Photosensitive resin composition, cured product, and semiconductor element

By using components such as maleimide compounds and crosslinking agents in the photosensitive resin composition, combined with thermal polymerization initiator and coupling agent, the problem of low Tg insulating film is solved, and high Tg and good mediation are achieved The resin composition with electrical properties is suitable for high-frequency semiconductor components.

CN119072660APending Publication Date: 2024-12-03RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480002266.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-01-19
Filing Date
2024-01-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

It is difficult for the conventional photosensitive resin composition to improve the glass transition temperature (Tg) of the insulating film while maintaining the fine processability and dielectric properties, affecting its stability and performance under high temperature conditions.

Method used

A photosensitive resin composition containing a maleimide compound, a crosslinking agent and a photopolymerization initiator is used to form a cured product with a high Tg through a combination of a specific reactant and a crosslinking agent, and is used during the curing process. Thermal polymerization initiator and coupling agent are used to improve the heat resistance and adhesion of the cured substance.

Benefits of technology

It realizes that the glass transition temperature of the insulating film is significantly improved while maintaining the fine processability and dielectric characteristics, and enhances its stability and performance under high temperature conditions, and is suitable for semiconductor components with high frequency characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005095831850000021
    Figure BDA0005095831850000021
  • Figure BDA0005095831850000061
    Figure BDA0005095831850000061
  • Figure BDA0005095831850000062
    Figure BDA0005095831850000062
Patent Text Reader

Abstract

This photosensitive resin composition contains a maleic imide compound, a crosslinking agent, and a photopolymerization initiator, the maleic imide compound being a reactant of a tetracarboxylic acid dianhydride (a1), an amine (a2), and a maleic anhydride (a3), the amine (a2) including a dimer diamine and a second amine other than the dimer diamine, and the photopolymerization initiator being a photopolymerization initiator. At least one of the tetracarboxylic dianhydride (a1) and the amine (a2) contains a compound having a fluorene skeleton.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive resin composition, a cured product and a semiconductor element. Background Art

[0002] With the high integration, miniaturization and micronization of semiconductor elements, the insulating films used for the surface protection layer, interlayer insulating layer, and rewiring layer of semiconductor elements are required to have better electrical properties, heat resistance, mechanical properties, etc. As a material for forming an insulating film having such properties, a photosensitive resin composition containing an alkali-soluble resin has been developed (for example, refer to patent documents 1, 2, and 3). These photosensitive resin compositions are applied and dried on a substrate to form a resin film, and a patterned resin film (a resin film having a pattern) is obtained by exposing and developing the resin film. Then, a patterned cured film (a cured film having a pattern) can be formed by heat curing the above-mentioned patterned resin film, and the patterned cured film can be used as an insulating film.

[0003] Previous technical literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2008-309885

[0006] Patent Document 2: Japanese Patent Application Publication No. 2007-057595

[0007] Patent Document 3: International Publication No. 2010 / 073948 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] For a photosensitive resin composition used to form an insulating film such as a redistribution layer, it is required to increase the glass transition temperature (Tg) of the insulating film while fully maintaining microfabrication and dielectric properties. Therefore, an object of the present invention is to provide a photosensitive resin composition that can form an insulating film with a high Tg while fully maintaining microfabrication and dielectric properties.

[0010] One aspect of the present invention relates to the following photosensitive resin composition, a cured product of the photosensitive resin composition, and a semiconductor device.

[0011] [1] A photosensitive resin composition comprising a maleic imide compound, a crosslinking agent and a photopolymerization initiator, wherein the maleic imide compound is a reaction product of tetracarboxylic dianhydride (a1), an amine (a2) and maleic anhydride (a3), the amine (a2) comprises a dimer diamine and a second amine other than the dimer diamine, and at least one of the tetracarboxylic dianhydride (a1) and the amine (a2) comprises a compound having a fluorene skeleton.

[0012] [2] The photosensitive resin composition according to [1], wherein the tetracarboxylic dianhydride (a1) comprises at least one of 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-c]furan-1,3-dione, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride.

[0013] [3] The photosensitive resin composition according to [1] or [2], wherein the second amine contains at least one of norbornanediamine and 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene.

[0014] [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein the dimer diamine contains at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2),

[0015]

[0016] In formulas (1) and (2), m, n, p and q represent integers greater than 1 selected so as to form m+n=6 to 17 and p+q=8 to 19, respectively. The bond represented by a dotted line refers to a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by a dotted line is a carbon-carbon double bond, formulas (1) and (2) become the following structure: the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond is subtracted by 1 from the number shown in formulas (1) and (2).

[0017] [5] The photosensitive resin composition according to any one of [1] to [4] above, wherein the amine (a2) further contains a triamine.

[0018] [6] The photosensitive resin composition according to any one of [1] to [5] above, wherein the weight average molecular weight of the maleimide compound is 3,000 to 40,000.

[0019] [7] The photosensitive resin composition according to any one of [1] to [6] above, wherein the crosslinking agent comprises a polymerizable crosslinking agent having a (meth)acryloyl group.

[0020] [8] The photosensitive resin composition according to any one of [1] to [7] above, wherein the crosslinking agent comprises a polymerizable crosslinking agent having an allyl group or a vinyl group.

[0021] [9] The photosensitive resin composition according to any one of [1] to [8], further comprising a thermal polymerization initiator.

[0022]

[10] A cured product, which is a cured product of the photosensitive resin composition according to any one of [1] to [9] above.

[0023]

[11] A semiconductor element having a redistribution layer formed from a cured product of the photosensitive resin composition according to any one of [1] to [9] above.

[0024] Effects of the Invention

[0025] According to the invention, there can be provided a photosensitive resin composition capable of forming an insulating film with a high Tg while fully maintaining micromachinability and dielectric properties, a cured product with a high Tg while fully maintaining micromachinability and dielectric properties, and a semiconductor element having a redistribution layer including the cured product. DETAILED DESCRIPTION

[0026] Hereinafter, preferred embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and various modifications can be made without departing from the gist of the present invention.

[0027] In this specification, the numerical range represented by "~" represents the range in which the numerical values ​​recorded before and after "~" are included as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of another stage. In the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. "A or B" can include any one of A and B, or both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. The content of each component in the composition, when there are multiple substances equivalent to each component in the composition, represents the total amount of the multiple substances present in the composition unless otherwise specified.

[0028] In this specification, "layer" and "film" include structures formed on a part of a surface in addition to structures formed on the entire surface when viewed from a top view. The term "process" includes not only independent processes, but also processes that achieve the desired purpose of the process even if they cannot be clearly distinguished from other processes.

[0029] In this specification, "(meth)acryloyl" refers to at least one of "acryloyl" and its corresponding "methacryloyl", and the same applies to other similar expressions such as (meth)acrylic acid and (meth)acrylate. In this specification, "solid content" refers to non-volatile components other than volatile substances (water, solvent, etc.) contained in the photosensitive resin composition, and also includes components that are liquid, syrupy, or waxy at room temperature (about 25°C).

[0030] [Photosensitive resin composition]

[0031] The photosensitive resin composition of the present embodiment contains a maleic imide compound having a specific structure, a crosslinking agent, and a photopolymerization initiator as essential components. The maleic imide compound is a reaction product of tetracarboxylic dianhydride (a1), an amine (a2), and maleic anhydride (a3), the amine (a2) contains a dimer diamine and a second amine other than the dimer diamine, and at least one of the tetracarboxylic dianhydride (a1) and the amine (a2) contains a compound having a fluorene skeleton.

[0032] The photosensitive resin composition of the present embodiment may further contain a thermal polymerization initiator, a coupling agent, a rust inhibitor, a polymerization inhibitor, etc. as needed. The photosensitive resin composition of the present embodiment is a negative photosensitive resin composition, and the cured product of the photosensitive resin composition can be appropriately used as an insulating film for a redistribution layer. Hereinafter, each component used in the photosensitive resin composition of the present embodiment will be described in more detail.

[0033] (Maleimide compound)

[0034] The maleic imide compound (hereinafter, also referred to as "component (A)") of the present embodiment can be obtained by reacting tetracarboxylic dianhydride (a1) (hereinafter, also referred to as "component (a1)"), amine (a2) (hereinafter, also referred to as "component (a2)") and maleic anhydride (a3) ​​(hereinafter, also referred to as "component (a3)"). That is, component (A) is a maleic imide compound formed by reacting component (a1), component (a2) and component (a3). Here, the above-mentioned component (a2) contains a dimer diamine and a second amine other than the dimer diamine. Furthermore, at least one of the above-mentioned component (a1) and the above-mentioned component (a2) contains a compound having a fluorene skeleton. Component (A) may have multiple maleic imide groups in the molecule. Component (A) may be a bismaleic imide compound. Component (A) may be used alone or in combination of two or more.

[0035] As the tetracarboxylic dianhydride of the component (a1), a material known as a raw material of polyimide can be used. As the component (a1), for example, pyromelitic dianhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-C] furan-1,3-dione, 3,3',4,4'-diphenylsulfonic acid tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 3,3',4,4'- -benzophenone tetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride, 1,2,3,4-butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, bicyclo[2.2.2]octane-7-ene-2,3,5,6-tetracarboxylic dianhydride anhydride, bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 1,4-phenylene, 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride, 4,4'-(ethynyl-1,2-diyl)diphthalic anhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, 3,4'-oxydi Phthalic anhydride, 4,4'-oxydiphthalic anhydride, 3,4'-diphthalic anhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane-5,5",6,6"-tetracarboxylic dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic acid-5,5',6,6'-dianhydride and 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride.

[0036] From the viewpoint of low dielectric properties or high Tg, the component (a1) preferably contains 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-C]furan-1,3-dione, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, propyl) diphthalic anhydride, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, dicyclohexyl-3,4,3',4'-tetracarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic 2,3:5,6-dianhydride, 5,5'-bis-2-norbornene-5,5',6,6'-tetracarboxylic 5,5',6,6'-dianhydride, 3,4'-diphthalic anhydride and 9,9-bis[ At least one selected from the group consisting of 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho[1,2-c]furan-1,3-dione, 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride, 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride It is more preferred that the present invention contains at least one selected from the group consisting of 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho [1,2-c] furan-1,3-dione, 9,9-bis (3,4-dicarboxyphenyl) fluorene dianhydride and 9,9-bis [4- (3,4-dicarboxyphenoxy) phenyl] fluorene dianhydride.

[0037] The component (a2) contains a dimer diamine (first amine) and a second amine other than the dimer diamine.

[0038] For example, as described in Japanese Patent Application Laid-Open No. 9-12712, dimer diamine is a compound derived from a dimer of unsaturated fatty acids such as oleic acid, i.e., dimer acid. By using dimer diamine as component (a2), a cured product with excellent dielectric properties can be obtained. In this embodiment, known dimer diamines can be used without particular limitation. The dimer diamine preferably includes at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2).

[0039]

[0040] In formulas (1) and (2), m, n, p and q each represent an integer greater than or equal to 1 selected so as to satisfy m+n=6 to 17 and p+q=8 to 19, and the bond represented by the dotted line refers to a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by the dotted line is a carbon-carbon double bond, formulas (1) and (2) have a structure in which the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond is subtracted by 1 from the number shown in formulas (1) and (2).

[0041] The dimer diamine may be a compound represented by the above general formula (2), and may be a compound represented by the following formula (3) from the viewpoints of solubility in organic solvents, heat resistance, heat-resistant adhesion, low viscosity, and the like.

[0042]

[0043] As a commercial item of dimer diamine, PRIAMINE 1075 and PRIAMINE 1074 (both manufactured by Croda Japan KK) etc. are mentioned, for example.

[0044] The second amine is an amine that does not conform to the above-mentioned dimer diamine. The second amine may be a diamine or a triamine, or may be a diamine. By using an alicyclic diamine as the second amine, the dielectric constant can be made lower. By using an aromatic diamine as the second amine, the elastic modulus and Tg of the cured product can be increased.

[0045] When the second amine is a diamine, examples of the diamine include 1,3-diaminopropane, norbornanediamine, 4,4-methylenedianiline, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)fluorene, 9,9-bis[3-fluoro-4-aminophenyl]fluorene, 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, 4,4'-(hexafluoroisopropylidene)diphenylamine, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.0 2,6] decane, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamino), 4,4'-methylenebis(2-methylcyclohexylamino), 1,1-bis(4-aminophenyl)cyclohexane, 2,7-diaminofluorene, 4,4'-ethylenedianiline, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2-ethyl-6-methylphenyl) amine), 2,2-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]methane, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ketone, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethylbiphenyl-4,4'-diamine , (4,4'-diamino) diphenyl ether, (3,3'-diamino) diphenyl ether, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, 4,4'-diamino-2,2'-diethyl biphenyl, 4,4'-diamino-3,3'-dimethyl biphenyl, 4,4'-diamino-3,3'-diethyl biphenyl, 4,4'-diamino-3,3',5,5'-tetramethyl biphenyl, 4,4'-diamino-3,3',5,5'- Tetraethylbiphenyl, 4,4'-diamino-2,2'-dimethoxybiphenyl, 4,4'-diamino-3,3'-dimethoxybiphenyl, m-xylene diamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 1,4'-bis(4-aminophenoxy)benzene, bis[4-(3-aminophenoxy)phenyl]sulfonamide and bis[4-(4-aminophenoxy)phenyl]sulfonamide.

[0046] When the second amine is a triamine, examples of the triamine include tris(2-aminomethyl)amine, tris(2-aminoethyl)amine, tris(2-aminopropyl)amine, 2-(aminomethyl)-2-methyl-1,3-propylenediamine, trimer triamine, 3,4,4'-triaminodiphenyl ether, 1,2,4-triaminobenzene, 1,3,5-triaminobenzene, 1,2,3-triaminobenzene, 1,3,5-triazine-2,4,6-triamine, 2,4,6-triaminopyrimidine, 1,3,5-tris(4-aminophenyl)benzene, 1,3,5-tris(4-aminophenoxy)benzene, and tris(4-aminophenyl)methane. Among these, aliphatic triamines are preferred from the viewpoint of solubility of the synthesized component (A) in an organic solvent, and tris(2-aminomethyl)amine and tris(2-aminoethyl)amine having a small number of carbon atoms are more preferred from the viewpoint of increasing Tg.

[0047] The second amine may include one of the above-mentioned diamines and triamines, or may include both. Furthermore, the second amine may include an amine other than diamines and triamines.

[0048] From the viewpoint of high Tg and high elastic modulus, the second amine preferably contains at least one of norbornanediamine and 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene.

[0049] In the component (a2), the molar ratio of the second amine to the total amount of amines (the number of moles of the second amine / (the number of moles of the dimer diamine+the number of moles of the second amine)) may be 70 mol% or less, or 50 mol% or less. If the ratio is 70 mol% or less, a cured product having lower dielectric properties can be formed.

[0050] When the second amine includes a diamine, in the component (a2), the molar ratio of the diamine in the second amine to the total amount of diamines (the number of moles of diamine in the second amine / (the number of moles of dimer diamine+the number of moles of diamine in the second amine)) may be 70 mol% or less, or 50 mol% or less. If the ratio is 70 mol% or less, a cured product having lower low dielectric properties can be formed.

[0051] By using dimer diamine as diamine, a cured product with lower low dielectric properties can be formed. On the other hand, when only dimer diamine is used as diamine, the elastic modulus and Tg of the cured product will decrease. In contrast, by using the second amine and dimer diamine together, the elastic modulus and Tg can be improved while maintaining the dielectric properties of the cured product.

[0052] At least one of the above-mentioned (a1) component and (a2) component includes a compound having a fluorene skeleton. By including at least one of the (a1) component and (a2) component constituting the maleimide compound having a compound having a fluorene skeleton, the cured product obtained using the maleimide compound becomes a cured product having a high elastic modulus and a high Tg while fully maintaining a low dielectric constant and a low dielectric loss tangent. From the viewpoint of further improving the elastic modulus and Tg of the cured product, the above-mentioned (a1) component and (a2) component can both include a compound having a fluorene skeleton.

[0053] (A) component can be produced by various known methods. For example, first, (a1) component and (a2) component are subjected to addition polymerization reaction at a temperature of about 60 to 120° C., preferably at a temperature of 70 to 90° C., usually for about 0.1 to 2 hours, preferably for 0.1 to 1.0 hours. Then, the obtained addition polymer is further subjected to an imidization reaction, i.e., a dehydration ring-closure reaction, at a temperature of about 80 to 250° C., preferably at a temperature of 100 to 200° C., for about 0.5 to 30 hours, preferably for 0.5 to 10 hours. Then, the substance obtained by the dehydration ring-closure reaction and (a3) ​​component are subjected to a maleimide reaction, i.e., a dehydration ring-closure reaction, at a temperature of about 60 to 250° C., preferably at a temperature of 80 to 200° C., for about 0.5 to 30 hours, preferably for 0.5 to 10 hours, thereby obtaining the target (A) component.

[0054] In the imidization reaction or the maleimide reaction, various known reaction catalysts, dehydrating agents and organic solvents can be used.

[0055] Examples of the reaction catalyst include aliphatic tertiary amines such as triethylamine, aromatic tertiary amines such as dimethylaniline, heterocyclic tertiary amines such as pyridine, picoline, and isoquinoline, and organic acids such as methanesulfonic acid and p-toluenesulfonic acid monohydrate. Examples of the dehydrating agent include aliphatic anhydrides such as acetic anhydride, and aromatic anhydrides such as benzoic anhydride.

[0056] Examples of the organic solvent include aromatic hydrocarbon solvents such as benzene, toluene, xylene, and trimethylol; alcohol solvents such as methanol, ethanol, isopropanol, butanol, amyl alcohol, hexanol, propylene glycol, and phenol; ether solvents such as anisole; ketone solvents such as acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, cyclopentanone, cyclohexanone, isophorone, and acetophenone; cellulose such as methyl cellulose and ethyl cellulose, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, butyl formate, γ- Ester solvents such as butyrolactone; glycol ether solvents such as ethylene glycol mono-n-butyl ether, ethylene glycol mono-isobutyl ether, ethylene glycol mono-tert-butyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol mono-isobutyl ether, triethylene glycol mono-n-butyl ether, and tetraethylene glycol mono-n-butyl ether; and amine solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide. The organic solvent can be used alone or in combination of two or more.

[0057] The (A) component can be purified by various known methods to improve the purity. For example, first, the (A) component dissolved in the organic solvent and pure water are placed in a separatory funnel. Then, the separatory funnel is shaken and left to stand. Then, after the aqueous layer and the organic layer are separated, only the organic layer is recovered, thereby purifying the (A) component.

[0058] An example of the assumed structure of the component (A) produced by the above method is shown in the following general formula (4).

[0059]

[0060] In the general formula (4), X independently represents a tetravalent organic group, Y independently represents a divalent organic group, and a represents an integer greater than 1. However, at least one of the multiple Ys represents a divalent organic group derived from the above-mentioned dimer diamine, and at least one of the multiple Ys represents a divalent organic group derived from the above-mentioned second amine (diamine). In addition, X and Y may be aliphatic groups, organic groups having alicyclic structures or aromatic rings, and they may contain heteroatoms. However, at least one of X and Y represents a tetravalent organic group having a fluorene skeleton.

[0061] The molecular weight of component (A) can be controlled by the molar numbers of component (a1) and component (a2). The smaller the molar number of component (a1) is than the molar number of component (a2), the lower the molecular weight can be. In order to easily achieve the effect of the present invention, it is usually preferred that the molar number of component (a1) relative to 1 mole of component (a2), i.e., [molar number of component (a1)] / [molar number of component (a2)] is about 0.30 to 1.00, preferably 0.30 to 0.95, more preferably 0.30 to 0.90, and further preferably 0.50 to 0.80.

[0062] The molecular weight of the component (A) may be 3000 or more, 5000 or more, 6000 or more, or 7000 or more, in terms of weight average molecular weight (Mw), or 40000 or less, 38000 or less, 35000 or less, 33000 or less, 30000 or less, 25000 or less, or 20000 or less. When the weight average molecular weight is 40000 or less, the solubility in organic solvents becomes good, and when it is 3000 or more, there is a tendency that the effect of improving heat resistance can be fully obtained. From the viewpoint of solubility in solvents and heat resistance, Mw may be 3000 to 40000, preferably 3000 to 30000, more preferably 5000 to 25000, further preferably 6000 to 23000, and particularly preferably 7000 to 20000. Mw can be measured by gel permeation chromatography (GPC) and converted using a calibration curve of standard polystyrene.

[0063] (Crosslinking agent)

[0064] The crosslinking agent (hereinafter also referred to as "component (B)") may be a polymerizable crosslinking agent. The polymerizable group may be a photopolymerizable group or a thermal polymerizable group. Examples of the polymerizable group include (meth)acryloyl, allyl and vinyl groups. Component (B) may be a polyfunctional compound having two or more polymerizable groups. Furthermore, regarding component (B), for example, when the photosensitive layer is exposed, the crosslinking agents may be crosslinked not only with each other but also with component (A). Furthermore, regarding component (B), for example, when the resin film after pattern formation is heated, the polymerizable crosslinking agents may be crosslinked with each other. Component (B) may be used alone or in combination of two or more.

[0065] From the viewpoint of dielectric properties, the resin composition of the present embodiment may contain a polymerizable crosslinking agent having a (meth)acryloyl group as a crosslinking agent. Regarding the polymerizable crosslinking agent having a (meth)acryloyl group, when the photosensitive layer is exposed, the crosslinking agents are not only crosslinked with each other, but also crosslinked with the (A) component. The polymerizable crosslinking agent having a (meth)acryloyl group may be an acrylate compound or a methacrylate compound. From the viewpoint of dielectric properties, the (B) component may contain a methacrylate compound.

[0066] Examples of the polymerizable crosslinking agent having a (meth)acryloyl group include tricyclodecane dimethanol di(meth)acrylate, tris-(2-(meth)acryloyloxyethyl)isocyanurate, dioxane glycol di(meth)acrylate, alkoxylated glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, alkoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, alkoxylated pentaerythritol tetra(meth)acrylate, 1, 6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, propoxylated ethoxylated bisphenol A (meth)acrylate, dipentatriol poly(meth)acrylate, alkoxylated dipentatriol poly(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, polyethylene glycol di(meth)acrylate and polypropylene glycol di(meth)acrylate.

[0067] From the viewpoints of heat resistance, dielectric properties and fine processing properties, the polymerizable crosslinking agent having a (meth)acryloyl group may include at least one selected from the group consisting of tricyclodecane dimethanol di(meth)acrylate, tris-(2-(meth)acryloyloxyethyl)isocyanurate and dioxane glycol di(meth)acrylate, and from the viewpoints of heat resistance and dielectric properties, may include tris-(2-(meth)acryloyloxyethyl)isocyanurate.

[0068] From the viewpoint of dielectric properties and heat resistance, the resin composition of the present embodiment may contain a polymerizable crosslinking agent having an allyl group or a vinyl group as a crosslinking agent. The polymerizable crosslinking agent having an allyl group or a vinyl group can crosslink the polymerizable crosslinking agents when the patterned resin film is heated.

[0069] Examples of the polymerizable crosslinking agent having an allyl group include 1,3,4,6-tetraallyl glycoluril, triallyl isocyanurate, diallyl monoglycidyl isocyanurate, diallyl monomethyl isocyanurate, diallyl isocyanurate, triallyl trimellitate, and triallyl orthoformate.

[0070] Examples of the polymerizable crosslinking agent having a vinyl group include polyvinyl benzyl compounds and polyvinyl benzyl ether compounds.

[0071] From the viewpoint of dielectric properties and fine processing properties, the polymerizable crosslinking agent having an allyl group or a vinyl group may include at least one selected from the group consisting of 1,3,4,6-tetraallyl glycoluril, triallyl isocyanurate, diallyl isocyanurate and polyvinyl benzyl ether compounds, and from the viewpoint of dielectric properties, may also include 1,3,4,6-tetraallyl glycoluril or triallyl isocyanurate.

[0072] From the viewpoint of further improving the balance between low dielectric properties and fine processing properties, when the total amount of component (A) and component (B) is set to 100 parts by mass, the content of component (B) is preferably less than 50 parts by mass, and can be 1 to 45 parts by mass, 5 to 40 parts by mass, 8 to 30 parts by mass, or 10 to 20 parts by mass.

[0073] (Photopolymerization Initiator)

[0074] The photopolymerization initiator (hereinafter also referred to as "component (C)") is not particularly limited as long as it is a compound that starts polymerization by irradiation with active light (ultraviolet rays, etc.), and examples thereof include alkyl phenone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, intramolecular hydrogen abstraction-type photopolymerization initiators, and oxime ester-based photopolymerization initiators.

[0075] Regarding the alkylphenone-based photopolymerization initiator, for example, it can be purchased as Omnirad 651, Omnirad 184, Omnirad 1173, Omnirad 2959, Omnirad 127, Omnirad 907, Omnirad 369, Omnirad 379EG, etc. manufactured by IGM Resins BV. Regarding the acylphosphine oxide-based photopolymerization initiator, for example, it can be purchased as Omnirad 819, Omnirad TPO H, etc. manufactured by IGM Resins B.V. Regarding the intramolecular hydrogen abstraction type photopolymerization initiator, for example, it can be purchased as Omnirad MBF, Omnirad 754, etc. manufactured by IGM Resins BV. Regarding the oxime ester-based photopolymerization initiator, for example, it can be purchased as Irgacure OXE01, Irgacure OXE02, etc. manufactured by BASF Japan Ltd. In order to promote the photoreaction, a titanocene-based photopolymerization initiator (for example, Irgacure 784 manufactured by BASF Japan Ltd.) may be used in combination.

[0076] From the perspective of easily obtaining excellent micromachinability, the content of component (C) may be 0.1 to 10.0 parts by mass, 0.5 to 8.0 parts by mass, 0.8 to 6.0 parts by mass, or 1.0 to 5.0 parts by mass relative to 100 parts by mass of the total amount of components (A) and (B).

[0077] (Thermal polymerization initiator)

[0078] From the viewpoint of promoting the polymerization reaction of the thermally polymerizable group, the photosensitive resin composition of the present embodiment may further contain a thermal polymerization initiator as the component (D). As the component (D), it is preferred that the compound decomposes by heating during curing to generate free radicals and promote the polymerization reaction of the components (A) and (B). As the component (D), for example, an organic peroxide can be cited.

[0079] Examples of the organic peroxide include methyl ethyl ketone peroxide, methyl cyclohexanone peroxide, methyl acetoacetate peroxide, acetylacetone peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(4,4-di-tert-butylperoxycyclohexyl)propane, 1,1-bis(tert-butylperoxy)cyclododecane, n-butyl-4,4-bis(tert-butylperoxy)valerate, 2,2-bis(tert-butylperoxy)butane, 1,1-bis(tert-butylperoxy)-2-methylcyclohexane, tert-butyl hydroperoxide, and p-butyl hydroperoxide. Menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, tert-hexyl hydroperoxide, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, α,α'-bis(tert-butylperoxy)diisopropylbenzene, tert-butylisopropylbenzene peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3, isobutyryl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, cinnamic acid peroxide, m-Toluoyl peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate Ester, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, α,α'-bis(neodecanoyl peroxy)diisopropylbenzene, isopropylbenzene peroxyneodecanoate, 1,1,3,3,-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoyl peroxy)hexane, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, 1-cyclohexyl Hexyl-1-methylethyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, tert-butyl peroxymaleic acid, tert-butyl peroxylaurate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, tert-butyl peroxyacetate, tert-hexyl peroxybenzoate, tert-butyl peroxy-m-toluoyl benzoate, tert-butyl peroxybenzoate, bis(tert-butylperoxy)isophthalate, tert-butyl peroxyallyl monocarbonate and 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone.

[0080] The content of the component (D) is not particularly limited and may be 0.1 to 10.0 parts by mass, 0.3 to 8.0 parts by mass, 0.5 to 5.0 parts by mass, 0.7 to 3.0 parts by mass, or 0.7 to 2.0 parts by mass relative to 100 parts by mass of the total amount of the components (A) and (B).

[0081] (Coupling agent)

[0082] From the viewpoint of improving the adhesion of the cured product of the photosensitive resin composition, the photosensitive resin composition of the present embodiment may further contain a coupling agent. The coupling agent may be a silane coupling agent. The silane coupling agent may have, for example, a vinyl group, an epoxy group, a styryl group, an acryl group, a methacryl group, an amino group, an ureide group, an isocyanate group, an isocyanurate group, a mercapto group, and the like.

[0083] As silane coupling agents having a vinyl group, KBM-1003, KBE-1003 (product names manufactured by Shin-Etsu Chemical Co., Ltd.. The same applies hereinafter.) and the like can be cited. As silane coupling agents having an epoxy group, KBM-303, 402, 403, KBE-402, 403, X-12-981S, X-12-984S and the like can be cited. As silane coupling agents having a styrene group, KBM-1403 and the like can be cited. As silane coupling agents having a methacryloyl group, KBM-502, 503, KBE-502, 503 and the like can be cited. As silane coupling agents having an acryl group, KBM-5103, X-12-1048, X-12-1050 and the like can be cited. As silane coupling agents having amino groups, KBM-602, 603, 903, 573, 575, KBE-903, 9103P, X-12-972F, etc. can be cited. As silane coupling agents having ureide groups, KBE-585, etc. can be cited. As silane coupling agents having isocyanate groups, KBE-9007, X-12-1159L, etc. can be cited. As silane coupling agents having isocyanurate groups, KBM-9659, etc. can be cited. As silane coupling agents having mercapto groups, KBM-802, 803, X-12-1154, X-12-1156, etc. can be cited. The silane coupling agent can be a silane coupling agent having a methacryloyl group. The silane coupling agent can be used alone or in combination of two or more.

[0084] The content of the silane coupling agent may be 0.01 to 10.0 parts by mass, 0.1 to 8.0 parts by mass, 0.3 to 6.0 parts by mass, 0.5 to 5.0 parts by mass, or 1.0 to 3.0 parts by mass based on 100 parts by mass of the total amount of the components (A) and (B).

[0085] (Rust Inhibitor)

[0086] From the viewpoint of inhibiting the corrosion of copper wiring or preventing the discoloration of copper wiring, the photosensitive resin composition of the present embodiment may further contain a rust inhibitor. As the rust inhibitor, for example, triazole derivatives such as benzotriazole, tetrazole derivatives, etc. can be cited. The rust inhibitor can be used alone or in combination of two or more.

[0087] The content of the rust inhibitor may be 0.01 to 10.0 parts by mass, 0.1 to 5.0 parts by mass, 0.3 to 4.0 parts by mass, 0.5 to 3.0 parts by mass, or 1.0 to 3.0 parts by mass based on 100 parts by mass of the total amount of the components (A) and (B).

[0088] (Polymerization Inhibitor)

[0089] The photosensitive resin composition of the present embodiment may further contain a polymerization inhibitor from the viewpoint of storage stability.

[0090] Examples of the polymerization inhibitor include 4-tert-butylcatechol, 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl radical, p-methoxyphenol, diphenyl-p-benzoquinone, benzoquinone, hydroquinone, gallol, phenothiazine, resorcinol, o-dinitrobenzene, p-dinitrobenzene, m-dinitrobenzene, phenanthraquinone, N-phenyl-2-naphthylamine, cupferroline, 2,5-methoxyquinone, tannic acid, p-benzylaminophenol, tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, and nitrosamines. The polymerization inhibitor may be used alone or in combination of two or more.

[0091] The content of the polymerization inhibitor may be 0.01 to 10.0 parts by mass, 0.05 to 5.0 parts by mass, 0.10 to 2.0 parts by mass, or 0.10 to 1.0 parts by mass based on 100 parts by mass of the total amount of the components (A) and (B).

[0092] (Sensitizer)

[0093] From the viewpoint of achieving both maintenance of the residual film rate in a wide range of exposure amounts and good resolution, the photosensitive resin composition may further contain a sensitizer.

[0094] Examples of the sensitizer include Michler's ketone, benzoin, 2-methylbenzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, 2-tert-butylanthraquinone, 1,2-benzo-9,10-anthraquinone, anthraquinone, methylanthraquinone, 4,4'-bis(diethylamino)benzophenone, acetophenone, benzophenone, thioxanthone, 1,5-acenaphthene, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-[4-(methylthio)phenyl]-2-morpholine-1-propanone, diacetylbenzyl, benzyl dimethyl ketal, benzyl ketal, 1,2-diethyl ketal, diphenyl disulfide, anthracene, phenanthrenequinone, riboflavin tetrabutyrate, acridine orange, erythrosine, phenanthrenequinone, 2-isopropylthioxanthone, 2,6-bis(p-diethylaminobenzylidene)-4-methyl-4-azacyclohexanone, 6-bis(p-dimethylaminobenzylidene)-cyclopentanone, 2,6-bis(p-diethylaminobenzylidene)-4-phenylcyclohexanone, aminophenyl ketone, 3-ketocoumarin compound, biscoumarin compound, N-phenylglycine, N-phenyldiethanolamine and 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone. The sensitizer may be used alone or in combination of two or more.

[0095] When the photosensitive resin composition contains a sensitizer, the content thereof is preferably 0.1 to 2.0 parts by mass, more preferably 0.2 to 1.5 parts by mass, based on 100 parts by mass of the total amount of the component (A) and the component (B).

[0096] (Solvent)

[0097] The photosensitive resin composition of the present embodiment contains a solvent for dissolving / dispersing each component, and can be easily applied on a substrate to form a coating film with uniform thickness. The solvent may be used alone or in combination of two or more.

[0098] As the solvent, for example, there can be mentioned ketone solvents such as methyl ethyl ketone, cyclohexanone, and cyclopentanone; aromatic hydrocarbon solvents such as toluene, xylene, tetramethylbenzene, mesitylene, and trimethylbenzene; glycol ether solvents such as methyl cellulose, butyl cellulose, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethyl cellulose acetate, carbitol acetate, and γ-butyrolactone; and amine solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide.

[0099] The amount of the solvent added is not particularly limited, and may be an amount such that the solid content in the photosensitive resin composition becomes 5 to 60% by mass, 10 to 50% by mass, or 15 to 40% by mass.

[0100] The preparation means and conditions of the photosensitive resin composition are not particularly limited. For example, a method in which each main component in a predetermined amount is sufficiently stirred and mixed with a stirrer or the like and then kneaded using a mixing roll, an extruder, a kneader, a roll, an extruder, etc. is cited. The kneading method is not particularly limited.

[0101] The relative dielectric constant of the cured product of the photosensitive resin composition of the present embodiment at 10 GHz may be 2.80 or less, 2.75 or less, or 2.70 or less. The dielectric loss tangent of the cured product of the photosensitive resin composition at 10 GHz may be 0.0060 or less, 0.0050 or less, 0.0045 or less, or 0.0040 or less. The relative dielectric constant and dielectric loss tangent may be measured using a cured film of the photosensitive resin composition by the method described in the Examples.

[0102] The photosensitive resin composition of the present embodiment can form a fine pattern. The photosensitive resin composition of the present embodiment can form an insulating film showing low dielectric properties and excellent insulation reliability. A semiconductor element having an interlayer insulating layer formed by a cured product of the above-mentioned photosensitive resin composition and an electronic device comprising the semiconductor element can be produced. The semiconductor element can improve high-frequency characteristics by having a redistribution layer comprising a cured product of the photosensitive resin composition of the present embodiment. The semiconductor element can be, for example, a memory, a package, etc. having a multi-layer wiring structure, a redistribution structure, etc. As an electronic device, for example, a mobile phone, a smart phone, a tablet terminal, a personal computer, and a hard disk suspension can be cited. By having a patterned cured film formed by the photosensitive resin composition of the present embodiment, a semiconductor element and an electronic device with excellent reliability can be provided.

[0103] Example

[0104] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.

[0105] (Synthesis example 1)

[0106] In a 0.3 L flask container equipped with a cooler, a nitrogen inlet pipe, a thermocouple, and a stirrer, 26.27 parts by mass of 9,9-bis(3,4-dicarboxyphenyl)fluorene anhydride (product name "BPAF" manufactured by JFE Chemical Corporation), 120.56 parts by mass of T-SOL 100 (product name, manufactured by ENEOS Corporation, aromatic high boiling point solvent), and 32.15 parts by mass of SOLMIX A-11 (product name, manufactured by Nippon Alcohol Trading Co., Ltd., alcohol solvent) were added. After the addition, the temperature was raised to 80° C., the temperature was maintained for 0.5 hours, and 28.20 parts by mass of dimer diamine (product name "PRIAMINE1075", manufactured by Croda Japan KK) was added dropwise. After the dropwise addition, 1.40 parts by mass of tris(2-aminoethyl)amine (manufactured by Tokyo Chemical Industry Co., Ltd.) and 4.42 parts by mass of norbornanediamine (manufactured by MITSUI FINE CHEMICALS, INC Co., Ltd.) were sequentially added dropwise, and the mixture was kept warm at 80°C for 0.5 hours. After the warming, 3.41 parts by mass of an aqueous solution of methanesulfonic acid (manufactured by BASF Japan Ltd., product name "Lutropur MSA") were added. Thereafter, the alcohol in the reaction solution was removed and the temperature was raised to 160°C. After the temperature was raised, 40.00 parts by mass of toluene (manufactured by Yamaichi Chemical Industries Co., Ltd.) was added, and a dehydration ring-closure reaction was carried out at 160°C for 2 hours to remove water and alcohol in the reaction solution, thereby obtaining a polyimide resin as an intermediate. Next, the obtained polyimide resin was cooled to 130° C., 11.24 parts by mass of maleic anhydride (manufactured by FUSO CHEMICAL CO., LTD.) was added, and the temperature was raised to 160° C., and a dehydration ring-closure reaction was performed at 160° C. for 4 hours to remove water in the reaction solution, thereby obtaining a maleimide compound.

[0107] The obtained maleic imide compound is placed in a separatory funnel, 500 parts by mass of pure water is added, and the separatory funnel is shaken and allowed to stand. After standing, the aqueous layer and the organic layer are separated, and only the organic layer is recovered. The recovered organic layer is placed in a 0.3L glass container equipped with a cooler, a nitrogen inlet pipe, a thermocouple, a stirrer, and a vacuum pump, and the temperature is raised to 88-93°C. After removing water, the temperature is raised to 100°C, and a portion of the solvent is removed over 0.5 hours under a state of reducing the pressure by 0.1MPa from the atmospheric pressure, thereby obtaining a solution of the maleic imide compound (A-1) as the (A) component.

[0108] (Synthesis example 2)

[0109] A solution of a maleimide compound (A-2) was obtained in the same manner as in Synthesis Example 1 except that tris(2-aminoethyl)amine was not used and the blending amounts of the components were changed as shown in Table 1.

[0110] (Synthesis example 3)

[0111] A solution of a maleimide compound (A-3) was obtained in the same manner as in Synthesis Example 1 except that tris(2-aminoethyl)amine was not used and the blending amounts of the components were changed as shown in Table 1.

[0112] (Synthesis Example 4)

[0113] A solution of maleimide compound (A-4) was obtained in the same manner as in Synthesis Example 1, except that BPAF was changed to 1,3,3a,4,5,9b-hexahydro-5(tetrahydro-2,5-dioxo-3-furanyl)naphtho[1,2-C]furan-1,3-dione (manufactured by New Japan Chemical Co., Ltd., product name "TDA-100"), norbornanediamine was changed to 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene (manufactured by JFE Chemical Corporation, product name "BPF-AN"), and tris(2-aminoethyl)amine was not used, and the formulation amounts of each component were changed as shown in Table 1.

[0114] (Synthesis Example 5)

[0115] A solution of maleimide compound (A-5) was obtained in the same manner as in Synthesis Example 1, except that tris(2-aminoethyl)amine was not used, T-SOL 100 was replaced with trimethylol (manufactured by Toyo Gosei Co., Ltd., an aromatic high-boiling point solvent) and N-methyl-2-pyrrolidone (NMP), and the blending amounts of each component were changed as shown in Table 1.

[0116] (Non-volatile ingredients)

[0117] After 0.75 g±0.25 g of the solution of the maleimide compound was weighed with a precision balance and placed in a metal petri dish, it was dried at 150° C. for 0.5 hours with a hot air dryer, and the nonvolatile content (NV) was calculated by the following formula.

[0118] NV (mass %) = {(W3-W1) / W2} × 100

[0119] W1: Mass of the empty metal petri dish (g)

[0120] W2: Mass of the maleimide compound solution before drying (g)

[0121] W3: Mass of the dried metal petri dish + maleimide compound (g)

[0122] (Weight average molecular weight)

[0123] The weight average molecular weight (Mw) of the maleic imide compound is measured by GPC (gel permeation chromatography). The maleic imide compound is dissolved in tetrahydrofuran (THF) to make a sample with a concentration of 3 mass%, and 50 μL is injected into a column (GL-R420×1 root, GL-R430×1 root, GL-R440×1 root (all manufactured by Hitachi High-Tech Corporation) heated to 30°C, THF is used as a developing solvent, and the flow rate is 1.6 mL / min. The condition is measured. In addition, the detector uses an L-3350RI detector (manufactured by Hitachi, Ltd.), and the Mw is converted from the dissolution time based on the molecular weight / dissolution time curve made using standard polystyrene (manufactured by TOSOH CORPORATION).

[0124] [Table 1]

[0125]

[0126] As the component (B), the following compounds were prepared.

[0127] A-9300: Tris-(2-acryloyloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name)

[0128] TA-G: 1,3,4,6-Tetraallyl glycoluril (manufactured by SHIKOKU KASEI HOLDINGS CORPORATION, product name)

[0129] TAIC: Triallyl isocyanurate (manufactured by Shinryo Corporation, product name)

[0130] The following compounds were prepared as the component (C), the component (D), a coupling agent, a polymerization inhibitor, a rust inhibitor, and a solvent.

[0131] (C) Component: Oxime ester photopolymerization initiator (manufactured by BASF Japan Ltd., product names "Irgacure OXE01" and "Irgacure OXE02")

[0132] (D) Component: α,α'-bis(tert-butylperoxy)diisopropylbenzene (manufactured by NOF CORPORATION, product name "PERBUTYL P")

[0133] Coupling agent: 3-methacryloxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-503")

[0134] Polymerization inhibitor: 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl radical (TEMPOL) (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0135] Rust inhibitor: 1,2,3-benzotriazole (manufactured by JOHOKU CHEMICAL CO., LTD., product name "BT-120")

[0136] Solvent: Mesitylene (manufactured by Toyo Gosei Co., Ltd.)

[0137] [Photosensitive resin composition]

[0138] The components in the amounts (parts by mass, solid content) shown in Table 2 and 210 parts by mass of a solvent were mixed, stirred at 25° C. for 30 minutes or more, and then filtered through a filter having a mesh size of 0.5 μm to prepare photosensitive resin compositions of Examples 1 to 8.

[0139] (Dielectric properties)

[0140] The photosensitive resin composition was applied onto the copper foil using a knife coater, air-dried for 15 minutes, and dried in a dryer at 90° C. for 15 minutes to form a coating film. The coating film was exposed to light using a high-pressure mercury lamp (exposure: 1000 mJ / cm 2 ) and post-exposure baking (100°C, 1 minute) was performed on a hot plate to form a resin film with a thickness of 100 μm. Thereafter, the resin film was cured at 200°C for 2 hours in a nitrogen atmosphere using a clean oven. Next, the copper foil was dissolved and removed using ammonium persulfate to obtain a cured film.

[0141] The cured film was cut into pieces of 80 mm in length and 80 mm in width to prepare evaluation samples. For the evaluation samples, the relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured at room temperature using a SPDR dielectric resonator (manufactured by QWED) and an analyzer (manufactured by Agilent Technologies, product name "PNA Network Analyzer N5227A").

[0142] (Mechanical properties)

[0143] The cured film was cut into a length of 40 mm and a width of 2 mm to prepare an evaluation sample. The evaluation sample was measured using a thermomechanical analyzer (manufactured by TA Instruments Japan Inc., product name "Q-400") under a nitrogen atmosphere, tensile mode, load 5 mN, measurement temperature range -50 to 220 ° C, heating rate 10 ° C / min, and chuck distance 10 mm. The linear expansion coefficient (CTE) was calculated from the displacement of 0 to 40 ° C.

[0144] (5% weight loss temperature)

[0145] 6.0 to 10.0 mg of the cured film was weighed and placed in an open sample container (manufactured by Hitachi High-Tech Corporation, product name "GCA-0055"), and the 5% weight loss temperature (T) was measured under the conditions of a nitrogen flow rate of 300 mL / min, a starting temperature of 40°C, and a heating rate of 10°C / min. d5 As a measuring apparatus, NEXTASTA200RV (manufactured by Hitachi High-Tech Corporation) was used.

[0146] (Tg)

[0147] The photosensitive resin composition was spin-coated on the silicon wafer with the Cu sputtered film and dried by heating at 90°C for 5 minutes to form a resin film with a thickness of 14 μm. Next, a mask alignment exposure machine (manufactured by Mikasa Corporation, MA-20) was used at an exposure dose of 1000 mJ / cm 2 After pattern exposure in a manner to form a resin film with a width of 10 mm under conditions of , it was heated at 100°C for 1 minute. After developing the exposed resin film with a developer (a mixture of cyclopentanone and propylene glycol monomethyl ether acetate) at 25°C for 30 seconds, it was washed with propylene glycol monomethyl ether acetate and cured at 200°C for 2 hours under a nitrogen atmosphere. The silicon wafer on which the patterned cured film was formed was immersed in an aqueous solution of ammonium persulfate, and the cured film was peeled off from the silicon wafer. The cured film was washed with pure water to obtain a short strip of resin film with a width of 10 mm. The resin film was cut into a length of 50 mm, and Tg was measured using a dynamic viscoelasticity measuring device (manufactured by TA Instruments Japan Inc., product name "RSAG2") at a distance of 20 mm between the chucks and a measuring temperature range of -50 to 350°C.

[0148] (Micromachinability)

[0149] The photosensitive resin composition was spin-coated on the silicon wafer and heated and dried at 90° C. for 5 minutes using a hot plate to form a resin film with a thickness of 7 μm. Next, an i-ray stepper (manufactured by CERMA PRECISION, INC., product name “Sc6k”) was used at an exposure dose of 300 mJ / cm 2 After the resin film was pattern exposed under the conditions of , it was heated at 100°C for 1 minute using a hot plate. Thereafter, it was developed using a developer (a mixture of cyclopentanone and propylene glycol monomethyl ether acetate) at 25°C for 30 seconds (twice for 15 seconds), and cleaned with propylene glycol monomethyl ether acetate. A metal microscope was used to confirm the peeling of the developed resin film from the silicon wafer, the cracks in the resin film, the roughness at the ends of the pattern, and the residue at the bottom of the pattern after the resin film was developed. The case where these undesirable conditions could not be confirmed and the minimum through-hole diameter was less than 20μm was evaluated as "A", and the case where the minimum through-hole diameter exceeded 20μm was evaluated as "B".

[0150] [Table 2]

[0151]

Claims

1. A photosensitive resin composition comprising a maleimide compound, a crosslinking agent and a photopolymerization initiator, The maleimide compound is a reaction product of tetracarboxylic dianhydride (a1), amine (a2) and maleic anhydride (a3). The amine (a2) includes a dimer diamine and a second amine other than the dimer diamine, At least one of the tetracarboxylic dianhydride (a1) and the amine (a2) includes a compound having a fluorene skeleton.

2. The photosensitive resin composition according to claim 1, wherein The tetracarboxylic dianhydride (a1) includes at least one of 1,3,3a,4,5,9b-hexahydro-5 (tetrahydro-2,5-dioxo-3-furanyl) naphtho [1,2-C] furan-1,3-dione, 9,9-bis (3,4-dicarboxyphenyl) fluorene dianhydride, and 9,9-bis [4- (3,4-dicarboxyphenoxy) phenyl] fluorene dianhydride.

3. The photosensitive resin composition according to claim 1, wherein The second amine contains at least one of norbornanediamine and 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene.

4. The photosensitive resin composition according to claim 1, wherein The dimer diamine contains at least one of a compound represented by the following general formula (1) and a compound represented by the following general formula (2), In formulas (1) and (2), m, n, p and q represent integers greater than 1 selected so as to form m+n=6 to 17 and p+q=8 to 19, respectively. The bond represented by a dotted line refers to a carbon-carbon single bond or a carbon-carbon double bond. When the bond represented by a dotted line is a carbon-carbon double bond, formulas (1) and (2) become the following structure: the number of hydrogen atoms bonded to each carbon atom constituting the carbon-carbon double bond is subtracted by 1 from the number shown in formulas (1) and (2).

5. The photosensitive resin composition according to claim 1, wherein The amine (a2) further comprises a triamine.

6. The photosensitive resin composition according to claim 1, wherein The weight average molecular weight of the maleimide compound is 3,000 to 40,000.

7. The photosensitive resin composition according to claim 1, wherein The crosslinking agent includes a polymerizable crosslinking agent having a (meth)acryloyl group.

8. The photosensitive resin composition according to claim 1, wherein The cross-linking agent includes a polymerizable cross-linking agent having an allyl group or a vinyl group. 9 . The photosensitive resin composition according to claim 1 , further comprising a thermal polymerization initiator. 10 . A cured product, which is a cured product of the photosensitive resin composition according to claim 1 . 11 . A semiconductor element comprising a redistribution layer comprising a cured product of the photosensitive resin composition according to claim 1 .