

[0158] 6.0 to 10.0 mg of the cured film was weighed in an open sample container (product name: P / N SSC000E030, manufactured by Seiko Instruments Inc.) and measured under the conditions of a nitrogen flow rate of 300 mL / min and a temperature increase rate of 10°C / min. The 5% weight loss temperature (T d5 TG / DTA7200 (manufactured by Hitachi High-Tech Science Corporation) was used as a measuring apparatus. The results are shown in Table 2.

[0159] <Evaluation of Dielectric Properties>

[0160] Using the cured film, a test piece with a sample size of 50 mm × 100 mm was made. Using the test piece, the relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured using a network analyzer (product name: P5003A, manufactured by KEYSIGHT Technologies) and a split cylinder resonator (manufactured by KEYSIGHT Technologies). Based on the measurement results, the evaluation was performed according to the following criteria. When the evaluation result is A, it can be said that the dielectric properties are sufficiently excellent. The results are shown in Table 2.

[0161] (Dk determination criteria)

[0162] A: less than 2.5

[0163] B: 2.5 or more and less than 2.8

[0164] C: 2.8 or above

[0165] (Df determination criteria)

[0166] A: less than 0.0030

[0167] B: 0.0030 or more and less than 0.0050

[0168] C: 0.0050 or more

[0169] <Determination of elongation at break>

[0170] Using the cured film, a test piece with a sample size of 50 mm × 10 mm was prepared. Using the test piece, both ends of the sample were fixed on an automatic stereogrammer (product name: AGS-X, manufactured by Shimadzu Corporation) with a 10 mm axis, and the elongation at break was measured at room temperature (25°C) at a tensile speed of 10 mm / min. The results are shown in Table 2.

[0171] [Table 2]

[0172]

[0173] As shown in Table 2, it was confirmed that the resin composition of Example 2-1 could form a cured film (cured product) having excellent dielectric properties (low Dk and low Df) and sufficient elongation at break.

[0174] Industrial Applicability

[0175] According to the present invention, a method for producing a resin composition capable of suppressing side reactions in the manufacture of polymaleimide resin can be provided. In addition, according to the present invention, a resin composition obtained by such a manufacturing method and a cured product thereof can be provided. By using the resin composition of the present invention, it is expected that the properties of the interlayer insulating material of a printed wiring board, the surface protection film of a semiconductor, the interlayer insulating film, the insulating film of a redistribution layer, etc. can be improved significantly.

Claims

1. A method for producing a resin composition, comprising the following steps: reacting tetracarboxylic dianhydride and polyamine in an organic solvent to obtain a polyimide resin; and reacting maleic anhydride with the polyimide resin to obtain a resin composition containing the polymaleimide resin and the organic solvent; The polyamine comprises a dimer diamine, The organic solvent includes 1,2,4-trimethylbenzene.

2. The method for producing a resin composition according to claim 1, wherein The dimer diamine is at least one selected from the group consisting of a compound represented by the following general formula (1) and a compound represented by the following general formula (2), In formulas (1) and (2), m, n, p, and q each independently represent an integer greater than 1, wherein m and n are integers satisfying the condition of m+n=6 to 17, p and q are integers satisfying the condition of p+q=8 to 19, and the bond represented by the dotted line represents a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by the dotted line is a carbon-carbon double bond, formulas (1) and (2) are structures obtained by subtracting 1 from the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond from the number represented by formulas (1) and (2).

3. The method for producing a resin composition according to claim 1 or 2, wherein: The blending amount of the dimer diamine is 20 mol% or more based on the total amount of the polyamine.

4. The method for producing a resin composition according to claim 1 or 2, wherein The weight average molecular weight of the polymaleimide resin is 3,000 to 40,000.

5. A resin composition comprising a polymaleimide resin which is a reaction product of tetracarboxylic dianhydride, polyamine, and maleic anhydride, and an organic solvent, The polyamine comprises a dimer diamine, The organic solvent includes 1,2,4-trimethylbenzene.

6. The resin composition according to claim 5, further comprising a polymerization initiator, The polymerization initiator includes a thermal polymerization initiator or a photopolymerization initiator. 7 . A cured product, which is a cured product of the resin composition according to claim 5 or 6 .