Photosensitive resin composition, cured product, and semiconductor element
By using a photosensitive resin composition with a maleimide compound and a crosslinking agent in a semiconductor device, the problem of difficult to achieve the characteristic balance of the insulating film in the prior art is solved, and excellent fine workability and mechanical characteristics are formed The resin film with dielectric characteristics improves the high frequency characteristics and reliability of semiconductor components.
Patent Information
- Application Number
- CN202480002265.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-01-19
- Filing Date
- 2024-01-18
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, it is difficult to form an insulating film with excellent fine machining, mechanical and dielectric characteristics in semiconductor components, especially in applications of re-wiring layers.
Using a photosensitive resin composition comprising a maleimide compound, a crosslinking agent and a photopolymerization initiator, a resin composition having a fluorene skeleton is formed by combining a specific reactant and a crosslinking agent, and the resin composition having a fluorene skeleton is formed, and the Curing is performed during exposure and heating to form a cured film with low dielectric constant and low dielectric loss tangent.
An insulating film with excellent fine workability, mechanical characteristics and dielectric characteristics is achieved in semiconductor components, and the high frequency characteristics and reliability of the re-wiring layer are improved.
Smart Images

Figure BDA0005095831500000021 
Figure BDA0005095831500000061 
Figure BDA0005095831500000062
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition, a cured product and a semiconductor element. Background Art
[0002] With the high integration, miniaturization and micronization of semiconductor elements, the insulating films used for the surface protection layer, interlayer insulating layer, and rewiring layer of semiconductor elements are required to have better electrical properties, heat resistance, mechanical properties, etc. As a material for forming an insulating film having such properties, a photosensitive resin composition containing an alkali-soluble resin has been developed (for example, refer to patent documents 1, 2, and 3). These photosensitive resin compositions are applied and dried on a substrate to form a resin film, and a patterned resin film (a resin film having a pattern) is obtained by exposing and developing the resin film. Then, a patterned cured film (a cured film having a pattern) can be formed by heat curing the above-mentioned patterned resin film, and the patterned cured film can be used as an insulating film.
[0003] Previous technical literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2008-309885
[0006] Patent Document 2: Japanese Patent Application Publication No. 2007-057595
[0007] Patent Document 3: International Publication No. 2010 / 073948 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] A photosensitive resin composition for forming an insulating film such as a redistribution layer is required to have an excellent balance among microfabrication, mechanical properties, and dielectric properties (low relative dielectric constant and low dielectric loss tangent). Therefore, an object of the present invention is to provide a photosensitive resin composition capable of forming an insulating film having an excellent balance among microfabrication, mechanical properties, and dielectric properties.
[0010] One aspect of the present invention relates to the following photosensitive resin composition, a cured product of the photosensitive resin composition, and a semiconductor device.
[0011] [1] A photosensitive resin composition comprising a maleimide compound, a crosslinking agent and a photopolymerization initiator, wherein the maleimide compound is a reaction product of tetracarboxylic dianhydride (a1), a diamine (a2), a triamine (a3) and maleic anhydride (a4), and the diamine (a2) comprises a dimer diamine.
[0012] [2] The photosensitive resin composition according to [1] above, wherein the diamine (a2) contains a second diamine other than the dimer diamine.
[0013] [3] The photosensitive resin composition according to [2] above, wherein the second diamine is an alicyclic diamine or an aromatic diamine.
[0014] [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein the dimer diamine contains at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2),
[0015]
[0016] In formulas (1) and (2), m, n, p and q represent integers greater than 1 selected so as to form m+n=6 to 17 and p+q=8 to 19, respectively. The bond represented by a dotted line refers to a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by a dotted line is a carbon-carbon double bond, formulas (1) and (2) become the following structure: the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond is subtracted by 1 from the number shown in formulas (1) and (2).
[0017] [5] The photosensitive resin composition according to any one of [1] to [4], wherein the tetracarboxylic dianhydride (a1) contains an anhydride selected from the group consisting of 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-c]furan-1,3-dione, 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenoxy)diphthalic anhydride, 4,4 At least one of the group consisting of '-(hexafluoroisopropylidene)diphthalic anhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic 2,3:5,6-dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic 5,5',6,6'-dianhydride and 3,4'-diphthalic anhydride.
[0018] [6] The photosensitive resin composition according to any one of [1] to [5] above, wherein the content of the triamine (a3) is 5 to 35 mol % based on the total amount of the diamine (a2) and the triamine (a3).
[0019] [7] The photosensitive resin composition according to any one of [1] to [6] above, wherein the weight average molecular weight of the maleimide compound is 3,000 to 40,000.
[0020] [8] The photosensitive resin composition according to any one of [1] to [7] above, wherein the maleimide compound has a fluorene skeleton.
[0021] [9] The photosensitive resin composition according to any one of [1] to [8] above, wherein the crosslinking agent comprises a polymerizable crosslinking agent having a (meth)acryloyl group.
[0022]
[10] The photosensitive resin composition according to any one of [1] to [9] above, wherein the crosslinking agent comprises a polymerizable crosslinking agent having an allyl group or a vinyl group.
[0023]
[11] The photosensitive resin composition according to any one of [1] to
[10] , further comprising a thermal polymerization initiator.
[0024]
[12] A cured product, which is a cured product of the photosensitive resin composition according to any one of [1] to
[11] .
[0025]
[13] A semiconductor element having a redistribution layer formed of a cured product of the photosensitive resin composition according to any one of [1] to
[11] above.
[0026] Effects of the Invention
[0027] According to the present invention, there can be provided a photosensitive resin composition capable of forming an insulating film having an excellent balance among microprocessibility, mechanical properties and dielectric properties, a cured product having an excellent balance among microprocessibility, mechanical properties and dielectric properties, and a semiconductor element having a redistribution layer including the cured product. DETAILED DESCRIPTION
[0028] Hereinafter, preferred embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and various modifications can be made without departing from the gist of the present invention.
[0029] In this specification, the numerical range represented by "~" represents the range in which the numerical values recorded before and after "~" are included as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of another stage. In the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. "A or B" can include any one of A and B, or both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. The content of each component in the composition, when there are multiple substances equivalent to each component in the composition, represents the total amount of the multiple substances present in the composition unless otherwise specified.
[0030] In this specification, "layer" and "film" include structures formed on a part of a surface in addition to structures formed on the entire surface when viewed from a top view. The term "process" includes not only independent processes, but also processes that achieve the desired purpose of the process even if they cannot be clearly distinguished from other processes.
[0031] In this specification, "(meth)acryloyl" refers to at least one of "acryloyl" and its corresponding "methacryloyl", and the same applies to other similar expressions such as (meth)acrylic acid and (meth)acrylate. In this specification, "solid content" refers to non-volatile components other than volatile substances (water, solvent, etc.) contained in the photosensitive resin composition, and also includes components that are liquid, syrupy, or waxy at room temperature (about 25°C).
[0032] [Photosensitive resin composition]
[0033] The photosensitive resin composition of this embodiment contains a maleimide compound having a specific structure, a crosslinking agent and a photopolymerization initiator as essential components. The maleimide compound is a reaction product of tetracarboxylic dianhydride (a1), diamine (a2), triamine (a3) and maleic anhydride (a4), and the diamine (a2) includes a dimer diamine.
[0034] The photosensitive resin composition of the present embodiment may further contain a thermal polymerization initiator, a coupling agent, a rust inhibitor, a polymerization inhibitor, etc. as needed. The photosensitive resin composition of the present embodiment is a negative photosensitive resin composition, and the cured product of the photosensitive resin composition can be appropriately used as an insulating film for a redistribution layer. Hereinafter, each component used in the photosensitive resin composition of the present embodiment will be described in more detail.
[0035] (Maleimide compound)
[0036] The maleic imide compound (hereinafter, also referred to as "(A) component") of the present embodiment can be obtained by reacting tetracarboxylic dianhydride (a1) (hereinafter, also referred to as "(a1) component"), diamine (a2) (hereinafter, also referred to as "(a2) component"), triamine (a3) (hereinafter, also referred to as "(a3) component") and maleic anhydride (a4) (hereinafter, also referred to as "(a4) component") . That is, component (A) is a maleic imide compound obtained by reacting component (a1), component (a2), component (a3) and component (a4). Here, the above-mentioned component (a2) contains a dimer diamine. Component (A) is a multifunctional maleic imide compound having two or more maleic imide groups. Component (A) can be used alone or in combination of two or more.
[0037] As the tetracarboxylic dianhydride of the component (a1), a material known as a raw material of polyimide can be used. As the component (a1), for example, pyromelitic dianhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-C] furan-1,3-dione, 3,3',4,4'-diphenylsulfonic acid tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 3,3',4,4'- -benzophenone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride, 1,2,3,4-butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, bicyclo[2.2.2]octane-7-ene-2,3,5,6-tetracarboxylic dianhydride anhydride, bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 1,4-phenylene, 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride, 4,4'-(ethynyl-1,2-diyl)diphthalic anhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, 3,4'-oxydi Phthalic anhydride, 4,4'-oxydiphthalic anhydride, 3,4'-diphthalic anhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic acid-5,5',6,6'-dianhydride and 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride.
[0038] From the viewpoint of low dielectric properties or high Tg, the component (a1) preferably contains an anhydride selected from 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-c]furan-1,3-dione, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic anhydride, bicyclo[2. 2.2] at least one selected from the group consisting of octane-2,3,5,6-tetracarboxylic acid 2,3:5,6-dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic acid-5,5',6,6'-dianhydride and 3,4'-diphthalic anhydride, more preferably at least one selected from the group consisting of 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-c]furan-1,3-dione, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride.
[0039] The component (a2) contains a dimer diamine (the first diamine) as an essential component. For example, as described in Japanese Patent Publication No. 9-12712, the dimer diamine is a compound derived from a dimer of unsaturated fatty acids such as oleic acid, i.e., a dimer acid. By using a dimer diamine as the component (a2), a cured product with excellent dielectric properties can be obtained. In this embodiment, known dimer diamines can be used without particular limitation. The component (a2) preferably includes at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2).
[0040]
[0041] In formulas (1) and (2), m, n, p and q each represent an integer greater than or equal to 1 selected so as to satisfy m+n=6 to 17 and p+q=8 to 19, and the bond represented by the dotted line refers to a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by the dotted line is a carbon-carbon double bond, formulas (1) and (2) have a structure in which the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond is subtracted by 1 from the number shown in formulas (1) and (2).
[0042] The dimer diamine may be a diamine represented by the above general formula (2), and may be a compound represented by the following formula (3) from the viewpoints of solubility in organic solvents, heat resistance, heat-resistant adhesion, low viscosity, and the like.
[0043]
[0044] As a commercial item of dimer diamine, PRIAMINE 1075, PRIAMINE 1074 (both manufactured by Croda Japan KK) etc. are mentioned, for example.
[0045] The component (a2) may further contain a diamine other than dimer diamine as the second diamine. By using an alicyclic diamine as the second diamine, the dielectric constant can be lowered. By using an aromatic diamine as the second diamine, the elastic modulus and Tg of the cured product can be increased.
[0046] The second diamine is a diamine that does not correspond to the above-mentioned dimer diamine. Examples of the second diamine include 1,3-diaminopropane, norbornanediamine, 4,4-methylenedianiline, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis[3-fluoro-4-aminophenyl]fluorene, 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, 4,4'-(hexafluoroisopropylidene)diphenylamine, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.0 2,6] decane, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamino), 4,4'-methylenebis(2-methylcyclohexylamino), 1,1-bis(4-aminophenyl)cyclohexane, 2,7-diaminofluorene, 4,4'-ethylenedianiline, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2-ethyl-6-methylphenyl) amine), 2,2-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]methane, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ketone, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethylbiphenyl-4,4'-diamine , (4,4'-diamino) diphenyl ether, (3,3'-diamino) diphenyl ether, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, 4,4'-diamino-2,2'-diethyl biphenyl, 4,4'-diamino-3,3'-dimethyl biphenyl, 4,4'-diamino-3,3'-diethyl biphenyl, 4,4'-diamino-3,3',5,5'-tetramethyl biphenyl, 4,4'-diamino-3,3',5,5'- Tetraethylbiphenyl, 4,4'-diamino-2,2'-dimethoxybiphenyl, 4,4'-diamino-3,3'-dimethoxybiphenyl, m-xylene diamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 1,4'-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]sulfonamide and bis[4-(4-aminophenoxy)phenyl]sulfonamide.
[0047] In the component (a2), the molar ratio of the second diamine (the number of moles of the second diamine / (the number of moles of the dimer diamine+the number of moles of the second diamine)) may be 70 mol% or less, or 50 mol% or less. If the ratio is 70 mol% or less, a cured product having lower dielectric properties can be formed.
[0048] As the triamine of the component (a3), a known triamine can be used. Examples of the component (a3) include tris(2-aminomethyl)amine, tris(2-aminoethyl)amine, tris(2-aminopropyl)amine, 2-(aminomethyl)-2-methyl-1,3-propylenediamine, trimerized triamine, 3,4,4'-triaminodiphenyl ether, 1,2,4-triaminobenzene, 1,3,5-triaminobenzene, 1,2,3-triaminobenzene, 1,3,5-triazine-2,4,6-triamine, 2,4,6-triaminopyrimidine, 1,3,5-tris(4-aminophenyl)benzene, 1,3,5-tris(4-aminophenoxy)benzene, and tris(4-aminophenyl)methane. Among these, aliphatic triamines are preferred from the viewpoint of solubility of the synthesized maleimide compound in an organic solvent, and tris(2-aminomethyl)amine and tris(2-aminoethyl)amine having a small number of carbon atoms are more preferred from the viewpoint of increasing Tg.
[0049] Based on the total amount of components (a2) and (a3), the content of component (a3) may be 5 mol% or more, 8 mol% or more, or 10 mol% or more, or 50 mol% or less, 40 mol% or less, or 35 mol% or less. If the ratio is 5 mol% or more, the elastic modulus and Tg of the cured product can be further improved, and if it is 50 mol% or less, it is easy to dissolve in a solvent and is also easy to synthesize.
[0050] From the above viewpoints, the content of the component (a3) may be 5 to 50 mol %, or 5 to 35 mol %, based on the total amount of the components (a2) and (a3).
[0051] By using dimer diamine as diamine, it is possible to form a cured product with lower low dielectric properties. On the other hand, as diamine, when only dimer diamine is used, the elastic modulus and Tg of the cured product can be reduced. In contrast, by using triamine and dimer diamine together, it is possible to improve elastic modulus and Tg while maintaining the dielectric properties of the cured product. And then, by using the second diamine and dimer diamine together, it is possible to further improve elastic modulus and Tg while maintaining the dielectric properties of the cured product.
[0052] The maleimide compound can have a fluorene skeleton. In this case, at least one of the above-mentioned (a1) component and (a2) component can contain a compound having a fluorene skeleton. By including a compound having a fluorene skeleton in at least one of the (a1) component and (a2) component constituting the maleimide compound, the cured product obtained using the maleimide compound becomes a cured product with high elastic modulus and high Tg while fully maintaining a low dielectric constant and a low dielectric loss tangent.
[0053] (A) component can be produced by various known methods. For example, first, component (a1), component (a2) and component (a3) are subjected to addition polymerization at a temperature of about 60 to 120° C., preferably at a temperature of 70 to 90° C., usually for about 0.1 to 2 hours, preferably 0.1 to 1.0 hours. Then, the obtained addition polymer is further subjected to an imidization reaction, i.e., a dehydration ring-closure reaction, at a temperature of about 80 to 250° C., preferably at a temperature of 100 to 200° C., for about 0.5 to 30 hours, preferably 0.5 to 10 hours. Then, the substance obtained by the dehydration ring-closure reaction and component (a4) are subjected to a maleimide reaction, i.e., a dehydration ring-closure reaction, at a temperature of about 60 to 250° C., preferably at a temperature of 80 to 200° C., for about 0.5 to 30 hours, preferably 0.5 to 10 hours, thereby obtaining the target (A) component.
[0054] In the imidization reaction or the maleimide reaction, various known reaction catalysts, dehydrating agents and organic solvents can be used.
[0055] Examples of the reaction catalyst include aliphatic tertiary amines such as triethylamine, aromatic tertiary amines such as dimethylaniline, heterocyclic tertiary amines such as pyridine, picoline, and isoquinoline, and organic acids such as methanesulfonic acid and p-toluenesulfonic acid monohydrate. Examples of the dehydrating agent include aliphatic anhydrides such as acetic anhydride, and aromatic anhydrides such as benzoic anhydride.
[0056] Examples of the organic solvent include aromatic hydrocarbon solvents such as benzene, toluene, xylene, and trimethylol; alcohol solvents such as methanol, ethanol, isopropanol, butanol, pentanol, hexanol, propylene glycol, and phenol; ether solvents such as anisole; ketone solvents such as acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclopentanone, cyclohexanone, isophorone, and acetophenone; cellulose such as methyl cellulose and ethyl cellulose, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, butyl formate, γ- Ester solvents such as butyrolactone; glycol ether solvents such as ethylene glycol mono-n-butyl ether, ethylene glycol mono-isobutyl ether, ethylene glycol mono-tert-butyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-isobutyl ether, triethylene glycol mono-n-butyl ether, and tetraethylene glycol mono-n-butyl ether; and amine solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide. The organic solvent can be used alone or in combination of two or more.
[0057] The (A) component can be purified by various known methods to improve the purity. For example, first, the (A) component dissolved in the organic solvent and pure water are placed in a separatory funnel. Then, the separatory funnel is shaken and left to stand. Then, after the aqueous layer and the organic layer are separated, only the organic layer is recovered, thereby purifying the (A) component.
[0058] The (A) component manufactured by the above method may contain one or more of the structural units represented by the following general formulae (4) to (6). The range of the number of functional groups (the number of maleimide groups) of the (A) component depends on the content of the triamine, but it is assumed that there are 2 to 6 functional groups per molecule. The (A) component may be a mixture of multiple compounds having different structures or different numbers of functional groups. The (A) component may contain a compound that contains one or more of the structural units represented by the following general formulae (5) to (6) and has 3 or more functional groups per molecule.
[0059]
[0060]
[0061] In formulae (4) to (6), X each independently represents a tetravalent organic group, Y each independently represents a divalent organic group, and Z each independently represents a trivalent organic group. X, Y, and Z may be an aliphatic group, an organic group having an alicyclic structure or an aromatic ring, and they may contain a heteroatom. Y may be an organic group derived from a dimer diamine, and Z may be an organic group derived from a triamine (a3).
[0062] An example of the assumed structure of the component (A) produced by the above method is shown in the following general formula (7).
[0063]
[0064] X, Y and Z in formula (7) have the same meanings as X, Y and Z in general formulae (4) to (6). Furthermore, a represents an integer of 0 to 20, b represents 0 to 30, c represents 0 to 20, and d represents an integer of 1 to 30. In general formula (7), the positions of the structural unit with symbol a (the structural unit represented by the above general formula (5)), the structural unit with symbol b (the structural unit represented by the above general formula (4)) and the structural unit with symbol c (the structural unit represented by the above general formula (6)) may be interchanged. Component (A) may contain a compound in which at least one of a and c is an integer greater than 1 and has three or more functional groups per molecule.
[0065] The molecular weight of component (A) can be controlled by the molar number of component (a1), component (a2) and component (a3). The smaller the molar number of component (a1) is compared to the molar number of component (a2) and component (a3), the lower the molecular weight can be. In order to easily achieve the effect of the present invention, it is usually preferred that [molar number of component (a1)] / [molar number of component (a2)+molar number of component (a3)] is about 0.30 to 1.00, preferably 0.30 to 0.95, more preferably 0.30 to 0.90, and further preferably 0.50 to 0.80.
[0066] The molecular weight of the component (A) may be 3000 or more, 5000 or more, 6000 or more, or 7000 or more, in terms of weight average molecular weight (Mw), or 40000 or less, 38000 or less, 35000 or less, 33000 or less, 30000 or less, 25000 or less, or 20000 or less. When the weight average molecular weight is 40000 or less, the solubility in organic solvents becomes good, and when it is 3000 or more, there is a tendency that the effect of improving heat resistance can be fully obtained. From the viewpoint of solubility in solvents and heat resistance, Mw may be 3000 to 40000, preferably 3000 to 30000, more preferably 5000 to 25000, further preferably 6000 to 23000, and particularly preferably 7000 to 20000. Mw can be measured by gel permeation chromatography (GPC) and converted using a calibration curve of standard polystyrene.
[0067] (Crosslinking agent)
[0068] The crosslinking agent (hereinafter also referred to as "component (B)") may be a polymerizable crosslinking agent. The polymerizable group may be a photopolymerizable group or a thermal polymerizable group. Examples of the polymerizable group include (meth)acryloyl, allyl and vinyl groups. Component (B) may be a polyfunctional compound having two or more polymerizable groups. Regarding the crosslinking agent, for example, when the photosensitive layer is exposed, the crosslinking agents can be crosslinked not only with each other but also with component (A). Furthermore, regarding the crosslinking agent, for example, when the resin film after pattern formation is heated, the polymerizable crosslinking agents can be crosslinked with each other. Component (B) may be used alone or in combination of two or more.
[0069] From the viewpoint of dielectric properties, the resin composition of the present embodiment may contain a polymerizable crosslinking agent having a (meth)acryloyl group as a crosslinking agent. Regarding the polymerizable crosslinking agent having a (meth)acryloyl group, when the photosensitive layer is exposed, the crosslinking agents are not only crosslinked with each other, but also crosslinked with the (A) component. The polymerizable crosslinking agent having a (meth)acryloyl group may be an acrylate compound or a methacrylate compound. From the viewpoint of dielectric properties, the (B) component may contain a methacrylate compound.
[0070] Examples of the polymerizable crosslinking agent having a (meth)acryloyl group include tricyclodecane dimethanol di(meth)acrylate, tris-(2-(meth)acryloyloxyethyl)isocyanurate, dioxane glycol di(meth)acrylate, alkoxylated glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, alkoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, alkoxylated pentaerythritol tetra(meth)acrylate, 1, 6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, propoxylated ethoxylated bisphenol A (meth)acrylate, dipentatriol poly(meth)acrylate, alkoxylated dipentatriol poly(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, polyethylene glycol di(meth)acrylate and polypropylene glycol di(meth)acrylate.
[0071] From the viewpoints of heat resistance, dielectric properties and fine processing properties, the polymerizable crosslinking agent having a (meth)acryloyl group may include at least one selected from the group consisting of tricyclodecane dimethanol di(meth)acrylate, tris-(2-(meth)acryloyloxyethyl)isocyanurate and dioxane glycol di(meth)acrylate, and from the viewpoints of heat resistance and dielectric properties, may include tris-(2-(meth)acryloyloxyethyl)isocyanurate.
[0072] From the viewpoint of dielectric properties and heat resistance, the resin composition of the present embodiment may contain a polymerizable crosslinking agent having an allyl group or a vinyl group as a crosslinking agent. The polymerizable crosslinking agent having an allyl group or a vinyl group can crosslink the polymerizable crosslinking agents when the patterned resin film is heated.
[0073] Examples of the polymerizable crosslinking agent having an allyl group include 1,3,4,6-tetraallyl glycoluril, triallyl isocyanurate, diallyl monoglycidyl isocyanurate, diallyl monomethyl isocyanurate, diallyl isocyanurate, triallyl trimellitate, and triallyl orthoformate.
[0074] Examples of the polymerizable crosslinking agent having a vinyl group include polyvinyl benzyl compounds and polyvinyl benzyl ether compounds.
[0075] From the viewpoint of dielectric properties and fine processing properties, the polymerizable crosslinking agent having an allyl group or a vinyl group may include at least one selected from the group consisting of 1,3,4,6-tetraallyl glycoluril, triallyl isocyanurate, diallyl isocyanurate and polyvinyl benzyl ether compounds, and from the viewpoint of dielectric properties, may also include 1,3,4,6-tetraallyl glycoluril or triallyl isocyanurate.
[0076] From the viewpoint of further improving the balance between low dielectric properties and fine processing properties, when the total amount of component (A) and component (B) is set to 100 parts by mass, the content of component (B) is preferably less than 50 parts by mass, and can be 1 to 45 parts by mass, 5 to 40 parts by mass, 8 to 30 parts by mass, or 10 to 20 parts by mass.
[0077] (Photopolymerization Initiator)
[0078] The photopolymerization initiator (hereinafter also referred to as "component (C)") is not particularly limited as long as it is a compound that starts polymerization by irradiation with active light (ultraviolet rays, etc.), and examples thereof include alkyl phenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, intramolecular hydrogen abstraction-type photopolymerization initiators, and oxime ester-based photopolymerization initiators.
[0079] Regarding the alkylphenone-based photopolymerization initiator, for example, it can be purchased as Omnirad 651, Omnirad 184, Omnirad 1173, Omnirad 2959, Omnirad 127, Omnirad 907, Omnirad 369, Omnirad 379EG, etc. manufactured by IGM Resins BV. Regarding the acylphosphine oxide-based photopolymerization initiator, for example, it can be purchased as Omnirad 819, Omnirad TPO H, etc. manufactured by IGM Resins B.V. Regarding the intramolecular hydrogen abstraction type photopolymerization initiator, for example, it can be purchased as Omnirad MBF, Omnirad 754, etc. manufactured by IGM Resins BV. Regarding the oxime ester-based photopolymerization initiator, for example, it can be purchased as Irgacure OXE01, Irgacure OXE02, etc. manufactured by BASF Japan Ltd. In order to promote the photoreaction, a titanocene-based photopolymerization initiator (for example, Irgacure 784 manufactured by BASF Japan Ltd.) may be used in combination.
[0080] From the perspective of easily obtaining excellent micromachinability, the content of component (C) may be 0.1 to 10.0 parts by mass, 0.5 to 8.0 parts by mass, 0.8 to 6.0 parts by mass, or 1.0 to 5.0 parts by mass relative to 100 parts by mass of the total amount of components (A) and (B).
[0081] (Thermal polymerization initiator)
[0082] From the viewpoint of promoting the polymerization reaction of the thermally polymerizable group, the photosensitive resin composition of the present embodiment may further contain a thermal polymerization initiator as the component (D). As the component (D), it is preferred that the compound decomposes by heating during curing to generate free radicals and promote the polymerization reaction of the components (A) and (B). As the component (D), for example, an organic peroxide can be cited.
[0083] Examples of the organic peroxide include methyl ethyl ketone peroxide, methyl cyclohexanone peroxide, methyl acetoacetate peroxide, acetylacetone peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(4,4-di-tert-butylperoxycyclohexyl)propane, 1,1-bis(tert-butylperoxy)cyclododecane, n-butyl-4,4-bis(tert-butylperoxy)valerate, 2,2-bis(tert-butylperoxy)butane, 1,1-bis(tert-butylperoxy)-2-methylcyclohexane, tert-butyl hydroperoxide, and p-butyl hydroperoxide. Menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, tert-hexyl hydroperoxide, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, α,α'-bis(tert-butylperoxy)diisopropylbenzene, tert-butylisopropylbenzene peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3, isobutyryl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, cinnamic acid peroxide, m-Toluoyl peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate Ester, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, α,α'-bis(neodecanoyl peroxy)diisopropylbenzene, isopropylbenzene peroxyneodecanoate, 1,1,3,3,-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoyl peroxy)hexane, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, 1-cyclohexyl Hexyl-1-methylethyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxymaleic acid, tert-butyl peroxylaurate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, tert-butyl peroxyacetate, tert-hexyl peroxybenzoate, tert-butyl peroxy-m-toluoyl benzoate, tert-butyl peroxybenzoate, bis(tert-butylperoxy)isophthalate, tert-butyl peroxyallyl monocarbonate and 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone.
[0084] The content of the component (D) is not particularly limited and may be 0.1 to 10.0 parts by mass, 0.3 to 8.0 parts by mass, 0.5 to 5.0 parts by mass, 0.7 to 3.0 parts by mass, or 0.7 to 2.0 parts by mass relative to 100 parts by mass of the total amount of the components (A) and (B).
[0085] (Coupling agent)
[0086] From the viewpoint of improving the adhesion of the cured product of the photosensitive resin composition, the photosensitive resin composition of the present embodiment may further contain a coupling agent. The coupling agent may be a silane coupling agent. The silane coupling agent may have, for example, a vinyl group, an epoxy group, a styryl group, an acryl group, a methacryl group, an amino group, an ureide group, an isocyanate group, an isocyanurate group, a mercapto group, and the like.
[0087] As silane coupling agents having a vinyl group, KBM-1003, KBE-1003 (product names manufactured by Shin-Etsu Chemical Co., Ltd.. The same applies hereinafter.) and the like can be cited. As silane coupling agents having an epoxy group, KBM-303, 402, 403, KBE-402, 403, X-12-981S, X-12-984S and the like can be cited. As silane coupling agents having a styrene group, KBM-1403 and the like can be cited. As silane coupling agents having a methacryloyl group, KBM-502, 503, KBE-502, 503 and the like can be cited. As silane coupling agents having an acryl group, KBM-5103, X-12-1048, X-12-1050 and the like can be cited. As silane coupling agents having amino groups, KBM-602, 603, 903, 573, 575, KBE-903, 9103P, X-12-972F, etc. can be cited. As silane coupling agents having ureide groups, KBE-585, etc. can be cited. As silane coupling agents having isocyanate groups, KBE-9007, X-12-1159L, etc. can be cited. As silane coupling agents having isocyanurate groups, KBM-9659, etc. can be cited. As silane coupling agents having mercapto groups, KBM-802, 803, X-12-1154, X-12-1156, etc. can be cited. The silane coupling agent can be a silane coupling agent having a methacryloyl group. The silane coupling agent can be used alone or in combination of two or more.
[0088] The content of the silane coupling agent may be 0.01 to 10.0 parts by mass, 0.1 to 8.0 parts by mass, 0.3 to 6.0 parts by mass, 0.5 to 5.0 parts by mass, or 1.0 to 3.0 parts by mass based on 100 parts by mass of the total amount of the components (A) and (B).
[0089] (Rust Inhibitor)
[0090] From the viewpoint of inhibiting the corrosion of copper wiring or preventing the discoloration of copper wiring, the photosensitive resin composition of the present embodiment may further contain a rust inhibitor. As the rust inhibitor, for example, triazole derivatives such as benzotriazole, tetrazole derivatives, etc. can be cited. The rust inhibitor can be used alone or in combination of two or more.
[0091] The content of the rust inhibitor may be 0.01 to 10.0 parts by mass, 0.1 to 5.0 parts by mass, 0.3 to 4.0 parts by mass, 0.5 to 3.0 parts by mass, or 1.0 to 3.0 parts by mass based on 100 parts by mass of the total amount of the components (A) and (B).
[0092] (Polymerization Inhibitor)
[0093] From the viewpoint of storage stability, the photosensitive resin composition of the present embodiment may further contain a polymerization inhibitor.
[0094] Examples of the polymerization inhibitor include 4-tert-butylcatechol, 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl radical, p-methoxyphenol, diphenyl-p-benzoquinone, benzoquinone, hydroquinone, gallol, phenothiazine, resorcinol, o-dinitrobenzene, p-dinitrobenzene, m-dinitrobenzene, phenanthraquinone, N-phenyl-2-naphthylamine, cupferroline, 2,5-methoxyquinone, tannic acid, p-benzylaminophenol, tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, and nitrosamines. The polymerization inhibitor may be used alone or in combination of two or more.
[0095] The content of the polymerization inhibitor may be 0.01 to 10.0 parts by mass, 0.05 to 5.0 parts by mass, 0.10 to 2.0 parts by mass, or 0.10 to 1.0 parts by mass based on 100 parts by mass of the total amount of the components (A) and (B).
[0096] (Sensitizer)
[0097] From the viewpoint of achieving both maintenance of the residual film rate in a wide range of exposure amounts and good resolution, the photosensitive resin composition may further contain a sensitizer.
[0098] Examples of the sensitizer include Michler's ketone, benzoin, 2-methylbenzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, 2-tert-butylanthraquinone, 1,2-benzo-9,10-anthraquinone, anthraquinone, methylanthraquinone, 4,4'-bis(diethylamino)benzophenone, acetophenone, benzophenone, thioxanthone, 1,5-acenaphthene, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-[4-(methylthio)phenyl]-2-morpholine-1-propanone, diacetylbenzyl, benzyl dimethyl ketal, benzyl ketal, 1,2-diethyl ketal, diphenyl disulfide, anthracene, phenanthrenequinone, riboflavin tetrabutyrate, acridine orange, erythrosine, phenanthrenequinone, 2-isopropylthioxanthone, 2,6-bis(p-diethylaminobenzylidene)-4-methyl-4-azacyclohexanone, 6-bis(p-dimethylaminobenzylidene)-cyclopentanone, 2,6-bis(p-diethylaminobenzylidene)-4-phenylcyclohexanone, aminophenyl ketone, 3-ketocoumarin compound, biscoumarin compound, N-phenylglycine, N-phenyldiethanolamine and 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone. The sensitizer may be used alone or in combination of two or more.
[0099] When the photosensitive resin composition contains a sensitizer, the content thereof is preferably 0.1 to 2.0 parts by mass, more preferably 0.2 to 1.5 parts by mass, based on 100 parts by mass of the total amount of the component (A) and the component (B).
[0100] (Solvent)
[0101] The photosensitive resin composition of the present embodiment contains a solvent for dissolving / dispersing each component, and can be easily applied on a substrate to form a coating film with uniform thickness. The solvent may be used alone or in combination of two or more.
[0102] As the solvent, for example, there can be mentioned ketone solvents such as methyl ethyl ketone, cyclohexanone, and cyclopentanone; aromatic hydrocarbon solvents such as toluene, xylene, tetramethylbenzene, mesitylene, and trimethylbenzene; glycol ether solvents such as methyl cellulose, butyl cellulose, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethyl cellulose acetate, carbitol acetate, and γ-butyrolactone; and amine solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide.
[0103] The amount of the solvent added is not particularly limited, and may be an amount such that the solid content in the photosensitive resin composition becomes 5 to 60% by mass, 10 to 50% by mass, or 15 to 40% by mass.
[0104] The preparation means and conditions of the photosensitive resin composition are not particularly limited. For example, a method in which each main component in a predetermined amount is sufficiently stirred and mixed with a stirrer or the like and then kneaded using a mixing roll, an extruder, a kneader, a roll, an extruder, etc. is cited. The kneading method is not particularly limited.
[0105] The relative dielectric constant of the cured product of the photosensitive resin composition of the present embodiment at 10 GHz may be 2.80 or less, 2.75 or less, or 2.70 or less. The dielectric loss tangent of the cured product of the photosensitive resin composition at 10 GHz may be 0.0060 or less, 0.0050 or less, 0.0045 or less, or 0.0040 or less. The relative dielectric constant and dielectric loss tangent may be measured using a cured film of the photosensitive resin composition by the method described in the Examples.
[0106] The photosensitive resin composition of the present embodiment can form a fine pattern. The photosensitive resin composition of the present embodiment can form an insulating film showing low dielectric properties and excellent insulation reliability. A semiconductor element having an interlayer insulating layer formed by a cured product of the above-mentioned photosensitive resin composition and an electronic device comprising the semiconductor element can be produced. The semiconductor element can improve high-frequency characteristics by having a redistribution layer comprising a cured product of the photosensitive resin composition of the present embodiment. The semiconductor element can be, for example, a memory, a package, etc. having a multi-layer wiring structure, a redistribution structure, etc. As an electronic device, for example, a mobile phone, a smart phone, a tablet terminal, a personal computer, and a hard disk suspension can be cited. By having a patterned cured film formed by the photosensitive resin composition of the present embodiment, a semiconductor element and an electronic device with excellent reliability can be provided.
[0107] Example
[0108] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.
[0109] (Synthesis example 1)
[0110] In a 0.3 L flask container equipped with a cooler, a nitrogen inlet tube, a thermocouple, and a stirrer, 30.79 parts by mass of 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride (manufactured by SABIC, product name "BISDA-1000"), 131.28 parts by mass of T-SOL 100 (product name, manufactured by ENEOS Corporation, aromatic high boiling point solvent), and 36.33 parts by mass of SOLMIX A-11 (product name, manufactured by Japan Alcohol Trading Co., Ltd., alcohol solvent) were added. After the addition, the temperature was raised to 80°C, the temperature was maintained for 0.5 hours, and 29.15 parts by mass of dimer diamine (product name "PRIAMINE 1075", manufactured by Croda Japan KK) was added dropwise. After the dropwise addition, 1.44 parts by mass of tris(2-aminoethyl)amine (manufactured by Tokyo Chemical Industry Co., Ltd.) and 4.57 parts by mass of norbornanediamine (manufactured by MITSUI FINE CHEMICALS, INC Co., Ltd.) were sequentially added dropwise, and the mixture was kept warm at 80°C for 0.5 hours. After the warming, 3.52 parts by mass of an aqueous solution of methanesulfonic acid (manufactured by BASF Japan Ltd., product name "Lutropur MSA") was added. Thereafter, the alcohol in the reaction solution was removed and the temperature was raised to 160°C. After the temperature was raised, 40.00 parts by mass of toluene (manufactured by Yamaichi Chemical Industries Co., Ltd.) was added, and a dehydration ring-closure reaction was carried out at 160°C for 2 hours to remove water and alcohol in the reaction solution, thereby obtaining a polyimide resin as an intermediate. Next, the obtained polyimide resin was cooled to 130° C., 11.61 parts by mass of maleic anhydride (manufactured by FUSO CHEMICAL CO., LTD.) was added, and the temperature was raised to 160° C., and a dehydration ring-closure reaction was performed at 160° C. for 4 hours to remove water in the reaction solution, thereby obtaining a maleimide compound.
[0111] The obtained maleic imide compound is placed in a separatory funnel, 500 parts by mass of pure water is added, and the separatory funnel is shaken and allowed to stand. After standing, the aqueous layer and the organic layer are separated, and only the organic layer is recovered. The recovered organic layer is placed in a 0.3L glass container equipped with a cooler, a nitrogen inlet pipe, a thermocouple, a stirrer, and a vacuum pump, and the temperature is raised to 88-93°C. After removing water, the temperature is raised to 100°C, and a portion of the solvent is removed over 0.5 hours under a state of reducing the pressure by 0.1MPa from the atmospheric pressure, thereby obtaining a solution of the maleic imide compound (A-1) as the (A) component.
[0112] (Synthesis example 2)
[0113] A solution of maleimide compound (A-2) was obtained in the same manner as in Synthesis Example 1, except that 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride was replaced with 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (manufactured by JFE Chemical Corporation, product name "BPAF") and the blending amounts of each component were changed as shown in Table 1.
[0114] (Synthesis example 3)
[0115] A solution of a maleimide compound (A-3) was obtained in the same manner as in Synthesis Example 1 except that tris(2-aminoethyl)amine was replaced with 1,3,5-tris(4-aminophenoxy)benzene (manufactured by SEIKA GROUP, product name “TAPOB”) and the blending amounts of the components were changed as shown in Table 1.
[0116] (Non-volatile ingredients)
[0117] After 0.75 g±0.25 g of the solution of the maleimide compound was weighed with a precision balance and placed in a metal petri dish, it was dried at 150° C. for 0.5 hours with a hot air dryer, and the nonvolatile content (NV) was calculated by the following formula.
[0118] NV (mass %) = {(W3-W1) / W2} × 100
[0119] W1: Mass of the empty metal petri dish (g)
[0120] W2: Mass of the maleimide compound solution before drying (g)
[0121] W3: Mass of the dried metal petri dish + maleimide compound (g)
[0122] (Weight average molecular weight)
[0123] The weight average molecular weight (Mw) of the maleic imide compound is measured by GPC (gel permeation chromatography). The maleic imide compound is dissolved in tetrahydrofuran (THF) to make a sample with a concentration of 3 mass%, and 50 μL is injected into a column (GL-R420×1 root, GL-R430×1 root, GL-R440×1 root (all manufactured by Hitachi High-Tech Corporation) heated to 30°C, THF is used as a developing solvent, and the flow rate is 1.6 mL / min. The condition is measured. In addition, the detector uses an L-3350RI detector (manufactured by Hitachi, Ltd.), and the Mw is converted from the dissolution time based on the molecular weight / dissolution time curve made using standard polystyrene (manufactured by TOSOH CORPORATION).
[0124] [Table 1]
[0125]
[0126] As the component (B), the following compounds were prepared.
[0127] A-9300: Tris-(2-acryloyloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name)
[0128] TA-G: 1,3,4,6-Tetraallyl glycoluril (manufactured by SHIKOKU KASEI HOLDINGS CORPORATION, product name)
[0129] TAIC: Triallyl isocyanurate (manufactured by Shinryo Corporation, product name)
[0130] The following compounds were prepared as the component (C), the component (D), a coupling agent, a polymerization inhibitor, a rust inhibitor, and a solvent.
[0131] (C) Component: Oxime ester photopolymerization initiator (manufactured by BASF Japan Ltd., product names "Irgacure OXE01" and "Irgacure OXE02")
[0132] (D) Component: α,α'-bis(tert-butylperoxy)diisopropylbenzene (manufactured by NOF CORPORATION, product name "PERBUTYL P")
[0133] Coupling agent: 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-503")
[0134] Polymerization inhibitor: 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl radical (TEMPOL) (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0135] Rust inhibitor: 1,2,3-benzotriazole (manufactured by JOHOKU CHEMICAL CO., LTD., product name "BT-120")
[0136] Solvent: Mesitylene (manufactured by Toyo Gosei Co., Ltd.)
[0137] [Photosensitive resin composition]
[0138] The components in the amounts (parts by mass, solid content) shown in Table 2 or 3 and 210 parts by mass of a solvent were mixed, stirred at 25° C. for 30 minutes or more, and then filtered through a filter with a mesh size of 0.5 μm to prepare a photosensitive resin composition of an example.
[0139] (Dielectric properties)
[0140] The photosensitive resin composition was applied onto the copper foil using a knife coater, air-dried for 15 minutes, and dried in a dryer at 90° C. for 15 minutes to form a coating film. The coating film was exposed to light using a high-pressure mercury lamp (exposure: 1000 mJ / cm 2 ) and post-exposure baking (100°C, 1 minute) was performed on a hot plate to form a resin film with a thickness of 100 μm. Thereafter, the resin film was cured at 200°C for 2 hours in a nitrogen atmosphere using a clean oven. Next, the copper foil was dissolved and removed using ammonium persulfate to obtain a cured film.
[0141] The cured film was cut into pieces of 80 mm in length and 80 mm in width to prepare evaluation samples. For the evaluation samples, the relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured at room temperature using a SPDR dielectric resonator (manufactured by QWED) and an analyzer (manufactured by Agilent Technologies, product name "PNA Network Analyzer N5227A").
[0142] (Mechanical properties)
[0143] The cured film was cut into a length of 40 mm and a width of 2 mm to prepare an evaluation sample. The evaluation sample was measured using a thermomechanical analyzer (manufactured by TA Instruments Japan Inc., product name "Q-400") under a nitrogen atmosphere, tensile mode, load 5 mN, measurement temperature range -50 to 220 ° C, heating rate 10 ° C / min, and chuck distance 10 mm. The linear expansion coefficient (CTE) was calculated from the displacement of 0 to 40 ° C.
[0144] (5% weight loss temperature)
[0145] 6.0 to 10.0 mg of the cured film was weighed and placed in an open sample container (manufactured by Hitachi High-Tech Corporation, product name "GCA-0055"), and the 5% weight loss temperature (T) was measured under the conditions of a nitrogen flow rate of 300 mL / min, a starting temperature of 40°C, and a heating rate of 10°C / min. d5 As a measuring apparatus, NEXTASTA200RV (manufactured by Hitachi High-Tech Corporation) was used.
[0146] (Micromachinability)
[0147] The photosensitive resin composition was spin-coated on the silicon wafer and heated and dried at 90° C. for 5 minutes using a hot plate to form a resin film with a thickness of 7 μm. Next, an i-ray stepper (manufactured by CERMA PRECISION, INC., product name “Sc6k”) was used at an exposure dose of 300 mJ / cm 2 After the resin film was pattern exposed under the conditions of , it was heated at 100°C for 1 minute using a hot plate. Thereafter, it was developed using a developer (a mixture of cyclopentanone and propylene glycol monomethyl ether acetate) at 25°C for 30 seconds (twice for 15 seconds), and cleaned with propylene glycol monomethyl ether acetate. A metal microscope was used to confirm the peeling of the developed resin film from the silicon wafer, the cracks in the resin film, the roughness at the ends of the pattern, and the residue at the bottom of the pattern after the resin film was developed. The case where these undesirable conditions could not be confirmed and the minimum through-hole diameter was less than 20μm was evaluated as "A", and the case where the minimum through-hole diameter exceeded 20μm was evaluated as "B".
[0148] [Table 2]
[0149]
[0150] [Table 3]
[0151]
Claims
1. A photosensitive resin composition comprising a maleimide compound, a crosslinking agent and a photopolymerization initiator, The maleimide compound is a reaction product of tetracarboxylic dianhydride (a1), diamine (a2), triamine (a3) and maleic anhydride (a4). The diamine (a2) includes a dimer diamine.
2. The photosensitive resin composition according to claim 1, wherein The diamine (a2) contains a second diamine other than the dimer diamine.
3. The photosensitive resin composition according to claim 2, wherein The second diamine is an alicyclic diamine or an aromatic diamine.
4. The photosensitive resin composition according to claim 1, wherein The dimer diamine contains at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2), In formulas (1) and (2), m, n, p and q represent integers greater than 1 selected so as to form m+n=6 to 17 and p+q=8 to 19, respectively. The bond represented by a dotted line refers to a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by a dotted line is a carbon-carbon double bond, formulas (1) and (2) become the following structure: the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond is subtracted by 1 from the number shown in formulas (1) and (2).
5. The photosensitive resin composition according to claim 1, wherein The tetracarboxylic dianhydride (a1) contains 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho [1,2-C] furan-1,3-dione, 9,9-bis (3,4-dicarboxyphenyl) fluorene dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'- (4,4'-isopropylidene diphenoxy) diphthalic anhydride, 4,4'- (hexafluoroisopropylidene) diphthalic anhydride At least one member selected from the group consisting of anhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic 2,3:5,6-dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic 5,5',6,6'-dianhydride and 3,4'-diphthalic anhydride.
6. The photosensitive resin composition according to claim 1, wherein The content of the triamine (a3) is 5 to 35 mol % based on the total amount of the diamine (a2) and the triamine (a3).
7. The photosensitive resin composition according to claim 1, wherein The weight average molecular weight of the maleimide compound is 3,000 to 40,000.
8. The photosensitive resin composition according to claim 1, wherein The maleimide compound has a fluorene skeleton.
9. The photosensitive resin composition according to claim 1, wherein The crosslinking agent includes a polymerizable crosslinking agent having a (meth)acryloyl group.
10. The photosensitive resin composition according to claim 1, wherein The cross-linking agent includes a polymerizable cross-linking agent having an allyl group or a vinyl group. The photosensitive resin composition according to claim 1 , further comprising a thermal polymerization initiator. 12 . A cured product, which is a cured product of the photosensitive resin composition according to claim 1 . 13 . A semiconductor element comprising a redistribution layer comprising a cured product of the photosensitive resin composition according to claim 1 .