Polymer modified lithium material, negative pole piece, secondary battery, power utilization device, method and application

CN119072795APending Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280095207.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-08-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing lithium metal rechargeable batteries suffer from rapid cycle life degradation and lithium dendrite formation, leading to decreased battery performance and safety risks.

Method used

By using polymer-modified lithium materials, a dense and flexible polymer layer is formed on the surface of the lithium anode. Through chemical bonding, it adheres tightly to the lithium metal surface, inhibiting the contact reaction between the electrolyte and lithium, regulating the deposition morphology of lithium ions, suppressing dendrite formation, and improving the interfacial conductivity.

Benefits of technology

It extends battery cycle life, reduces electrolyte and lithium consumption, lowers short-circuit risk, improves coulombic efficiency and lithium-ion transfer efficiency, and enhances battery safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072795A_ABST
    Figure CN119072795A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer modified lithium material, which comprises a lithium-containing metal and a polymer Poly chemically connected to the lithium surface of the lithium-containing metal, and the polymer Poly comprises a structure as shown in a formula I; each group appears at each time, Rf is independently a fluorine-substituted aliphatic group, X is independently H or an electron withdrawing group, A is independently O, S or NR11, R11 is H or C1-3 alkyl, Z2 is independently a bond, carbonyl,-(O =) P (-O-) 2,-S (= O) 2-,-C (= O)-NH-or LC-Z0, Lc is C1-3 alkylene, and Z0 is a coupling linker; n > = 10; m < = 10; at least one cyano group in Poly forms a chemical connection with lithium in the lithium-containing metal. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Polymer-modified lithium material, negative electrode sheet, secondary battery, power-consuming device, method and application Technical Field

[0001] The present application relates to the technical field of lithium metal secondary batteries, and more specifically to polymer-modified lithium materials, negative electrode sheets, electrode assemblies, secondary batteries, battery modules, battery packs, electrical devices, methods, and applications. Background Art

[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0003] With the accelerated pace of life and the development of various electronic products such as smart phones, tablets, smart wearables, power tools and electric vehicles, lithium metal secondary batteries with high energy density are becoming more and more popular, and high energy density is an irreversible trend in the future development of lithium metal secondary batteries.

[0004] However, lithium metal secondary batteries currently on the market often suffer from problems such as rapid decay of cycle life and lithium dendrites.

[0005] Summary of the Invention

[0006] In view of the above problems, the present application provides a polymer-modified lithium material, a negative electrode plate, an electrode assembly, a secondary battery, a battery module, a battery pack, an electrical device, a method and an application. By using this polymer-modified lithium material, a tightly fitting, dense, flexible polymer layer can be formed on the surface of the lithium negative electrode, effectively inhibiting the contact reaction between the electrolyte and lithium, reducing the consumption of lithium for the electrolyte, extending the battery life, and further, effectively inhibiting the dendrite short-circuit problem.

[0007] In a first aspect, the present application provides a polymer-modified lithium material, which includes a lithium-containing metal and a polymer Poly chemically connected to the lithium in the lithium-containing metal, wherein the polymer Poly comprises a structure shown in Formula I;

[0008]

[0009] in,

[0010] Each occurrence of Rf is independently a fluorine-substituted aliphatic group;

[0011] Each occurrence of X is independently H or an electron withdrawing group;

[0012] Each occurrence of A is independently O, S or NR 11 ; Among them, R 11 H or C 1-3 alkyl;

[0013] Each occurrence of Z2 is independently a bond, carbonyl, -(O=)P(-O-)2, -S(=O)2--C(=O)-NH- or L C -Z0, where Lc is C 1-3 Alkylene, Z0 is a coupling type linking group;

[0014] * indicates the site of attachment of the terminal groups;

[0015] n is an integer selected from ≥10;

[0016] m is a positive integer ≤ 10;

[0017] At least one cyano group in the polymer Poly forms a chemical connection with lithium in the lithium-containing metal.

[0018] In this polymer-modified lithium material, the polymer "Poly" forms a dense and uniform flexible polymer layer on the surface of the lithium-containing metal. This flexible polymer layer can tightly adhere to the lithium-containing metal surface. When formed on the lithium-containing metal surface of the lithium metal battery negative electrode, this polymer layer can act as a protective layer at the lithium metal battery negative electrode, effectively inhibiting the contact reaction between the electrolyte and lithium, reducing the consumption of electrolyte and lithium, improving coulombic efficiency, and extending cycle life. The polymer Poly carries a large number of cyano groups, one or more of which can form a stable chemical bond (further, a covalent bond) with the lithium in the lithium-containing metal, firmly binding the polymer layer to the surface of the lithium-containing metal. Therefore, when the volume of the negative electrode changes during the charge and discharge process, the polymer layer can be prevented from peeling off from the surface of the lithium-containing metal. The polymer Poly contains a large number of fluorine-substituted aliphatic groups as side groups. On the one hand, these aliphatic side groups with a certain length can enhance the elasticity of the polymer layer and prevent the polymer layer from breaking under large volume deformation. On the other hand, the introduction of fluorine elements can effectively regulate the uniform deposition of lithium ions, improve the deposition morphology of lithium dendrites in lithium metal batteries under a certain charging current density, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium negative electrode side. The side chain of the polymer Poly also introduces an EO segment (composed of m ethylene oxide units), which can improve the flexibility and elasticity of the polymer layer, facilitate the close fit between the protective layer and the electrode and diaphragm, and reduce the interface impedance. In addition, the dense and uniform flexible polymer layer can also be swollen by the electrolyte and can provide a relatively high ionic conductivity (such as 10 -3 S / cm), thereby ensuring efficient lithium ion transfer within the polymer layer and at the lithium interface, greatly reducing interfacial polarization in the battery cell. The various structural units of the polymer Poly work together to form a technical whole that provides the aforementioned multi-dimensional comprehensive excellent effects.

[0019] In some embodiments, each occurrence of m is independently 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10.

[0020] In some embodiments, each occurrence of m is independently 1, 2, 3, 4, 5, 6, 7, or 8.

[0021] Also preferably, m is independently 1, 2, 3, 4, 5 or 6 at each occurrence.

[0022] Also preferably, m is independently 1, 2, 3, 4 or 5 at each occurrence.

[0023] Also preferably, m is independently 1, 2 or 3 at each occurrence.

[0024] Also preferably, m is independently 2, 3, 4, 5 or 6 at each occurrence.

[0025] Also preferably, m is independently 2, 3, 4 or 5 at each occurrence.

[0026] Also preferably, m is independently 2 or 3 at each occurrence.

[0027] In the general formula (I), m reflects the number of EO units (ethylene oxide units) with the structure of "CH2CH2O". By introducing EO segments, the flexibility and elasticity of the polymer layer can be improved, which is beneficial to the close fit between the protective layer and the electrode and the diaphragm, and the interface impedance is reduced. By adjusting the size of m, the number of EO units can be controlled (that is, the length of the EO segment can be controlled), the flexibility and elasticity of the polymer can be regulated, and the elastic deformation of the protective layer and the degree of fit between the protective layer and the substrate and the diaphragm can be regulated. Larger elastic deformation can well adapt to the larger volume expansion of the negative electrode side during charging and prevent the protective layer from breaking; better flexibility is beneficial to the close fit between the protective layer and the lithium metal and diaphragm side, reducing the interface impedance. By controlling m within a suitable range or size, it can also work synergistically with other structural units of the polymer Poly (such as Rf chain, X group) to achieve the aforementioned multi-dimensional comprehensive excellent effect. When the polymer Poly is prepared by in-situ polymerization, by controlling m within a suitable range or size, the flexibility of the polymer layer can be effectively adjusted while maintaining a high reaction rate and effective grafting density, thereby maintaining high density of the polymer layer.

[0028] In some embodiments, each occurrence of Rf has a fluorine substitution ratio of >50% independently;

[0029] Preferably, the fluorine substitution rate in Rf independently satisfies ≥55%;

[0030] Preferably, the fluorine substitution rate in Rf independently satisfies ≥60%;

[0031] Preferably, the fluorine substitution rate in Rf independently satisfies ≥65%;

[0032] Preferably, the fluorine substitution rate in Rf independently satisfies ≥70%;

[0033] Preferably, the fluorine substitution rate in Rf independently satisfies ≥80%;

[0034] Preferably, at least 50% of the Rf in the polymer Poly satisfies a fluorine substitution rate ≥80%, or ≥90%;

[0035] Preferably, at least 60% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥70%, or ≥80%, or ≥90%;

[0036] Preferably, at least 70% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥60%, or ≥70%, or ≥80%, or ≥90%;

[0037] Preferably, at least 80% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥50%, or ≥60%, or ≥70%, or ≥80%, or ≥90%.

[0038] In some embodiments, at each occurrence of Rf, the number of fluorine atoms in Rf is independently an integer ≥ 4;

[0039] Preferably, the number of fluorine atoms in Rf is independently an integer selected from 4 to 20;

[0040] Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 16;

[0041] Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 15;

[0042] Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 13;

[0043] Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 10;

[0044] Also preferably, the number of fluorine atoms in Rf is independently 4, 5, 6, 7, 8, 9, 10, 11, 12 or 13.

[0045] In some embodiments, the mass percentage of fluorine element in the polymer Poly is selected from 10% to 50%;

[0046] Preferably, the mass proportion of fluorine element in the polymer Poly is selected from 15% to 50%;

[0047] Another preferred embodiment is that the mass proportion of fluorine element in the polymer Poly is selected from 20% to 50%.

[0048] By controlling the fluorine substitution rate in Rf, the number of fluorine atoms in Rf, and the mass fraction of fluorine in the polymer (Poly), the uniform deposition of lithium ions can be optimally controlled, the formation of lithium dendrites can be suppressed, the lithium ion cycle life can be improved, the risk of short circuits can be reduced, and the volume expansion of the lithium negative electrode can be alleviated. Taking the mass fraction of fluorine in the polymer (Poly) as an example, it is beneficial to improve the morphology of lithium dendrite deposition and alleviate the volume expansion of the lithium negative electrode in lithium metal batteries at a certain charging current density.

[0049] In some embodiments, each occurrence of Rf contains 2 to 10 backbone carbon atoms;

[0050] Preferably, Rf contains 2 to 8 main chain carbon atoms;

[0051] Another preferred embodiment is that Rf contains 2 to 7 main chain carbon atoms;

[0052] Also preferably, Rf contains 3, 4, 5, 6, 7 or 8 main chain carbon atoms;

[0053] Another preferred embodiment is: The chain length is selected from 5 to 40, preferably from 5 to 35, preferably from 5 to 30, preferably from 6 to 40, preferably from 6 to 35, preferably from 6 to 30, preferably from 8 to 40, preferably from 8 to 35, preferably from 8 to 30, preferably from 10 to 40, preferably from 10 to 35, preferably from 10 to 30; the chain length refers to the number of backbone atoms of the longest backbone connecting the carbonyl site and the terminal group in Rf.

[0054] In some embodiments, each occurrence of Rf has an integer number of carbon atoms selected from 2 to 10;

[0055] Preferably, the number of carbon atoms in Rf is an integer selected from 2 to 8;

[0056] Another preferred embodiment is that the number of carbon atoms in Rf is an integer selected from 2 to 7;

[0057] Also preferably, the number of carbon atoms in Rf is 3, 4, 5, 6, 7 or 8.

[0058] By controlling the main chain carbon atoms in Rf, the length of the Rf side group can be adjusted by further controlling the number of carbon atoms in Rf, thereby giving the polymer layer appropriate elasticity and better preventing the polymer layer from rupturing under large volume deformation.

[0059] By controlling the chain length of the EO-Rf chain to an appropriate length, the advantages of the aforementioned Rf and EO segments can be achieved, the corresponding monomers can have a higher reaction rate, and the steric effect of the chain length can be avoided from affecting the distribution density of the connection points between the polymer Poly and the lithium-containing metal, thereby achieving a firmly connected, tightly fitting, and dense polymer layer.

[0060] In some embodiments, each occurrence of Rf further comprises one or more heteroatoms selected from the group consisting of iodine, nitrogen, oxygen, sulfur, silicon, boron, and phosphorus.

[0061] In some embodiments, for each occurrence of Rf, the number of any one of said heteroatoms in Rf is 1 or more;

[0062] Preferably, the number of any one of the heteroatoms in Rf is selected from 1 to 5;

[0063] Also preferably, the number of any one of the heteroatoms in Rf is selected from 1, 2, 3 or 4.

[0064] In some embodiments, for each occurrence of Rf, the number of heteroatoms in Rf satisfies one or more of the following:

[0065] The number of oxygen atoms in Rf is 1, 2, 3, 4 or 5;

[0066] The number of nitrogen atoms in Rf is 1, 2 or 3;

[0067] The number of sulfur atoms in Rf is 1, 2, or 3;

[0068] The number of phosphorus atoms in Rf is 1 or 2;

[0069] The number of iodine atoms in Rf is 1, 2, 3, 4, 5 or 6;

[0070] The number of silicon atoms in Rf is 1 or 2; and

[0071] The number of boron atoms in Rf is 1 or 2.

[0072] In some embodiments, each occurrence of Rf contains one or more selected from iodo, -NR 12 -, -O-, -S-, -S(O)2-, >Si<, >B- and >P(=O)-, wherein R 12 H or C 1-3 alkyl;

[0073] Preferably, R 12 is H or methyl;

[0074] Another preferred embodiment is that R 12 For H.

[0075] In some embodiments, each occurrence of Rf contains one or more atoms or groups of atoms selected from the group consisting of -O-, -S(O)2-, and -(O=)P(-O-)2;

[0076] Preferably, Rf contains one or more -O-;

[0077] Another preferred embodiment is that Rf contains -S(O)2F;

[0078] Another preferred embodiment is that Rf contains -(O=)P(-O-)2.

[0079] By introducing heteroatoms other than fluorine atoms into Rf, such as one or more heteroatoms from iodine, nitrogen, oxygen, sulfur, silicon, boron, and phosphorus, special properties can be imparted to the polymer layer. For example, phosphorus has a certain flame retardant effect. Iodine can also play a role in regulating lithium ion deposition. For another example, sulfonyl fluoride groups have a certain effect on improving the ionic conductivity of the polymer layer.

[0080] In some embodiments, each occurrence of the fluorine-substituted aliphatic group is independently a linear or branched structure.

[0081] The linear Rf is beneficial to improving the flexibility of the polymer material, while the branched Rf is beneficial to improving the swelling capacity of the electrolyte membrane, thereby improving the ionic conductivity.

[0082] In some embodiments, each occurrence of Rf has a structure independently represented by Formula III-1, Formula III-2, or Formula III-3:

[0083]

[0084] Among them, R 31 、R 32 and R 3 Each occurrence is independently H or F; each occurrence of m3 is independently an integer selected from 2 to 10; in formula III-1, there are at least 4 F atoms;

[0085] Preferably, m3 is an integer selected from 3 to 10;

[0086] Another preferred embodiment is that m3 is an integer selected from 3 to 8;

[0087] Another preferred embodiment is that m3 is 3, 4, 5, 6, 7 or 8;

[0088] R 41a 、R 42a 、R 4a 、R 41b 、R 42b and R 4bEach occurrence is independently H or F; m 4a and m4 4b Each occurrence is independently an integer selected from 1 to 9 (1, 2, 3, 4, 5, 6, 7, 8 and 9); contains at least 4 F atoms in formula III-2;

[0089] Preferably, m 4a and m4 4b are each independently an integer selected from 2 to 9;

[0090] Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 2 to 8;

[0091] Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 3 to 8;

[0092] Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 3 to 6;

[0093] R 51 and R 52 Each occurrence is independently H or F; each occurrence of m5 is independently an integer selected from 2 to 10; in formula III-3, there are at least 4 F atoms;

[0094] Preferably, m5 is an integer selected from 3 to 10;

[0095] Another preferred embodiment is that m5 is an integer selected from 3 to 8;

[0096] Another preferred embodiment is that m5 is 3, 4, 5, 6, 7 or 8.

[0097] In some embodiments, each occurrence of Rf has a structure as shown in Formula III-1;

[0098] Alternatively, each time Rf appears, the structure of Rf is as shown in Formula III-2;

[0099] Alternatively, each time Rf appears, the structure of Rf is as shown in Formula III-3.

[0100] Among them, the structure of formula III-1 is a linear saturated fluorinated aliphatic chain. On the one hand, it can give the polymer layer better elasticity to prevent the polymer layer from breaking under large volume deformation. On the other hand, the fluorine element can effectively regulate the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium negative electrode side.

[0101] The structure of formula III-2 can be introduced with a phosphorus element, and further Z2 is a bond (ie, does not exist), at this time -(CH2CH2O) m -Rf form a phosphate group, which has a flame retardant effect and is beneficial to improving the safety performance of the battery cell.

[0102] The structure of formula III-3 can introduce a sulfonyl fluoride group, which has a certain positive effect on improving the ionic conductivity of the polymer layer.

[0103] In some embodiments, each occurrence of Formula III-1 has 0, 1, 2, 3, or 4 H atoms; each occurrence of Formula III-2 has 0, 1, 2, 3, 4, 5, or 6 H atoms; each occurrence of Formula III-3 has 0, 1, 2, 3, or 4 H atoms;

[0104] Preferably, each time Formula III-1 appears, the number of H atoms therein is 0; each time Formula III-2 appears, the number of H atoms therein is 0; each time Formula III-3 appears, the number of H atoms therein is 0.

[0105] By controlling the number of H atoms, the number of sites available for fluorine substitution can be controlled.

[0106] In some embodiments, each occurrence of Rf is independently selected from any one of the following structures:

[0107]

[0108] In some embodiments, each occurrence of X is independently H or an electron withdrawing group containing 1 to 6 non-hydrogen atoms.

[0109] In some embodiments, each occurrence of X is independently H or cyano, nitro, or -NR 21 R 22 ; Among them, R 21 and R 22 Each independently is H or C 1-3 alkyl;

[0110] Preferably, R 21 and R 22 are each independently H or methyl;

[0111] Another preferred embodiment is that R 21 and R 22 All are methyl.

[0112] The introduction of an electron-withdrawing group at the X position is beneficial to increasing the reactivity of the carbon-carbon double bond in the cyanoacrylic acid derivative monomer during the formation of the polymer layer, thereby promoting the in-situ polymerization reaction.

[0113] In some embodiments, each occurrence of A is independently O, S, or NH;

[0114] Preferably, each occurrence of A is independently O or NH;

[0115] Another preferred embodiment is that each occurrence of A is O;

[0116] Alternatively, each occurrence of A is NH.

[0117] Linker A can be formed by coupling -COOH or its derivatives (e.g., acyl chlorides, activated N-succinimidyl esters of carboxyl groups) in cyanoacrylate derivative monomers with various reactive functional groups to form reactive functional group pairs. These pairs can then form different types of chemical bonds through coupling reactions. For example, when A is O, S, or NH, it can be formed through coupling reactions between -COOH or its derivatives (e.g., -OH, -SH, or -NH2) in cyanoacrylate derivative monomers. The diverse nature of A is the result of flexible combinations of reactive monomers.

[0118] In some embodiments, Rf in Formula I is the same; each occurrence of X in Formula I is the same; each occurrence of A in Formula I is the same; and further, each occurrence of Z2 in Formula I is the same. In this case, a single type of monomer can be used for the polymerization reaction.

[0119] In some embodiments, n is an integer selected from 10 to 1000, preferably an integer selected from 10 to 950, preferably an integer selected from 10 to 800, preferably an integer selected from 15 to 800, preferably an integer selected from 20 to 800, preferably an integer selected from 40 to 800, preferably an integer selected from 50 to 800, preferably an integer selected from 100 to 800, preferably an integer selected from 10 to 750, preferably an integer selected from 15 to 750, preferably an integer selected from 20 to 750. An integer, further preferably an integer selected from 40 to 750, further preferably an integer selected from 50 to 750, further preferably an integer selected from 80 to 750, further preferably an integer selected from 100 to 750, further preferably an integer selected from 10 to 600, further preferably an integer selected from 15 to 600, further preferably an integer selected from 20 to 600, further preferably an integer selected from 40 to 600, further preferably an integer selected from 50 to 600, further preferably an integer selected from 100 to 600, further preferably an integer selected from 100 to 200.

[0120] In some embodiments, the number average molecular weight of the polymer Poly is selected from 10 kDa to 200 kDa;

[0121] Preferably, the number average molecular weight of the polymer Poly is selected from 50 kDa to 100 kDa.

[0122] In Formula I, n is numerically equal to the degree of polymerization (DP) of the polymer (Poly). Controlling n allows for regulation of the molecular weight of the polymer (Poly). Adjusting the DP or molecular weight allows for adjusting the molecular chain length of the polymer (Poly), effectively encapsulating the lithium-containing metal while maintaining a stable chemical connection and affecting the density and uniformity of the polymer layer.

[0123] In some embodiments, the amount of lithium in the lithium-containing metal relative to the polymer Poly is greater than the amount of the catalyst, calculated on a molar ratio;

[0124] Preferably, the lithium-containing metal comprises lithium metal or lithium alloy;

[0125] In another embodiment, the lithium alloy contains lithium and further contains one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium.

[0126] In this polymer-modified lithium material, the lithium metal can successfully catalyze the in-situ polymerization of cyanoacrylate derivative monomers on the lithium metal surface as long as the lithium metal provides a catalytic amount. The amount of lithium metal relative to the polymer Poly only requires contact with the catalyst to catalyze the in-situ polymerization of cyanoacrylate monomers on the lithium metal surface.

[0127] In a second aspect, the present application provides a negative electrode sheet, wherein the negative electrode sheet comprises a stacked negative electrode sheet substrate and a polymer layer; the negative electrode sheet substrate comprises a lithium-containing layer in contact with the polymer layer, the lithium-containing layer contains lithium, and the polymer layer is chemically connected to at least a portion of the lithium in the lithium-containing layer;

[0128] Wherein, the polymer layer comprises the polymer Poly defined in the first aspect of the present application.

[0129] A dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer on at least one side of the negative electrode plate. The flexible polymer layer can be tightly adhered to the surface of the lithium-containing layer, and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve coulombic efficiency, and extend the cycle life.

[0130] In some embodiments, the amount of lithium in the lithium-containing layer relative to the polymer Poly is greater than the amount of the catalyst, calculated on a molar ratio;

[0131] Preferably, the lithium-containing layer comprises lithium metal or a lithium alloy.

[0132] Also preferably, the lithium-containing layer consists essentially of lithium metal.

[0133] Alternatively, the lithium-containing layer is a lithium alloy.

[0134] Preferably, the lithium alloy contains lithium and further contains one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium;

[0135] Also preferably, the lithium-containing layer consists essentially of lithium metal;

[0136] Alternatively, the lithium-containing layer is a lithium alloy.

[0137] In some embodiments, the polymer layer further contains an electrolyte, which is beneficial for providing better ionic conductivity.

[0138] In some embodiments, the electrolyte contains a lithium salt and an electrolyte solvent.

[0139] In some embodiments, the lithium salt is selected from one or more of lithium hexafluorophosphate, tetrafluoroboric acid, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate, and lithium bis(oxalatoborate);

[0140] Preferably, the electrolyte solvent is selected from one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, diphenyl carbonate, dibutyl carbonate, butylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, dioxolane, methyl nonafluoro-n-butyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, octafluoropentyl-tetrafluoroethyl ether, 1,2-bis(cyanoethoxy)ethane, diphenyl ether and 18-crown-6.

[0141] In some embodiments, the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 5 mol / L;

[0142] Preferably, the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 4 mol / L;

[0143] Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 2 mol / L to 4 mol / L;

[0144] Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 3 mol / L;

[0145] Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 2 mol / L.

[0146] The concentration of lithium salt in the electrolyte will also affect the deposition morphology of lithium ions. +The solvation effect affects the composition of the solid electrolyte interface film (SEI film) and the deposition morphology of lithium ions. By controlling the lithium salt in the electrolyte at an appropriate concentration, dense and uniform lithium ion deposition and minimal volume expansion can be achieved. In addition, by controlling the lithium salt in the electrolyte at an appropriate concentration, the polymer layer can also have suitable mechanical properties, avoiding the detrimental effect of excessive lithium salt concentration on mechanical properties. It can also achieve better lithium ion conductivity during charging and discharging, avoiding poor lithium ion conductivity due to insufficient lithium salt concentration.

[0147] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:2;

[0148] Preferably, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:1;

[0149] Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:2;

[0150] Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:1;

[0151] Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1.5:1;

[0152] Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 4:1 to 1.5:1.

[0153] In some embodiments, the electrolyte accounts for a mass percentage of 9.5% to 65% in the polymer layer;

[0154] Preferably, the mass proportion of the electrolyte in the polymer layer is selected from 10% to 60%;

[0155] Another preferred embodiment is that the mass proportion of the electrolyte in the polymer layer is selected from 20% to 60%;

[0156] Another preferred embodiment is that the mass proportion of the electrolyte in the polymer layer is selected from 25% to 40%;

[0157] In another embodiment, the mass proportion of the electrolyte in the polymer layer is selected from 30% to 50%.

[0158] The mass ratio of the electrolyte in the polymer layer can be adjusted by controlling the mass ratio of the polymer Poly and the electrolyte within a suitable range. The mass ratio of the electrolyte in the polymer layer will affect the elasticity and ionic conductivity of the protective layer. The presence of a certain amount of lithium salt and solvent has a plasticizing effect on the polymer layer, which can improve the elasticity of the polymer layer. In addition, during the in-situ polymerization process of the polymer layer, the lithium salt and solvent are incorporated into the interior of the polymer layer. On a microscopic scale, the polymer layer has a sponge-like loose porous structure, and the pores are filled with electrolyte, providing a path for the subsequent transmission of lithium ions.

[0159] In some embodiments, the thickness of the polymer layer is selected from 5 nm to 10 μm;

[0160] Preferably, the thickness of the polymer layer is selected from 50 nm to 8 μm;

[0161] Another preferred embodiment is that the thickness of the polymer layer is selected from 50 nm to 5 μm;

[0162] Another preferred embodiment is that the thickness of the polymer layer is selected from 100 nm to 5 μm.

[0163] The polymer layer structure on the lithium-containing metal surface can be controlled at the nanoscale, which is conducive to the assembled battery cells showing smaller interface impedance.

[0164] In some embodiments, the elastic modulus of the polymer layer at 25° C. is 0.1 MPa to 70 MPa;

[0165] Preferably, the elastic modulus of the polymer layer at 25° C. is 0.5 MPa to 50 MPa;

[0166] Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is 1 MPa to 50 MPa;

[0167] Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is selected from 10 MPa to 47 MPa;

[0168] Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is 10 MPa to 45 MPa;

[0169] Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is selected from 20 MPa to 45 MPa.

[0170] In some embodiments, the elastic deformation range of the polymer layer at 25° C. is 50% to 700%;

[0171] Preferably, the elastic deformation range of the polymer layer at 25° C. is 50% to 400%;

[0172] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 50% to 300%;

[0173] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 80% to 300%;

[0174] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 80% to 265%;

[0175] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 700%;

[0176] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 600%;

[0177] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 400%;

[0178] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 300%;

[0179] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 250%;

[0180] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 200%;

[0181] Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 190%.

[0182] In some embodiments, based on the electrolyte, the swelling ratio of the polymer layer at 25° C. is selected from 10% to 60%;

[0183] Preferably, the swelling ratio of the polymer layer at 25° C. is selected from 15% to 60%;

[0184] Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 15% to 55%;

[0185] Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 15% to 45%;

[0186] Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 20% to 45%;

[0187] Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 20% to 40%;

[0188] Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 25% to 50%.

[0189] In some embodiments, based on the electrolyte, the ionic conductivity of the swollen polymer layer at 25° C. is 8×10 -3 S / cm to 1×10 -6 S / cm;

[0190] Preferably, the ionic conductivity of the swollen polymer layer at 25°C is selected from 5×10 -3 S / cm to 1×10 -6 S / cm;

[0191] Preferably, the ionic conductivity of the swollen polymer layer at 25°C is selected from 8×10 -3 S / cm to 1×10 -5 S / cm;

[0192] Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 5×10 -3 S / cm to 1×10 -5 S / cm;

[0193] Preferably, the ionic conductivity of the swollen polymer layer at 25°C is selected from 8×10 -3 S / cm to 1×10 -4 S / cm;

[0194] Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 5×10 -3 S / cm to 1×10 -4 S / cm;

[0195] Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 3×10 -3 S / cm to 1×10 -4 S / cm;

[0196] Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 3×10 -3 S / cm to 5×10 -4 S / cm.

[0197] In some embodiments, the negative electrode substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.

[0198] In some embodiments, a second negative electrode active material layer may or may not be provided between the negative electrode current collector and the lithium-containing layer, and the components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.

[0199] In the third aspect, the present application provides an electrode assembly, which includes a positive electrode plate, an isolation membrane and the negative electrode plate described in the second aspect of the present application, wherein the isolation membrane is arranged between the negative electrode plate and the positive electrode plate; the polymer layer is arranged at least on the surface of the aforementioned negative electrode plate substrate close to the isolation membrane.

[0200] A dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer on at least one side of the negative electrode plate in the electrode assembly. The flexible polymer layer can be tightly adhered to the surface of the lithium-containing layer, and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve coulombic efficiency, and extend the cycle life.

[0201] In a fourth aspect, the present application provides a secondary battery comprising a cell electrolyte and the electrode assembly described in the third aspect of the present application, wherein the cell electrolyte is disposed between the polymer layer and the positive electrode plate.

[0202] A dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer on at least one side of the negative electrode plate in the secondary battery. The flexible polymer layer can be tightly adhered to the surface of the lithium-containing layer, and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve coulombic efficiency, and extend the cycle life.

[0203] In some embodiments, the components of the core electrolyte and the electrolyte in the polymer layer may be the same or different.

[0204] In some embodiments, the charging current density of the secondary battery is selected from 0.3 mA / cm 2 ~12mA / cm 2 ;

[0205] Preferably, the charging current density of the secondary battery is selected from 1 mA / cm 2 ~10mA / cm 2 ;

[0206] Another preferred embodiment is that the charging current density of the secondary battery is selected from 1 mA / cm 2 ~6mA / cm 2 ;

[0207] Another preferred embodiment is that the charging current density of the secondary battery is selected from 1 mA / cm 2 ~3mA / cm 2 .

[0208] In a fifth aspect, the present application provides a battery module, which includes the secondary battery described in the fourth aspect of the present application.

[0209] In a sixth aspect, the present application provides a battery pack comprising the battery module described in the fifth aspect of the present application.

[0210] In a seventh aspect, the present application provides an electrical device comprising one or more of the secondary battery described in the fourth aspect of the present application, the battery module described in the fifth aspect of the present application, and the battery pack described in the sixth aspect of the present application.

[0211] In an eighth aspect, the present application provides an application of a monomer compound II in preparing a negative electrode sheet, wherein the structure of the monomer compound II is as shown in Formula II:

[0212]

[0213] Wherein, Rf, A, Z2, X and m are respectively as defined in the first aspect of the present application.

[0214] In some embodiments, the monomer compound II contacts lithium in the lithium-containing layer of the negative electrode substrate and forms a polymer layer through in-situ polymerization.

[0215] The monomer compound II is a cyanoacrylic acid derivative compound, the cyano group of which can contact the lithium in the outermost layer of the negative electrode substrate to form a chemical connection, and the carbon-carbon double bond therein can undergo an in-situ polymerization reaction under lithium catalysis, thereby preparing the polymer-modified lithium material described in the first aspect of the present application. At this time, a firmly connected, tightly fitted, dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer of the negative electrode, which can play the role of the aforementioned protective layer.

[0216] In a ninth aspect, the present application provides a method for preparing a negative electrode sheet, comprising the following steps:

[0217] Providing a negative electrode substrate, wherein the outermost layer of at least one side of the negative electrode substrate is a lithium-containing layer, and the lithium-containing layer includes lithium-containing metal; and also providing a reaction mixture containing monomer compound II and an electrolyte;

[0218] The reaction mixture is coated on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, and the monomer compound II is polymerized in situ to form a polymer layer;

[0219]

[0220] wherein Rf, A, Z2, X and m are as defined in the first aspect of this application;

[0221] Wherein, the electrolyte is as defined in the second aspect of this application.

[0222] In the presence of an electrolyte, the cyano group in the monomer compound II can contact the lithium in the outermost layer of the negative electrode substrate to form a chemical connection (covalent connection), and the carbon-carbon double bond therein can undergo an in-situ polymer reaction under lithium catalysis to form the polymer Poly shown in the aforementioned formula I, thereby preparing the polymer-modified lithium material described in the first aspect of the present application. At this time, a firmly connected, tightly fitted, dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer, which can play the role of the aforementioned protective layer. Compared with the physical coating effect in traditional technologies, it not only stably binds to the surface of the lithium-containing layer through chemical connection, avoiding falling off from the surface of the lithium-containing layer during the charge and discharge process, but also the coating is dense and uniform, and the coating thickness can be controlled at the nanoscale, and the assembled battery cell can exhibit a smaller interface impedance.

[0223] In some embodiments, the present application provides that the monomer compound II is exposed to at least a catalytic amount of lithium, which provides chemical connection sites for the polymer layer and effectively catalyzes the in-situ polymerization reaction of cyanoacrylic acid derivative monomers.

[0224] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:2;

[0225] Preferably, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:1;

[0226] Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 5:1 to 1:1;

[0227] Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 5:1 to 1.5:1;

[0228] Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 4:1 to 1.5:1.

[0229] By controlling the mass ratio of the monomer compound II and the electrolyte, the mass ratio of the polymer Poly to the electrolyte in the generated polymer layer can be controlled.

[0230] In some embodiments, in the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating method is selected from any one of a coating method, a spraying method, a spin coating method and a vapor deposition method.

[0231] In some embodiments, the reaction temperature of the in situ polymerization is selected from 30°C to 100°C;

[0232] Preferably, the reaction temperature of the in-situ polymerization is selected from 30°C to 50°C;

[0233] Another preferred embodiment is that the reaction temperature of the in-situ polymerization is selected from 40°C to 60°C.

[0234] In some embodiments, the reaction time of the in situ polymerization is selected from 0.1 h to 24 h;

[0235] Preferably, the reaction time of the in-situ polymerization is selected from 0.1h to 12h;

[0236] Another preferred embodiment is that the reaction time of the in-situ polymerization is selected from 0.1 h to 6 h.

[0237] In some embodiments, in the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating thickness of the reaction mixture is selected from 100 nm to 8 μm;

[0238] Preferably, the coating thickness of the reaction mixture is selected from 50 nm to 5 μm;

[0239] Another preferred embodiment is that the coating thickness of the reaction mixture is selected from 50 nm to 8 μm.

[0240] In some embodiments, the formed polymer layer is as defined in the second aspect of the present application.

[0241] In some embodiments, the negative electrode substrate is a pure lithium sheet. In this case, the negative electrode sheet can also be equipped with a negative current collector to facilitate the assembly of the tab. Alternatively, a pure lithium sheet covered with a polymer layer can be used as the negative electrode sheet.

[0242] In some embodiments, the negative electrode substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.

[0243] In some embodiments, a second negative electrode active material layer may or may not be provided between the negative electrode current collector and the lithium-containing layer, and the components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.

[0244] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0245] In order to better describe and illustrate the embodiments or examples of the applications disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the drawings should not be considered as limiting the scope of the disclosed applications, the embodiments or examples currently described, and any of the best modes of these applications currently understood. Moreover, the same figure numbers are used to represent the same components throughout the drawings. It should also be noted that the drawings are drawn in a simplified form and are only used to assist in explaining the invention conveniently and clearly. The various dimensions of each component shown in the drawings are arbitrarily shown and may be accurate or not drawn to scale. For example, in order to make the illustrations clearer, the dimensions of the components are appropriately exaggerated in some places in the drawings. Unless otherwise specified, the components in the drawings are not drawn to scale. The present invention does not limit every dimension of each component. In the drawings:

[0246] FIG1 is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer is provided on one side of the negative electrode plate;

[0247] FIG2 is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer and a negative electrode current collector are provided on one side of the negative electrode plate;

[0248] FIG3 is a schematic structural diagram of a negative electrode sheet according to an embodiment of the present application, wherein a second negative electrode active material layer is provided between the lithium-containing layer and the negative electrode current collector;

[0249] FIG4 is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application, wherein polymer layers are provided on both sides of the negative electrode plate;

[0250] FIG5 is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer is provided on both sides of the negative electrode plate, and a second negative electrode active material layer is provided between the lithium-containing layer and the negative electrode current collector on both sides;

[0251] FIG6 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0252] FIG7 is an exploded view of the secondary battery of one embodiment of the present application shown in FIG6 ;

[0253] FIG8 is a schematic diagram of a battery module according to an embodiment of the present application;

[0254] FIG9 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0255] FIG10 is an exploded view of the battery pack shown in FIG9 according to an embodiment of the present application;

[0256] FIG. 11 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application.

[0257] Explanation of the accompanying drawings: 100, negative electrode substrate; 110, negative electrode current collector; 120, second negative electrode active material layer; 130, lithium-containing layer; 200, polymer layer; 1, battery pack; 2, upper case; 3, lower case; 4, battery module; 5, secondary battery; 51, shell; 52, electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0258] Below, the embodiments of the polymer-modified lithium material, negative electrode sheet, electrode assembly, secondary battery, battery module, battery pack, electrical device, method and application of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0259] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0260] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0261] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0262] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0263] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0264] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0265] In this application, "plurality", "multiple", "multiple times", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.

[0266] As used herein, "combination thereof", "any combination thereof", "any combination thereof" and the like include all suitable combinations of any two or more of the listed items.

[0267] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc. shall be based on the technical solution that can implement the present application.

[0268] Herein, the terms "preferred," "better," "more preferred," and "suitable" are used solely to describe preferred implementations or examples and should not be construed as limiting the scope of protection of this application. If multiple "preferred" terms appear in a technical solution, each "preferred" term is considered independent unless otherwise specified and there are no contradictions or mutual constraints.

[0269] In this application, "optionally" means optional.

[0270] In this application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be understood as limiting the scope of protection of this application.

[0271] In this application, the terms "first," "second," "third," "fourth," etc. in "the first aspect," "the second aspect," "the third aspect," "the fourth aspect," etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or quantity, nor should they be understood as implicitly indicating the importance or quantity of the indicated technical features. Furthermore, "first," "second," "third," "fourth," etc. serve only as non-exhaustive enumeration and description, and should be understood not to constitute a closed-ended limitation on quantity.

[0272] High energy density is an irreversible trend in the development of lithium metal batteries in the future. It has high specific capacity (3860mAh / g), extremely low potential (-3.04V vs.H2 / H + ) has therefore received widespread attention in the industry, but the high reactivity of lithium metal and the problem of dendrite short-circuiting have greatly restricted its further development. Lithium metal has high reactivity and is prone to side reactions with the electrolyte, consuming the electrolyte and lithium metal, producing a thicker passivation layer, and causing the battery cycle life to decay rapidly. In addition, during the charging process, lithium ions are unevenly deposited due to regional differences in ion flow and electron flow, resulting in dendrites. On the one hand, lithium dendrites have a high specific surface area, which will aggravate the consumption of electrolyte and even cause battery diving; on the other hand, the rapid growth of lithium dendrites will penetrate the diaphragm, bringing the risk of battery short circuit.

[0273] A highly elastic lithium metal protective layer that has the function of lithium ion transport and regulation and is tightly bonded to lithium metal may solve the above problems. First, the presence of the protective layer can reduce the direct contact between the electrolyte and the lithium metal, inhibit the occurrence of side reactions, and reduce the consumption of the electrolyte and lithium metal. Secondly, the high ionic conductivity and functional group design of the protective layer can not only ensure the effective transfer of lithium ions within the protective layer and at the interface with the lithium metal, but also regulate the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, reduce the consumption of electrolyte, and avoid dendrites piercing the diaphragm and short-circuiting. Furthermore, the close bonding between the protective layer and the lithium metal can prevent the coating from peeling off from the lithium metal surface due to volume changes on the negative electrode side during charging and discharging.

[0274] The inventors of this application discovered that currently, protective layers are attached to the lithium metal surface through physical coating. The protective layer and lithium metal are bonded via intermolecular van der Waals forces, which are weak. During long cycles, the protective layer can easily lose contact with the lithium metal due to volume changes on the negative electrode side. The functional groups contained in the protective layer have no regulatory effect on lithium deposition. Furthermore, if the protective layer is independently obtained and then attached between the lithium metal and the separator, the process becomes complex and the smoothness of the thin layer is difficult to ensure. To ensure good wettability of the lithium metal surface, a highly viscous polymer solution is used to coat the lithium metal surface, but this results in a thicker protective layer.

[0275] In response to the above-mentioned common technical problems, in the first aspect, the present application includes a lithium-containing metal and a polymer Poly chemically connected to the lithium surface of the lithium-containing metal, the polymer Poly having a repeating unit structure formed by a cyanoacrylic acid derivative monomer, and carrying a large number of cyano groups and fluorine-substituted aliphatic groups Rf, and also having an oxyethylene chain segment (EO segment) between the main chain and the Rf side chain, and at least one cyano group in the polymer Poly forms a chemical connection (further, forms a covalent connection) with the lithium in the lithium-containing metal.

[0276] In some embodiments, a polymer-modified lithium material is provided, comprising a lithium-containing metal and a polymer Poly chemically bonded to the lithium surface of the lithium-containing metal, wherein the polymer Poly comprises a structure shown in Formula I;

[0277]

[0278] in,

[0279] Each occurrence of Rf is independently a fluorine-substituted aliphatic group;

[0280] Each occurrence of X is independently H or an electron withdrawing group;

[0281] Each occurrence of A is independently O, S or NR 11 ; Among them, R 11 H or C 1-3 alkyl;

[0282] Each occurrence of Z2 is independently a bond (i.e., absent), carbonyl, -(O=)P(-O-)2, -S(=O)2-, -C(=O)-NH-, or L C -Z0, where Lc is C 1-3 Alkylene, Z0 is a coupling type linking group;

[0283] * indicates the site of attachment of the terminal groups;

[0284] n is an integer selected from ≥10;

[0285] m is a positive integer ≤ 10;

[0286] At least one cyano group in the polymer Poly forms a chemical connection (further, a covalent connection) with lithium in the lithium-containing metal.

[0287] When Z2 is -(O=)P(-O-)2, the number of Rf connected to Z2 can be 1 or 2. In this case, Z2-Rf can be -(O=)P(-O-Rf)2 or R e is a terminal group different from Rf, such as an alkyl group, further such as C 1-20 Alkyl, further such as C 1-10 Alkyl, further such as C 1-6 Alkyl (including C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl and C6 alkyl), further such as C 1-3 Alkyl; R e It may be a linear alkyl group or a main chain alkyl group.

[0288] In the main chain of the polymer "Poly," the carbon atom to which the Rf side group is attached is also connected to a cyano group. The inventors have discovered that the cyano group at this position facilitates the polymerization reaction of cyanoacrylic acid derivative monomers. This is because the cyano group is an electron-withdrawing group. During the polymerization reaction, the carbon atom connected to the cyano group can form a relatively stable anionic active center, thereby continuing the chain growth until the chain terminates.

[0289] In this application, the term "lithium-containing metal" may be essentially composed of lithium (Li) metal, may be a lithium alloy, or may be a combination of lithium metal and a lithium alloy. "Essentially composed of lithium metal" means that the weight proportion of metallic lithium is very high, and the proportion described in "essentially" here is, for example, greater than 80%, greater than 85%, greater than 90%, greater than 95%, greater than 96%, greater than 97%, greater than 98%, greater than 99%, 100%, etc.

[0290] In this application, the term "lithium metal" or "metallic lithium" refers to lithium in a metallic state.

[0291] In this application, the term "lithium" used independently, unless otherwise specified, refers to metallic lithium, for example, "lithium" in lithium-containing metals.

[0292] In this application, the term "lithium alloy" refers to an alloy containing lithium. In addition to lithium, a lithium alloy may also contain one or more other types of metals. All lithium alloys reported to be used as negative electrode active materials in lithium metal batteries fall within the scope of this application. For example, a lithium alloy can be an alloy of lithium and one or more metals selected from silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium. Non-limiting examples of lithium alloys include lithium-magnesium alloys and lithium-aluminum alloys. In this application, the "chemical connection" between a cyano group and lithium refers to a covalent connection unless otherwise specified.

[0293] In this application, the term "cyanoacrylic acid derivative monomer" refers to a The derivatives of the skeleton shown, the end marked with an asterisk "*" can be connected to the aforementioned ethylene oxide segment (EO segment) through a linking group such as an ester group or an amide group.

[0294] In the present application, an oxyethylene group segment, also referred to as an EO segment, refers to a segment having one or more EO units (units having the structure -CH2CH2O-).

[0295] As used herein, the term "aliphatic group" refers to a group containing at least one carbon atom and no aromatic group, and when the aliphatic group contains only one carbon atom, the carbon atom is connected to four adjacent atoms by four single bonds (i.e., excluding substituted methylene groups such as carbonyl groups). The aliphatic group is permitted to contain one or more heteroatoms, examples of which include, but are not limited to, fluorine, iodine, nitrogen, oxygen, sulfur, silicon, boron, and phosphorus.

[0296] The aliphatic group may be an aliphatic hydrocarbon group, an aliphatic hydrocarbon group in which one or more hydrogen atoms may be independently replaced by a non-fluorine heteroatom, or an aliphatic hydrocarbon group in which one or more carbon atoms may be independently replaced by a heteroatom. Simultaneous substitution of hydrogen atoms and carbon atoms is permitted.

[0297] In this application, the term "hydrocarbyl" refers to a monovalent group composed of carbon and hydrogen. The hydrocarbyl group can be in the form of an alkyl, alkenyl, alkynyl, etc.

[0298] In this application, the term "alkyl" refers to a monovalent residue formed by the loss of a hydrogen atom from a saturated hydrocarbon containing a primary carbon atom, a secondary carbon atom, a tertiary carbon atom, a quaternary carbon atom, or a combination thereof. Phrases containing this term, for example, "C1- 10 "Alkyl" refers to an alkyl group containing 1 to 10 carbon atoms, each occurrence of which can be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl, C9 alkyl or C 10Alkyl. Examples of suitable alkyl groups include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (n-Pr, n-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl, -CH (CH3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl ( -CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH (CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 and octyl (-(CH2)7CH3).

[0299] In this application, the term "alkenyl" refers to a group containing at least one unsaturated site (ie, carbon-carbon sp 2 A monovalent residue formed by losing a hydrogen atom from a hydrocarbon (with a double bond) containing this term. Phrases containing this term, for example, "C2~C 10 "Alkenyl" or "C2-9 alkenyl" refers to an alkenyl group containing 2 to 9 carbon atoms, each occurrence of which is independently C2 alkenyl, C3 alkenyl, C4 alkenyl, C5 alkenyl, C6 alkenyl, C7 alkenyl, C8 alkenyl, C9 alkenyl or C 10Suitable examples include, but are not limited to, vinyl (-CH=CH2), allyl (-CH2CH=CH2), cyclopentenyl (-C5H7), and 5-hexenyl (-CH2CH2CH2CH2CH=CH2).

[0300] In this application, the term "alkynyl" refers to a monovalent residue containing a hydrocarbon having at least one unsaturated site, i.e., a carbon-carbon sp triple bond, which loses a hydrogen atom. Phrases containing this term, for example, "C2-C 10 "Alkynyl" refers to an alkynyl group containing 2 to 9 carbon atoms, each occurrence of which can be independently C2 alkynyl, C3 alkynyl, C4 alkynyl, C5 alkynyl, C6 alkynyl, C7 alkynyl, C8 alkynyl, C9 alkynyl or C 10 Suitable examples include, but are not limited to, ethynyl (-C≡CH) and propargyl (-CH2C≡CH).

[0301] In this application, the term "C 1-3 "Alkylene" refers to an alkylene group containing 1, 2 or 3 carbon atoms, suitable examples of which include methylene (-CH2-), ethylene (-CH2CH2- or -CH(CH3)-), propylene (-CH2CH2CH2-, -CH2CH(CH3)- or -C(CH3)2-). In some embodiments, L C Each occurrence is independently ethylene or propylene. In some embodiments, L C Each occurrence is independently 1,2-ethylene or 1,3-propylene. In some embodiments, L C Each occurrence is independently 1,2-ethylene. In some embodiments, L C Each occurrence is independently 1,3-propylene. In some embodiments, L in formula (I) C All the same.

[0302] In this application, the term "coupling type linker" refers to a covalent linker that can be formed by a coupling reaction between two reactive groups. When Z2 is absent (i.e., a bond), -(CH2CH2O) in formula (I) m - and Rf form a coupling type linking group; when Z2 exists (in this case, Z2 is a linking group containing at least one atom), -(CH2CH2O) in Formula I m- and Z2 constitute a coupled linking group. Non-limiting examples of the "coupled linking group" in the present application include -O-, -OC(=O)-, -O-(O=)P(-O-)2, -OS(=O)2-, -OC(=O)-NH-, -NH-, -NH-C(=O)-, -NH-C(=O)-O-, -C(=O)-NH-, -C(=O)-O-, -S-, -S(=O)2-O-, -S(=O)2-NH-, -S(=O)2-O-, etc. For example, -O-, -NH-, and -S- can be generated through the alkylation reaction of -OH, -NH2, and -SH; for example, -OC(=O)- and -C(=O)-O- can be generated through the condensation reaction between -OH and -COOH; for example, -NH-C(=O)- and -C(=O)-NH- can be generated through the condensation reaction between -NH2 and -COOH or an active carboxylate (such as succinimidyl acetate); for example, -OC(=O)-NH- and -NH-C(=O)-O- can be generated through the condensation reaction between -NH2 and an active carbonate (such as succinimidyl carbonate), and can also be generated through a coupling reaction between -OH and -NCO groups; etc. Those skilled in the art can obtain these different types of coupling-type linking groups according to existing reaction methods in the field of organic synthesis technology, which will not be described in detail here.

[0303] In the present application, non-limiting examples of Z0 include -O-, -OC(=O)-, -O-(O=)P(-O-)2, -OS(=O)2-, -OC(=O)-NH-, -NH-, -NH-C(=O)-, -NH-C(=O)-O-, -C(=O)-NH-, -C(=O)-O-, -S-, -S(=O)2-O-, -S(=O)2-NH-, -S(=O)2-O-, etc. In some embodiments, each occurrence of Z0 is independently -O-, -OC(=O)-, -OS(=O)2-, -OC(=O)-NH-, -NH-, -NH-C(=O)-, -NH-C(=O)-O-, -C(=O)-NH-, -C(=O)-O-, -S-, -S(=O)2-O-, -S(=O)2-NH-, or -S(=O)2-O-. In some embodiments, each occurrence of Z0 is independently -O-, -OC(=O)-, -OC(=O)-NH-, -NH-, -NH-C(=O)-, -NH-C(=O)-O-, -C(=O)-NH-, or -C(=O)-O-. In some embodiments, Z0 in Formula (I) is the same. When Z0 is -(O=)P(-O-)2, the number of Rf connected to Z0 can be 1 or 2. In this case, Z0-Rf can be -(O=)P(-O-Rf)2 or Re The definition is consistent with the above.

[0304] In the present application, the end group of the polymer Poly, unless otherwise specified, refers to the end group formed by the polymerization reaction of the carbon-carbon double bond. The type of the end group is related to factors such as the initiator used and the end-capping group in the termination reaction. When "*" is used to describe the end group of the polymer Poly, it can be understood in conjunction with the relevant description of the polymer reaction in this application, and those skilled in the art can correctly understand the structure of the polymer Poly.

[0305] In some embodiments, Rf is a fluoro-substituted hydrocarbon group.

[0306] In some embodiments, Rf is fluoro-substituted alkyl.

[0307] In some embodiments, Rf is fluoro-substituted alkenyl.

[0308] In some embodiments, Rf is fluoro-substituted alkynyl.

[0309] In this polymer-modified lithium material, the polymer Poly forms a dense and uniform flexible polymer layer on the surface of the lithium-containing metal. The flexible polymer layer can be tightly attached to the surface of the lithium-containing metal and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve the coulombic efficiency, and extend the cycle life. The polymer Poly carries a large number of cyano groups, one or more of which can form a stable chemical connection (covalent connection) with the lithium in the lithium-containing metal, firmly binding the polymer layer to the surface of the lithium-containing metal. Therefore, when the volume of the negative electrode side changes during the charge and discharge process, the polymer layer can be prevented from peeling off from the lithium-containing metal surface; the polymer Poly contains a large number of fluorine-substituted aliphatic groups as side groups. On the one hand, these aliphatic side groups with a certain length can enhance the elasticity of the polymer layer and prevent the polymer layer from breaking under large volume deformation. On the other hand, the introduction of fluorine can effectively regulate the uniform deposition of lithium ions, improve the deposition morphology of lithium dendrites in lithium metal batteries under a certain charging current density, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium negative electrode side. The EO segment (composed of m ethylene oxide units) is also introduced into the side chain of the polymer Poly, which can improve the flexibility and elasticity of the polymer layer, facilitate the close fit between the protective layer and the electrode and the diaphragm, and reduce the interface impedance. In addition, the dense and uniform flexible polymer layer can also be swollen by the electrolyte and can provide a relatively high ionic conductivity after swelling (such as 10 -3 S / cm), thereby ensuring efficient lithium ion transfer within the polymer layer and at the lithium interface, greatly reducing interfacial polarization in the battery cell. The various structural units of the polymer Poly work together to form a technical whole that provides the aforementioned multi-dimensional comprehensive excellent effects.

[0310] In some embodiments, each occurrence of m is independently an integer selected from 2-6.

[0311] In some embodiments, each occurrence of m is independently an integer selected from 2-5.

[0312] In some embodiments, each occurrence of m is independently an integer selected from 2-4.

[0313] In some embodiments, each occurrence of m is independently an integer selected from 2 to 3.

[0314] In some embodiments, each occurrence of m is independently 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10.

[0315] In some embodiments, each occurrence of m is independently 1, 2, 3, 4, 5, 6, 7, or 8.

[0316] In some embodiments, each occurrence of m is independently 1, 2, 3, 4, 5, or 6.

[0317] In some embodiments, each occurrence of m is independently 1, 2, 3, 4, or 5.

[0318] In some embodiments, each occurrence of m is independently 1, 2, or 3.

[0319] In some embodiments, each occurrence of m is independently 2, 3, 4, 5, or 6.

[0320] In some embodiments, each occurrence of m is independently 2, 3, 4, or 5.

[0321] In some embodiments, each occurrence of m is independently 2 or 3.

[0322] In the general formula (I), m reflects the number of EO units (ethylene oxide units) with the structure of "CH2CH2O". By introducing EO segments, the flexibility and elasticity of the polymer layer can be improved, which is beneficial to the close fit between the protective layer and the electrode and the diaphragm, and the interface impedance is reduced. By adjusting the size of m, the number of EO units can be controlled (that is, the length of the EO segment can be controlled), the flexibility and elasticity of the polymer can be regulated, and the elastic deformation of the protective layer and the degree of fit between the protective layer and the substrate and the diaphragm can be regulated. Larger elastic deformation can well adapt to the larger volume expansion of the negative electrode side during charging and prevent the protective layer from breaking; better flexibility is beneficial to the close fit between the protective layer and the lithium metal and diaphragm side, reducing the interface impedance. By controlling m within a suitable range or size, it can also work synergistically with other structural units of the polymer Poly (such as Rf chain, X group) to achieve the aforementioned multi-dimensional comprehensive excellent effect. When the polymer Poly is prepared by in-situ polymerization, by controlling m within a suitable range or size, the flexibility of the polymer layer can be effectively adjusted while maintaining a high reaction rate and effective grafting density, thereby maintaining high density of the polymer layer.

[0323] In some embodiments, each occurrence of Rf independently satisfies a fluorine substitution ratio >50%.

[0324] In some embodiments, the fluorine substitution ratio in Rf independently satisfies ≥ 55%.

[0325] In some embodiments, the fluorine substitution ratio in Rf independently satisfies ≥ 60%.

[0326] In some embodiments, the fluorine substitution ratio in Rf independently satisfies ≥ 65%.

[0327] In some embodiments, the fluorine substitution ratio in Rf independently satisfies ≥ 70%.

[0328] In some embodiments, the fluorine substitution ratio in Rf independently satisfies ≥ 80%.

[0329] In some embodiments, at least 50% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥80%, or ≥90%.

[0330] In some embodiments, at least 60% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥70%, or ≥80%, or ≥90%.

[0331] In some embodiments, at least 70% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥60%, or ≥70%, or ≥80%, or ≥90%.

[0332] In some embodiments, at least 80% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥50%, or ≥60%, or ≥70%, or ≥80%, or ≥90%.

[0333] In this application, for percentage intervals defined by “≥”, such as ≥50% and ≥60%, unless otherwise specified, the upper limit is 100%, that is, ≥50% and ≥60% have the same meanings as 50% to 100% and 60% to 100%, respectively.

[0334] In this application, the "fluorine substitution rate in Rf" refers to the molar percentage of fluorine atoms, based on the number of replaceable hydrogen atoms in the Rf group. The "number of replaceable hydrogen atoms" can be understood as the number of replaceable sites in the Rf group, that is, the maximum number of hydrogen atoms that can be attached to carbon atoms and any heteroatoms (such as phosphorus atoms, nitrogen atoms, sulfur atoms, etc.). The hydrogen atoms can also be replaced by other elements (in this case, the sites occupied by other elements are also included in the base number).

[0335] The fluorine substitution rate in Rf can also be selected from any one of the following percentages or an interval consisting of any two percentages: 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 100%. Non-limiting examples of the interval consisting of any two percentages include 30% to 100%, 35% to 100%, etc.

[0336] In some embodiments, at each occurrence of Rf, the number of fluorine atoms in Rf is independently an integer ≥4.

[0337] In some embodiments, the number of fluorine atoms in Rf is independently an integer selected from 4 to 20.

[0338] In some embodiments, the number of fluorine atoms in Rf is independently an integer selected from 4-16.

[0339] In some embodiments, the number of fluorine atoms in Rf is independently an integer selected from 4 to 15.

[0340] In some embodiments, the number of fluorine atoms in Rf is independently an integer selected from 4-13.

[0341] In some embodiments, the number of fluorine atoms in Rf is independently an integer selected from 4 to 10.

[0342] In some embodiments, the number of fluorine atoms in Rf is independently 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13.

[0343] The number of fluorine atoms in Rf can also be selected from any one of the following values ​​or an interval consisting of any two values: 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, etc. Non-limiting examples of an interval consisting of any two values ​​include 4 to 20, 4 to 16, etc.

[0344] In some embodiments, the mass proportion of fluorine element in the polymer Poly is selected from 10% to 50%.

[0345] In some embodiments, the mass proportion of fluorine element in the polymer Poly is selected from 15% to 50%.

[0346] In some embodiments, the mass proportion of fluorine element in the polymer Poly is selected from 20% to 50%.

[0347] The mass percentage of fluorine in the polymer Poly can also be selected from any one of the following percentages or a range consisting of any two percentages: 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, and 50%. Non-limiting examples of the range consisting of any two percentages include 30% to 50%.

[0348] By controlling the fluorine substitution rate in Rf, the number of fluorine atoms in Rf, and the mass fraction of fluorine in the polymer (Poly), one or more of the following can be used to better regulate the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, improve the lithium ion cycle life, reduce the risk of short circuits, and mitigate the volume expansion of the lithium negative electrode. For example, controlling the mass fraction of fluorine in the polymer (Poly) is beneficial for improving the morphology of lithium dendrite deposition and mitigating the volume expansion of the lithium negative electrode in lithium metal batteries at a certain charging current density.

[0349] In some embodiments, each occurrence of Rf contains 2 to 10 backbone carbon atoms.

[0350] In some embodiments, Rf contains 2 to 8 backbone carbon atoms.

[0351] In some embodiments, Rf contains 2 to 7 backbone carbon atoms.

[0352] In some embodiments, Rf contains 3, 4, 5, 6, 7, or 8 backbone carbon atoms.

[0353] In some embodiments, each occurrence of Rf has an integer number of carbon atoms selected from 2 to 10.

[0354] In some embodiments, the number of carbon atoms in Rf is an integer selected from 2-8.

[0355] In some embodiments, the number of carbon atoms in Rf is an integer selected from 2-7.

[0356] In some embodiments, the number of carbon atoms in Rf is 3, 4, 5, 6, 7, or 8.

[0357] In some embodiments, depending on the number of carbon atoms in Rf, Rf is a fluorine-substituted C 2-10 The number of carbon atoms in the aliphatic group can be selected from any one of the following values ​​or an interval consisting of any two of the following values, such as 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0358] In some embodiments, Rf is a fluorine-substituted C 2-10 Hydrocarbon. C 2-10 The hydrocarbon group may be, but is not limited to, C 2-10 Alkyl, C 2-10 Alkenyl, C 2-10 Alkynyl, etc.

[0359] In some embodiments, Rf is a fluorine-substituted C 2-10 The number of carbon atoms can be selected from any one of the following values ​​or an interval consisting of any two of the following values, such as 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0360] In some embodiments, C 2-10 The alkyl group may be, but is not limited to, for example, ethylpropyl, butyl, pentyl, hexyl, heptyl, octyl, isopropyl, isobutyl, tert-butyl, isopentyl, tert-pentyl, neopentyl, 2-methylpentyl, 3-methylpentyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 2-methylhexyl, 3-methylhexyl, 2,2-dimethylpentyl, 3,3-dimethylpentyl, 2,3-dimethylpentyl, 2,4-dimethylpentyl, 3-ethylpentyl. , 2,2,3-trimethylbutyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 2,2-dimethylhexyl, 3,3-dimethylhexyl, 2,3-dimethylhexyl, 2,4-dimethylhexyl, 2,5-dimethylhexyl, 3,4-dimethylhexyl, 3-ethylhexyl, 2,2,3-trimethylpentanyl, 2,2,4-trimethylpentanyl, 2,3,3-trimethylpentanyl, 2,3,4-trimethylpentanyl, 2-methyl-3-ethylpentanyl, 3-methyl-3-ethylpentanyl, 2,2,3,3-tetramethylbutanyl, nonyl, decyl, etc.

[0361] In some embodiments, Rf is a fluorine-substituted C 2-10 The number of carbon atoms can be selected from any one of the following values ​​or an interval consisting of any two values, such as 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0362] In some embodiments, C 2-10The alkenyl group may be, for example, but is not limited to, ethenyl, propenyl, butenyl, butadienyl, pentenyl, pentadienyl, hexenyl, and the like.

[0363] In some embodiments, Rf is a fluorine-substituted C 2-10 The number of carbon atoms can be selected from any one of the following values ​​or an interval consisting of any two of the following values, such as 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0364] In some embodiments, C 2-10 The alkynyl group can be, for example, but is not limited to, ethynyl, propynyl, butynyl, butadiynyl, pentynyl, pentadiynyl, hexynyl, and the like.

[0365] By controlling the main chain carbon atoms in Rf, the length of the Rf side group can be adjusted by further controlling the number of carbon atoms in Rf, thereby giving the polymer layer appropriate elasticity and better preventing the polymer layer from rupturing under large volume deformation.

[0366] In some embodiments, each occurrence of Rf further comprises one or more heteroatoms selected from the group consisting of iodine, nitrogen, oxygen, sulfur, silicon, boron, and phosphorus.

[0367] In some embodiments, for each occurrence of Rf, the number of any one of the heteroatoms in Rf is one or more.

[0368] In some embodiments, the number of any one of the heteroatoms in Rf is selected from 1 to 5.

[0369] In some embodiments, the number of any of the heteroatoms in Rf is selected from 1, 2, 3, or 4.

[0370] In some embodiments, for each occurrence of Rf, the number of heteroatoms in Rf satisfies one or more of the following:

[0371] The number of oxygen atoms in Rf is 1, 2, 3, 4 or 5;

[0372] The number of nitrogen atoms in Rf is 1, 2 or 3;

[0373] The number of sulfur atoms in Rf is 1, 2, or 3;

[0374] The number of phosphorus atoms in Rf is 1 or 2;

[0375] The number of iodine atoms in Rf is 1, 2, 3, 4, 5 or 6;

[0376] The number of silicon atoms in Rf is 1 or 2; and

[0377] The number of boron atoms in Rf is 1 or 2.

[0378] In some embodiments, the number of oxygen atoms in Rf is 1, 2, 3, 4, or 5.

[0379] In some embodiments, the number of nitrogen atoms in Rf is 1, 2, or 3.

[0380] In some embodiments, the number of sulfur atoms in Rf is 1, 2, or 3.

[0381] In some embodiments, the number of phosphorus atoms in Rf is 1 or 2.

[0382] In some embodiments, the number of iodine atoms in Rf is 1, 2, 3, 4, 5, or 6.

[0383] In some embodiments, the number of silicon atoms in Rf is 1 or 2.

[0384] In some embodiments, the number of boron atoms in Rf is 1 or 2.

[0385] In some embodiments, each occurrence of Rf contains one or more selected from iodo, -NR 12 -, -O-, -S-, -S(O)2-, >Si<, >B- and >P(=O)-, wherein R 12 H or C 1-3 alkyl.

[0386] In some embodiments, R 12 is H or methyl.

[0387] In some embodiments, R 12 For H.

[0388] In some embodiments, each occurrence of Rf contains one or more atoms or groups of atoms selected from the group consisting of -O-, -S(O)2-, and -(O=)P(-O-)2.

[0389] In some embodiments, Rf contains one or more -O- groups.

[0390] In some embodiments, Rf contains -S(O)2F.

[0391] In some embodiments, Rf contains -(O=)P(-O-)2.

[0392] In this application, the term "radical" refers to a group having two or more atoms.

[0393] By introducing heteroatoms other than fluorine atoms into Rf, such as one or more heteroatoms from iodine, nitrogen, oxygen, sulfur, silicon, boron, and phosphorus, special properties can be imparted to the polymer layer. For example, phosphorus has a certain flame retardant effect. Iodine can also play a role in regulating lithium ion deposition. For another example, sulfonyl fluoride groups have a certain positive effect on improving the ionic conductivity of the polymer layer.

[0394] In some embodiments, each occurrence of the fluorine-substituted aliphatic group is independently a straight chain structure or a branched chain structure. For example, a fluorine-substituted hydrocarbon group (such as a fluorine-substituted C 2-10 Hydrocarbon), fluorine-substituted alkyl (such as fluorine-substituted C 2-10 Alkyl), fluorine-substituted alkenyl (such as fluorine-substituted C 2-10 alkenyl), fluorine-substituted alkynyl (such as fluorine-substituted C 2-10 Each occurrence of alkynyl) and the like may independently be a linear structure, a branched structure or a ring-containing structure, but is preferably a linear structure or a branched structure.

[0395] The linear Rf is beneficial to improving the flexibility of the polymer material, while the branched Rf is beneficial to improving the swelling capacity of the electrolyte membrane, thereby improving the ionic conductivity.

[0396] In some embodiments, each occurrence of the fluorine-substituted aliphatic group is independently saturated or unsaturated.

[0397] In some embodiments, the fluorine-substituted aliphatic group contains one or more unsaturated bonds selected from the group consisting of carbon-carbon double bonds and carbon-carbon triple bonds.

[0398] In some embodiments, Rf is a fluorine-substituted C 2-10 See the above definition.

[0399] In some embodiments, Rf is a fluorine-substituted C 2-10 Alkynyl. See above definition.

[0400] When the fluorine-substituted aliphatic group has a saturated structure, it can give the molecular chain of the polymer Poly better flexibility, which is beneficial for improving the elasticity regulation of the polymer layer; in addition, the introduction of a certain amount of unsaturated bonds in Rf can moderately increase the cross-linking degree of the polymer protective layer, which is beneficial for improving the elastic modulus of the material.

[0401] In some embodiments, each occurrence of Rf has a structure independently represented by Formula III-1, Formula III-2, or Formula III-3:

[0402]

[0403] Among them, R 31 、R 32and R 3 Each occurrence is independently H or F; each occurrence of m3 is independently an integer selected from 2 to 10; in formula III-1, there are at least 4 F atoms;

[0404] Preferably, m3 is an integer selected from 3 to 10 (such as 3, 4, 5, 6, 7, 8, 9 or 10);

[0405] Another preferred embodiment is that m3 is an integer selected from 3 to 8;

[0406] Another preferred embodiment is that m3 is 3, 4, 5, 6, 7 or 8;

[0407] R 41a 、R 42a 、R 4a 、R 41b 、R 42b and R 4b Each occurrence is independently H or F; m 4a and m4 4b Each occurrence is independently an integer selected from 1 to 9; in formula III-2, contains at least 4 F atoms;

[0408] Preferably, m 4a and m4 4b are each independently an integer selected from 2 to 9 (such as 2, 3, 4, 5, 6, 7, 8 or 9);

[0409] Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 2 to 8;

[0410] Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 3 to 8;

[0411] Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 3 to 6;

[0412] R 51 and R 52 Each occurrence is independently H or F; each occurrence of m5 is independently an integer selected from 2 to 10; in formula III-3, there are at least 4 F atoms;

[0413] Preferably, m5 is an integer selected from 3 to 10 (such as 3, 4, 5, 6, 7, 8, 9 or 10);

[0414] Another preferred embodiment is that m5 is an integer selected from 3 to 8;

[0415] Another preferred embodiment is that m5 is 3, 4, 5, 6, 7 or 8.

[0416] In some embodiments, R 31 、R 32 and R 3 Each time it appears, it is F.

[0417] In some embodiments, each occurrence of m3 is independently an integer selected from 2 to 10.

[0418] In some embodiments, m3 is an integer selected from 3 to 10 (eg, 3, 4, 5, 6, 7, 8, 9, or 10).

[0419] In some embodiments, m3 is an integer selected from 3-8.

[0420] In some embodiments, m3 is 3, 4, 5, 6, 7 or 8.

[0421] In some embodiments, R 41a 、R 42a 、R 4a 、R 41b 、R 42b and R 4b Each time it appears, it is F.

[0422] In some embodiments, m 4a and m4 4b Each is independently an integer selected from 2 to 9 (eg, 2, 3, 4, 5, 6, 7, 8 or 9).

[0423] In some embodiments, m 4a and m4 4b Each independently represents an integer selected from 2 to 8.

[0424] In some embodiments, m 4a and m4 4b Each independently represents an integer selected from 3 to 8.

[0425] In some embodiments, m 4a and m4 4b Each independently represents an integer selected from 3 to 6.

[0426] In some embodiments, R 51 and R 52 Each time it appears, it is F.

[0427] In some embodiments, m5 is an integer selected from 3 to 10 (eg, 3, 4, 5, 6, 7, 8, 9, or 10).

[0428] In some embodiments, m5 is an integer selected from 3-8.

[0429] In some embodiments, m5 is 3, 4, 5, 6, 7 or 8.

[0430] In some embodiments, each occurrence of Rf has a structure as shown in Formula III-1.

[0431] In some embodiments, each occurrence of Rf has a structure as shown in Formula III-2.

[0432] In some embodiments, each occurrence of Rf has a structure as shown in Formula III-3.

[0433] Among them, the structure of formula III-1 is a linear saturated fluorinated aliphatic chain. On the one hand, it can give the polymer layer better elasticity to prevent the polymer layer from breaking under large volume deformation. On the other hand, the fluorine element can effectively regulate the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium negative electrode side.

[0434] The structure of formula III-2 can be introduced with a phosphorus element, and further Z2 is a bond (ie, does not exist), at this time -(CH2CH2O) m -Rf form a phosphate group, which has a flame retardant effect and is beneficial to improving the safety performance of the battery cell.

[0435] In some embodiments, each time Z2-Rf appears in Formula I, Z2 is a linking group containing at least one atom, and Rf is a structure shown in Formula III-1 or Formula III-3. Further, Z2 is a divalent linking group containing at least one atom. In this case, as a non-limiting example, Z2 can be a carbonyl group, -(O=)P(-O-)2, -S(=O)2--C(=O)-NH- or L C -Z 02 , Z 02 For the divalent Z0, L C The definitions of and Z0 are consistent with those above.

[0436] In some embodiments, each occurrence of Z2-Rf in Formula I is -(O=)P(-O-)2, and Z2-Rf is -(O=)P(-O-Rf)2 (i.e. ), further, Rf is a structure represented by formula III-1 or formula III-3. -(CH2CH2O) m -Z2 form a phosphate group, which can play a flame retardant role and is beneficial to improving the safety performance of the battery cell.

[0437] In some embodiments, each occurrence of Z2-Rf in formula (I) is -L C -O-(O=)P(-O-)2, Z2-Rf is -L C -O-(O=)P(-O-Rf)2(i.e. ), further, Rf is a structure represented by formula III-1 or formula III-3. -(CH2CH2O) m -Z2 form a phosphate group, which can play a flame retardant role and is beneficial to improving the safety performance of the battery cell.

[0438] The structure of formula III-3 can introduce a sulfonyl fluoride group, which has a certain positive effect on improving the ionic conductivity of the polymer layer.

[0439] In some embodiments, each occurrence of Formula III-1 has 0, 1, 2, 3, or 4 H atoms.

[0440] In some embodiments, each occurrence of Formula III-1 has 0 H atoms.

[0441] In some embodiments, each occurrence of Formula III-2 has 0, 1, 2, 3, 4, 5, or 6 H atoms.

[0442] In some embodiments, each occurrence of Formula III-2 has 0 H atoms.

[0443] In some embodiments, each occurrence of Formula III-3 has 0, 1, 2, 3, or 4 H atoms.

[0444] In some embodiments, each occurrence of Formula III-3 has 0 H atoms.

[0445] By controlling the number of H atoms, the number of sites available for fluorine substitution can be controlled.

[0446] In some embodiments, each occurrence of Rf is independently selected from any one of the following structures:

[0447] Rf 10 It is a branched structure Rf. 01 、Rf 02 、Rf 03 、Rf 04 、Rf 05 、Rf 06 、Rf 07 、Rf 08 and Rf 09 All of them are linear structures.

[0448] In some embodiments, each occurrence of Z2-Rf in Formula I is independently selected from any of the following structures: Rf 01 、Rf 02 、Rf 03 、Rf 04 、Rf 05, Rf 06 , Rf 07 , Rf 08 , Rf 09 , Rf 10 , -C(=O)-Rf 01 , -C(=O)-Rf 02 , -C(=O)-Rf 03 , -C(=O)-Rf 04 , -C(=O)-Rf 05 , -C(=O)-Rf 06 , -C(=O)-Rf 07 , -C(=O)-Rf 08 , -C(=O)-Rf 09 , -C(=O)-NH-Rf 01 , -C(=O)-NH-Rf 02 , -C(=O)-NH-Rf 03 , -C(=O)-NH-Rf 04 , -C(=O)-NH-Rf 05 , -C(=O)-NH-Rf 06 , -C(=O)-NH-Rf 07 , -C(=O)-NH-Rf 08 , -C(=O)-NH-Rf 09 , -S(=O)2-Rf 01 , -S(=O)2-Rf 02 , -S(=O)2-Rf 03 , -S(=O)2-Rf 04 , -S(=O)2-Rf 05 , -S(=O)2-Rf 06 , -S(=O)2-Rf 07 , -S(=O)2-Rf 08 , -S(=O)2-Rf 09 , -(O=)P(-O-Rf Z )2, -L C -Z 02 -Rf Z , -L C -O-Rf 10 or -L C -O-(O=)P(-O-Rf Z )2; wherein, L C is defined as above; Rf Z Each occurrence can independently be Rf 01 , Rf 02 , Rf 03 , Rf04 、Rf 05 、Rf 06 、Rf 07 、Rf 08 or Rf 09 ; Z 02 is a divalent Z0; in some embodiments, Z 02 Each occurrence is independently -O-, -OC(=O)-, -OS(=O)2-, -OC(=O)-NH-, -NH-, -NH-C(=O)-, -NH-C(=O)-O-, -C(=O)-NH-, -C(=O)-O-, -S-, -S(=O)2-O-, -S(=O)2-NH-, -S(=O)2-O-; in some embodiments, Z 02 Each occurrence is independently -O-, -OC(=O)-, -OC(=O)-NH-, -NH-, -NH-C(=O)-, -NH-C(=O)-O-, -C(=O)-NH-, or -C(=O)-O-.

[0449] In some embodiments, Z2 in Formula I is a divalent linking group, and each occurrence of Z2-Rf includes only one Rf. In this case, Z2-Rf is not -(O=)P(-O-Rf) in the above example. Z )2. -L C -O-Rf 10 and -L C -O-(O=)P(-O-Rf Z )2.

[0450] The side group structure in formula (I) is The side chains shown (wherein, represents the linking site to the main chain carbon atom), which can be recorded as EO-Rf chain.

[0451] In this application, unless otherwise specified, the chain length of the EO-Rf chain refers to the number of backbone atoms of the longest backbone connecting the carbonyl site and the terminal group in Rf.

[0452] In some embodiments, the EO-Rf chain ( ) has a chain length of ≤40, further, further ≥5, further ≥6, further ≥7, further ≥8, further ≥9, further ≥10.

[0453] In some embodiments, the chain length of the EO-Rf chain is ≤35, further, further ≥5, further ≥6, further ≥7, further ≥8, further ≥9, further ≥10.

[0454] In some embodiments, the chain length of the EO-Rf chain is ≤30, further, further ≥5, further ≥6, further ≥7, further ≥8, further ≥9, further ≥10.

[0455] In some embodiments, the chain length of the EO-Rf chain can also be selected from any one or any two of the following ranges: 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, etc. Regarding "any two ranges", non-limiting examples of the chain length of the EO-Rf chain include 5-40, 5-35, 5-30, 6-40, 6-35, 6-30, 8-40, 8-35, 8-30, 10-40, 10-35, 10-30, etc.

[0456] For example, the EO-Rf chain is The chain length is 10;

[0457] EO-Rf chain is The chain length is 16;

[0458] EO-Rf chain is The chain length is 21;

[0459] EO-Rf chain is The chain length is 29;

[0460] EO-Rf chain is The chain length is 12;

[0461] EO-Rf chain is When , the skeleton structure is branched, and the chain length is 10.

[0462] By controlling the chain length of the EO-Rf chain to an appropriate length, the advantages of the aforementioned Rf and EO segments can be achieved, the corresponding monomers can have a higher reaction rate, and the steric effect of the chain length can be avoided from affecting the distribution density of the connection points between the polymer Poly and the lithium-containing metal, thereby achieving a firmly connected, tightly fitting, and dense polymer layer.

[0463] In some embodiments, each occurrence of X is independently H or an electron-withdrawing group containing 1 to 6 non-hydrogen atoms, wherein the number of non-hydrogen atoms can be selected from any one or two of the following values: 1, 2, 3, 4, 5, 6.

[0464] In some embodiments, each occurrence of X is independently H or cyano, nitro, or -NR 21 R 22 ; Among them, R 21and R 22 Each independently is H or C 1-3 alkyl.

[0465] In some embodiments, R 21 and R 22 are each independently H or methyl.

[0466] In some embodiments, R 21 and R 22 All are methyl.

[0467] In some embodiments, each occurrence of X is independently -N(CH3)2.

[0468] The introduction of an electron-withdrawing group (such as a cyano group) at the X position is beneficial for increasing the reactivity of the carbon-carbon double bond in the cyanoacrylic acid derivative monomer during the formation of the polymer layer, thereby promoting the in-situ polymerization reaction.

[0469] In some embodiments, each occurrence of A is independently O, S, or NH.

[0470] In some embodiments, each occurrence of A is independently O or NH.

[0471] In some embodiments, each occurrence of A is O.

[0472] In some embodiments, each occurrence of A is NH.

[0473] Linker A can be formed by coupling -COOH or its derivatives (e.g., acyl chlorides, activated N-succinimidyl esters of carboxyl groups) in cyanoacrylate derivative monomers with various reactive functional groups to form reactive functional group pairs. These pairs can then form different types of chemical bonds through coupling reactions. For example, when A is O, S, or NH, it can be formed through coupling reactions between -COOH or its derivatives (e.g., -OH, -SH, or -NH2) in cyanoacrylate derivative monomers. The diverse nature of A is the result of flexible combinations of reactive monomers.

[0474] In some embodiments, Rf in Formula I is the same; each occurrence of X in Formula I is the same; and each occurrence of A in Formula I is the same.

[0475] In some embodiments, Rf in Formula I is the same; each occurrence of X in Formula I is the same; each occurrence of A in Formula I is the same; and further, each occurrence of Z2 in Formula I is the same. In this case, a single type of monomer (Formula (II)) can be used for the polymerization reaction.

[0476]

[0477] In some embodiments, the general structure of the polymer Poly can be selected from the structure formed by polymerization of any monomer polymer in Table 1. The molecular weight can be the same as or different from that of the corresponding polymer in Table 1.

[0478] The monomer corresponding to Example 1 in Table 1 For example, the structure formed by polymerization is: In formula I, X is H, A is O, m is 1, Z2 is a bond, and Rf is The EO-Rf chain length is 10.

[0479] In some embodiments, in Formula I, X is H, Rf is Further, A is O, further, Z2 is a bond, further, m is a positive integer selected from 1 to 10, for example, m is 1.

[0480] In some embodiments, monomers may be used In this case, in Formula I, X is -N(CH3)2, A is O, m is 3, Z2 is a bond, and Rf is The EO-Rf chain length is 16.

[0481] In some embodiments, in Formula I, X is -N(CH3)2, Rf is Further, A is O, further, Z2 is a bond, further, m is a positive integer selected from 1 to 10, for example, m is 3.

[0482] In some embodiments, monomers may be used In this case, in Formula I, X is H, A is O, m is 3, Z2 is a bond, and Rf is The EO-Rf chain length is 21.

[0483] In some embodiments, in Formula I, X is H, Rf is Further, A is O, further, Z2 is a bond, further, m is a positive integer selected from 1 to 10, for example, m is 3.

[0484] In some embodiments, in Formula I, X is H, A is O or NH, m is any integer selected from 1 to 1, Z2 is a bond, and Rf is When m=8, the EO-Rf chain length is 30.

[0485] In some embodiments, monomers may be used In this case, in Formula I, X is -NO2, A is O, m is 1, Z2 is a bond, and Rf is The EO-Rf chain length is 12.

[0486] In some embodiments, in Formula I, X is -NO2, Rf is Further, A is O, further, Z2 is a bond, further, m is a positive integer selected from 1 to 10, for example, m is 1.

[0487] In some embodiments, in Formula I, X is H, A is O or NH (preferably O), and Rf is The definitions of m and Z2 are the same as above. In one embodiment, A is 0; in another embodiment, A is NH.

[0488] In some embodiments, monomers may be used In this case, in Formula I, X is H, A is O, m is 8, Z2 is a bond, and Rf is The EO-Rf chain length is 29.

[0489] In some embodiments, in Formula I, X is H, Rf is Further, A is O, further, Z2 is a bond, further, m is a positive integer selected from 1 to 10, for example, m is 8.

[0490] In some embodiments, in Formula I, X is H, A is O or NH, and Rf is The definitions of m and Z2 are the same as above. In one embodiment, A is 0; in another embodiment, A is NH.

[0491] In some embodiments, monomers may be used In this case, in Formula I, X is H, A is O, m is 1, Z2 is a bond, and Rf is The EO-Rf chain length is 10. The following embodiment can also be used: In Formula I, X is H, A is O, m is 1, Z2 is -(O=)P(-O-)2, Z2 connects two Rf, and both Rf are -CH2CF2CHF2.

[0492] In some embodiments, in Formula I, X is H, Rf is Further, A is O, further, Z2 is a bond, further, m is a positive integer selected from 1 to 10, for example, m is 1. The following embodiment can also correspond: in Formula I, X is H, Z2 is -(O=)P(-O-)2, Z2 connects two Rf, and both Rf are -CH2CF2CHF2.

[0493] In some embodiments, n is an integer selected from 10 to 1000, preferably an integer selected from 10 to 950, preferably an integer selected from 10 to 800, preferably an integer selected from 15 to 800, preferably an integer selected from 20 to 800, preferably an integer selected from 40 to 800, preferably an integer selected from 50 to 800, preferably an integer selected from 100 to 800, preferably an integer selected from 10 to 750, preferably an integer selected from 15 to 750, preferably an integer selected from 20 to 750, preferably an integer selected from 40 to 750, preferably an integer selected from 50 to 750, preferably an integer selected from 80 to 750, preferably an integer selected from 100 to 750. The integers are preferably selected from 10 to 600, 15 to 600, 20 to 600, 40 to 600, 50 to 600, 100 to 600, 100 to 200, 10 to 650, 15 to 650, 20 to 650, 40 to 650, 50 to 650, 100 to 650, 150 to 500, 200 to 350.

[0494] In some embodiments, n can be selected from any one of the following values ​​or an interval consisting of any two of the following values: 10, 20, 30, 40, 50, 60, 70, 80, 100, 150, 200, 250, 300, 400, 500, 600, 700, 800, 850, 900, 950, 1000, etc.

[0495] In some embodiments, the number average molecular weight of the polymer Poly is selected from 10 kDa to 200 kDa.

[0496] In some embodiments, the number average molecular weight of the polymer Poly is selected from 50 kDa to 100 kDa.

[0497] In some embodiments, the number average molecular weight of the polymer Poly can be selected from any one of the following molecular weights or an interval consisting of any two molecular weights (in kDa): 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 22, 25, 26, 28, 30, 35, 40, 44, 45, 46, 48, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, etc.

[0498] In Formula I, n is numerically equal to the degree of polymerization (DP) of the polymer (Poly). Controlling n allows for regulation of the molecular weight of the polymer (Poly). Adjusting the DP or molecular weight allows for adjusting the molecular chain length of the polymer (Poly), effectively encapsulating the lithium-containing metal while maintaining a stable chemical connection and affecting the density and uniformity of the polymer layer.

[0499] In some embodiments, the amount of lithium in the lithium-containing metal relative to the polymer Poly is greater than the amount of the catalyst, calculated on a molar ratio.

[0500] In this polymer-modified lithium material, the lithium metal can successfully catalyze the in-situ polymerization of cyanoacrylate derivative monomers on the lithium metal surface as long as the lithium metal provides a catalytic amount. The amount of lithium metal relative to the polymer Poly only requires contact with the catalyst to catalyze the in-situ polymerization of cyanoacrylate monomers on the lithium metal surface.

[0501] In some embodiments, the lithium-containing metal comprises lithium metal or a lithium alloy.

[0502] Lithium metal has the highest specific capacity (3860 mAh / g) and the lowest electrochemical potential (-3.04 V, relative to standard hydrogen electrode) among all negative electrode materials for lithium-based batteries. It is an optimal negative electrode material for lithium metal batteries and helps to achieve high energy density.

[0503] In some embodiments, the lithium alloy contains lithium and further contains one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel, titanium, etc.

[0504] In a second aspect, the present application provides a negative electrode sheet, wherein the negative electrode sheet comprises a stacked negative electrode sheet substrate and a polymer layer; the negative electrode sheet substrate comprises a lithium-containing layer in contact with the polymer layer, the lithium-containing layer contains lithium, and the polymer layer is chemically connected to at least a portion of the lithium in the lithium-containing layer;

[0505] Wherein, the polymer layer comprises the polymer Poly defined in the first aspect of the present application.

[0506] In the present application, the "negative electrode sheet substrate" can provide a negative electrode active material for a lithium metal battery. The negative electrode sheet substrate in the negative electrode sheet includes at least a lithium-containing layer in contact with the polymer layer, that is, the lithium-containing layer is located at the outermost layer of the negative electrode sheet substrate. In other words, the outermost layer of at least one side of the negative electrode sheet substrate is a lithium-containing layer. In one embodiment, the negative electrode sheet substrate is composed of a lithium-containing layer. The polymer layer is chemically connected to at least a portion of the lithium in the lithium-containing layer. Further, "chemical connection" here refers to covalent connection. The thickness of the negative electrode sheet substrate can be the thickness of the lithium negative electrode in a conventional lithium metal battery. The "lithium negative electrode" here refers to the thickness of the negative electrode active material layer provided by lithium metal or lithium alloy. Non-limiting examples of the thickness of the lithium-containing layer are 5 μm to 40 μm. The thickness of the lithium-containing layer can also be selected from the interval consisting of any one or two of the following thicknesses: 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 40 μm, etc.

[0507] In this application, the term "lithium-containing layer" refers to a structural layer containing metallic lithium. The lithium-containing layer can be essentially composed of lithium (Li) metal, or a lithium alloy, or a composition comprising lithium metal and a lithium alloy (e.g., a composition essentially composed of lithium metal and a lithium alloy). The lithium in the lithium-containing layer can play multiple roles. On the one hand, it can catalyze the in-situ polymerization reaction of cyanoacrylic acid derivative monomers, on the other hand, it can form a stable covalent bond with the cyano group carried by the polymer Poly, and on the other hand, it can also serve as a lithium source for the negative electrode active material. The thickness of the lithium-containing layer can be any suitable thickness, as long as it is sufficient to provide an amount of catalyst that can support the in-situ polymerization reaction of cyanoacrylic acid derivative monomers. For example, it can also be the thickness of a lithium negative electrode in a conventional lithium metal battery. When the thickness of the lithium-containing layer is relatively thin, a second negative electrode active material layer can be provided on the side of the lithium-containing layer away from the polymer layer. In this case, the negative electrode substrate includes the lithium-containing layer and the second negative electrode active material layer. The composition and content of the lithium-containing layer and the second negative electrode active material layer can be the same or different.

[0508] A dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer on at least one side of the negative electrode plate. The flexible polymer layer can be tightly adhered to the surface of the lithium-containing layer, and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve coulombic efficiency, and extend the cycle life.

[0509] In some embodiments, the amount of lithium in the lithium-containing layer relative to the polymer (Poly) is greater than the amount of the catalyst, measured on a molar basis. Generally, sufficient lithium (considerably greater than the amount of the catalyst) is required in the negative electrode to significantly increase the energy density of the battery cell while ensuring the initial coulombic efficiency of the negative electrode and reducing or avoiding lithium consumption at the positive electrode.

[0510] In some embodiments, the lithium-containing layer comprises lithium metal or a lithium alloy.

[0511] In some embodiments, the lithium alloy contains lithium and further contains one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel, and titanium.

[0512] In some embodiments, the lithium-containing layer consists essentially of lithium metal.

[0513] In some embodiments, the lithium-containing layer is a lithium alloy.

[0514] In some embodiments, the polymer layer further contains an electrolyte, which is beneficial for providing better ionic conductivity.

[0515] In some embodiments, the electrolyte contains a lithium salt and an electrolyte solvent.

[0516] In some embodiments, the lithium salt is selected from one or more of lithium hexafluorophosphate (LiPF6), tetrafluoroboric acid (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiDFOB), lithium perchlorate (LiClO4) and lithium bis(oxaloyl)borate (LiBOB).

[0517] In some embodiments, the electrolyte solvent is selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), diphenyl carbonate (DPhC), dibutyl carbonate (DBC), butylene carbonate (BC), ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), dioxolane (DOL), methyl nonafluorobutyl ether (MFE), 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE-458), octafluoropentyl-tetrafluoroethyl ether (F-EAE), 1,2-bis(cyanoethoxy)ethane (DENE), diphenyl ether (DPE) and 18-crown-6.

[0518] In some embodiments, the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 5 mol / L.

[0519] In some embodiments, the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 4 mol / L.

[0520] In some embodiments, the concentration of the lithium salt in the electrolyte is selected from 2 mol / L to 4 mol / L.

[0521] In some embodiments, the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 3 mol / L.

[0522] In some embodiments, the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 2 mol / L.

[0523] In some embodiments, the concentration of the lithium salt in the electrolyte can be selected from any one of the following values ​​or an interval consisting of any two of the following values ​​(in mol / L): 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, etc.

[0524] The concentration of lithium salt in the electrolyte will also affect the deposition morphology of lithium ions. + The solvation effect affects the composition of the solid electrolyte interface film (SEI film) and the deposition morphology of lithium ions. By controlling the lithium salt in the electrolyte at an appropriate concentration, dense and uniform lithium ion deposition and minimal volume expansion can be achieved. In addition, by controlling the lithium salt in the electrolyte at an appropriate concentration, the polymer layer can also have suitable mechanical properties, avoiding the detrimental effect of excessive lithium salt concentration on mechanical properties. It can also achieve better lithium ion conductivity during charging and discharging, avoiding poor lithium ion conductivity due to insufficient lithium salt concentration.

[0525] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:2, wherein "9:1 to 1:2" and (9-0.5):1 have the same meaning and can be used interchangeably.

[0526] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:1.

[0527] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:2.

[0528] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:1.

[0529] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1.5:1.

[0530] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 4:1 to 1.5:1.

[0531] In some embodiments, the mass ratio of polymer Poly to electrolyte may be 9:1, 8.5:1, 8:1, 7.5:1, 7:1, 6.5:1, 6:1, 5.5:1, 5:1, 4.5:1, 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 0.9:1, 0.8:1, 0.7:1, 0.6:1, 0.5:1, etc. The mass ratio may also be selected from a range consisting of any two of the above ratios, such as (9-2):1, etc.

[0532] In some embodiments, the electrolyte accounts for a mass percentage of 9.5% to 65% in the polymer layer.

[0533] In some embodiments, the electrolyte accounts for 10% to 60% by mass in the polymer layer.

[0534] In some embodiments, the electrolyte accounts for 20% to 60% by mass in the polymer layer.

[0535] In some embodiments, the electrolyte accounts for 30% to 60% by mass in the polymer layer.

[0536] In some embodiments, the electrolyte accounts for 9.5% to 50% by mass in the polymer layer.

[0537] In some embodiments, the electrolyte accounts for 10% to 50% by mass in the polymer layer.

[0538] In some embodiments, the electrolyte accounts for 20% to 50% by mass in the polymer layer.

[0539] In some embodiments, the electrolyte accounts for 30% to 45% by mass in the polymer layer.

[0540] In some embodiments, the electrolyte accounts for 9.5% to 45% by mass in the polymer layer.

[0541] In some embodiments, the electrolyte accounts for 10% to 45% by mass in the polymer layer.

[0542] In some embodiments, the electrolyte accounts for 20% to 45% by mass in the polymer layer.

[0543] In some embodiments, the electrolyte accounts for 30% to 50% by mass in the polymer layer.

[0544] In some embodiments, the mass proportion of the electrolyte in the polymer layer can be selected from any one of the following percentages or a range consisting of any two percentages: 9.5%, 10%, 11%, 12%, 14%, 15%, 16%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, etc. Non-limiting examples of the range consisting of any two percentages include 9% to 55%, 9.5% to 50%, etc.

[0545] The mass ratio of the electrolyte in the polymer layer can be adjusted by controlling the mass ratio of the polymer Poly and the electrolyte within a suitable range. The mass ratio of the electrolyte in the polymer layer will affect the elasticity and ionic conductivity of the protective layer. The presence of a certain amount of lithium salt and solvent has a plasticizing effect on the polymer layer, which can improve the elasticity of the polymer layer. In addition, during the in-situ polymerization process of the polymer layer, the lithium salt and solvent are incorporated into the interior of the polymer layer. On a microscopic scale, the polymer layer has a sponge-like loose porous structure, and the pores are filled with electrolyte, providing a path for the subsequent transmission of lithium ions.

[0546] In some embodiments, the thickness of the polymer layer is selected from 5 nm to 10 μm.

[0547] In some embodiments, the thickness of the polymer layer is selected from 50 nm to 8 μm.

[0548] In some embodiments, the thickness of the polymer layer is selected from 50 nm to 5 μm.

[0549] In some embodiments, the thickness of the polymer layer is selected from 100 nm to 5 μm.

[0550] In some embodiments, the thickness of the polymer layer can be selected from any one of the following thicknesses or an interval consisting of any two of the following thicknesses: 5nm, 5.5nm, 6nm, 6.5nm, 7nm, 7.5nm, 8nm, 8.5nm, 9nm, 9.5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 6μm, 7μm, 8μm, 9μm, 9.5μm, 10μm, etc.

[0551] The polymer layer structure on the lithium-containing metal surface can be controlled at the nanoscale, which is conducive to the assembled battery cells showing smaller interface impedance.

[0552] In some embodiments, the elastic modulus of the polymer layer is 0.1 MPa to 70 MPa.

[0553] In some embodiments, the elastic modulus of the polymer layer is 0.5 MPa to 50 MPa.

[0554] In some embodiments, the elastic modulus of the polymer layer is 1 MPa to 50 MPa.

[0555] In some embodiments, the elastic modulus of the polymer layer is 10 MPa to 50 MPa.

[0556] In some embodiments, the elastic modulus of the polymer layer is selected from 10 MPa to 47 MPa.

[0557] In some embodiments, the elastic modulus of the polymer layer is 10 MPa to 45 MPa.

[0558] In some embodiments, the polymer layer has an elastic modulus selected from 20 MPa to 45 MPa.

[0559] In some embodiments, the elastic modulus of the polymer layer can be selected from any one of the following values ​​or an interval consisting of any two of the following values: 0.1 MPa, 0.2 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, 14 MPa, 15 MPa, 16 MPa, 18 MPa, 20 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 60 MPa, 65 MPa, 70 MPa, etc. Non-limiting examples of the elastic modulus of the polymer layer include: 0.5 MPa to 70 MPa, 1 MPa to 70 MPa, 15 MPa to 70 MPa, 20 MPa to 70 MPa, 20 MPa to 50 MPa, 0.1 MPa to 47 MPa, 0.5 MPa to 47 MPa, 1 MPa to 47 MPa, 15 MPa to 47 MPa, 20 MPa to 47 MPa, 0.1 MPa to 45 MPa, 0.5 MPa to 45 MPa, 1 MPa to 45 MPa, 15 MPa to 45 MPa, etc.

[0560] In the present application, the “elastic modulus of the polymer layer” generally refers to a test value at 20° C. to 30° C. unless otherwise specified.

[0561] In some embodiments, the elastic modulus of the polymer layer refers to the elastic modulus at 25°C.

[0562] In some embodiments, the elastic deformation range of the polymer layer is 50% to 700%.

[0563] In some embodiments, the elastic deformation range of the polymer layer is 50% to 400%.

[0564] In some embodiments, the elastic deformation range of the polymer layer is 50% to 300%.

[0565] In some embodiments, the elastic deformation range of the polymer layer is 80% to 300%.

[0566] In some embodiments, the elastic deformation range of the polymer layer is 80% to 265%.

[0567] In some embodiments, the elastic deformation range of the polymer layer is 100% to 700%.

[0568] In some embodiments, the elastic deformation range of the polymer layer is 100% to 600%.

[0569] In some embodiments, the elastic deformation range of the polymer layer is 100% to 400%.

[0570] In some embodiments, the elastic deformation range of the polymer layer is 100% to 300%.

[0571] In some embodiments, the elastic deformation range of the polymer layer is 100% to 250%.

[0572] In some embodiments, the elastic deformation range of the polymer layer is 100% to 200%.

[0573] In some embodiments, the elastic deformation range of the polymer layer is 100% to 190%.

[0574] In some embodiments, the elastic deformation range of the polymer layer can be selected from any one or two of the following percentages: 50%, 55%, 60%, 65%, 70%, 80%, 90%, 100%, 150%, 200%, 220%, 240%, 250%, 260%, 265%, 270%, 280%, 300%, 350%, 400%, 450%, 500%, 600%, 700%, etc. Non-limiting examples of the elastic deformation range of the polymer layer include: 50% to 265%, 50% to 250%, 80% to 700%, 80% to 600%, 80% to 500%, 80% to 400%, 100% to 500%, 100% to 265%, etc.

[0575] In the present application, the "elastic deformation range of the polymer layer" generally refers to the test value under the conditions of 20°C to 30°C unless otherwise specified.

[0576] In some embodiments, the elastic deformation range of the polymer layer refers to the elastic deformation range at 25°C.

[0577] In some embodiments, based on the electrolyte, the swelling ratio of the polymer layer at 25° C. is selected from 10% to 60%.

[0578] In some embodiments, the swelling ratio of the polymer layer is selected from 15% to 60%.

[0579] In some embodiments, the swelling ratio of the polymer layer is selected from 15% to 55%.

[0580] In some embodiments, the swelling ratio of the polymer layer is selected from 15% to 45%.

[0581] In some embodiments, the swelling ratio of the polymer layer is selected from 20% to 45%.

[0582] In some embodiments, the swelling ratio of the polymer layer is selected from 20% to 40%.

[0583] In some embodiments, the swelling ratio of the polymer layer is selected from 25% to 50%.

[0584] In some embodiments, the swelling ratio of the polymer layer based on the electrolyte can be selected from any one or a range consisting of any two of the following percentages: 10%, 11%, 12%, 14%, 15%, 16%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc. Non-limiting examples of the swelling ratio of the polymer layer based on the electrolyte include 20% to 60%, 10% to 55%, 20% to 55%, 10% to 45%, 10% to 40%, 15% to 40%, etc.

[0585] In the present application, the "swelling rate of the polymer layer" generally refers to a test value at 20°C to 30°C unless otherwise specified.

[0586] In some embodiments, the swelling ratio of the polymer layer refers to the swelling ratio at 25° C. For details, please refer to the test method in the “Structure and Performance Test” in the Examples section below.

[0587] In some embodiments, based on the electrolyte, the ionic conductivity of the swollen polymer layer is selected from 8×10 -3 S / cm to 1×10 -6 S / cm.

[0588] In some embodiments, based on the electrolyte, the ionic conductivity of the swollen polymer layer is selected from 5×10 -3 S / cm to 1×10 -6S / cm.

[0589] In some embodiments, the ionic conductivity of the swollen polymer layer is selected from 8×10 -3 S / cm to 1×10 -5 S / cm.

[0590] In some embodiments, the ionic conductivity of the swollen polymer layer is selected from 5×10 -3 S / cm to 1×10 -5 S / cm.

[0591] In some embodiments, the ionic conductivity of the swollen polymer layer is selected from 8×10 -3 S / cm to 1×10 -4 S / cm.

[0592] In some embodiments, the ionic conductivity of the swollen polymer layer is selected from 5×10 -3 S / cm to 1×10 -4 S / cm.

[0593] In some embodiments, the ionic conductivity of the swollen polymer layer is selected from 3×10 -3 S / cm to 1×10 -4 S / cm.

[0594] In some embodiments, the ionic conductivity of the swollen polymer layer is selected from 3×10 -3 S / cm to 5×10 -4 S / cm.

[0595] In some embodiments, based on the electrolyte, the ionic conductivity of the swollen polymer layer can be selected from any one of the following values ​​or any two of the following ranges: 8×10 -3 S / cm, 7×10 -3 S / cm, 6×10 -3 S / cm, 5×10 -3 S / cm, 4.5×10 -3 S / cm, 4×10 -3 S / cm, 3.5×10 -3 S / cm, 3×10 -3 S / cm, 2.5×10 -3 S / cm, 2×10 -3 S / cm, 1.5×10 -3 S / cm, 1×10 -3 S / cm, 9×10 -4 S / cm, 8×10 -4 S / cm, 7×10 -4 S / cm, 6×10-4 S / cm, 5×10 -4 S / cm, 4×10 -4 S / cm, 3×10 -4 S / cm, 2×10 -4 S / cm, 1×10 -4 S / cm, 9×10 -5 S / cm, 8×10 -5 S / cm, 7×10 -5 S / cm, 6×10 -5 S / cm, 5×10 -5 S / cm, 4×10 -5 S / cm, 3×10 -5 S / cm, 2×10 -5 S / cm, 1×10 -5 S / cm, etc.

[0596] In the present application, the “ionic conductivity of the swollen polymer layer” generally refers to a test value at 20° C. to 30° C. unless otherwise specified.

[0597] In some embodiments, the ionic conductivity of the swollen polymer layer refers to the ionic conductivity at 25°C.

[0598] In some embodiments, the volume expansion rate of the negative electrode plate is less than 92%, and further, is selected from 6% to 92%. The volume expansion rate of the negative electrode plate can also be selected from any one or two percentage ranges as follows: 6%, 7%, 8%, 9%, 10%, 11%, 12%, 14%, 15%, 16%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 92%, etc.

[0599] In this application, the “volume expansion rate of the electrode”, unless otherwise specified, generally refers to the test value under the conditions of 20°C to 30°C.

[0600] In some embodiments, the volume expansion rate of the pole piece refers to the volume expansion rate at 25°C.

[0601] In some embodiments, the negative electrode substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.

[0602] In some embodiments, the negative electrode current collector is located between the negative electrode current collector and the lithium-containing layer with or without a second negative electrode active material layer. Furthermore, the components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.

[0603] In some embodiments, a lithium-containing layer is provided only on the outermost layer of one side of the negative electrode substrate (see FIG. 1 , FIG. 2 and FIG. 3 ).

[0604] In some embodiments, a lithium-containing layer is provided on the outermost layers of both sides of the negative electrode substrate (see Figures 4 and 5). The lithium-containing layers on both sides may contain the same or different amounts of lithium. The lithium content in the lithium-containing layer may refer to the above definition. The lithium content in the second negative electrode active material may be selected from the lithium content in the negative electrode active material layer of a conventional lithium metal battery. Non-limiting examples of the second negative electrode active material layer include lithium metal, lithium alloy, or a combination of the two groups.

[0605] In this application, the "second negative electrode active material layer" can be any suitable negative electrode active material layer among the active material layers reported for lithium metal batteries. The second negative electrode active material layer can be essentially composed of lithium (Li) metal, a lithium alloy, or a combination essentially composed of lithium metal and a lithium alloy.

[0606] In some embodiments, a lithium-containing layer is provided on the outermost layers on both sides of the negative electrode substrate, and a polymer layer is provided on the surface of the lithium-containing layer on both sides (see Figures 4 and 5); the chemical composition and content of the polymer layers on both sides can be the same or different.

[0607] In some embodiments, the negative electrode plate includes a structure as shown in Figure 1, including a stacked lithium-containing layer 130 and a polymer layer 200. The lithium-containing layer contains lithium, a lithium alloy, or a combination of the two, and the lithium-containing layer here serves as a negative electrode active material layer; the polymer layer contains a polymer Poly, which carries a large number of cyano groups. These cyano groups are covalently bonded to the lithium in the lithium-containing layer to form a stable chemical connection, so that the polymer layer is firmly connected to the surface of the lithium-containing layer. The polymer Poly can be selected from the polymer Poly described in any embodiment of the first aspect. The definition of the electrolyte is as described above.

[0608] In some embodiments, the negative electrode sheet comprises a structure as shown in FIG2 , including a stacked negative electrode sheet substrate 100 and a polymer layer 200 ; the negative electrode sheet substrate 100 includes a stacked negative electrode current collector 110 and a lithium-containing layer 130 , and the polymer layer 200 is located on the surface of the lithium-containing layer 130 away from the negative electrode current collector 110 . Furthermore, the polymer layer comprises a polymer Poly and an electrolyte. The lithium-containing layer contains lithium, a lithium alloy, or a combination of the two, and the polymer layer contains a polymer Poly that carries a large number of cyano groups. These cyano groups are covalently bonded to the lithium in the lithium-containing layer to form a stable chemical connection, so that the polymer layer is firmly connected to the surface of the negative electrode sheet substrate.

[0609] In some embodiments, the negative electrode sheet includes a structure shown in Figure 3, including a negative electrode sheet substrate 100 and a polymer layer 200 that are stacked and distributed; the negative electrode sheet substrate 100 includes a negative electrode current collector 110, a second negative electrode active material layer 120 and a lithium-containing layer 130 that are stacked and distributed in sequence, and the polymer layer is located on the surface of the lithium-containing layer 130 away from the negative electrode current collector 110.

[0610] In some embodiments, the negative electrode plate comprises a structure as shown in FIG4 , including a negative electrode plate substrate 100 and two polymer layers 200 disposed on both sides of the negative electrode plate substrate 110; the negative electrode plate substrate comprises a negative electrode current collector 110, and two lithium-containing layers 130 disposed on both sides of the negative electrode current collector 110. The lithium-containing layers 130 on both sides of the negative electrode plate are directly connected to the corresponding polymer layers 200 (chemically connected by covalent interaction). The chemical composition and content of the polymer layers 130 on both sides can be the same or different. The chemical composition and content of the lithium-containing layers 130 on both sides can be the same or different.

[0611] In some embodiments, the negative electrode sheet includes a structure as shown in Figure 5, including a negative electrode sheet substrate 100 and two polymer layers 200 respectively disposed on the surfaces of both sides of the negative electrode sheet substrate 110; the negative electrode sheet substrate includes a negative electrode current collector 110, two second negative electrode active material layers 120 respectively disposed on the surfaces of both sides of the negative electrode current collector 110, and two lithium-containing layers 130 respectively disposed on the surface of the two second negative electrode active material layers 120 away from the negative electrode current collector 110. The lithium-containing layers 130 on both sides of the negative electrode sheet are directly connected to the corresponding polymer layers 200 (chemical connection is achieved through covalent interaction). The chemical composition and content of the polymer layers 130 on both sides can be the same or different. The chemical composition and content of the second negative electrode active material layers 120 on both sides can be the same or different. The chemical composition and content of the lithium-containing layers 130 on both sides can be the same or different.

[0612] Negative electrode

[0613] In some embodiments, the negative electrode plate generally includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. The negative electrode film layer includes the aforementioned lithium-containing layer and further includes a polymer layer formed on at least one surface of the lithium-containing layer remote from the interior of the negative electrode film layer. That is, the polymer layer is located on the surface of the lithium-containing layer remote from the negative electrode current collector. The polymer layer is located on the outermost layer of the negative electrode plate. Furthermore, the polymer layer and the lithium-containing layer are chemically bonded via a covalent interaction.

[0614] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0615] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0616] In some embodiments, the negative electrode active material in the negative electrode active material layer may be a negative electrode active material for lithium metal batteries that is well known in the art. As an example, the negative electrode active material suitable for the present application may include one or more of lithium metal and lithium alloys. In addition to lithium, the lithium alloy may also contain one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel, titanium, etc. The lithium-containing layer in the present application may serve as the first negative electrode active material layer, and a second negative electrode active material layer may be provided between the lithium-containing layer and the negative electrode current collector. The composition and content of the second negative electrode active material layer may be the same as or different from the composition and content of the lithium-containing layer.

[0617] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0618] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0619] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0620] In the third aspect, the present application provides an electrode assembly, which includes a positive electrode plate, an isolation membrane and the negative electrode plate described in the second aspect of the present application, wherein the isolation membrane is arranged between the negative electrode plate and the positive electrode plate; the polymer layer is arranged at least on the surface of the negative electrode plate substrate close to the isolation membrane.

[0621] A dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer on at least one side of the negative electrode plate in the electrode assembly. The flexible polymer layer can be tightly adhered to the surface of the lithium-containing layer, and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve coulombic efficiency, and extend the cycle life.

[0622] In some embodiments, a lithium-containing layer is provided on the outermost layer of one side of the negative electrode substrate.

[0623] In some embodiments, lithium-containing layers are provided on the outermost layers of both sides of the negative electrode substrate. The lithium-containing layers on both sides may contain the same or different amounts of lithium.

[0624] In some embodiments, a lithium-containing layer is provided on the outermost layers on both sides of the negative electrode substrate, and a polymer layer is provided on the surface of the lithium-containing layer on both sides. The chemical composition and content of the polymer layers on both sides can be the same or different.

[0625] In a fourth aspect, the present application provides a secondary battery comprising a cell electrolyte and the electrode assembly described in the third aspect of the present application, wherein the cell electrolyte is disposed between the polymer layer and the positive electrode plate.

[0626] A dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer on at least one side of the negative electrode plate in the secondary battery. The flexible polymer layer can be tightly adhered to the surface of the lithium-containing layer, and can act as a protective layer at the negative electrode of the lithium metal battery. It can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of electrolyte and lithium, improve coulombic efficiency, and extend the cycle life.

[0627] Typically, a secondary battery consists of a positive electrode, a negative electrode, a cell electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The cell electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.

[0628] Positive electrode

[0629] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.

[0630] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0631] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0632] In some embodiments, the positive electrode active material may adopt the positive electrode active material for batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ),

[0633] LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0634] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0635] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0636] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0637] Battery electrolyte

[0638] The cell electrolyte conducts ions between the positive and negative electrodes. This application does not specifically limit the type of cell electrolyte, and the type can be selected based on needs. For example, the cell electrolyte can be liquid, gel, or solid.

[0639] In some embodiments, the battery cell electrolyte is a second electrolyte. The second electrolyte includes an electrolyte salt and a solvent. The composition of the second electrolyte and the electrolyte in the polymer layer can be the same or different.

[0640] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0641] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0642] In some embodiments, the battery cell electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0643] Isolation film

[0644] In this application, unless otherwise specified, “separator membrane” and “diaphragm” have the same meaning and can be used interchangeably.

[0645] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0646] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0647] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0648] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the battery cell electrolyte.

[0649] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0650] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG6 shows a secondary battery 5 with a square structure as an example.

[0651] In some embodiments, referring to Figure 7, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0652] In some embodiments, the components of the core electrolyte and the electrolyte in the polymer layer may be the same or different.

[0653] When the composition of the cell electrolyte in the secondary battery is the same as that of the electrolyte in the polymer layer, the consistency of lithium ion transmission in the cell can be maintained, and the interference of multiple factors such as electrolyte solvation and interface side reactions can be reduced.

[0654] When the composition of the core electrolyte in the secondary battery is different from that of the electrolyte in the polymer layer, the formation of a stable SEI can be induced in a directionally manner on the lithium-containing layer side, thereby regulating the deposition morphology of lithium ions.

[0655] In some embodiments, the charging current density of the secondary battery is selected from 0.3 mA / cm 2 ~12mA / cm 2 .

[0656] In some embodiments, the charging current density of the secondary battery is selected from 1 mA / cm 2 ~10mA / cm 2 .

[0657] In some embodiments, the charging current density of the secondary battery is selected from 1 mA / cm 2 ~6mA / cm 2 .

[0658] In some embodiments, the charging current density of the secondary battery is selected from 1 mA / cm 2 ~3mA / cm 2 .

[0659] In some embodiments, the charging current density of the secondary battery can be selected from any one of the following values ​​or an interval consisting of any two values: 0.3 mA / cm 2 , 0.4mA / cm 2 , 0.5mA / cm 2 , 0.6mA / cm 2 , 0.7mA / cm 2, .8mA / cm 2 , 0.9mA / cm 2 , 1mA / cm 2 , 1.5mA / cm 2 , 2mA / cm 2 , 2.5mA / cm 2 , 3mA / cm 2 , 3.5mA / cm 2 , 4mA / cm 2 , 4.5mA / cm 2 , 5mA / cm 2 , 5.5mA / cm 2 , 6mA / cm 2 , 7mA / cm 2 , 8mA / cm 2 , 9mA / cm 2 , 10mA / cm 2 , 11mA / cm 2 , 12mA / cm 2 wait.

[0660] In some embodiments, the applicable charging current density may also be 0.3 mA / cm 2 ~0.5mA / cm 2 , 0.5mA / cm 2 ~1mA / cm 2 , 1mA / cm 2 ~1.5mA / cm 2 , 1.5mA / cm 2 ~2mA / cm 2 , 2mA / cm 2 ~2.5mA / cm 2 , 2.5mA / cm 2 ~3mA / cm 2 , 3mA / cm 2 ~3.5mA / cm 2 , 3.5mA / cm 2 ~4mA / cm 2 , 4mA / cm 2 ~4.5mA / cm 2 , 4.5mA / cm 2 ~5mA / cm 2 , 5mA / cm 2 ~5.5mA / cm 2 , 5.5mA / cm 2 ~ 6mA / cm 2 , 6mA / cm 2 ~8mA / cm 2 , 8mA / cm2 ~10mA / cm 2 or 10mA / cm 2 ~12mA / cm 2 .

[0661] The secondary battery provided in the present application can be cycled under the aforementioned charging current density conditions.

[0662] In some embodiments, the capacity retention rate of the secondary battery after 50 cycles is selected from 85% to 97%. The capacity after 50 cycles can also be selected from any one or two of the following percentages: 85%, 86%, 88%, 90%, 92%, 94%, 95%, 96%, etc.

[0663] In the present application, the "capacity retention rate after 50 cycles" of a secondary battery generally refers to a test value at 20°C to 30°C unless otherwise specified.

[0664] In some embodiments, the capacity retention rate of a secondary battery after 50 cycles refers to a volume expansion rate at 25°C.

[0665] In a fifth aspect, the present application provides a battery module, which includes the secondary battery described in the fourth aspect of the present application.

[0666] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0667] Figure 8 shows an example battery module 4. Referring to Figure 8 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0668] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0669] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0670] In a sixth aspect, the present application provides a battery pack comprising the battery module described in the fifth aspect of the present application.

[0671] Figures 9 and 10 illustrate an example battery pack 1. Referring to Figures 9 and 10 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0672] In a seventh aspect, the present application provides an electrical device comprising one or more of the secondary battery described in the fourth aspect of the present application, the battery module described in the fifth aspect of the present application, and the battery pack described in the sixth aspect of the present application.

[0673] The electrical device includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptop computers, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to these.

[0674] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0675] Figure 11 shows an example of an electric device 6. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module can be used.

[0676] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0677] In an eighth aspect, the present application provides an application of a monomer compound II in preparing a negative electrode sheet, wherein the structure of the monomer compound II is as shown in Formula II:

[0678]

[0679] Wherein, Rf, A, Z2, X and m are respectively as defined in the first aspect of the present application.

[0680] Non-limiting examples of monomeric compounds II are shown in Table 1.

[0681] In some embodiments, the monomer compound II contacts lithium in the lithium-containing layer of the negative electrode substrate and forms a polymer layer through in-situ polymerization.

[0682] The monomer compound II is a cyanoacrylic acid derivative compound, the cyano group of which can contact the lithium in the outermost layer of the negative electrode substrate to form a chemical connection, and the carbon-carbon double bond therein can undergo an in-situ polymerization reaction under lithium catalysis, thereby preparing the polymer-modified lithium material described in the first aspect of the present application. At this time, a firmly connected, tightly fitted, dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer, which can play the role of the aforementioned protective layer.

[0683] In a ninth aspect, the present application provides a method for preparing a negative electrode sheet, comprising the following steps:

[0684] Providing a negative electrode substrate, wherein the outermost layer of at least one side of the negative electrode substrate is a lithium-containing layer, and the lithium-containing layer includes lithium-containing metal; and also providing a reaction mixture containing monomer compound II and an electrolyte;

[0685] The reaction mixture is coated on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, and the monomer compound II is polymerized in situ to form a polymer layer;

[0686]

[0687] wherein Rf, A, Z2, X and m are as defined in the first aspect of this application;

[0688] Wherein, the electrolyte is as defined in the second aspect of this application.

[0689] The definition of the negative electrode substrate provided in this aspect can refer to the above definition. The negative electrode substrate provided in this aspect at least includes a lithium-containing layer capable of contacting the monomer compound II to catalyze the in-situ polymerization reaction.

[0690] In the presence of an electrolyte, the cyano group in the monomer compound II can contact the lithium in the outermost layer of the negative electrode substrate to form a chemical connection (covalent connection), and the carbon-carbon double bond therein can undergo an in-situ polymer reaction under lithium catalysis to form the polymer Poly shown in the aforementioned formula I, thereby preparing the polymer-modified lithium material described in the first aspect of the present application. At this time, a firmly connected, tightly fitted, dense and uniform flexible polymer layer is formed on the surface of the lithium-containing layer, which can play the role of the aforementioned protective layer. Compared with the physical coating effect in traditional technologies, it not only stably binds to the surface of the lithium-containing layer through chemical connection, avoiding falling off from the surface of the lithium-containing layer during the charge and discharge process, but also the coating is dense and uniform, and the coating thickness can be controlled at the nanoscale, and the assembled battery cell can exhibit a smaller interface impedance.

[0691] In some embodiments, the negative electrode sheet substrate can be prepared by the following method: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet substrate can be obtained.

[0692] In some embodiments, the present application provides that the monomer compound II contacts at least a catalytic amount of lithium in the lithium-containing metal, thereby providing chemical connection sites for the polymer layer and effectively catalyzing the in-situ polymerization reaction of cyanoacrylic acid derivative monomers.

[0693] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:2.

[0694] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:1.

[0695] In some embodiments, the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:1.

[0696] In some embodiments, the mass ratio of the monomer compound II to the electrolyte is selected from 5:1 to 1.5:1.

[0697] In some embodiments, the mass ratio of the monomer compound II to the electrolyte is selected from 4:1 to 1.5:1.

[0698] In some embodiments, the mass ratio of the polymer Poly to the electrolyte can also be any of the following ratios or an interval consisting of any two ratios: 9:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 1:1.5, etc.

[0699] By controlling the mass ratio of the monomer compound II and the electrolyte, the mass ratio of the polymer Poly to the electrolyte in the generated polymer layer can be controlled.

[0700] In some embodiments, in the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating method is selected from any one of a coating method, a spraying method, a spin coating method and a vapor deposition method.

[0701] In some embodiments, the reaction temperature of the in-situ polymerization is selected from 30°C to 100°C.

[0702] In some embodiments, the reaction temperature of the in-situ polymerization is selected from 30°C to 50°C.

[0703] In some embodiments, the reaction temperature of the in-situ polymerization is selected from 40°C to 60°C.

[0704] In some embodiments, the reaction temperature of the in situ polymerization can be selected from any one of the following values ​​or an interval consisting of any two of the following values: 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.

[0705] In some embodiments, the reaction time of the in-situ polymerization is selected from 0.1 h to 24 h.

[0706] In some embodiments, the reaction time of the in-situ polymerization is selected from 0.1 h to 12 h.

[0707] In some embodiments, the reaction time of the in-situ polymerization is selected from 0.1 h to 6 h.

[0708] In some embodiments, the reaction time of the in situ polymerization can be selected from any one of the following time lengths or an interval consisting of any two of the following time lengths: 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.8h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 11h, 12h, 14h, 15h, 16h, 18h, 20h, 21h, 22h, 24h, etc.

[0709] In some embodiments, in the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating thickness of the reaction mixture is selected from 100 nm to 8 μm.

[0710] In some embodiments, the coating thickness of the reaction mixture is selected from 50 nm to 5 μm.

[0711] In some embodiments, the coating thickness of the reaction mixture is selected from 50 nm to 8 μm.

[0712] In some embodiments, the coating thickness of the reaction mixture can be selected from any one of the following values ​​or an interval consisting of any two of the following values: 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, etc.

[0713] In some embodiments, the formed polymer layer is as defined in the second aspect of the present application.

[0714] In some embodiments, the negative electrode substrate is a pure lithium sheet. In this case, the negative electrode sheet can also be equipped with a negative current collector to facilitate the assembly of the tab. Alternatively, a pure lithium sheet covered with a polymer layer can be used as the negative electrode sheet.

[0715] In some embodiments, the negative electrode substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.

[0716] In some embodiments, a second negative electrode active material layer may or may not be provided between the negative electrode current collector and the lithium-containing layer, and the components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.

[0717] In some embodiments, the method of forming the second active material layer or the lithium-containing layer on the negative electrode current collector can be selected from: (1) a method of transferring lithium metal or lithium alloy rolled by rolling to the negative electrode current collector; (2) a method of evaporating lithium metal or lithium alloy on the negative electrode current collector, etc.

[0718] In some embodiments, the method of forming a lithium-containing layer on the second active material layer may be selected from: (1) a method of transferring lithium metal or lithium alloy rolled by rolling onto the second active material layer; (2) a method of evaporating lithium metal or lithium alloy on the second active material layer, etc.

[0719] In the tenth aspect, the present application provides a method for preparing a secondary battery, wherein the secondary battery is the secondary battery described in the fourth aspect of the present application, and the preparation method comprises the following steps: injecting the battery cell electrolyte into the battery shell containing the electrode assembly described in the third aspect of the present application.

[0720] Some embodiments of the present application are described below.

[0721] The parameter characterizations mentioned above, including but not limited to elastic modulus, elastic deformation range, polymer swelling rate, ionic conductivity, flexibility test, electrode expansion rate, battery cycle performance, etc., can be achieved by adopting or referring to the test methods below, including but not limited to the "Structure and Performance Test" section.

[0722] The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. Where specific techniques or conditions are not indicated in the embodiments, they are carried out according to the description above, or according to the technology or conditions described in the document in this area or according to the product specification. Reagents used or instruments that are not indicated by the manufacturer are conventional products that can be obtained commercially, or can be synthesized in a conventional manner by commercially available products.

[0723] In the following examples, unless otherwise specified, room temperature refers to 20°C to 30°C.

[0724] In the following embodiments, unless otherwise specified, the monomer-electrolyte mixture is applied by coating.

[0725] Preparation of fluorinated monomer (corresponding monomer compound II)

[0726] The fluorinated monomers used in the following examples can be obtained commercially or prepared by the following method. For the preparation of intermediates and synthetic products, those skilled in the art can use (but not limited to) Fourier transform infrared spectroscopy (FT-IR) testing, 1 Structural characterization can be performed using methods such as H NMR testing, gel permeation chromatography (GPC), and X-ray photoelectron spectroscopy (XPS) to confirm whether the structure of the synthesized product conforms to the structural design, which is achievable for those skilled in the art.

[0727] Step 1: Preparation of side chain molecule Cp3: Compound Cp1 (P A -AH-terminated polyethylene glycol, A is O or NH, AH is OH or NH2, PA is a protecting group of AH, corresponding to a hydroxyl protecting group or an amino protecting group) and Cp2 are reacted by condensation or addition reaction to obtain compound Cp31, and then the protecting group P of AH is removed. A Compound Cp3 is obtained. The reaction conditions can refer to existing methods in the field of organic chemistry and can be easily implemented by those skilled in the art.

[0728] Step 2: Preparation of monomer compound II shown in formula II

[0729]

[0730] When X in monomer compound II is H, the fluorinated monomer shown in formula II-1 can be prepared by a condensation reaction between compound Cp4 (2-cyanoacrylic acid, commercially available) and compound Cp3, and the reaction generates a linker A, wherein, when A is O, an ester bond (C(=O)-O) is generated by a condensation reaction between the carboxyl group and the hydroxyl group; when A is NH, an amide bond (C(=O)-NH) is generated by a condensation reaction between the carboxyl group and -NH2.

[0731] When X in monomer compound II is not H, taking X as -N(CH3)2 as an example, reference can be made to the method in the literature "Bredereck, Hellmut, et al. Chemische Berichte, 1964, 97(12), 3397-3406", using acetal compound Cp5 and 2-cyanoacrylate compound Cp6 to prepare acrylate compound Cp7 containing 1-X and 2-cyano groups, hydrolyze to form compound Cp8, and then condense with compound Cp3 to produce the fluorinated monomer shown in formula II-2.

[0732] The reaction formula in step 1 is as follows:

[0733]

[0734] Step 2, taking X as H as an example, the fluorinated monomer shown in Formula II-1 can be prepared by referring to the following reaction formula:

[0735]

[0736] Step 2: Taking X as -N(CH3)2 as an example, the fluorinated monomer shown in Formula II-1 can be prepared by referring to the following reaction formula:

[0737]

[0738] Whether the product compound is formed may be determined based on at least one of the molecular weight test result and the viscosity test result.

[0739] Example 1. Preparation of a lithium metal anode containing a polymer layer

[0740] (1) At 25°C, 10 g of fluorinated monomer (see Table 1), 0.955 g of lithium bis(fluorosulfonyl)imide (LiFSI), and 4.425 g of ethylene glycol dimethyl ether (DME) were stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1.

[0741] (2) The resulting monomer-electrolyte mixture was coated on the surface of a lithium sheet and allowed to react at 30°C for 2 h to obtain a lithium sheet containing a transparent, dense polymer layer. The operating parameters are shown in Table 2. The sheet was cut into Φ16 mm diameter discs to serve as the negative electrode.

[0742] (3) Preparation of positive electrode sheet:

[0743] The positive electrode active material LiCoO2, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 96:2:2, and the solvent N-methylpyrrolidone (NMP) was added and stirred until the system became uniform to obtain a positive electrode slurry. The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying. Then, it was cut into discs with a diameter of Φ14mm as positive electrode sheets. The positive electrode surface capacity was 3mAh / cm 2 .

[0744] (4) Preparation of electrolyte:

[0745] Lithium bis(fluorosulfonyl)imide (LiFSI) was slowly added to ethylene glycol dimethyl ether (DME) to prepare an electrolyte with a LiFSI concentration of 1 mol / L.

[0746] (5) Isolation film: Use polypropylene film.

[0747] (6) Battery preparation:

[0748] Place the above-mentioned positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role, inject the electrolyte prepared in (4) above, and assemble into a button battery.

[0749] Before the battery test, the lithium metal battery was charged at 3.0 mA / cm 2 The constant current was charged to 4.25V, and then 3.0mA / cm 2 The constant current discharges to 3.0V.

[0750] Examples 2 to 13 adopt methods substantially the same as those of Example 1, except that step (1) is different.

[0751] In Examples 2 to 13, the monomer fluorinated monomer, the fluorine substitution rate in Rf in the monomer, the mass content of the electrolyte in the monomer-electrolyte mixture, the lithium salt concentration in the electrolyte of step (1), the coating thickness, the temperature and time of the in situ polymerization reaction can be found in Tables 1 and 2.

[0752] Steps (1) of Example 2 to Example 13 are as follows.

[0753] Example 2

[0754] Step (1): At 25° C., 10 g of a fluorinated monomer, 0.540 g of a lithium salt, and 4.840 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0755] Example 3

[0756] Step (1): At 25° C., 10 g of a fluorinated monomer, 0.540 g of a lithium salt, and 4.840 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0757] Example 4

[0758] Step (1): At 25° C., 10 g of a fluorinated monomer, 0.955 g of a lithium salt, and 4.425 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0759] Example 5

[0760] Step (1): At 25° C., 10 g of fluorinated monomer, 0.4397 g of lithium salt and 4.940 g of electrolyte solvent were mixed uniformly and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for fluorinated monomer.

[0761] Example 6

[0762] Step (1): At 25° C., 10 g of fluorinated monomer, 0.5795 g of lithium salt and 4.800 g of electrolyte solvent were mixed uniformly and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for fluorinated monomer.

[0763] Example 7

[0764] Step (1): At 25° C., 10 g of a fluorinated monomer, 0.540 g of a lithium salt, and 4.840 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0765] Example 8

[0766] Step (1): At 25° C., 18 g of a fluorinated monomer, 0.201 g of a lithium salt, and 1.799 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0767] Example 9

[0768] Step (1): At 25° C., 6 g of fluorinated monomer, 0.904 g of lithium salt and 8.096 g of electrolyte solvent were mixed uniformly and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for fluorinated monomer.

[0769] Examples 10-13

[0770] Step (1): At 25° C., 10 g of a fluorinated monomer, 0.955 g of a lithium salt, and 4.425 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0771] Comparative Examples 1-11 are prepared according to the method of Example 1, with the differences shown in Tables 1 and 2.

[0772] Comparative Example 1

[0773] Step (1): At 25° C., 20 g of fluorinated monomer, 0.041 g of lithium salt and 0.367 g of electrolyte solvent were mixed uniformly and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for fluorinated monomer.

[0774] Comparative Example 2

[0775] Step (1): At 25° C., 3 g of fluorinated monomer, 1.206 g of lithium salt and 10.794 g of electrolyte solvent were mixed uniformly and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for fluorinated monomer.

[0776] Comparative Examples 3-11

[0777] Step (1): At 25° C., 10 g of a fluorinated monomer, 0.955 g of a lithium salt, and 4.425 g of an electrolyte solvent were mixed uniformly, and stirred uniformly at room temperature to obtain a monomer-electrolyte mixture, see Table 1 for the fluorinated monomer.

[0778] Comparative Example 1 and Comparative Example 2 respectively adopt methods substantially the same as Example 1, except that the mass content of the electrolyte in the monomer-electrolyte mixture is different, as shown in Tables 1 and 2.

[0779] Comparative Examples 3 and 4 respectively adopt methods substantially the same as those of Example 1, except that the concentration of lithium salt in the electrolyte in step (1) is different, as shown in Tables 1 and 2.

[0780] Comparative Example 5 and Comparative Example 6 respectively adopt the method basically the same as Example 1, and the difference is that the coating thickness is different, which can be seen in Table 1 and Table 2.

[0781] Comparative Example 7 adopts a method that is substantially the same as that of Example 1, except that the structure of monomer compound II is different (no EO segment in the side chain, m=0), as shown in Tables 1 and 2.

[0782] Comparative Example 8 adopts a method that is substantially the same as that of Example 1, except that the structure of monomer compound II is different (the side chain is not substituted by fluorine), as shown in Tables 1 and 2.

[0783] Comparative Example 9: A polymer solution having a molecular weight of 1000 kDa was sprayed onto the surface of a pure lithium sheet and dried to obtain a coated polymer layer, as shown in Tables 1 and 2. The polymer solution was prepared by dissolving 18 g of a polymer in 50 mL of a solvent, wherein the polymer was a PVdF-HFP (polyvinylidene fluoride-hexafluoropropylene) copolymer having a weight-average molecular weight of 500 kDa, and the solvent was tetrahydrofuran (THF).

[0784] In Comparative Example 10, a pure lithium sheet is used as the negative electrode sheet, that is, there is no polymer layer.

[0785] The PEG segment used in Comparative Example 11 was replaced with a polyoxypropylene PPO segment, and the remaining parameters were the same as in Example 1.

[0786] Table 1.

[0787]

[0788]

[0789]

[0790] Table 2.

[0791]

[0792]

[0793] Note 1: “About” in the average degree of polymerization means ±2; the average degree of polymerization corresponds to the average value of n of the polymer Poly represented by formula I in the polymer layer.

[0794] Test sample preparation

[0795] 1. Preparation of polymer layer membrane

[0796] (1) At 25°C, 30 g of fluorinated monomer, 2.4 g of lithium bis(fluorosulfonyl)imide (LiFSI), and 15 g of ethylene glycol dimethyl ether (DME) were stirred at room temperature to obtain a uniform solution.

[0797] (2) 0.48 g of lithium powder was added to the uniform solution obtained in step (1), and the mixture was quickly stirred and evenly coated on a glass plate. The mixture was allowed to stand for reaction at 30° C. for 2 h to obtain a transparent polymer layer film with a thickness of 15 μm.

[0798] Structure and performance testing

[0799] 1. Characterization of polymer components in the polymer layer (lithium metal protection layer)

[0800] The lithium sheet containing the polymer layer is immersed in isopropanol. The lithium sheet will be corroded and consumed. The generated lithium isopropoxide can be dissolved in isopropanol. The polymer is insoluble in isopropanol and precipitates. After centrifugal drying, a solid sample of the polymer can be obtained.

[0801] 1.1. Fourier transform infrared spectroscopy (FT-IR) test: ATR mode, 4cm -1 Resolution, 32 scans, wave number range 4000cm -1 ~400cm -1 .

[0802] 1.2. 1 H NMR nuclear magnetic test: 1 The H resonance frequency was 400 MHz, the solvent was deuterated dimethyl sulfoxide (DMSO-d6), and tetramethylsilane (TMS) was used as the internal standard.

[0803] 1.3. Molecular weight test: The polymer sample was dissolved in NMP and the molecular weight was tested by gel permeation chromatography (GPC) to obtain the weight average molecular weight, number average molecular weight and molecular weight polydispersity index (PDI).

[0804] 1.4. Polymer layer thickness test: The polymer coating thickness was measured using a laser thickness gauge.

[0805] 1.5. Viscosity Test: The viscosity of the polymer solution was tested using a viscometer. The polymer solution was prepared as follows: 5 g of polymer was dissolved in 30 mL of NMP. The test temperature was 25°C.

[0806] 2. Fluorine content

[0807] The content of fluorine in the polymer layer can be detected by X-ray photoelectron spectroscopy (XPS).

[0808] 3. Swelling parameters

[0809] The swelling parameters of the polymer layer were tested using the following method:

[0810] The test temperature was 25°C. The lithium metal sheet containing the polymer layer was cut into 30 mm x 30 mm square samples, with three replicates per group. Each sample was weighed. The sample was then immersed in a 1 mol / L LiFSI-based DME electrolyte for 2 hours to allow it to swell. After swelling, the sample was gently wiped with filter paper to remove any residual electrolyte, and the swollen sample was weighed. The swelling rate of the polymer layer was calculated as the percentage of the increased mass of the swollen sample to the original sample mass.

[0811] 4. Ionic conductivity

[0812] The test temperature was 25°C. The polymer membrane was punched into a Φ16mm diameter disc. The disc was immersed in electrolyte for 1 hour, removed, and the electrolyte on the membrane surface was wiped with filter paper. The ionic conductivity of the polymer membrane after swelling in the electrolyte was calculated using the formula σ = d / RA, where d is the membrane thickness, measured with a micrometer, A is the membrane area, and R is the membrane impedance. The impedance of the symmetrical cell was measured using an electrochemical workstation at a test frequency of 10 -6 ~10 -1 Hz, the voltage amplitude is 5mV; the intersection of the graph and the horizontal axis is the impedance R of the polymer film.

[0813] 5. Elastic modulus and elastic deformation

[0814] Elastic Modulus: Tested at 25°C. Cut the polymer film into strips with a length L0 of 150 mm and a width of 20 mm. Measure the elastic modulus of the polymer film using a universal testing machine at a stretching distance of 100 mm and a stretching speed of 50 mm / min. The maximum tensile force of the polymer film is the elastic modulus.

[0815] Elastic deformation: The test temperature is 25° C. When a polymer film is stretched, the length at the time of film rupture is L, and the elastic deformation of the film can be calculated as (L-L0) / L0×100%.

[0816] 6. Polymer layer bonding performance test (peeling degree)

[0817] By controlling the reaction time, the thickness of the polymer layer on the lithium metal surface is controlled to be around 5μm. A 50×100 mm area is used as a peeling test sample. A sharp blade (with a sharp angle of 15° to 30°) is used to draw 10×10 1mm×1mm small grids on the surface of the protective layer sample. Each line should be deep enough to reach the bottom layer of the protective layer. Use a brush to clean the debris in the test area. Use an adhesive force of 350g / cm 2 ~400g / cm 2 Firmly adhere the small grid to be tested with adhesive tape (3M No. 600 tape or equivalent) and vigorously rub the tape with an eraser to increase the contact area and strength between the tape and the tested area. Grab one end of the tape and quickly pull it off vertically (90°). Perform the same test twice at the same location. Finally, observe the grid area with a magnifying glass. If there is no peeling or it occurs within the protective layer, it is qualified. However, if the peeling occurs between the metal and the protective layer and the area is greater than 65%, it is rated 0B; if the area is 35%-65%, it is rated 1B; if the area is 15%-35%, it is rated 2B; if the area is 5%-15%, it is rated 3B; if the area is less than or equal to 5%, it is rated 4B. If the cut edge is completely smooth and there is no peeling at the grid edge, it is rated 5B.

[0818] 7. Flexibility testing of polymer materials

[0819] Differential Scanning Calorimetry (DSC) was performed to characterize the glass transition temperature (Tg) of the polymer material. A lower Tg indicates greater molecular weight flexibility. The DSC test temperature range was 35-800°C, with a heating rate of 5°C / min and an argon atmosphere.

[0820] 8. Pole performance test

[0821] Pole sheet volume expansion rate: The test temperature is 25°C. The thickness of the fresh lithium sheet is d1. After the battery is cycled 50 times to a fully discharged state, the battery is disassembled and the thickness of the lithium sheet is measured using an optical microscope to be d2. The pole sheet expansion rate is (d2-d1) / d1×100%.

[0822] 9. Battery performance test

[0823] (1) Cycling performance test: The test temperature is 25°C. The lithium metal battery is first charged to 4.25V at a constant current and then discharged to 3.0V to obtain the first-cycle discharge capacity (Cd1). This charge and discharge cycle is repeated for 50 cycles. The discharge capacity of the lithium metal battery after n cycles is recorded as Cdn. Capacity retention rate = discharge capacity after n cycles (Cdn) / first-cycle discharge capacity (Cd1) × 100%. The battery charging current density can be referred to in Table 3.

[0824] (2) Observation of the lithium negative electrode surface: After the battery was fully discharged at the 50th cycle, the uniformity of lithium deposition / dissolution and the flatness of the lithium negative electrode surface were observed under an optical microscope.

[0825] Test results

[0826] The test results of the polymer molecular weight in the polymer layer, the mass percentage of fluorine in the polymer, and the thickness of the polymer layer can be found in Table 2. The test results of the swelling rate, ionic conductivity, elastic modulus, and elastic deformation of the polymer layer, as well as the battery charging current density, capacity retention after 50 cycles, lithium dendrites, pole piece volume expansion rate, and degree of peeling of lithium-ion batteries prepared using negative electrode sheets containing the polymer layer of the present application can be found in Table 3.

[0827] Example 1:

[0828] FTIR: 2853–2962 cm -1 , CH stretching vibration; 2245cm -1 ,-CN stretching vibration; 1742cm -1 ,-C=O stretching vibration; 1100–1300 cm -1 , -CF stretching vibration; 400–700 cm -1, -CF bending vibration; 1036cm -1 ,-CO stretching vibration.

[0829] Tg: -10℃.

[0830] Example 2:

[0831] FTIR: 2889cm-2965cm -1 , CH stretching vibration; 2241cm -1 ,-CN stretching vibration; 1735cm -1 ,-C=O stretching vibration; 1192cm -1 , CN stretching vibration; 1100–1300 cm -1 , -CF stretching vibration; 400–700 cm -1 , -CF bending vibration; 1019cm -1 ,-CO stretching vibration.

[0832] Tg: -15℃.

[0833] Example 3:

[0834] FTIR: 2850–2962 cm -1 , CH stretching vibration; 2243cm -1 ,-CN stretching vibration; 1739cm -1 ,-C=O stretching vibration; 1100–1300 cm -1 , -CF stretching vibration; 400–700 cm -1 , -CF bending vibration; 1021cm -1 ,-CO stretching vibration.

[0835] Tg: -23℃.

[0836] Example 4:

[0837] FTIR: 2853–2962 cm -1 , CH stretching vibration; 2245cm -1 ,-CN stretching vibration; 1692cm -1 ,-C=O stretching vibration; 3345cm -1 , -NH stretching vibration; 1623cm -1 , -NH bending vibration; 1100–1300 cm-1 , -CF stretching vibration; 400–700 cm -1 , -CF bending vibration; 1026cm -1 ,-CO stretching vibration.

[0838] Tg: -19℃.

[0839] Example 5:

[0840] FTIR: 2883–2964 cm -1 , CH stretching vibration; 2238cm -1 ,-CN stretching vibration; 1742cm -1 ,-C=O stretching vibration; 1100–1300 cm -1 , -CF stretching vibration; 400–700 cm -1 , -CF bending vibration; 1032cm -1 ,-CO stretching vibration; 1360cm -1 ,-NO stretching vibration.

[0841] Tg: -8℃.

[0842] Example 6:

[0843] FTIR: 2856–2962 cm -1 , CH stretching vibration; 2245cm -1 ,-CN stretching vibration; 1751cm -1 ,-C=O stretching vibration; 1100–1300 cm -1 , -CF stretching vibration; 400–700 cm -1 , -CF bending vibration; 1037cm -1 ,-CO stretching vibration.

[0844] Tg: -13℃.

[0845] Example 7:

[0846] FTIR: 2856–2953 cm -1 , CH stretching vibration; 2245cm -1 ,-CN stretching vibration; 1751cm -1 ,-C=O stretching vibration; 1100–1300 cm -1 ,-CF stretching vibration; 400–700 cm -1 , -CF bending vibration; 1023cm -1 ,-CO stretching vibration; 1315cm -1 , -P=O stretching vibration; 1160cm -1 , -PO stretching vibration.

[0847] Tg: -16℃.

[0848] Compared with Comparative Examples 8 and 9, after containing the polymer layer of the present application (Examples 1 to 13, Comparative Examples 3 to 6), the volume expansion of the lithium negative electrode is significantly suppressed after the lithium metal battery is cycled multiple times, which is beneficial for the battery to maintain a good capacity retention rate.

[0849] By comparing Example 1 and Comparative Example 7, it can be seen that the EO segment is beneficial to improving the flexibility and elasticity of the polymer layer. After the lithium metal battery is cycled multiple times, the volume expansion of the lithium negative electrode is significantly suppressed, which is beneficial for the battery to maintain a good capacity retention rate.

[0850] Comparing Examples 1 to 4, it can be seen that the longer EO chain segment can improve the flexibility and elasticity of the polymer coating. After the lithium metal battery is cycled multiple times, the volume expansion of the lithium negative electrode is significantly suppressed, which is beneficial for the battery to maintain a good capacity retention rate.

[0851] By regulating the monomer structure in the polymer layer, different fluorine substitution rates and fluorine contents can be achieved. Compared to Comparative Example 8, the introduction of fluorine in Examples 1 to 13 helps enhance the protective film's ability to regulate lithium ion deposition, improve dendrite morphology, and reduce volume expansion.

[0852] By comparing Example 1 and Example 4, it can be seen that when the fluorine-substituted aliphatic group is connected to the polymer main chain through an amide group (A is NH in Example 4), the polymer protective layer can improve the ionic conductivity and elastic modulus of the polymer layer, improve the battery charging current density of the secondary battery, the capacity retention rate and volume expansion performance after 50 cycles, and significantly inhibit lithium dendrites.

[0853] Comparing Example 1 and Example 6, it can be seen that when the fluorine-substituted aliphatic group is connected to the polymer backbone through the phosphate group (in Example 6, A is O and Rf is close to the EO segment side ), the polymer protective layer can improve the ionic conductivity of the polymer layer, improve the battery charging current density of the secondary battery, the capacity retention rate and volume expansion performance after 50 cycles, and significantly inhibit lithium dendrites.

[0854] Comparison of Examples 7-8 and Comparative Examples 1-2 shows that controlling the electrolyte content in the polymer layer can regulate the swelling rate and mechanical properties of the polymer layer. In Comparative Example 1, although the high electrolyte content is beneficial to the improvement of ionic conductivity, the rigidity of the membrane is low, which is not conducive to the 3mA / cm 2 The above high current charge and discharge results in severe dendrites, large volume expansion, and rapid capacity decay. In Comparative Example 2, the ionic conductivity decreases, which is not conducive to 3mA / cm 2 The above large current charging and discharging will cause serious dendrites, large volume expansion, and rapid capacity decay.

[0855] Comparison of Examples 9-10 and Comparative Examples 3-4 demonstrates that varying the deposition morphology and expansion rate of the polymer layer can be achieved by adjusting the lithium salt concentration in the polymer layer. Lower lithium salt concentrations result in lower ionic conductivity and elastic modulus in the polymer protective layer, hindering the suppression of dendrite formation and negative electrode volume expansion. Higher lithium salt concentrations, however, compromise the mechanical strength of the material.

[0856] By comparing Examples 11 to 12 and Comparative Examples 5 to 6, it can be seen that the thickness of the polymer layer needs to be controlled within a certain range. If it is too thick, the polarization of the battery cell is large, the ionic conductivity is low, and the cycle decay is fast; if it is too thin, the mechanical strength is poor, which is not conducive to suppressing dendrites and uneven deposition of lithium.

[0857] Comparing the embodiments with Comparative Example 11, it can be seen that the EO segment has obvious advantages over other types of polymer segments in terms of ionic conductivity, cycle performance, reduction of lithium dendrites and control of electrode expansion.

[0858] In summary, by adjusting the fluorine content, EO segment length, lithium salt concentration, electrolyte content and thickness of the protective layer membrane, the membrane can achieve higher electrical conductivity and mechanical strength, which is beneficial for the application of the protective layer in lithium metal batteries that are charged and discharged at high current density.

[0859] Table 3.

[0860]

[0861]

[0862] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0863] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and within the scope of the technical solution of the present application, embodiments that have substantially the same structure as the technical idea and exert the same effect are all included in the technical scope of the present application. The above-mentioned embodiments only express several embodiments of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent. In addition, without departing from the scope of the subject matter of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of constructing by combining some of the constituent elements in the embodiments are also included in the scope of the present application. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all fall within the scope of protection of the present application. Therefore, the scope of protection of the present application shall be based on the attached claims, and the description and drawings may be used to explain the content of the claims.

Claims

1. A polymer-modified lithium material comprising a lithium-containing metal and a polymer (Poly) chemically bonded to the surface of lithium in the lithium-containing metal, wherein the polymer (Poly) comprises a structure represented by Formula I; in, Each occurrence of Rf is independently a fluorine-substituted aliphatic group; Each occurrence of X is independently H or an electron withdrawing group; Each occurrence of A is independently O, S or NR 11 ; Among them, R 11 H or C 1-3 alkyl; Each occurrence of Z2 is independently a bond, carbonyl, -(O=)P(-O-)2, -S(=O)2-, -C(=O)-NH- or L C -Z0, where Lc is C 1-3 Alkylene, Z0 is a coupling type linking group; * indicates the site of attachment of the terminal groups; n is an integer ≥10; m is a positive integer ≤ 10; At least one cyano group in the polymer Poly forms a chemical connection with lithium in the lithium-containing metal.

2. The polymer-modified lithium material according to claim 1, wherein Each occurrence of m is independently 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10; Preferably, each occurrence of m is independently 1, 2, 3, 4, 5, 6, 7 or 8; Also preferably, each occurrence of m is independently 1, 2, 3, 4, 5 or 6; Also preferably, each occurrence of m is independently 1, 2, 3, 4 or 5; Also preferably, each occurrence of m is independently 1, 2 or 3; Also preferably, each occurrence of m is independently 2, 3, 4, 5 or 6; Also preferably, each occurrence of m is independently 2, 3, 4 or 5; Also preferably, m is independently 2 or 3 at each occurrence.

3. The polymer-modified lithium material according to claim 1 or 2, wherein: Each time Rf appears, the fluorine substitution rate in Rf independently satisfies >50%; Preferably, the fluorine substitution rate in Rf independently satisfies ≥55%; Preferably, the fluorine substitution rate in Rf independently satisfies ≥60%; Preferably, the fluorine substitution rate in Rf independently satisfies ≥65%; Preferably, the fluorine substitution rate in Rf independently satisfies ≥70%; Preferably, the fluorine substitution rate in Rf independently satisfies ≥80%; Preferably, at least 50% of the Rf in the polymer Poly satisfies a fluorine substitution rate ≥80%, or ≥90%; Preferably, at least 60% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥70%, or ≥80%, or ≥90%; Preferably, at least 70% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥60%, or ≥70%, or ≥80%, or ≥90%; Preferably, at least 80% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥50%, or ≥60%, or ≥70%, or ≥80%, or ≥90%.

4. The polymer-modified lithium material according to any one of claims 1 to 3, wherein: Each time Rf appears, the number of fluorine atoms in Rf is independently an integer ≥ 4; Preferably, the number of fluorine atoms in Rf is independently an integer selected from 4 to 20; Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 16; Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 15; Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 13; Another preferred embodiment is that the number of fluorine atoms in Rf is independently an integer selected from 4 to 10; Also preferably, the number of fluorine atoms in Rf is independently 4, 5, 6, 7, 8, 9, 10, 11, 12 or 13.

5. The polymer-modified lithium material according to any one of claims 1 to 4, wherein: The mass proportion of fluorine element in the polymer Poly is selected from 10% to 50%; Preferably, the mass proportion of fluorine element in the polymer Poly is selected from 15% to 50%; Another preferred embodiment is that the mass proportion of fluorine element in the polymer Poly is selected from 20% to 50%.

6. The polymer-modified lithium material according to any one of claims 1 to 5, wherein: Each time Rf appears, Rf contains 2 to 10 main chain carbon atoms; Preferably, Rf contains 2 to 8 main chain carbon atoms; Another preferred embodiment is that Rf contains 2 to 7 main chain carbon atoms; Also preferably, Rf contains 3, 4, 5, 6, 7 or 8 main chain carbon atoms; Another preferred embodiment is: The chain length is selected from 5 to 40, preferably from 5 to 35, preferably from 5 to 30, preferably from 6 to 40, preferably from 6 to 35, preferably from 6 to 30, preferably from 8 to 40, preferably from 8 to 35, preferably from 8 to 30, preferably from 10 to 40, preferably from 10 to 35, preferably from 10 to 30; the chain length refers to the number of backbone atoms of the longest backbone connecting the carbonyl site and the terminal group in Rf.

7. The polymer-modified lithium material according to claim 6, wherein: Each time Rf appears, the number of carbon atoms in Rf is an integer selected from 2 to 10; Preferably, the number of carbon atoms in Rf is an integer selected from 2 to 8; Another preferred embodiment is that the number of carbon atoms in Rf is an integer selected from 2 to 7; Also preferably, the number of carbon atoms in Rf is 3, 4, 5, 6, 7 or 8.

8. The polymer-modified lithium material according to any one of claims 1 to 7, wherein: Each occurrence of Rf further comprises one or more heteroatoms selected from the group consisting of iodine, nitrogen, oxygen, sulfur, silicon, boron and phosphorus; Preferably, each time Rf occurs, the number of any one of the heteroatoms in Rf is 1 or more; Another preferred embodiment is that the number of any one of the heteroatoms in Rf is selected from 1 to 5; Also preferably, the number of any one of the heteroatoms in Rf is selected from 1, 2, 3 or 4.

9. The polymer-modified lithium material according to claim 8, wherein: Each time Rf appears, the number of heteroatoms in Rf satisfies one or more of the following: The number of oxygen atoms in Rf is 1, 2, 3, 4 or 5; The number of nitrogen atoms in Rf is 1, 2 or 3; The number of sulfur atoms in Rf is 1, 2, or 3; The number of phosphorus atoms in Rf is 1 or 2; The number of iodine atoms in Rf is 1, 2, 3, 4, 5 or 6; The number of silicon atoms in Rf is 1 or 2; and The number of boron atoms in Rf is 1 or 2.

10. The polymer-modified lithium material according to any one of claims 1 to 8, wherein: Each occurrence of Rf contains one or more iodine groups, -NR 12 -, -O-, -S-, -S(O)2-, >Si<, >B- and >P(=O)-, wherein R 12 H or C 1-3 alkyl; Preferably, R 12 is H or methyl; Another preferred embodiment is that R 12 For H.

11. The polymer-modified lithium material according to claim 10, wherein: Each occurrence of Rf contains one or more atoms or groups of atoms selected from the group consisting of -O-, -S(O)2- and -(O=)P(-O-)2; Preferably, Rf contains one or more -O-; Another preferred embodiment is that Rf contains -S(O)2F; Another preferred embodiment is that Rf contains -(O=)P(-O-)2.

12. The polymer-modified lithium material according to any one of claims 1 to 11, wherein: Each occurrence of the fluorine-substituted aliphatic group is independently a straight-chain structure or a branched-chain structure.

13. The polymer-modified lithium material according to any one of claims 1 to 6, wherein: Each time Rf appears, the structure of Rf is independently as shown in Formula III-1, Formula III-2 or Formula III-3: Among them, R 31 、R 32 and R 3 Each occurrence is independently H or F; each occurrence of m3 is independently an integer selected from 2 to 10; in formula III-1, there are at least 4 F atoms; Preferably, m3 is an integer selected from 3 to 10; Another preferred embodiment is that m3 is an integer selected from 3 to 8; Another preferred embodiment is that m3 is 3, 4, 5, 6, 7 or 8; R 41a 、R 42a 、R 4a 、R 41b 、R 42b and R 4b Each occurrence is independently H or F; m 4a and m4 4b Each occurrence is independently an integer selected from 1 to 9; in formula III-2, contains at least 4 F atoms; Preferably, m 4a and m4 4b are each independently an integer selected from 2 to 9; Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 2 to 8; Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 3 to 8; Another preferred embodiment is that m 4a and m4 4b are each independently an integer selected from 3 to 6; R 51 and R 52 Each occurrence is independently H or F; each occurrence of m5 is independently an integer selected from 2 to 10; in formula III-3, there are at least 4 F atoms; Preferably, m5 is an integer selected from 3 to 10; Another preferred embodiment is that m5 is an integer selected from 3 to 8; Another preferred embodiment is that m5 is 3, 4, 5, 6, 7 or 8.

14. The polymer-modified lithium material according to claim 13, wherein: Each time Rf appears, the structure of Rf is as shown in Formula III-1; Alternatively, each time Rf appears, the structure of Rf is as shown in Formula III-2; Alternatively, each time Rf appears, the structure of Rf is as shown in Formula III-3.

15. The polymer-modified lithium material according to claim 13 or 14, wherein: Each occurrence of Formula III-1 has 0, 1, 2, 3, or 4 H atoms; each occurrence of Formula III-2 has 0, 1, 2, 3, 4, 5, or 6 H atoms; each occurrence of Formula III-3 has 0, 1, 2, 3, or 4 H atoms; Preferably, each time Formula III-1 appears, the number of H atoms therein is 0; each time Formula III-2 appears, the number of H atoms therein is 0; each time Formula III-3 appears, the number of H atoms therein is 0.

16. The polymer-modified lithium material according to any one of claims 13 to 15, wherein: Each occurrence of Rf is independently selected from any one of the following structures:

17. The polymer-modified lithium material according to any one of claims 1 to 16, wherein: Each occurrence of X is independently H or an electron withdrawing group containing 1 to 6 non-hydrogen atoms.

18. The polymer-modified lithium material according to claim 17, wherein: Each occurrence of X is independently H or cyano, nitro or -NR 21 R 22 ; Among them, R 21 and R 22 Each independently is H or C 1-3 alkyl; Preferably, R 21 and R 22 are each independently H or methyl; Another preferred embodiment is that R 21 and R 22 All are methyl.

19. The polymer-modified lithium material according to any one of claims 1 to 18, wherein: Each occurrence of A is independently O, S or NH; Preferably, each occurrence of A is independently O or NH; Another preferred embodiment is that each occurrence of A is O; Alternatively, each occurrence of A is NH.

20. The polymer-modified lithium material according to any one of claims 1 to 19, wherein Rf in Formula I are all the same; In formula I, each occurrence of X is the same; A in Formula I is the same at each occurrence; Preferably, each occurrence of Z2 in formula I is the same.

21. The polymer-modified lithium material according to any one of claims 1 to 20, wherein: n is an integer selected from 10 to 1000, preferably an integer selected from 10 to 950, preferably an integer selected from 10 to 800, preferably an integer selected from 15 to 800, preferably an integer selected from 20 to 800, preferably an integer selected from 40 to 800, preferably an integer selected from 50 to 800, preferably an integer selected from 100 to 800, preferably an integer selected from 10 to 750, preferably an integer selected from 15 to 750, preferably an integer selected from 20 to 750, and preferably an integer selected from 20 to 750. It is preferably an integer selected from 40 to 750, further preferably an integer selected from 50 to 750, further preferably an integer selected from 80 to 750, further preferably an integer selected from 100 to 750, further preferably an integer selected from 10 to 600, further preferably an integer selected from 15 to 600, further preferably an integer selected from 20 to 600, further preferably an integer selected from 40 to 600, further preferably an integer selected from 50 to 600, further preferably an integer selected from 100 to 600, further preferably an integer selected from 100 to 200.

22. The polymer-modified lithium material according to any one of claims 1 to 20, wherein: The number average molecular weight of the polymer Poly is selected from 10kDa to 200kDa; Preferably, the number average molecular weight of the polymer Poly is selected from 50 kDa to 100 kDa.

23. The polymer-modified lithium material according to any one of claims 1 to 22, wherein: The amount of lithium in the lithium-containing metal relative to the polymer Poly is greater than the amount of the catalyst, calculated on a molar ratio; Preferably, the lithium-containing metal comprises lithium metal or lithium alloy; In another embodiment, the lithium alloy contains lithium and further contains one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium.

24. A negative electrode sheet, wherein: The negative electrode plate includes a stacked negative electrode plate substrate and a polymer layer; the negative electrode plate substrate includes a lithium-containing layer in contact with the polymer layer, the lithium-containing layer contains lithium, and the polymer layer is chemically connected to at least a portion of the lithium in the lithium-containing layer; Wherein, the polymer layer comprises the polymer Poly defined in any one of claims 1 to 22.

25. The negative electrode sheet according to claim 24, wherein: The amount of lithium in the lithium-containing layer relative to the polymer Poly is greater than the amount of the catalyst, calculated on a molar ratio; Preferably, the lithium-containing layer comprises lithium metal or a lithium alloy; Preferably, the lithium alloy contains lithium and further contains one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium; Also preferably, the lithium-containing layer consists essentially of lithium metal; Alternatively, the lithium-containing layer is a lithium alloy.

26. The negative electrode sheet according to any one of claims 24 to 25, wherein: The polymer layer also contains an electrolyte.

27. The negative electrode sheet according to claim 26, wherein: The electrolyte contains lithium salt and electrolyte solvent.

28. The negative electrode sheet according to claim 27, wherein: The lithium salt is selected from one or more of lithium hexafluorophosphate, tetrafluoroboric acid, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate and lithium bis(oxalate)borate; Preferably, the electrolyte solvent is selected from one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, diphenyl carbonate, dibutyl carbonate, butylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, dioxolane, methyl nonafluoro-n-butyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, octafluoropentyl-tetrafluoroethyl ether, 1,2-bis(cyanoethoxy)ethane, diphenyl ether and 18-crown-6.

29. The negative electrode sheet according to any one of claims 27 to 28, wherein: The concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 5 mol / L; Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 4 mol / L; Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 2 mol / L to 4 mol / L; Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 3 mol / L; Another preferred embodiment is that the concentration of the lithium salt in the electrolyte is selected from 0.5 mol / L to 2 mol / L.

30. The negative electrode sheet according to any one of claims 26 to 29, wherein: The mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:2; Preferably, the mass ratio of the polymer Poly to the electrolyte is selected from 9:1 to 1:1; Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:2; Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1:1; Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 5:1 to 1.5:1; Another preferred embodiment is that the mass ratio of the polymer Poly to the electrolyte is selected from 4:1 to 1.5:

1.

31. The negative electrode sheet according to any one of claims 26 to 30, wherein: The mass proportion of the electrolyte in the polymer layer is selected from 9.5% to 65%; Preferably, the mass proportion of the electrolyte in the polymer layer is selected from 10% to 60%; Another preferred embodiment is that the mass proportion of the electrolyte in the polymer layer is selected from 20% to 60%; Another preferred embodiment is that the mass proportion of the electrolyte in the polymer layer is selected from 25% to 40%; In another embodiment, the mass proportion of the electrolyte in the polymer layer is selected from 30% to 50%.

32. The negative electrode sheet according to any one of claims 24 to 31, wherein: The thickness of the polymer layer is selected from 5 nm to 10 μm; Preferably, the thickness of the polymer layer is selected from 50 nm to 8 μm; Another preferred embodiment is that the thickness of the polymer layer is selected from 50 nm to 5 μm; Another preferred embodiment is that the thickness of the polymer layer is selected from 100 nm to 5 μm.

33. The negative electrode sheet according to any one of claims 24 to 32, wherein: The elastic modulus of the polymer layer at 25° C. is 0.1 MPa to 70 MPa; Preferably, the elastic modulus of the polymer layer at 25° C. is selected from 0.5 MPa to 50 MPa; Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is selected from 1 MPa to 50 MPa; Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is selected from 10 MPa to 47 MPa; Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is selected from 10 MPa to 45 MPa; Another preferred embodiment is that the elastic modulus of the polymer layer at 25° C. is selected from 20 MPa to 45 MPa.

34. The negative electrode sheet according to any one of claims 24 to 33, wherein: The elastic deformation range of the polymer layer at 25° C. is 50% to 700%; Preferably, the elastic deformation range of the polymer layer at 25° C. is 50% to 400%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 50% to 300%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 80% to 300%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 80% to 265%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 700%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 600%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 400%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 300%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 250%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 200%; Another preferred embodiment is that the elastic deformation range of the polymer layer at 25° C. is 100% to 190%.

35. The negative electrode sheet according to any one of claims 24 to 34, wherein: Based on the electrolyte, the swelling rate of the polymer layer at 25° C. is 10% to 60%; Preferably, the swelling ratio of the polymer layer at 25° C. is selected from 15% to 60%; Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 15% to 55%; Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 15% to 45%; Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 20% to 45%; Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 20% to 40%; Another preferred embodiment is that the swelling ratio of the polymer layer at 25° C. is selected from 25% to 50%.

36. The negative electrode sheet according to claim 35, wherein: Based on the electrolyte, the ionic conductivity of the swollen polymer layer at 25°C is 8×10 -3 S / cm to 1×10 -6 S / cm; Preferably, the ionic conductivity of the swollen polymer layer at 25°C is 5×10 -3 S / cm to 1×10 -6 S / cm; Preferably, the ionic conductivity of the swollen polymer layer at 25°C is selected from 8×10 -3 S / cm to 1×10 -5 S / cm; Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 5×10 -3 S / cm to 1×10 -5 S / cm; Preferably, the ionic conductivity of the swollen polymer layer at 25°C is selected from 8×10 -3 S / cm to 1×10 -4 S / cm; Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 5×10 -3 S / cm to 1×10 -4 S / cm; Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 3×10 -3 S / cm to 1×10 -4 S / cm; Another preferred embodiment is that the ionic conductivity of the swollen polymer layer at 25°C is selected from 3×10 -3 S / cm to 5×10 -4 S / cm.

37. The negative electrode sheet according to any one of claims 24 to 36, wherein: The negative electrode sheet substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.

38. The negative electrode sheet according to claim 37, wherein: A second negative electrode active material layer may or may not be provided between the negative electrode current collector and the lithium-containing layer. The components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.

39. An electrode assembly comprising a positive electrode plate, a separator and the negative electrode plate according to any one of claims 24 to 38, wherein the separator is arranged between the negative electrode plate and the positive electrode plate; and the polymer layer is arranged at least on the surface of the negative electrode plate substrate close to the separator.

40. A secondary battery comprising a core electrolyte and the electrode assembly according to claim 39, wherein the core electrolyte is disposed between the polymer layer and the positive electrode plate.

41. The secondary battery according to claim 40, wherein: The components of the core electrolyte and the electrolyte in the polymer layer may be the same or different.

42. The secondary battery according to claim 40 or 41, wherein: The charging current density of the secondary battery is selected from 0.3 mA / cm 2 ~12mA / cm 2 ; Preferably, the charging current density of the secondary battery is selected from 1 mA / cm 2 ~10mA / cm 2 ; Another preferred embodiment is that the charging current density of the secondary battery is selected from 1 mA / cm 2 ~6mA / cm 2 ; Another preferred embodiment is that the charging current density of the secondary battery is selected from 1 mA / cm 2 ~3mA / cm 2 . 43 . A battery module comprising the secondary battery according to claim 40 .

44. A battery pack comprising the battery module according to claim 43.

45. An electrical device comprising one or more of the secondary battery according to any one of claims 40 to 42, the battery module according to claim 43, and the battery pack according to claim 44.

46. ​​Application of monomer compound II in the preparation of negative electrode sheets, wherein: The structure of the monomer compound II is shown in Formula II: wherein Rf, A, Z2, X and m are as defined in any one of claims 1 to 20.

47. The use according to claim 46, wherein The monomer compound II contacts the lithium in the lithium-containing layer of the negative electrode substrate and forms a polymer layer through in-situ polymerization.

48. A method for preparing a negative electrode sheet, comprising the following steps: Providing a negative electrode substrate, wherein the outermost layer of at least one side of the negative electrode substrate is a lithium-containing layer, and the lithium-containing layer includes lithium-containing metal; and also providing a reaction mixture containing monomer compound II and an electrolyte; The reaction mixture is coated on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, and the monomer compound II is polymerized in situ to form a polymer layer; in, Rf, A, Z2, X and m are defined as any one of claims 1 to 20; Wherein, the electrolyte is as defined in any one of claims 26 to 30.

49. The preparation method according to claim 48, wherein The monomeric compound II is contacted with at least a catalytic amount of lithium.

50. The preparation method according to claim 48 or 49, wherein The mass ratio of the monomer compound II to the electrolyte is 9:1 to 1:2; Preferably, the mass ratio of the monomer compound II to the electrolyte is selected from 9:1 to 1:1; Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 5:1 to 1:2; Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 5:1 to 1:1; Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 5:1 to 1.5:1; Another preferred embodiment is that the mass ratio of the monomer compound II to the electrolyte is selected from 4:1 to 1.5:

1.

51. The preparation method according to any one of claims 48 to 50, wherein In the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating method is selected from any one of a coating method, a spraying method, a spin coating method and a vapor deposition method.

52. The preparation method according to any one of claims 48 to 51, wherein The reaction temperature of the in-situ polymerization is selected from 30°C to 100°C; Preferably, the reaction temperature of the in-situ polymerization is selected from 30°C to 50°C; Another preferred embodiment is that the reaction temperature of the in-situ polymerization is selected from 40°C to 60°C.

53. The preparation method according to any one of claims 48 to 52, wherein The reaction time of the in-situ polymerization is selected from 0.1h to 24h; Preferably, the reaction time of the in-situ polymerization is selected from 0.1h to 12h; Another preferred embodiment is that the reaction time of the in-situ polymerization is selected from 0.1 h to 6 h.

54. The preparation method according to any one of claims 48 to 53, wherein In the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating thickness of the reaction mixture is selected from 100 nm to 8 μm; Preferably, the coating thickness of the reaction mixture is selected from 50 nm to 5 μm; Another preferred embodiment is that the coating thickness of the reaction mixture is selected from 50 nm to 8 μm.

55. The preparation method according to any one of claims 48 to 54, wherein The polymer layer formed is as defined in any one of claims 32 to 36.

56. The preparation method according to any one of claims 48 to 55, wherein The negative electrode plate substrate is a pure lithium plate.

57. The preparation method according to any one of claims 48 to 56, wherein The negative electrode sheet substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.

58. The preparation method according to claim 57, wherein A second negative electrode active material layer may or may not be provided between the negative electrode current collector and the lithium-containing layer. The components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.