AI Technical Summary
Existing secondary batteries have challenges in balancing good cycle performance and kinetic performance. In particular, high-capacity graphite is difficult to simultaneously improve the cycle performance and kinetic performance of secondary batteries.
A carbon material including a pore structure is used. The material has two diffraction peaks in the peak split pattern of the X-ray diffraction pattern. The peak intensity ratio is in the range of 10:90-40:60. By adjusting the pore structure and filling material The type, softening point, coking value and other parameters are used to prepare carbon materials with stable structure and high energy density.
The secondary battery achieves both good cycle performance and kinetic performance, improves energy density and first Coulomb efficiency, and reduces irreversible capacity loss and the occurrence of side reactions.
Smart Images

Figure CN119072797A_ABST
Abstract
Description
Carbon material and preparation method thereof, as well as secondary battery and electric device containing the same Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a carbon material and a preparation method thereof, as well as a secondary battery and an electrical device containing the same. Background Art
[0002] In recent years, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As the scope of application of secondary batteries becomes wider and wider, people have put forward severe challenges to the performance of secondary batteries, such as requiring secondary batteries to take into account various properties such as energy density, dynamic performance, and service life. The negative electrode active material is an important component of the secondary battery, which affects the performance of the secondary battery. At present, the negative electrode active material mainly includes graphite. However, the problem faced in the existing technology is that it is difficult for high-capacity graphite to make the secondary battery have good cycle performance and dynamic performance.
[0003] Summary of the Invention
[0004] The purpose of the present application is to provide a carbon material and a preparation method thereof, as well as a secondary battery and an electrical device containing the same, which can enable the secondary battery to have both good cycle performance and kinetic performance.
[0005] In a first aspect, the present application provides a carbon material comprising a pore structure. In a peak separation spectrum of an X-ray diffraction pattern of the carbon material, two diffraction peaks exist within a range of 2θ of 25.5°-27.5°.
[0006] During the research process, the inventors of this application found that when the carbon material includes a pore structure and there are two diffraction peaks in the peak spectrum of the X-ray diffraction pattern of the carbon material within the range of 2θ of 25.5°-27.5°, the secondary battery can have both good cycle performance and kinetic performance.
[0007] In any embodiment of the present application, of the two diffraction peaks, the one with the smaller 2θ is recorded as the first peak, and the one with the larger 2θ is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is 10:90-40:60, optionally 15:85-35:65. When the ratio of the peak intensity of the first peak to the peak intensity of the second peak is within the above range, a secondary battery using the carbon material can have better cycle performance and kinetic performance, while also having a higher energy density.
[0008] In any embodiment of the present application, the carbon material comprises one or more pores with an area greater than or equal to 0.1 μm 2The pore structure may include one or more pores with an area of 0.15 μm 2 -3.0μm 2 When the carbon material includes a pore structure with the above-mentioned pore area, the pore structure can reserve the required expansion space for the volume change of the carbon material particles, thereby further reducing the risk of carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance of the secondary battery.
[0009] In any embodiment of the present application, the carbon material includes an outer region and an inner region located inside the outer region, wherein the outer region refers to a region extending from the surface of the carbon material particle to the interior of the particle by a distance of 0.25L, where L refers to the minor axis length of the carbon material particle, the total pore area of the outer region is denoted as S1, the total pore area of the inner region is denoted as S2, and S2>S1. When the carbon material further satisfies S2>S1, the irreversible capacity loss of the secondary battery can be effectively reduced, the capacity utilization characteristics of the secondary battery can be improved, and the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycle performance and kinetic performance.
[0010] In any embodiment of the present application, 1.5≤S2 / S1≤450, optionally, 2≤S2 / S1≤400. When S2 / S1 is also within the above range, the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycle performance and kinetic performance.
[0011] In any embodiment of the present application, 0.01 μm 2 ≤S1≤8.0μm 2 , optionally, 0.02 μm 2 ≤S1≤4.5μm 2 When the total pore area of the outer region of the carbon material is within the above range, on the one hand, the carbon material particles can have a more stable structure, and the electrolyte can be prevented from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions and reducing the consumption of active ions by the formation of the SEI film inside the carbon material particles. On the other hand, it will not affect the transmission performance of active ions and electrons.
[0012] In any embodiment of the present application, 2.5 μm 2 ≤S2≤25.0μm 2 , optionally, 3.0 μm 2 ≤S2≤22.5μm 2When the total pore area of the internal region of the carbon material is within the above range, on the one hand, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, reducing the risk of carbon material particles breaking to produce new interfaces, reducing the occurrence of side reactions on the new interface surface, and reducing the consumption of active ions by the formation of the SEI film on the new interface surface. On the other hand, it can also improve the capacity and first coulombic efficiency of the carbon material.
[0013] In any embodiment of the present application, L≥4 μm, optionally, 4 μm≤L≤20 μm.
[0014] In any embodiment of the present application, the area of the pore structure in the outer region of the carbon material is less than or equal to 0.2 μm 2 , can be selected to be less than or equal to 0.1μm 2 By controlling the area of the pore structure in the outer region of the carbon material within the above range, the outer region of the carbon material can have a dense structure, thereby effectively improving the structural stability of the carbon material and preventing the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby effectively improving the cycle performance of the secondary battery.
[0015] In any embodiment of the present application, the inner region of the carbon material includes one or more areas greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.15 μm 2 -3.0μm 2 By including the aforementioned pore structure in the internal region of the carbon material, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, reducing the risk of carbon material particle breakage. On the other hand, the compaction density of the carbon material can be increased, thereby improving the energy density of the secondary battery.
[0016] In any embodiment of the present application, the specific surface area of the carbon material is 0.5 m 2 / g-3.1m 2 / g, optional 0.7m 2 / g-2.8m 2 The carbon material of the present application has a low specific surface area, thereby reducing the consumption of active ions in the formation of the SEI film and improving the first coulombic efficiency of the carbon material.
[0017] In any embodiment of the present application, the volume distribution particle size Dv50 of the carbon material is 8.0 μm-23.0 μm, and optionally 9.0 μm-22.0 μm. When the volume distribution particle size Dv50 of the carbon material is within the above range, it is beneficial to improve the transport performance of active ions and electrons, thereby further improving the cycle performance and kinetic performance of the secondary battery.
[0018] In any embodiment of the present application, the ratio (Dv90-Dv10) / Dv50 of the carbon material is ≤1.55, and can be 0.5-1.50. This helps to increase the compaction density of the carbon material, thereby further improving the energy density of the secondary battery, and also helps to form a reasonable pore structure between the particles of the negative electrode film layer, thereby improving the cycle performance and / or dynamic performance of the secondary battery.
[0019] In any embodiment of the present application, the morphology of the carbon material includes one or more of block, spherical, and quasi-spherical, which is beneficial to improving the compaction density of the negative electrode sheet and thus improving the energy density of the secondary battery.
[0020] In any embodiment of the present application, the powder resistivity of the carbon material at a pressure of 8 MPa is 0.006 Ω.cm-0.051 Ω.cm, and optionally 0.010 Ω.cm-0.040 Ω.cm. When the powder resistivity of the carbon material is within the above range, it is beneficial to improve the electron transport performance, thereby further improving the cycle performance and kinetic performance of the secondary battery.
[0021] In any embodiment of the present application, the powder compaction density of the carbon material under a pressure of 20000N is 1.70g / cm 3 -1.95g / cm 3 , optional 1.72g / cm 3 -1.92g / cm 3 When the compaction density of the carbon material powder is within the above range, the compaction density of the negative electrode sheet can be increased, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.
[0022] In any embodiment of the present application, the tap density of the carbon material is 0.90 g / cm 3 -1.35g / cm 3 , optional 0.95g / cm 3 -1.32g / cm 3 When the tap density of the carbon material is within the above range, it can increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.
[0023] In any embodiment of the present application, the gram capacity of the carbon material is 350 mAh / g-372 mAh / g, and optionally 353 mAh / g-371 mAh / g. When the gram capacity of the carbon material is within the above range, the energy density of the secondary battery can be improved.
[0024] In any embodiment of the present application, the graphitization degree of the carbon material is 91.5%-98.5%, optionally 92.5%-98.0%. When the graphitization degree of the carbon material is within the above range, it is beneficial to improve the cycle performance, storage performance and dynamic performance of the secondary battery.
[0025] In any embodiment of the present application, the carbon material has no diffraction peak of the 3R phase C(012) crystal plane in its X-ray diffraction pattern. As a result, the carbon material particles have fewer internal defects, thereby further reducing the irreversible consumption of active ions.
[0026] The second aspect of the present application provides a method for preparing a carbon material, comprising the following steps: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and a filler material in a predetermined proportion, and then keeping the mixture at a first temperature T1 for a first time t1 to obtain an intermediate; step 3, keeping the obtained intermediate at a second temperature T2 for a second time t2 to obtain a carbon material, wherein the carbon material includes a pore structure, and in the peak spectrum of the X-ray diffraction pattern of the carbon material, there are two diffraction peaks in the range of 2θ of 25.5°-27.5°.
[0027] The preparation method of the carbon material of the present application is simple and safe, does not require a preset pressure or vacuum treatment, and does not require an additional depolymerization step during the heat treatment process. The carbon material prepared in the present application has a small volume expansion, high structural stability, and a fast active ion diffusion rate, thereby achieving a high gram capacity, a high first coulombic efficiency, and a small volume change, and can also enable the secondary battery to have good cycle performance and kinetic performance. In addition, the secondary battery can also have a high first coulombic efficiency and a high energy density.
[0028] In any embodiment of the present application, the raw material includes natural graphite. Optionally, the natural graphite includes one or more of flake graphite, natural spherical graphite and microcrystalline graphite.
[0029] In any embodiment of the present application, the volume distribution particle size Dv50 of the raw material is 7.5 μm-23.0 μm, and can be optionally 9.0 μm-22.0 μm.
[0030] In any embodiment of the present application, the graphitization degree of the raw material is ≥93.0%.
[0031] In any embodiment of the present application, the carbon content in the raw material is ≥98 wt%.
[0032] In any embodiment of the present application, the softening point temperature of the filling material is 120°C-300°C, and can be optionally 125°C-250°C.
[0033] In any embodiment of the present application, the coking value of the filler material is 25%-70%, and optionally 30%-60%.
[0034] In any embodiment of the present application, the volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be optionally 1 μm-5 μm.
[0035] In any embodiment of the present application, the filling material includes one or more of coal-based asphalt, oil-based asphalt, resin and polymer material, and can optionally include one or more of coal-based asphalt and oil-based asphalt.
[0036] In any embodiment of the present application, the mass ratio of the filling material to the raw material is 10:90-25:75, and can be optionally 12:88-25:75.
[0037] By adjusting one or more parameters such as the type, softening point, coking value, and addition amount of the filling material within the above-mentioned range, on the one hand, it is beneficial to adjust the ratio of the peak intensity of the first peak to the peak intensity of the second peak within an appropriate range, and on the other hand, it is beneficial to adjust the pore size and / or pore content in the external region and the internal region of the carbon material within an appropriate range; in addition, after the filling material is heated and melted, the viscosity is not high, and good fluidity is maintained, and it is not easy to adhere to the raw material particles, which can reduce the agglomeration of the raw material particles in the subsequent preparation process, thereby reducing the problems of increased surface defects of the carbon material particles and increased surface side reaction active sites due to the need to add a depolymerization process.
[0038] In any embodiment of the present application, the first temperature T1 is 1000°C-1400°C, and can be optionally 1050°C-1250°C.
[0039] In any embodiment of the present application, the first time t1 is 1 hour to 5 hours, and can be optionally 2 hours to 4 hours.
[0040] In any embodiment of the present application, the temperature is increased to the first temperature T1 at a rate of 1°C / min-10°C / min, optionally 1.5°C / min-5°C / min.
[0041] By adjusting one or more of the heating rate, the first temperature, the first time, etc. within the above-mentioned range, it is beneficial to prepare a carbon material with a desired structure, for example, it is beneficial to adjust the pore size and / or pore content in the outer region and the inner region of the carbon material within a suitable range.
[0042] In any embodiment of the present application, the second temperature T2 is 2000°C-2720°C, and can be optionally 2150°C-2550°C.
[0043] In any embodiment of the present application, the second time t2 is 1.5 hours to 6 hours, and can be optionally 2 hours to 5 hours.
[0044] By adjusting one or more of the second temperature and the second time within the above-mentioned range, two diffraction peaks can be present in the peak spectrum of the X-ray diffraction pattern of the carbon material within the range of 2θ of 25.5°-27.5°, which is also beneficial for adjusting the ratio of the peak intensity of the first peak to the peak intensity of the second peak within an appropriate range.
[0045] A third aspect of the present application provides a secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises the carbon material of the first aspect of the present application or the carbon material prepared by the method of the second aspect of the present application.
[0046] A fourth aspect of the present application provides an electrical device comprising the secondary battery according to the third aspect of the present application.
[0047] The carbon material provided in this application can enable the secondary battery to have both good cycle performance and kinetic performance. In addition, it can enable the secondary battery to have both high first coulombic efficiency and high energy density. The electrical device of this application includes the secondary battery provided in this application, and thus has at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0049] FIG1 is a peak spectrum of an X-ray diffraction spectrum of an embodiment of the carbon material of the present application.
[0050] FIG2 is a schematic diagram of a cross-sectional image of a particle of the carbon material of the present application.
[0051] FIG3 is a schematic diagram of an embodiment of a secondary battery of the present application.
[0052] FIG. 4 is an exploded schematic diagram of an embodiment of a secondary battery of the present application.
[0053] FIG5 is a schematic diagram of an embodiment of a battery module of the present application.
[0054] FIG6 is a schematic diagram of an embodiment of a battery pack of the present application.
[0055] FIG. 7 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 6 .
[0056] FIG8 is a schematic diagram of an embodiment of an electric device including the secondary battery of the present application as a power source.
[0057] In the accompanying drawings, which are not necessarily drawn to scale, reference numerals are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 housing, 52 electrode assembly, 53 cover plate, 100 carbon material, 101 external region, 102 internal region. DETAILED DESCRIPTION
[0058] Below, the carbon material and its preparation method, as well as the embodiments of the secondary battery and the electrical device containing the carbon material of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0059] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0060] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0061] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0062] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0063] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0064] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0065] Unless otherwise specified, the terms used in this application have the common meanings generally understood by those skilled in the art.
[0066] Unless otherwise specified, the values of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in this application.
[0067] Unless otherwise specified, in this application, the term "active ions" refers to ions that can be intercalated and extracted back and forth between the positive electrode and the negative electrode of a secondary battery, including but not limited to lithium ions.
[0068] In this application, the terms "plurality" and "multiple" refer to two or more.
[0069] Graphite can be divided into artificial graphite and natural graphite based on its preparation process or source. Artificial graphite generally undergoes a high-temperature graphitization process, which is energy-intensive and costly, resulting in a higher cost. Natural graphite, derived from nature, offers the advantage of being relatively inexpensive. Furthermore, natural graphite has the advantages of high capacity and / or high compacted density.
[0070] Natural graphite mainly includes flake graphite, natural spherical graphite, and microcrystalline graphite. Unlike artificial graphite, natural graphite particles generally have a large number of pores and defects inside and outside. During the first charge of a secondary battery, the electrolyte produces many side reactions with the pores on the surface and inside the particles, resulting in a high first irreversible capacity loss, low first coulombic efficiency, and poor cycle performance of the secondary battery. In particular, flake graphite and natural spherical graphite have high crystallinity and high graphitization degree, and their microstructure is mostly layered. This structure causes the volume of natural graphite to change significantly during the extraction and insertion of active ions, which easily leads to the fragmentation of the graphite layer structure and particle breakage. After the particles are broken, the exposed fresh surface will continue to react with the electrolyte, further increasing the irreversible capacity loss of the secondary battery. In addition, natural graphite has high anisotropy and slow diffusion of active ions, which also leads to its poor kinetic performance.
[0071] Currently, the properties of natural graphite are mainly improved by surface coating treatment of particles and / or internal filling treatment of particles.
[0072] The particle surface coating treatment mainly involves mixing natural graphite with a coating agent (such as asphalt, polymer compounds, etc.) and then heat-treating it to coat the surface of the natural graphite particles with an amorphous carbon layer, slightly repairing the surface defects of the particles. However, during the research process, the inventors of this application found that the surface-coated amorphous carbon layer can reduce the specific capacity and / or compacted density of natural graphite, affecting the energy density of the secondary battery. At the same time, the surface-coated amorphous carbon layer cannot effectively prevent the electrolyte from penetrating into the pore structure inside the particles, resulting in limited improvement in the initial coulombic efficiency and cycle performance of the secondary battery.
[0073] The particle internal filling process mainly involves mixing natural graphite with a filler (such as asphalt, a polymer compound, etc.), and filling the filler into the particle internal pores by means of preset pressure, vacuuming, and heating, so as to obtain natural graphite without pores in the particle interior. However, the inventors of the present application have found in the research process that the carbon filled in a large amount inside the particle causes the gram capacity and compacted density of natural graphite to be reduced, affecting the energy density of the secondary battery; simultaneously, since the pores inside the natural graphite particles are all filled with carbon, the volume change of natural graphite produced during the active ion escape and embedding process is large, and the particles are more easily broken, thereby causing the SEI film on the particle surface to be repeatedly destroyed and reconstructed, further increasing the irreversible consumption of active ions, increasing the irreversible capacity loss of the secondary battery, and shortening the service life of the secondary battery. The prior art also continues to coat a layer of amorphous carbon layer on the surface of the natural graphite without pores in the above-mentioned particle interior, which causes the gram capacity and / or compacted density of natural graphite to be further reduced, and at this time, the particle surface side reaction activity is high, thus the service life of the secondary battery can not be effectively improved.
[0074] Therefore, after modifying natural graphite through the above-mentioned particle surface coating treatment and / or particle internal filling treatment, although the irreversible capacity loss of the secondary battery can be reduced to a certain extent and the first coulombic efficiency of the secondary battery can be improved, its improvement effect on the first coulombic efficiency of the secondary battery is limited, and the energy density of the secondary battery will also be lost. In addition, it is difficult for the secondary battery to have both good cycle performance and kinetic performance.
[0075] In view of this, the inventors of the present application have proposed a new type of carbon material after extensive research, which can enable secondary batteries to have both good cycle performance and kinetic performance.
[0076] carbon materials
[0077] A first aspect of an embodiment of the present application provides a carbon material comprising a pore structure, wherein in a peak separation spectrum of an X-ray diffraction spectrum of the carbon material, two diffraction peaks exist within a range of 2θ of 25.5°-27.5°.
[0078] FIG1 is a peak spectrum of an X-ray diffraction pattern of an embodiment of the carbon material of the present application. As can be seen from FIG1, two diffraction peaks can be separated in the range of 25.5°-27.5° (corresponding to the diffraction peak of the carbon 002 crystal plane). The inventors of the present application found during the research process that when the carbon material includes a pore structure and there are two diffraction peaks in the peak spectrum of the X-ray diffraction pattern of the carbon material in the range of 25.5°-27.5°, the secondary battery can have both good cycle performance and kinetic performance. Possible reasons include at least the following points.
[0079] When the peak spectrum of the X-ray diffraction pattern of the carbon material has two diffraction peaks in the range of 2θ of 25.5°-27.5°, the carbon material simultaneously contains a crystalline carbon component with a higher degree of graphitization (for example, crystalline carbon with a degree of graphitization ≥95%) and a crystalline carbon component with a lower degree of graphitization (for example, crystalline carbon with a degree of graphitization of 70%-90%). The crystalline carbon component with a lower degree of graphitization can have a larger interlayer spacing, which is conducive to the diffusion of active ions, so that the secondary battery can have good dynamic performance; the crystalline carbon component with a higher degree of graphitization can, on the one hand, make the carbon material have a high gram capacity and / or compaction density, thereby improving the energy density of the secondary battery, and on the other hand, can also make the carbon material have a stable structure, and the irreversible consumption of active ions during the cycle of the secondary battery is low, thereby also making the secondary battery have good cycle performance.
[0080] The carbon material provided in this application includes a pore structure. In this application, "the carbon material includes a pore structure" means that the carbon material has a pore structure that can be directly observed from a cross-sectional image (e.g., a scanning electron microscope image with a magnification of 1000 times), that is, the pore structure in the raw material used to prepare the carbon material is not completely filled. The pore structure in the carbon material can reserve the required expansion space for the volume change of the carbon material particles, thereby reducing the risk of the carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions and improving the cycle performance of the secondary battery.
[0081] Therefore, the carbon material provided in this application can enable the secondary battery using the carbon material to have both good cycle performance and kinetic performance.
[0082] When the carbon material does not include a pore structure, the volume of the carbon material particles changes greatly during the charge and discharge process of the secondary battery, which leads to a higher risk of carbon material particles breaking and producing new interfaces, more side reactions inside the secondary battery, and thus poor cycle performance and kinetic performance of the secondary battery.
[0083] When the peak pattern of the X-ray diffraction pattern of a carbon material has only one diffraction peak within the range of 25.5°-27.5° 2θ, the carbon material is mainly composed of the same crystalline phase microstructure, that is, the carbon material only has crystalline carbon with a high degree of graphitization or crystalline carbon with a low degree of graphitization. When the carbon material refers to crystalline carbon with only a low degree of graphitization, the specific capacity and / or compacted density of the carbon material is low, and the energy density of the secondary battery is low; when the carbon material only has crystalline carbon with a high degree of graphitization, the interlayer spacing of the carbon material is small, which is not conducive to the diffusion of active ions, and thus the kinetic performance of the secondary battery is poor, and the secondary battery cannot achieve both good cycle performance and kinetic performance.
[0084] In some embodiments, among the two diffraction peaks, the one with smaller 2θ is recorded as the first peak, and the one with larger 2θ is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is 10:90-40:60, which can be optionally 12:88-35:65, 15:85-35:65, or 15:85-30:70.
[0085] The inventors found in further research that when the ratio of the peak intensity of the first peak to the peak intensity of the second peak is within the above range, the secondary battery using the carbon material can have better cycle performance and kinetic performance while also having a higher energy density.
[0086] When the ratio of the peak intensity of the first peak to the peak intensity of the second peak is within the above range, the content of crystalline carbon components with higher graphitization degree in the carbon material is higher and the content of crystalline carbon components with lower graphitization degree is lower, thereby making the structure of the carbon material more stable and the irreversible consumption of active ions during the secondary battery cycle lower, thereby enabling the secondary battery to have further improved cycle performance, while the secondary battery can also take into account high energy density.
[0087] And it can effectively avoid the following situations: when the ratio of the peak intensity of the first peak to the peak intensity of the second peak is small, the carbon material contains fewer crystalline carbon components with a lower degree of graphitization, which may affect the diffusion of active ions and further affect the improvement effect of the kinetic performance of the secondary battery; when the ratio of the peak intensity of the first peak to the peak intensity of the second peak is large, the carbon material contains too many crystalline carbon components with a lower degree of graphitization, and thus the surface side reaction activity of the carbon material particles may be higher, and there are more side reactions between the electrolyte and the carbon material particles, which may affect the cycle performance of the secondary battery; at the same time, when the carbon material contains more crystalline carbon components with a lower degree of graphitization, the gram capacity and / or compaction density of the carbon material will also decrease, and the energy density of the secondary battery may also be reduced.
[0088] In the peak spectrum of the X-ray diffraction spectrum of the carbon material of the present application, the 2θ of the first peak is located between 26.256° and 26.456°, and the 2θ of the second peak is located between 26.509° and 26.569°.
[0089] The peak spectrum of the X-ray diffraction pattern of the carbon material is obtained by using Topas software and the Rietveld full spectrum fitting refinement method to refine the X-ray diffraction pattern of the carbon material. The 2θ of 25.5°-27.5° corresponds to the peak position of the carbon 002 crystal plane.
[0090] The ratio of the peak intensity of the first peak to the peak intensity of the second peak is the ratio of the integrated area of the first peak to the integrated area of the second peak.
[0091] In some embodiments, the carbon material comprises at least one pore with an area greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.15 μm 2 -3.0μm 2 The inventors discovered in further research that when a carbon material includes a pore structure with the aforementioned pore area, the pore structure can reserve the required expansion space for the volume change of the carbon material particles, thereby further reducing the risk of carbon material particles breaking and generating new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance of the secondary battery.
[0092] In some embodiments, the carbon material includes an external region and an internal region located inside the external region, wherein the external region refers to a region extending 0.25L from the particle surface of the carbon material to the interior of the particle, L refers to the short axis length of the carbon material particle, the total pore area of the external region is denoted as S1, the total pore area of the internal region is denoted as S2, and S2>S1.
[0093] In the present application, the total pore area S1 of the outer region and the total pore area S2 of the inner region of the carbon material can be obtained by testing a cross-sectional image of the carbon material.
[0094] In the present application, the cross-sectional image of the carbon material includes a cross-sectional image passing through the center of the carbon material particle. "Particle center" refers to the range within a radius of 0.1 μm extending from the geometric center of the particle to the particle surface.
[0095] In this application, the minor axis length of a particle refers to the minimum value when a line connecting two points on the particle surface passes through the geometric center of the particle.
[0096] FIG2 is a schematic diagram of a cross-sectional image of a particle of the carbon material 100 of the present application, and the cross-sectional image passes through the center of the particle of carbon material 100. As shown in FIG2 , L represents the minor axis length of the particle of carbon material 100, and the region extending from the surface of the particle of carbon material 100 to the interior of the particle by a distance of 0.25L is the outer region 101, and the region inside the outer region 101 is the inner region 102.
[0097] The cross-section of the carbon material can be prepared using a cross-section polisher (e.g., the IB-09010CP argon ion cross-section polisher from JEOL, Japan); then, referring to JY / T010-1996, a scanning electron microscope (e.g., the Sigma 300 scanning electron microscope from ZEISS, Germany) is used to scan the cross-section of the carbon material; finally, the total pore area S1 of the outer region and the total pore area S2 of the inner region of the carbon material are calculated using image processing software (e.g., AVIZO).
[0098] The inventors discovered in further research that when the carbon material further satisfies S2>S1, the carbon material particles may have the following characteristics: the pore content in the inner region is high and / or the pore size is large, while the pore content in the outer region is low and / or the pore size is small. The pore content in the inner region of the carbon material particles is high and / or the pore size is large, so that the pore structure can reserve the required expansion space for the volume change of the carbon material particles, thereby reducing the risk of carbon material particles breaking and producing new interfaces, thereby reducing the occurrence of side reactions, reducing the irreversible capacity loss of the secondary battery, and improving the cycle performance and kinetic performance of the secondary battery; the pore content in the outer region of the carbon material particles is low and / or the pore size is small, thereby making the carbon material particles have a more stable structure and avoiding the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions, reducing the consumption of active ions by the SEI film formation inside the particles, thereby improving the first coulombic efficiency of the carbon material, and further improving the cycle performance of the secondary battery.
[0099] Therefore, when the carbon material further satisfies S2>S1, it can effectively reduce the irreversible capacity loss of the secondary battery, improve the capacity utilization characteristics of the secondary battery, and enable the secondary battery to better balance high first coulombic efficiency, high energy density, and good cycle performance and kinetic performance.
[0100] In some embodiments, 1.5≤S2 / S1≤450, 2≤S2 / S1≤400, 2.1≤S2 / S1≤300, 2.2≤S2 / S1≤200, 2.3≤S2 / S1≤100, and 2.4≤S2 / S1≤80. The inventors have further discovered that when S2 / S1 is also within the above range, the secondary battery can better balance high initial coulombic efficiency, high energy density, and good cycling and kinetic performance.
[0101] In some embodiments, 0.01 μm 2 ≤S1≤8.0μm 2 , optionally, 0.02 μm 2 ≤S1≤6.5μm 2 , 0.02μm 2 ≤S1≤5.0μm 2 , 0.02μm 2 ≤S1≤4.5μm 2 , 0.05m 2 ≤S1≤4.0μm 2When the total pore area of the outer region of the carbon material is within the above range, on the one hand, the carbon material particles can have a more stable structure, and the electrolyte can be prevented from penetrating into the pore structure inside the carbon material particles as much as possible, thereby reducing the occurrence of side reactions and reducing the consumption of active ions by the formation of the SEI film inside the carbon material particles. On the other hand, it will not affect the transmission performance of active ions and electrons.
[0102] In some embodiments, 2.5 μm 2 ≤S2≤25.0μm 2 , optionally, 3.0 μm 2 ≤S2≤22.5μm 2 , 4.0μm 2 ≤S2≤20μm 2 , 5.0μm 2 ≤S2≤17.5μm 2 , 6.0μm 2 ≤S2≤15μm 2 When the total pore area of the internal region of the carbon material is within the above range, on the one hand, sufficient and stable expansion space can be reserved for the volume change of the carbon material particles, reducing the risk of carbon material particles breaking to produce new interfaces, reducing the occurrence of side reactions on the new interface surface, and reducing the consumption of active ions by the formation of the SEI film on the new interface surface. On the other hand, it can also improve the capacity and first coulombic efficiency of the carbon material.
[0103] In some embodiments, L≧4 μm, optionally, 4 μm≤L≤20 μm, 6 μm≤L≤20 μm, 8 μm≤L≤20 μm, 8 μm≤L≤18 μm, 8 μm≤L≤16 μm.
[0104] In some embodiments, the area of the pore structure in the outer region of the carbon material is less than or equal to 0.2 μm 2 , can be selected to be less than or equal to 0.1μm 2 In further research, the inventors also found that by controlling the area size of the pore structure in the outer region of the carbon material within the above range, the outer region of the carbon material can have a dense structure, thereby effectively improving the structural stability of the carbon material and preventing the electrolyte from penetrating into the pore structure inside the carbon material particles as much as possible, thereby effectively improving the cycle performance of the secondary battery. Of course, this application does not intend to limit the area of all pore structures in the outer region of the carbon material to be less than or equal to 0.2 μm. 2 For example, the area of the pore structure can be controlled to be less than or equal to 0.2 μm by controlling more than 95%, or more than 99%. 2 , can be selected to be less than or equal to 0.1μm 2 .
[0105] In some embodiments, the inner region of the carbon material includes at least one area greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.15 μm 2 -3.0μm 2 The inventors further discovered that by including the aforementioned pore structure in the internal region of the carbon material, sufficient and stable expansion space can be reserved for the volume changes of the carbon material particles, reducing the risk of carbon material particle breakage. Furthermore, the compaction density of the carbon material can be increased, thereby improving the energy density of the secondary battery.
[0106] In some embodiments, the carbon material has no diffraction peaks for the 3R phase C(012) crystal plane in its X-ray diffraction pattern. The 3R (Rhombohedral) phase refers to rhombohedral crystalline carbon having an ABCABC... stacking structure. The carbon material of the present application has no diffraction peaks for the 3R phase C(012) crystal plane, and thus the carbon material particles have fewer internal defects, thereby further reducing the irreversible consumption of active ions. In the present application, the 2θ of the diffraction peak for the 3R phase C(012) crystal plane is in the range of 46°-47°.
[0107] In some embodiments, the carbon material has a morphology of one or more of block, spherical, and quasi-spherical, which is beneficial for increasing the compaction density of the negative electrode sheet and thus improving the energy density of the secondary battery.
[0108] In some embodiments, the carbon material includes primary particles. Optionally, the primary particles in the carbon material account for ≥50%, for example, 55%-95%, 60%-100%, 65%-90%, 65%-80%, 70%-100%, 75%-90%, 80%-100%, 90%-100%, or 95%-100%. The carbon material containing an appropriate proportion of primary particles can provide it with higher structural stability and reduce the occurrence of side reactions. In addition, it can also increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the secondary battery.
[0109] In some embodiments, the carbon materials may all be primary particles, that is, the number of the primary particles in the carbon materials accounts for 100%.
[0110] Primary particles and secondary particles are both well-known in the art. Primary particles refer to non-agglomerated particles. Secondary particles refer to agglomerated particles formed by the aggregation of two or more primary particles. Primary particles and secondary particles can be distinguished using scanning electron microscopy (SEM) images.
[0111] In the present application, the number ratio of primary particles in the carbon material can be tested according to the following method: randomly select a test sample in the negative electrode film layer, randomly select multiple test areas in the test sample, use a scanning electron microscope to obtain images of the multiple test areas, and count the proportion of the number of carbon material particles with primary particle morphology in each image to the total number of carbon material particles. The average value of multiple statistical results is the number ratio of primary particles in the carbon material.
[0112] In some embodiments, the carbon material has a degree of graphitization of 91.5% to 98.5%, optionally 92.5% to 98.0%, 93.5% to 98.0%, or 94.5% to 98.0%. When the degree of graphitization of the carbon material is within the above range, it is beneficial to improve the cycle performance, storage performance, and kinetic performance of the secondary battery.
[0113] The degree of graphitization of carbon materials is well known in the art and can be measured using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for testing. The test can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain the average interlayer spacing d of the (002) crystal plane in the carbon material crystal structure. 002 Then according to the formula g=(0.344-d 002 ) / (0.344-0.3354)×100% to calculate the degree of graphitization. In the above formula, d 002 It is the average interlayer distance between (002) planes in the carbon material crystal structure expressed in nanometers (nm).
[0114] In some embodiments, the specific surface area of the carbon material is 0.5 m 2 / g-3.1m 2 / g, optional 0.7m 2 / g-2.8m 2 The carbon material of the present application has a low specific surface area, thereby reducing the consumption of active ions in the formation of the SEI film and improving the first coulombic efficiency of the carbon material.
[0115] The specific surface area of a carbon material is well known in the art and can be measured using instruments and methods known in the art. For example, the specific surface area can be measured using the nitrogen adsorption specific surface area analysis test method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed using a Micromeritics Tri-Star 3020 specific surface area pore size analyzer.
[0116] In some embodiments, the volume distribution particle size Dv50 of the carbon material is 8.0 μm-23.0 μm, optionally 9.0 μm-22.0 μm.
[0117] When the volume distribution particle size Dv50 of the carbon material is within the above range, it is beneficial to improve the transport performance of active ions and electrons, thereby further improving the cycle performance and kinetic performance of the secondary battery.
[0118] In some embodiments, the (Dv90-Dv10) / Dv50 ratio of the carbon material is ≤1.55, and can optionally be 0.5-1.50. When the (Dv90-Dv10) / Dv50 ratio of the carbon material is within the above range, it is beneficial to increase the compaction density of the carbon material, thereby further increasing the energy density of the secondary battery. It is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, thereby improving the cycle performance and / or kinetic performance of the secondary battery.
[0119] The volume distribution particle sizes Dv10, Dv50, and Dv90 of carbon materials are well known in the art and represent the particle sizes corresponding to the 10%, 50%, and 90% cumulative volume distribution percentages of the material, respectively. These can be measured using instruments and methods known in the art. For example, they can be conveniently measured using a laser particle size analyzer, as described in GB / T 19077-2016: Particle Size Distribution Laser Diffraction Method. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0120] In some embodiments, the powder resistivity of the carbon material at a pressure of 8 MPa is 0.006 Ω.cm-0.051 Ω.cm, and optionally 0.010 Ω.cm-0.040 Ω.cm. When the powder resistivity of the carbon material is within the above range, it is beneficial to improve the electron transport performance, thereby further improving the cycle performance and kinetic performance of the secondary battery.
[0121] The powder resistivity of carbon materials is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder resistivity tester (e.g., Suzhou Jingge ST2722, Sansi Zongheng UTM7305) using the four-probe method, with reference to GB / T 30835-2014. An exemplary test method is as follows: a certain amount of sample powder to be tested is weighed and placed in a dedicated mold. A test pressure is set to obtain the powder resistivity at different pressures. In this application, the test pressure can be set to 8 MPa.
[0122] In some embodiments, the powder compaction density of the carbon material under a pressure of 20,000 N is 1.70 g / cm 3 -1.95g / cm 3 , optional 1.72g / cm3 -1.92g / cm 3 .
[0123] When the powder compaction density of the carbon material is within the above range, the compaction density of the negative electrode sheet can be increased, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transmission performance, and improve the cycle performance and kinetic performance of the secondary battery.
[0124] In this application, the compacted density of carbon material powder is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured by an electronic pressure testing machine (for example, a UTM7305 electronic pressure testing machine) with reference to GB / T 24533-2009. An exemplary test method is as follows: 1g of carbon material powder is weighed and added to a container with a bottom area of 1.327cm 2 The mold was pressurized to 2000 kg (equivalent to 20000 N), maintained for 30 seconds, then released and maintained for 10 seconds, and then the powder compaction density of the carbon material under a pressure of 20000 N was recorded and calculated.
[0125] In some embodiments, the tap density of the carbon material is 0.90 g / cm 3 -1.35g / cm 3 , optional 0.95g / cm 3 -1.32g / cm 3 When the tap density of the carbon material is within the above range, it can increase the compaction density of the negative electrode sheet, thereby increasing the energy density of the secondary battery; it is also beneficial to improve the active ion and electron transport performance, and improve the cycle performance and kinetic performance of the secondary battery.
[0126] The tap density of carbon materials is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder tap density tester in accordance with GB / T 5162-2006. A suitable tester is the Dandong Better BT-301.
[0127] In some embodiments, the gram capacity of the carbon material is 350 mAh / g-372 mAh / g, optionally 353 mAh / g-371 mAh / g. When the gram capacity of the carbon material is within the above range, the energy density of the secondary battery can be increased.
[0128] The gram capacity of carbon materials is a well-known meaning in the art and can be tested using methods known in the art. An exemplary test method is as follows: a carbon material sample is thoroughly stirred and mixed with a binder of styrene-butadiene rubber (SBR), a thickener of sodium carboxymethyl cellulose (CMC), and a conductive agent of carbon black in a mass ratio of 96.2:1.8:1.2:0.8 in an appropriate amount of solvent deionized water to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil and dried in an oven for later use; ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L; a metal lithium sheet is then used as a counter electrode and a polyethylene (PE) film is used as an isolation membrane to assemble a CR2430 button cell in an argon-protected glove box. At 25°C, the prepared button cell was first discharged at a constant current of 0.15 mA to 0.005 V, allowed to stand for 5 minutes, and then discharged at a constant current of 10 μA to 0.005 V. The first-cycle discharge capacity of the button cell was recorded. The cell was then charged at a constant current of 0.3 mA to 2.0 V, and the charge capacity of the button cell was recorded. The ratio of the charge capacity of the button cell to the mass of the carbon material sample is the gram capacity of the carbon material.
[0129] Preparation method
[0130] A second aspect of the embodiments of the present application provides a method for preparing a carbon material, which can prepare the carbon material of the first aspect of the embodiments of the present application.
[0131] The preparation method of the carbon material includes the following steps: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and the filler material in a predetermined proportion, and then keeping the mixture at a first temperature T1 for a first time t1 to obtain an intermediate; step 3, keeping the obtained intermediate at a second temperature T2 for a second time t2 to obtain a carbon material, wherein the carbon material includes a pore structure, and in the peak spectrum of the X-ray diffraction pattern of the carbon material, there are two diffraction peaks in the range of 2θ of 25.5°-27.5°.
[0132] In some embodiments, the raw material for preparing the carbon material includes natural graphite. Optionally, the natural graphite includes one or more of flake graphite, natural spherical graphite, and microcrystalline graphite, and more preferably includes natural spherical graphite.
[0133] In this application, "natural spherical graphite" refers to natural graphite having a spherical or quasi-spherical shape, and not all natural graphite particles are controlled to be ideal spheres. In some embodiments, natural spherical graphite of a desired particle size and morphology can be obtained by pre-treating flake graphite. Optionally, the pre-treatment includes processes such as crushing, classification, spheroidization, and purification.
[0134] In some embodiments, the morphology of the raw material includes one or more of spherical and spheroidal shapes.
[0135] In some embodiments, the volume distribution particle size Dv50 of the raw material is 7.5 μm-23.0 μm, optionally 9.0 μm-22.0 μm. When the volume distribution particle size of the raw material is within the above range, it is beneficial to the subsequent filling process.
[0136] In some embodiments, the graphitization degree of the raw material is ≥93.0%, optionally ≥93.5%, ≥94.0%, ≥94.5%, or ≥95.0%, thereby facilitating the carbon material to have a high gram capacity.
[0137] In some embodiments, the carbon content in the raw material is ≥98 wt %.
[0138] In some embodiments, the softening point temperature of the filling material is 120℃-300℃, optionally 120℃-250℃, 120℃-225℃, 120℃-200℃, 120℃-180℃, 120℃-170℃, 120℃-160℃, 125℃-250℃, 125℃-225℃, 125℃-200℃, 125℃-180℃, 125℃-170℃, 125℃-160℃.
[0139] During the research process, the inventors found that when the softening point temperature of the filling material is within the above-mentioned range, it is beneficial to adjust the pore size and / or pore content in the external and internal regions of the carbon material within a suitable range, and it is also beneficial to adjust the ratio of the peak intensity of the first peak to the peak intensity of the second peak within a suitable range. And it can effectively avoid the following situations: when the softening point temperature of the filling material is too high, the filling material is not easy to flow and fill into the pore structure of the raw material, thereby failing to effectively modify the internal defects of the particles, and failing to effectively prevent the electrolyte from penetrating into the pore structure inside the obtained carbon material particles, thereby affecting the initial coulombic efficiency and cycle performance of the secondary battery; when the softening point temperature of the filling material is too low, the filling material contains more small molecules, which are easily volatilized when heated. Therefore, although the filling material is easy to flow and fill into the pore structure of the raw material, when step 2 and / or step 3 is heat treated, the small molecules in the filling material volatilize, thereby resulting in the actual residual carbon in the filling area failing to effectively fill the pore structure of the raw material, failing to achieve an effective filling effect, or the actual residual carbon in the filling area has more pore structures, thereby failing to reduce the consumption of active ions by SEI film formation and reduce the irreversible capacity loss of the secondary battery, and at the same time affecting the cycle performance, kinetic performance and / or storage performance of the secondary battery.
[0140] In some embodiments, the coking value of the filler material is 25%-70%, optionally 30%-60%. The inventors found during research that when the coking value of the filler material is within the above range, it is beneficial to adjust the pore size and / or pore content in the outer region and the inner region of the carbon material within a suitable range, and it is also beneficial to adjust the ratio of the peak intensity of the first peak to the peak intensity of the second peak within a suitable range.
[0141] The coking value of the filler material is well known in the art and can be measured using instruments and methods known in the art, for example, according to GB / T 8727-2008.
[0142] In some embodiments, the volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be selected from 1 μm-6 μm, 2 μm-5 μm, and 3 μm-5 μm. This facilitates the filler material to fill into the pore structure of the raw material and improves the dispersion uniformity of the filler material and the raw material.
[0143] In some embodiments, the filling material includes one or more of coal-based asphalt, oil-based asphalt, resin and polymer material, and can optionally include one or more of coal-based asphalt and oil-based asphalt.
[0144] In some embodiments, the mass ratio of the filler material to the raw material is 10:90-25:75, optionally 12:88-25:75. This is beneficial for adjusting the pore size and / or pore content in the outer region and the inner region of the carbon material within a suitable range, and is also beneficial for adjusting the ratio of the peak intensity of the first peak to the peak intensity of the second peak within a suitable range. And it can effectively avoid the following situations: when the mass ratio of the filler material to the raw material is too small, the dispersion uniformity of the filler material and the raw material may deteriorate. At this time, the filler material cannot effectively modify the internal defects of the particles, nor can it effectively prevent the electrolyte from penetrating into the pore structure inside the obtained carbon material particles, thereby affecting the first coulomb efficiency and cycle performance of the secondary battery; when the mass ratio of the filler material to the raw material is too small, the ratio of the peak intensity of the first peak to the peak intensity of the second peak is also easy to be small, thereby also affecting the dynamic performance of the secondary battery; when the mass ratio of the filler material to the raw material is too large, it is easy to cause the internal pore structure of the raw material to be completely filled, and at this time the obtained The volume of the obtained carbon material changes greatly, the particles are easier to break, the consumption of active ions for SEI film formation increases, and the irreversible capacity loss of the secondary battery increases; when the mass ratio of the filler material to the raw material is too large, a large amount of filler material will remain on the surface of the particles. At this time, the particles are more likely to agglomerate, which not only increases the depolymerization process, but also reduces the gram capacity and / or compaction density of the obtained carbon material; when the mass ratio of the filler material to the raw material is too large, the ratio of the peak intensity of the first peak to the peak intensity of the second peak is also likely to be large, and the content of crystalline carbon components with lower graphitization degree in the obtained carbon material is higher, thereby affecting the energy density and cycle performance of the secondary battery.
[0145] By adjusting one or more parameters such as the type, softening point, coking value, and addition amount of the filling material within the above-mentioned range, on the one hand, it is beneficial to adjust the ratio of the peak intensity of the first peak to the peak intensity of the second peak within an appropriate range, and on the other hand, it is beneficial to adjust the pore size and / or pore content in the external region and the internal region of the carbon material within an appropriate range; in addition, after the filling material is heated and melted, the viscosity is not high, and good fluidity is maintained, and it is not easy to adhere to the raw material particles, which can reduce the agglomeration of the raw material particles in the subsequent preparation process, thereby reducing the problems of increased surface defects of the carbon material particles and increased surface side reaction active sites due to the need to add a depolymerization process.
[0146] In some embodiments, in step 2, the first temperature T1 is 1000° C.-1400° C., optionally 1000° C.-1350° C., 1000° C.-1300° C., 1050° C.-1350° C., 1050° C.-1300° C., or 1050° C.-1250° C. The inventors have found during research that when the first temperature is within the above range, it is beneficial to adjust the pore size and / or pore content in the outer region and the inner region of the carbon material to be within an appropriate range.
[0147] In some embodiments, the first time t1 is 1 hour to 5 hours. For example, the first time t1 can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, or any range thereof. Alternatively, the first time t1 is 2 hours to 4 hours. The inventors have found during research that when the first time is within the above range, it is beneficial to adjust the pore size and / or pore content in the outer region and the inner region of the carbon material to be within a suitable range.
[0148] In some embodiments, in step 2, the temperature is raised to the first temperature T1 at a rate of 1°C / min-10°C / min. For example, the heating rate can be 1.5°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, or any range thereof. Alternatively, the heating rate is 1°C / min-8°C / min, 1.5°C / min-6°C / min, 1.5°C / min-5°C / min, or 1.5°C / min-4°C / min.
[0149] During the research process, the inventors found that when the heating rate is within the above range, it is beneficial to adjust the pore size and / or pore content in the outer region and inner region of the carbon material within an appropriate range. It can also effectively avoid the following situations: when the heating rate is too high, the filler material may be carbonized on the surface of the raw material particles, resulting in the filler material being difficult to fill into the pore structure of the raw material, thereby failing to effectively modify the internal defects of the particles and failing to effectively prevent the electrolyte from penetrating into the pore structure inside the obtained carbon material particles, thereby affecting the initial coulombic efficiency and cycle performance of the secondary battery; when the heating rate is too low, the filler material easily flows and fills into the entire pore structure of the raw material, resulting in a large volume change of the carbon material during the process of active ion extraction and embedding, and the particles are more easily broken, thereby increasing the consumption of active ions by the SEI film formation, increasing the irreversible capacity loss of the secondary battery, and also affecting the cycle performance and kinetic performance of the secondary battery.
[0150] In some embodiments, in step 2, the heat treatment may be performed in a box furnace, a medium frequency furnace, a roller kiln, a rotary kiln, or a pusher kiln.
[0151] In some embodiments, in step 2, the heat treatment atmosphere may be a protective gas atmosphere, which may include one or more of nitrogen, argon, and helium.
[0152] In step 2, by adjusting one or more of the heating rate, the first temperature, the first time, etc. within the above-mentioned range, it is beneficial to prepare a carbon material with a desired structure, for example, it is beneficial to adjust the pore size and / or pore content in the outer region and the inner region of the carbon material within a suitable range.
[0153] In some embodiments, the second temperature T2 is 2000° C.-2720° C., for example, 2050° C., 2100° C., 2150° C., 2200° C., 2250° C., 2300° C., 2350° C., 2400° C., 2450° C., 2500° C., 2550° C., 2600° C., 2650° C., 2700° C., or any range thereof. Optionally, the second temperature T2 is 2050° C.-2550° C., 2100° C.-2550° C., 2150° C.-2550° C., 2150° C.-2500° C., or 2150° C.-2400° C.
[0154] During the research process, the inventors found that when the second temperature is within the above range, the peak spectrum of the X-ray diffraction pattern of the carbon material can be made to have two diffraction peaks in the range of 2θ of 25.5°-27.5°, which is also conducive to adjusting the ratio of the peak intensity of the first peak to the peak intensity of the second peak within a suitable range. And it can effectively avoid the following situation: when the second temperature is too low, the ratio of the peak intensity of the first peak to the peak intensity of the second peak is large, and the content of components with low graphitization degree and / or amorphous carbon (such as soft carbon, etc.) in the obtained carbon material is large, thereby resulting in a high defect content in the carbon material, affecting the first coulombic efficiency, gram capacity and cycle performance of the carbon material; when the second temperature is too high, the peak spectrum of the X-ray diffraction pattern of the carbon material will not have two diffraction peaks in the range of 2θ of 25.5°-27.5°, or the ratio of the peak intensity of the first peak to the peak intensity of the second peak is small, which is not conducive to the rapid release and embedding of active ions, thereby affecting the kinetic performance of the secondary battery.
[0155] In some embodiments, the second time t2 is 1.5 hours to 6 hours. For example, the second time t1 can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, or any range thereof. Alternatively, the second time t2 is 2 hours to 5 hours.
[0156] During the research process, the inventors found that when the second time is within the above range, the peak spectrum of the X-ray diffraction pattern of the carbon material can be made to have two diffraction peaks in the range of 2θ of 25.5°-27.5°, which is also conducive to adjusting the ratio of the peak intensity of the first peak to the peak intensity of the second peak within a suitable range. It can also effectively avoid the following situations: when the second time is too short, the ratio of the peak intensity of the first peak to the peak intensity of the second peak is large, thereby resulting in a high defect content in the carbon material, affecting the initial coulombic efficiency, gram capacity and cycle performance of the carbon material; when the second time is too long, the peak spectrum of the X-ray diffraction pattern of the carbon material does not have two diffraction peaks in the range of 2θ of 25.5°-27.5°, or the ratio of the peak intensity of the first peak to the peak intensity of the second peak is small, which is not conducive to the rapid extraction and embedding of active ions, thereby affecting the kinetic performance of the secondary battery.
[0157] In some embodiments, in step 3, the heat treatment may be performed in a medium frequency furnace, a box-type graphitization furnace, an Acheson graphitization furnace, a continuous graphitization furnace, or an inner-string graphitization furnace.
[0158] In some embodiments, in step 3, the medium frequency furnace and the continuous graphitization heat treatment atmosphere may be a protective gas atmosphere. The protective gas may include one or more of nitrogen, argon, and helium.
[0159] By adjusting one or more of the second temperature and the second time within the above-mentioned range, two diffraction peaks can be present in the peak spectrum of the X-ray diffraction pattern of the carbon material within the range of 2θ of 25.5°-27.5°, which is also beneficial for adjusting the ratio of the peak intensity of the first peak to the peak intensity of the second peak within an appropriate range.
[0160] The preparation method of the carbon material of the present application is simple and safe, does not require a preset pressure or vacuum treatment, and does not require an additional depolymerization step during the heat treatment process. The carbon material prepared in the present application has a small volume expansion, high structural stability, and a fast active ion diffusion rate, thereby achieving a high gram capacity, a high first coulombic efficiency, and a small volume change, and can also enable the secondary battery to have good cycle performance and kinetic performance. In addition, the secondary battery can also have a high first coulombic efficiency and a high energy density.
[0161] The preparation method of the present application is low-cost, highly practical, and suitable for large-scale production.
[0162] secondary batteries
[0163] A third aspect of the embodiments of the present application provides a secondary battery.
[0164] The present application has no particular restrictions on the type of secondary battery. For example, the secondary battery can be a lithium-ion battery, etc. In general, a secondary battery includes a positive electrode plate, a negative electrode plate, and an electrolyte, etc. During the charge and discharge process of the secondary battery, active ions are embedded and released back and forth between the positive electrode plate and the negative electrode plate, and the electrolyte plays a role in conducting active ions between the positive electrode plate and the negative electrode plate. The present application has no particular restrictions on the type of the electrolyte, and it can be selected according to actual needs. For example, the electrolyte can be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte). Secondary batteries using electrolytes and some secondary batteries using solid electrolytes can also include an isolation membrane, which is arranged between the positive electrode plate and the negative electrode plate to play an isolation role.
[0165] [Negative electrode]
[0166] In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces that are opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0167] In some embodiments, the negative electrode film layer comprises the carbon material of the first aspect of the embodiment of the present application or the carbon material prepared by the method described in the second aspect of the embodiment of the present application, thereby enabling the secondary battery to have both good cycle performance and kinetic performance.
[0168] In some embodiments, the negative electrode film layer may further include other negative electrode active materials in addition to the above-mentioned carbon materials. In some embodiments, the other negative electrode active materials include, but are not limited to, one or more of conventional natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy materials. The tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials.
[0169] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. As examples, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0170] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As examples, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0171] In some embodiments, the negative electrode film layer may further include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.
[0172] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0173] The negative electrode film layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring until uniformly mixed. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0174] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode plate described in the present application further includes a protective layer covering the surface of the negative electrode film layer.
[0175] [Positive electrode]
[0176] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces that are opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0177] The positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0178] The positive electrode film layer generally comprises a positive electrode active material, an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating a positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is generally formed by dispersing a positive electrode active material, an optional conductive agent, an optional binder and any other components in a solvent and stirring evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto. As an example, the binder for the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. As an example, the conductive agent for the positive electrode film layer includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0179] The positive electrode active material may be a positive electrode active material for a secondary battery known in the art.
[0180] When the secondary battery of the present application is a lithium-ion battery, the positive electrode active material may include, but is not limited to, one or more of lithium-containing transition metal oxides, lithium-containing phosphates, and their respective modified compounds. Examples of the lithium transition metal oxide may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of the lithium-containing phosphate may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.
[0181] In some embodiments, in order to further improve the energy density of the secondary battery, the positive electrode active material for the lithium ion battery may include a general formula of Li a Nib Co c M d O e A f One or more lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M is selected from one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A is selected from one or more of N, F, S and Cl.
[0182] In some embodiments, as examples, the positive electrode active material for lithium ion batteries may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 One or more of O2, LiFePO4 and LiMnPO4.
[0183] In the present application, the modified compounds of the above-mentioned positive electrode active materials may be the ones subjected to doping modification and / or surface coating modification on the positive electrode active materials.
[0184] [Electrolytes]
[0185] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0186] The type of the electrolyte salt is not particularly limited and can be selected according to actual needs.
[0187] When the secondary battery of the present application is a lithium ion battery, as an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0188] The type of the solvent is not specifically limited and can be selected according to actual needs. In some embodiments, for example, the solvent may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE). One or more.
[0189] In some embodiments, the electrolyte may further optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives capable of improving certain properties of the secondary battery, such as additives that improve the overcharge performance of the secondary battery, additives that improve the high-temperature performance of the secondary battery, and additives that improve the low-temperature power performance of the secondary battery.
[0190] [Isolation film]
[0191] The present application has no particular limitation on the type of the isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected.
[0192] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different.
[0193] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process.
[0194] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0195] In some embodiments, the outer packaging can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0196] The present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. FIG3 shows a secondary battery 5 with a square structure as an example.
[0197] In some embodiments, as shown in FIG4 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.
[0198] The preparation method of the secondary battery of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The secondary battery is then vacuum packaged, allowed to stand, formed, and shaped.
[0199] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.
[0200] Figure 5 is a schematic diagram of an exemplary battery module 4. As shown in Figure 5 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured using fasteners.
[0201] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0202] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0203] Figures 6 and 7 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 6 and 7, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.
[0204] Electrical devices
[0205] The present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0206] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0207] Figure 8 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0208] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.
[0209] Example
[0210] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.
[0211] Example 1
[0212] (1) Preparation of carbon materials
[0213] Step 1: Mechanically crush, classify, spheroidize, and purify 100-mesh flake graphite to obtain natural spherical graphite with a volume distribution particle size Dv50 of 15 μm, a carbon content of 99.9%, and a degree of graphitization of 95%.
[0214] Step 2: The obtained natural spherical graphite and petroleum pitch (softening point temperature of 150°C, volume distribution particle size Dv50 of 5 μm, and coking value of 35%) were mixed in a VC mixer at a mass ratio of 80:20 for 30 minutes. The mixed materials were placed in a crucible and then heated to 1100°C in a box furnace at a rate of 2°C / min and maintained at this temperature for 2 hours. After the mixture was cooled naturally to room temperature, an intermediate was obtained.
[0215] Step 3: Place the obtained intermediate in an Acheson graphitization furnace, heat it to 2400°C and keep it warm for 3 hours. After the graphitization is completed, demagnetize and sieve to obtain the carbon material.
[0216] (2) Preparation of button cells (half-cells)
[0217] The carbon material prepared above was thoroughly stirred and mixed with the binder styrene-butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC), and the conductive agent carbon black in an appropriate amount of deionized water at a mass ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry. The negative electrode slurry was evenly coated on the surface of the negative electrode current collector copper foil and dried in an oven for later use. Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed at a volume ratio of 1:1:1 to obtain an organic solvent, and LiPF6 was dissolved in the organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L. A metal lithium sheet was then used as the counter electrode and a polyethylene (PE) film as the separator to assemble a CR2430 button cell in an argon-protected glove box.
[0218] (3) Preparation of secondary batteries (full batteries)
[0219] The carbon material prepared above, the conductive agent carbon black (Super P), the binder styrene-butadiene rubber, and the thickener sodium carboxymethyl cellulose were thoroughly stirred and mixed in an appropriate amount of deionized water at a weight ratio of 96:1:1:2 to form a negative electrode slurry. The negative electrode slurry was coated on both surfaces of the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0220] LiNi 0.5 Co 0.2 Mn 0.3O2 (NCM523) is mixed with conductive carbon black and polyvinylidene fluoride in a weight ratio of 96:2.5:1.5. An appropriate amount of NMP solvent is added and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil. After drying and cold pressing, the positive electrode sheet is obtained.
[0221] A polypropylene film with a thickness of 12 μm is used as an isolation membrane, and is placed in order with the positive electrode sheet and the negative electrode sheet prepared above, so that the isolation membrane is located between the positive electrode sheet and the negative electrode sheet to play an isolation role, and then the electrode assembly is obtained by winding; the electrode assembly is placed in an outer package, dried, and then injected with the same electrolyte as the button battery prepared above, and after vacuum packaging, standing, formation, capacity and other processes, a secondary battery is obtained.
[0222] Comparative Example 1
[0223] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.
[0224] 100 mesh flake graphite is mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 15 μm, a carbon content of 99.9% and a graphitization degree of 95%.
[0225] Comparative Example 2
[0226] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.
[0227] 100 mesh flake graphite was mechanically crushed, classified, spheroidized, and purified to obtain natural spherical graphite having a volume distribution particle size Dv50 of 15 μm, a carbon content of 99.9%, and a degree of graphitization of 95%. The obtained natural spherical graphite was mixed with petroleum asphalt (softening point temperature of 150°C, volume distribution particle size Dv50 of 5 μm, and coking value of 35%) in a mass ratio of 80:20 in a VC mixer for 30 minutes. The mixed material was then graphitized at 3200°C for 10 hours and then cooled to room temperature to obtain a carbon material.
[0228] Comparative Example 3
[0229] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.
[0230] 100 mesh flake graphite was mechanically crushed, classified, spheroidized, and purified to obtain natural spherical graphite having a volume distribution particle size Dv50 of 15 μm, a carbon content of 99.9%, and a degree of graphitization of 95%. The obtained natural spherical graphite was mixed with petroleum pitch (softening point temperature of 150°C, volume distribution particle size Dv50 of 5 μm, and coking value of 35%) in a mass ratio of 80:20 in a VC mixer for 30 minutes. The mixed material was then carbonized at 1200°C for 3 hours and then cooled to room temperature to obtain a carbon material.
[0231] Comparative Example 4
[0232] The preparation methods of half cells and full cells are similar to those in Example 1, except for the preparation process of the carbon material.
[0233] 100 mesh flake graphite is mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite with a volume distribution particle size Dv50 of 15 μm, a carbon content of 99.9% and a graphitization degree of 95%.
[0234] The obtained natural spherical graphite and petroleum asphalt (softening point temperature of 150 ° C, volume distribution particle size Dv50 of 5 μm, coking value of 35%) were mixed in a VC mixer for 30 minutes. The mixed materials were then put into a reactor, and the reactor was gradually heated at a heating rate of 2 ° C / min. While heating, the reactor was kept in a uniform stirring state, and the temperature was raised to 190 ° C. The reactor was pumped to a pressure of -0.1 MPa, and then kept warm for 2 hours. After the insulation was completed, the reactor was heated to 650 ° C and kept warm for 2 hours. After that, the reactor was cooled to about 160 ° C, and then petroleum asphalt was slowly added to the reactor. The mass ratio of the amount of petroleum asphalt added this time to the previous petroleum asphalt was 1:1. After that, the reactor was heated to 190 ° C again, the reactor was pumped to a pressure of -0.1 MPa, and then kept warm for 2 hours. After that, the reactor was heated to 650 ° C and kept warm for 2 hours. After that, the temperature was cooled by condensation cooling. Finally, the material processed by the above process was heat-treated at 1200°C for 3 hours, and the heat-treated sample was crushed and sieved to obtain a carbon material with no pores inside.
[0235] Example 2-21
[0236] The preparation methods of half cells and full cells are similar to those in Example 1, except that the preparation process parameters of the carbon material are adjusted. See Table 1 for details.
[0237] Table 1
[0238]
[0239]
[0240] Performance Testing
[0241] (1) X-ray diffraction test of carbon materials
[0242] The carbon material was tested using an X-ray diffractometer according to JIS K 0131-1996 and JB / T 4220-2011 to determine its physical structure. The X-ray diffraction pattern of the carbon material was refined using Topas software and the Rietveld full spectrum fitting refinement method.
[0243] In Table 2, the 2θ of the first peak is between 26.256° and 26.456°, and the 2θ of the second peak is between 26.509° and 26.569°. The ratio of the peak intensity of the first peak to the peak intensity of the second peak is the ratio of the integrated area of the first peak to the integrated area of the second peak. The testing instrument can be a Bruker D8 Discover X-ray diffractometer. In the X-ray diffraction analysis test, the test conditions can be as follows: the carbon material is prepared by a flat plate sample preparation method, a copper target is used as an anode target, CuKα rays are used as a radiation source, the voltage is 40KV, the current is 40mA, the anti-scattering slit is 1mm, the scanning 2θ angle range is 20°-80°, the step size is 0.01671°, the time per step is 0.24s, and the scanning rate is 4° / min.
[0244] (2) Total pore area test in the outer and inner regions of carbon materials
[0245] Mix the sample preparation binder and carbon material powder evenly, then apply the mixture to copper foil and dry at 60°C for 30 minutes. Cut the sample into 6mm x 6mm pieces and affix them to the sample stage of a CP-type argon ion cross-section polisher. Use a plasma beam to cut the sample to obtain a cross section of the carbon material, with the cross section passing through the center of the carbon material particle. The testing instrument can be the IB-09010CP-type argon ion cross-section polisher from JEOL, Japan.
[0246] The cross section of the carbon material was scanned using a scanning electron microscope. The test may refer to JY / T010-1996. The testing instrument may be a Sigma 300 scanning electron microscope from the German ZEISS company.
[0247] The area extending 0.25L from the particle surface of the carbon material to the interior of the particle is recorded as the outer area, and the area inside the outer area is recorded as the inner area, where L represents the minor axis length of the carbon material particle. The total pore area S1 of the outer area of the carbon material and the total pore area S2 of the inner area of the carbon material are calculated using image processing software. The image processing software can be AVIZO.
[0248] (3) Maximum charge rate test of secondary batteries
[0249] At 25°C, the secondary battery is discharged at a constant current rate of 1C to the lower cutoff voltage (corresponding to 0% SOC). Then, it is charged at a constant current rate of 1C to the upper cutoff voltage (corresponding to 100% SOC), and the constant voltage charging is continued until the current reaches 0.05C. At this time, the secondary battery is fully charged. After the fully charged secondary battery is allowed to stand for 5 minutes, it is discharged at a constant current rate of 1C to the lower cutoff voltage (corresponding to 0% SOC). The discharge capacity at this time is the actual capacity of the secondary battery at 1C rate, recorded as C0. The secondary battery is charged at a constant current rate of x C0 (representing a gradient charge rate, for example, 1C0, 1.05C0, 1.1C0, 1.15C0, 1.2C0...) to the upper cutoff voltage (corresponding to 100% SOC), and the constant voltage charging is continued until the current reaches 0.05C0. After standing for 5 minutes, the secondary battery is disassembled to observe the lithium deposition on the surface of the negative electrode. If no lithium is deposited on the surface of the negative electrode, increase the charge rate and test again until lithium is deposited on the surface of the negative electrode. Record the maximum charge rate at which no lithium is deposited on the surface of the negative electrode.
[0250] (4) Cycle performance test of secondary batteries
[0251] At 25°C, the prepared secondary battery was charged at a constant current of 1C to the upper cutoff voltage (corresponding to 100% SOC), then charged at a constant voltage to a current of 0.05C. After standing for 5 minutes, the secondary battery was discharged at a constant current of 1C to the lower cutoff voltage (corresponding to 0% SOC). The discharge capacity at this point was recorded as the first cycle discharge capacity. The secondary battery was subjected to a cyclic charge and discharge test according to the above method, and the discharge capacity after each cycle was recorded. Capacity retention rate (%) of the secondary battery after 2500 cycles at 25°C = discharge capacity after 2500 cycles / discharge capacity after 1st cycle × 100%.
[0252] Table 2
[0253]
[0254] The specific surface area, volume distribution particle size, powder resistivity, powder compaction density and other parameters of the carbon materials prepared in Examples 1-21 are all within the range described in the specification of this application, and there is no diffraction peak of the 3R phase C(012) crystal plane in the X-ray diffraction pattern of the carbon material.
[0255] The test results in Table 2 indicate that when the X-ray diffraction pattern of the carbon material exhibits two diffraction peaks within the 2θ range of 25.5°-27.5°, the battery can achieve both good cycling and kinetic performance. Furthermore, when the ratio of the peak intensity of the first peak to the peak intensity of the second peak is further between 10:90 and 40:60, or optionally between 15:85 and 35:65, the battery can achieve both good cycling and kinetic performance while also achieving high energy density.
[0256] The test results in Table 2 also show that when the carbon material particles further meet S2>S1, optionally meet 1.5≤S2 / S1≤450, and more optionally meet 2≤S2 / S1≤400, the overall performance of the battery is further improved. In this case, the carbon material particles further have the following characteristics: the inner region has a high pore content and / or large pore size, while the outer region has a low pore content and / or small pore size. The pore structure in the inner region of the carbon material can reserve the required expansion space for the volume change of the carbon material particles, thereby reducing the risk of carbon material particles breaking and forming new interfaces, thereby reducing the occurrence of side reactions and reducing the irreversible capacity loss of the battery; the low pore content and / or small pore size in the outer region of the carbon material can make the carbon material particles have a more stable structure and minimize the infiltration of electrolyte into the pore structure inside the carbon material particles, thereby reducing the occurrence of side reactions and reducing the consumption of active ions by the formation of the SEI film inside the particles. Therefore, carbon materials that further meet the above structural characteristics can further improve the overall performance of the battery.
[0257] The X-ray diffraction patterns of the carbon materials prepared in Comparative Examples 1-4 have only one diffraction peak in the range of 2θ of 25.5°-27.5°, and none of them can enable the battery to have both good cycle performance and kinetic performance.
[0258] Comparative Example 1 uses untreated natural spherical graphite as the carbon material. The carbon material particles have a large number of pores, and in the peak spectrum of the X-ray diffraction pattern of the carbon material, there is only one diffraction peak in the range of 2θ of 25.5°-27.5°. Combined with the test results in Table 2, it can be seen that the cycle performance and kinetic performance of the battery prepared in this way are poor.
[0259] The carbon material prepared in Comparative Example 2 is a carbon layer coating formed on the surface of natural spherical graphite. Due to the high heat treatment temperature and the long heat treatment time, the degree of graphitization of the carbon layer is close to that of the natural spherical graphite matrix. Therefore, the peak spectrum of the X-ray diffraction pattern of the carbon material has only one diffraction peak in the range of 2θ of 25.5°-27.5°, and the interlayer spacing of the carbon material is small at this time. Combined with the test results in Table 2, it can be seen that the dynamic performance of the battery prepared thereby is poor; in addition, the coating layer only exists on the surface of the natural spherical graphite, fails to achieve an effective filling effect, and cannot effectively prevent the electrolyte from penetrating into the pore structure inside the particles, which in turn leads to limited improvement in the battery cycle performance.
[0260] The carbon material prepared in Comparative Example 3 is a carbon layer coating formed on the surface of natural spherical graphite. Due to the low heat treatment temperature, the main component of the coating at this time is amorphous carbon, and no crystalline carbon phase with different degrees of graphitization will appear in the carbon material. In addition, the peak spectrum of the X-ray diffraction pattern of the carbon material has only one diffraction peak in the range of 2θ of 25.5°-27.5°; in addition, the coating only exists on the surface of natural spherical graphite, fails to achieve an effective filling effect, and cannot effectively prevent the electrolyte from penetrating into the pore structure inside the particles, which in turn leads to limited improvement in the battery cycle performance and kinetic performance.
[0261] In Comparative Example 4, when preparing the carbon material, the filling material is filled into all the pore structures inside the natural spherical graphite particles by vacuuming. Due to the low heat treatment temperature, a large amount of amorphous carbon exists inside and / or on the surface of the carbon material particles at this time, and no crystalline carbon phase with different degrees of graphitization appears in the carbon material. The peak spectrum of the X-ray diffraction pattern of the carbon material has only one diffraction peak in the range of 2θ of 25.5°-27.5°; in addition, there is no pore structure inside the carbon material particles obtained at this time, which leads to a large volume change of the carbon material during the extraction and embedding of active ions, and the particles are more easily broken, which in turn leads to limited improvement in the cycle performance and kinetic performance of the battery.
[0262] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A carbon material, wherein The carbon material includes a pore structure. In the peak spectrum of the X-ray diffraction spectrum of the carbon material, two diffraction peaks exist within the range of 2θ of 25.5°-27.5°.
2. The carbon material according to claim 1, wherein Among the two diffraction peaks, the one with smaller 2θ is recorded as the first peak, and the one with larger 2θ is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is 10:90-40:60, and can be optionally 15:85-35:
65.
3. The carbon material according to claim 1 or 2, wherein The carbon material includes at least one pore with an area greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.15 μm 2 -3.0μm 2 pore structure.
4. The carbon material according to any one of claims 1 to 3, wherein The carbon material includes an external region and an internal region located inside the external region, wherein the external region refers to a region extending from the particle surface of the carbon material to the interior of the particle by a distance of 0.25L, and L refers to the minor axis length of the carbon material particle. The total pore area of the external region is recorded as S1, and the total pore area of the internal region is recorded as S2, and S2>S1. Optionally, 1.5≤S2 / S1≤450, 2≤S2 / S1≤400.
5. The carbon material according to claim 4, wherein 0.01μm 2 ≤S1≤8.0μm 2 , optionally, 0.02 μm 2 ≤S1≤4.5μm 2 and / or, 2.5μm 2 ≤S2≤25.0μm 2 , optionally, 3.0 μm 2 ≤S2≤22.5μm 2 and / or, L≥4μm, optionally, 4μm≤L≤20μm.
6. The carbon material according to claim 4 or 5, wherein The area of the pore structure in the outer region of the carbon material is less than or equal to 0.2 μm 2 , can be selected to be less than or equal to 0.1μm 2 and / or, The inner region of the carbon material includes at least one area greater than or equal to 0.1 μm 2 The pore structure may optionally include one or more pores with an area of 0.15 μm 2 -3.0μm 2 pore structure.
7. The carbon material according to any one of claims 1 to 6, wherein The carbon material satisfies at least one of the following: (1) The specific surface area of the carbon material is 0.5 m 2 / g-3.1m 2 / g, optional 0.7m 2 / g-2.8m 2 / g; (2) The volume distribution particle size Dv50 of the carbon material is 8.0 μm-23.0 μm, and can be optionally 9.0 μm-22.0 μm; (3) (Dv90-Dv10) / Dv50 of the carbon material is ≤1.55, and can be optionally 0.5-1.50; (4) The morphology of the carbon material includes one or more of block, spherical and quasi-spherical shapes.
8. The carbon material according to any one of claims 1 to 7, wherein The carbon material satisfies at least one of the following: (1) The powder resistivity of the carbon material under a pressure of 8 MPa is 0.006 Ω.cm-0.051 Ω.cm, and can be optionally 0.010 Ω.cm-0.040 Ω.cm; (2) The powder compaction density of the carbon material under a pressure of 20000N is 1.70g / cm 3 -1.95g / cm 3 , optional 1.72g / cm 3 -1.92g / cm 3 ; (3) The tap density of the carbon material is 0.90 g / cm 3 -1.35g / cm 3 , optional 0.95g / cm 3 -1.32g / cm 3 ; (4) The gram capacity of the carbon material is 350 mAh / g-372 mAh / g, and can be optionally 353 mAh / g-371 mAh / g; (5) The graphitization degree of the carbon material is 91.5%-98.5%, and can be optionally 92.5%-98.0%; (6) The X-ray diffraction pattern of the carbon material does not contain a diffraction peak of the 3R phase C(012) crystal plane.
9. A method for preparing a carbon material, comprising the following steps: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and a filler material in a predetermined ratio, and then maintaining the mixture at a first temperature T1 for a first time t1 to obtain an intermediate; step 3, maintaining the obtained intermediate at a second temperature T2 for a second time t2 to obtain a carbon material, wherein: The carbon material includes a pore structure. In the peak spectrum of the X-ray diffraction spectrum of the carbon material, two diffraction peaks exist within the range of 2θ of 25.5°-27.5°.
10. The method according to claim 9, wherein: The raw materials satisfy at least one of the following: (1) The raw material includes natural graphite, and optionally, the natural graphite includes one or more of flake graphite, natural spherical graphite and microcrystalline graphite; (2) The volume distribution particle size Dv50 of the raw material is 7.5 μm-23.0 μm, and can be optionally 9.0 μm-22.0 μm; (3) The graphitization degree of the raw material is ≥93.0%; (4) The carbon content in the raw material is ≥98wt%.
11. The method according to claim 9 or 10, wherein: The filling material satisfies at least one of the following: (1) The softening point temperature of the filling material is 120°C-300°C, and can be optionally 125°C-250°C; (2) The coking value of the filler material is 25%-70%, and can be optionally 30%-60%; (3) The volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be optionally 1 μm-5 μm; (4) The filling material includes one or more of coal-based asphalt, oil-based asphalt, resin and polymer material, and can optionally include one or more of coal-based asphalt and oil-based asphalt.
12. The method according to any one of claims 9 to 11, wherein: The mass ratio of the filling material to the raw material is 10:90-25:75, and can be optionally 12:88-25:
75.
13. The method according to any one of claims 9 to 12, wherein: The first temperature T1 is 1000° C.-1400° C., optionally 1050° C.-1250° C.; and / or, The first time t1 is 1 hour to 5 hours, and can be optionally 2 hours to 4 hours; and / or, The second temperature T2 is 2000° C.-2720° C., optionally 2150° C.-2550° C.; and / or, The second time t2 is 1.5 hours to 6 hours, and can be optionally 2 hours to 5 hours.
14. The method according to any one of claims 9 to 13, wherein: The temperature is raised to the first temperature T1 at a rate of 1°C / min-10°C / min, optionally 1.5°C / min-5°C / min. 15 . A secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises the carbon material according to claim 1 or the carbon material prepared by the method according to claim 9 .
16. An electrical device comprising the secondary battery according to claim 15.
Citation Information
Patent Citations
Natural graphite-based modified composite material and preparation method thereof, and lithium ion battery comprising modified composite material
CN108063229A
Carbon catalyst, battery electrode, and battery
CN110869121A
Natural graphite, modified natural graphite material prepared from natural graphite, preparation method and application
CN111244450A
Anode active material for lithium secondary battery and lithium secondary battery comprising same
CN111316481A
Carbonaceous-coated graphite particle for lithium ion secondary battery negative electrode material and method for producing the same, lithium ion secondary battery negative electrode, and lithium ion secondary battery
JP2015135809A