Positive electrode active material, lithium ion battery, electronic device, and vehicle

By using positive electrode active substances and electrolytes with specific structures in lithium-ion batteries, the problem of poor discharge capacity and energy density of lithium-ion batteries in low temperature environments is solved, and higher battery performance and safety are achieved.

CN119072799APending Publication Date: 2024-12-03SEMICON ENERGY LAB CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035560.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have poor performance in low-temperature environments and are difficult to maintain charging characteristics under low-temperature conditions, resulting in a degradation of battery performance.

Method used

A positive electrode active material containing cobalt, oxygen, magnesium, aluminum and nickel is used, with a particle size of more than 1 μm and less than 12 μm. The surface layer contains magnesium and aluminum, and is distributed through specific crystal structures and additive elements, including the spatial group R-3m. The base and end regions of the layered rock salt crystal structure and the surface part are distributed, and the electrolytes of lithium hexafluorophosphate, vinyl carbonate, methyl ethyl carbonate and dimethyl carbonate are optimized.

Benefits of technology

In low temperature environments, significantly improve the discharge capacity and energy density of lithium-ion batteries, reduce the reduction rate of discharge capacity and energy density, improve the charging voltage and safety of the battery, and extend the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072799A_ABST
    Figure CN119072799A_ABST
Patent Text Reader

Abstract

Provided is a lithium ion battery having good charge characteristics and discharge characteristics even in a low-temperature environment. A lithium ion battery including a positive electrode active material, the positive electrode active material including cobalt, oxygen, magnesium, aluminum, and nickel, the positive electrode active material having a median diameter of 1 [mu] m or more and 12 [mu] m or less, the surface layer portion including magnesium and aluminum, the surface layer portion being a region 50 nm from the surface of the positive electrode active material, the positive electrode active material includes a region in which magnesium is distributed closer to the surface side of the positive electrode active material than aluminum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention disclosed in this specification and the like (hereinafter sometimes referred to as "the present invention" in this specification and the like) relates to a power storage device, a secondary battery, etc. In particular, it relates to a lithium ion battery.

[0002] In addition, the present invention relates to an object, a method or a manufacturing method. In addition, the present invention relates to a process, a machine, a product or a composition of matter. In addition, the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, a vehicle or a manufacturing method thereof. Background Art

[0003] In recent years, the research and development of various power storage devices such as lithium-ion batteries, lithium-ion capacitors and air batteries has become increasingly popular. In particular, with the development of the semiconductor industry such as mobile phones, smartphones or portable information terminals such as notebook computers, portable music players, digital cameras, medical equipment or electric vehicles such as hybrid electric vehicles (HV), electric vehicles (EV) or plug-in hybrid electric vehicles (PHV), the demand for high-output and high-energy-density lithium-ion batteries has increased. As a rechargeable energy supply source, lithium-ion batteries have become a necessity in the modern information society.

[0004] The charging characteristics and / or discharging characteristics of a lithium-ion battery vary depending on the battery charging environment and / or battery discharging environment. For example, it is known that the discharge capacity of a lithium-ion battery varies depending on the temperature during discharge.

[0005] Therefore, there is a need for a lithium ion battery having good battery characteristics even in a low-temperature environment (for example, refer to Patent Document 1).

[0006] In addition, as image processing software, for example, ImageJ is known (Non-Patent Documents 1 to 3). By using this software, for example, the shape of the positive electrode active material can be analyzed. [Prior technical literature] [Patent Document]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2015-026608 [Non-patent literature]

[0008] [Non-patent document 1] Rasband, WS, ImageJ, USNational Institutes of Health, Bethesda, Maryland, USA, http: / / rsb.info.nih.gov / ij / , 1997-2012. [Non-patent document 2] Schneider, CA, Rasband, WS, Eliceiri, KW "NIH Image to ImageJ: 25 years of image analysis". Nature Methods 9, 671-675, 2012. [Non-patent document 3] Abramoff, MD, Magelhaes, PJ, Ram, SJ "Image Processing with ImageJ". Biophotonics International, volume 11, issue 7, pp. 36-42, 2004. Summary of the invention Technical problem to be solved by the invention

[0009] Patent Document 1 describes that a lithium ion battery that can operate even in a low temperature environment (e.g., below 0° C.) can be realized by using the non-aqueous solvent described in Patent Document 1. However, even the lithium ion battery described in Patent Document 1 cannot be said to have a large discharge capacity when discharged in a low temperature environment, and further improvements are expected.

[0010] In addition, in order to realize lithium-ion batteries that can also work in low-temperature environments, it is necessary not only to develop non-aqueous solvents (electrolytes), but also to develop positive and negative electrodes suitable for lithium-ion batteries that can also work in low-temperature environments. More specifically, the positive electrode is required to develop a positive electrode active material suitable for lithium-ion batteries that can also work in low-temperature environments.

[0011] One of the purposes of one embodiment of the present invention is to provide a positive electrode active material for a lithium ion battery having good discharge characteristics in a low temperature environment. Specifically, one of the purposes of one embodiment of the present invention is to provide a positive electrode active material for a lithium ion battery having a large discharge capacity and / or a large discharge energy density even when discharged in a low temperature environment.

[0012] Note that in this specification, "under low temperature environment" means below 0°C. Also, in this specification, when "under low temperature environment" is described, any temperature below 0°C can be selected. For example, in this specification, when "under low temperature environment" is described, one of below 0°C, below -10°C, below -20°C, below -30°C, below -40°C, below -50°C, below -60°C, below -80°C, and below -100°C can be selected.

[0013] Another object of one embodiment of the present invention is to provide a lithium ion battery having good discharge characteristics even in a low temperature environment. Another object of one embodiment of the present invention is to provide a lithium ion battery having good charge characteristics even in a low temperature environment.

[0014] Specifically, one of the purposes of one embodiment of the present invention is to provide a lithium ion battery that has a large discharge capacity and / or discharge energy density even when discharged in a low temperature environment (e.g., below 0°C, -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C). In addition, one of the purposes of one embodiment of the present invention is to provide a lithium ion battery that has a small reduction rate in the discharge capacity value when discharged in a low temperature environment (e.g., below 0°C, -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C) relative to the discharge capacity value when discharged at 25°C. In addition, one of the purposes of one embodiment of the present invention is to provide a lithium ion battery as follows: relative to the discharge energy density value when discharged at 25°C, the reduction rate of the discharge energy density value when discharged in a low temperature environment (for example, below 0°C, -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C) is small.

[0015] In addition, one of the purposes of one embodiment of the present invention is to provide a secondary battery with a high charging voltage. In addition, one of the purposes of one embodiment of the present invention is to provide a secondary battery with high safety or reliability. In addition, one of the purposes of one embodiment of the present invention is to provide a secondary battery with less degradation. In addition, one of the purposes of one embodiment of the present invention is to provide a secondary battery with a long life. In addition, one of the purposes of one embodiment of the present invention is to provide a novel secondary battery.

[0016] Another object of one embodiment of the present invention is to provide a novel substance, an active material, a power storage device, or a method for producing the same.

[0017] Note that the description of these purposes does not prevent the existence of other purposes. One embodiment of the present invention does not need to solve all of the above purposes. In addition, purposes other than the above purposes can be extracted from the description of this specification, drawings, claims, etc. Solutions to technical problems

[0018] One embodiment of the present invention is a positive electrode active material containing cobalt, oxygen, magnesium, aluminum and nickel, wherein the particle size of the positive electrode active material has a median particle size of greater than 1 μm and less than 12 μm, and the positive electrode active material contains magnesium and aluminum in a surface portion, the surface portion being a region within 50 nm from the surface of the positive electrode active material, and when performing EDX line analysis in the depth direction, the positive electrode active material includes magnesium distributed in a region on the surface side of the positive electrode active material that is closer to the surface of the positive electrode active material than aluminum.

[0019] In the above structure, it is preferred that the positive electrode active material has a layered rock salt type crystal structure belonging to the space group R-3m, the surface portion includes a basal region having a surface parallel to the (001) plane of the crystal structure and an edge region having a surface in a direction intersecting the (001) plane, and when performing EDX line analysis in the depth direction, the positive electrode active material includes an area in the end region where the distribution of magnesium overlaps with the distribution of nickel.

[0020] In the above structure, sometimes the base region does not substantially contain nickel.

[0021] In any of the above structures, it is preferred that, when the positive electrode active material is subjected to XPS analysis, the number of magnesium atoms relative to the number of cobalt atoms (Mg / Co) is greater than 0.400 and less than 1.500, and the number of nickel atoms relative to the number of cobalt atoms (Ni / Co) is greater than 0.050 and less than 0.150.

[0022] In the above structure, preferably, the positive electrode active material contains fluorine, and when the positive electrode active material is subjected to XPS analysis, the number of fluorine atoms relative to the number of cobalt atoms (F / Co) is 0.100 or more and 1.000 or less.

[0023] In addition, one embodiment of the present invention is a lithium ion battery including a positive electrode including the positive electrode active material described in any of the above structures and an electrolyte, wherein the electrolyte includes lithium hexafluorophosphate, ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate.

[0024] In the above lithium ion battery, preferably, when the total volume of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate in the electrolyte is 100 vol%, the volume ratio of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate is x:y:100-xy (note, 5≤x≤35 and 0 <y<65)。

[0025] In the above lithium ion battery, the electrolyte preferably contains 0.5 mol / L or more and 1.5 mol / L or less of lithium hexafluorophosphate relative to the volume of the total content of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate.

[0026] Another embodiment of the present invention is an electronic device including the lithium ion battery.

[0027] Another embodiment of the present invention is a vehicle including the above-mentioned lithium-ion battery. Effects of the Invention

[0028] According to one embodiment of the present invention, a positive electrode active material for a lithium ion battery having good discharge characteristics in a low temperature environment can be provided. Specifically, according to one embodiment of the present invention, a positive electrode active material for a lithium ion battery having a large discharge capacity and / or a large discharge energy density can be provided even when discharged in a low temperature environment.

[0029] In addition, according to one embodiment of the present invention, a lithium ion battery can be provided: even when discharged at a temperature in a low temperature environment (e.g., below 0°C, -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C), the discharge capacity and / or discharge energy density are large. In addition, according to one embodiment of the present invention, a lithium ion battery can be provided: relative to the discharge capacity value when discharged at 25°C, the reduction rate of the discharge capacity value when discharged in a low temperature environment (e.g., below 0°C, -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C) is small. In addition, according to one embodiment of the present invention, a lithium ion battery can be provided in which the rate of decrease in the discharge energy density value when discharged in a low temperature environment (e.g., below 0°C, -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C) is small relative to the discharge energy density value when discharged at 25°C.

[0030] In addition, according to one embodiment of the present invention, a secondary battery with high charging voltage can be provided. In addition, according to one embodiment of the present invention, a secondary battery with high safety or reliability can be provided. In addition, according to one embodiment of the present invention, a secondary battery with less degradation can be provided. In addition, according to one embodiment of the present invention, a secondary battery with long life can be provided. In addition, according to one embodiment of the present invention, a novel secondary battery can be provided.

[0031] Furthermore, according to one embodiment of the present invention, a novel substance, an active material, a power storage device, or a method for producing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1A is a cross-sectional view illustrating the internal structure of a secondary battery, Figure 1B It is a cross-sectional view illustrating a positive electrode and an electrolyte of a secondary battery. Figure 2A and Figure 2B It is a cross-sectional view illustrating a positive electrode active material. FIG. 3A to FIG. 3F It is a cross-sectional view illustrating a positive electrode active material. Figure 4 It is a diagram illustrating the crystal structure of the positive electrode active material. Figure 5 This is a diagram illustrating the crystal structure of a conventional positive electrode active material. Figure 6 is a diagram showing an XRD pattern calculated from a crystal structure. Figure 7 is a diagram showing an XRD pattern calculated from a crystal structure. FIG. 8A to FIG. 8D It is a diagram for explaining a method for producing a positive electrode active material. Fig. 9 It is a diagram for explaining a method for producing a positive electrode active material. FIG. 10A to FIG. 10C It is a diagram for explaining a method for producing a positive electrode active material. FIG. 11A to FIG. 11D It is a cross-sectional view illustrating an example of a positive electrode of a secondary battery. Fig. 12A This is an exploded perspective view of a coin-type secondary battery. Fig. 12B is a perspective view of a coin-type secondary battery. Fig. 12C It is a cross-sectional stereogram. Fig.13A An example of a cylindrical secondary battery is shown. Fig. 13B An example of a cylindrical secondary battery is shown. Fig. 13C A plurality of examples of cylindrical secondary batteries are shown. Fig.13D An example of a power storage system including a plurality of cylindrical secondary batteries is shown. Fig.14A and Fig. 14B is a diagram illustrating an example of a secondary battery, Fig. 14C It is a diagram showing the internal state of a secondary battery. FIG. 15A to FIG. 15C It is a diagram for explaining an example of a secondary battery. Fig.16A and Fig. 16B It is a diagram showing the appearance of a secondary battery. FIG. 17A to FIG. 17C It is a diagram for explaining a method for manufacturing a secondary battery. 18A to 18C is a diagram showing a structural example of a battery pack. Fig.19A is a perspective view showing a battery pack according to one embodiment of the present invention. Fig.19B is the block diagram of the battery pack, Fig.19C is a block diagram of a vehicle including a battery pack. FIG. 20A to FIG. 20D It is a diagram illustrating an example of a transport vehicle. Fig.20E This is a diagram illustrating an example of an artificial satellite. Fig.21A and Fig.21B It is a diagram for explaining a power storage device according to one embodiment of the present invention. Fig.22A is a diagram showing an electric bicycle, Fig. 22B is a diagram showing a secondary battery of an electric bicycle, Fig. 22C It is a figure explaining a small motorcycle. FIG. 23A to FIG. 23D It is a diagram for explaining an example of an electronic device. Fig.24A Showing an example of a wearable device, Fig. 24B showing a perspective view of a watch type device, Fig.24C It is a diagram illustrating the side view of a wristwatch-type device. Fig.25A and Fig.25B This is a graph showing the particle size distribution of the lithium cobalt oxide described in Example 1. Fig.26A and Fig.26B is the SEM image of the sample. FIG. 27A to FIG. 27C This is a diagram for explaining one method of quantifying the smoothness of a positive electrode active material. FIG. 28A to FIG. 28C This is a diagram for explaining one method of quantifying the smoothness of a positive electrode active material. Fig.29A and Fig.29B This is a graph showing the discharge curve of the temperature-dependent charge and discharge test 1 described in Example 2. Fig.30 This is a graph showing the discharge curve of the temperature-dependent charge and discharge test 2 described in Example 2. Fig.31 3 is a graph showing the discharge capacity of the fractional rate discharge capacity test at -40°C described in Example 2. Fig.32A and Fig.32B This is a graph showing the charge and discharge cycle test described in Example 3. Fig.33A and Fig.33B This is a graph showing the charge and discharge cycle test described in Example 3. FIG. 34A to FIG. 34C This is a graph showing the XRD analysis of the high voltage charging state described in Example 3. Fig.35A and Fig.35B This is a graph showing the STEM-EDX analysis described in Example 3. FIG. 36A to FIG. 36C This is a graph showing the STEM-EDX analysis described in Example 3. FIG. 37A to FIG. 37C This is a graph showing the STEM-EDX analysis described in Example 3. Modes for Carrying Out the Invention

[0033] The present embodiment is described with appropriate reference to the accompanying drawings. Note that the present invention is not limited to the following description. It is readily understood by those skilled in the art that the modes and details of the present invention can be changed in various ways without departing from the spirit and scope of the present invention. Therefore, in the embodiments shown below, the reference numerals representing the same components of the present invention are common in different drawings.

[0034] Note that, unless otherwise specified, the following embodiment modes and examples can be implemented in combination with the embodiment modes and examples described in this specification and the like as appropriate.

[0035] In this specification, etc., "electronic equipment" refers to any device having a power storage device. An electro-optical device having a power storage device, an information terminal device having a power storage device, etc. are all electronic equipment.

[0036] Note that in this specification, etc., "power storage device" refers to all elements and devices that have a power storage function, including, for example, power storage devices such as lithium ion batteries (also called "secondary batteries"), lithium ion capacitors, and electric double layer capacitors.

[0037] In addition, in this specification, etc., the space group is represented by the short notation of the international symbol (or Hermann-Mauguin symbol). In addition, the Miller index is used to represent the crystal plane and the crystal direction. In crystallography, the space group, crystal plane and crystal direction are represented by a superscript horizontal bar to the number. Each face representing the crystal plane is represented by "()". (minus sign) is used to represent the space group, crystal plane and crystal direction, instead of attaching a superscript horizontal bar to the number. In addition, "[]" is used to represent the individual orientation of the orientation within the crystal, "<>" is used to represent the collective orientation of all equivalent orientations, "()" is used to represent the individual face of the crystal plane, and "{}" is used to represent the collective face with equivalent symmetry. In addition, in general, in order to facilitate the understanding of the structure, the trigonal system represented by the space group R-3m is represented by a compound hexagonal lattice of the hexagonal lattice. In this specification, etc., unless otherwise specified, the space group R-3m is also represented by a compound hexagonal lattice. In addition to (hkl), (hkil) is sometimes used as the Miller index. Here, i is -(h+k).

[0038] In addition, h, k, i, and l may represent any integer greater than 1. For example, (001) includes (001), (003), and (006).

[0039] In addition, the space group of the crystal structure is identified by XRD, electron diffraction, neutron diffraction, etc. Therefore, in this specification, etc., belonging to a certain space group or a space group means being identified as a certain space group.

[0040] In this specification, etc., the theoretical capacity of the positive electrode active material refers to the amount of electricity when all the lithium that can be inserted and separated in the positive electrode active material is separated. For example, the theoretical capacity of LiCoO2 is 274mAh / g, the theoretical capacity of LiNiO2 is 275mAh / g, and the theoretical capacity of LiMn2O4 is 148mAh / g.

[0041] In addition, x in the composition formula can be, for example, Li x x in CoO2 (Li occupancy rate at lithium position) represents the amount of lithium remaining in the positive electrode active material that can be inserted and removed. In the case of the positive electrode active material in a secondary battery, x = (theoretical capacity - charging capacity) / theoretical capacity. For example, when a secondary battery using LiCoO2 as the positive electrode active material is charged to 219.2 mAh / g, it can be said that Li 0.2 CoO2 or x = 0.2. Li x The state where x in CoO2 is small is, for example, x≤0.24. When considering the actual range when used as a positive electrode active material for a secondary battery, for example, it is 0.1 <x≤0.24。

[0042] When lithium cobalt oxide roughly satisfies the stoichiometric ratio, it is LiCoO2 and x=1. In addition, the lithium cobalt oxide in the secondary battery at the end of discharge can also be said to be LiCoO2 and x=1. In addition, in general, the discharge voltage of a lithium-ion battery using LiCoO2 drops sharply before reaching 2.5V. Therefore, in this specification, for example, a state in which a voltage of 2.5V (the electrode is lithium) is reached at a current of less than 100mA / g is regarded as a state in which discharge is completed, and x=1. Therefore, in order to obtain lithium cobalt oxide when x=0.2, for example, charging of 219.2mAh / g is sufficient from the state in which discharge is completed.

[0043] To calculate Li x The charge capacity and / or discharge capacity of x in CoO2 is preferably measured under conditions without or with little effect of short circuit and / or electrolyte decomposition. For example, data of a secondary battery in which a sharp change in voltage that may be a short circuit occurs is preferably not used for the calculation of x.

[0044] In addition, when the configuration of anions is roughly close to cubic closest packing, it can be regarded as cubic closest packing. The anion configuration of cubic closest packing refers to the following state: the anions of the second layer are configured on the gaps of the anions filled in the first layer, and the anions of the third layer are configured just on the gaps of the anions of the second layer and not just on the anions of the first layer. Therefore, the anions may not be strictly cubic lattices. In addition, in fact, crystallization has defects, so the analysis result may not be based on theory. For example, spots may also occur on a position slightly different from the theoretical position in the fast Fourier transform (FFT) pattern of an electron diffraction pattern or a transmission electron microscope (TEM) image, etc. For example, it can be said that there is a cubic closest packing structure when the difference in orientation between the theoretical position is less than 5 degrees or less than 2.5 degrees.

[0045] In addition, in this specification, etc., "a layered rock salt type crystal structure of a composite oxide containing lithium and a transition metal" refers to a crystal structure having a rock salt type ion arrangement in which cations and anions are alternately arranged, and transition metals and lithium are regularly arranged to form a two-dimensional plane, so that lithium can diffuse in two dimensions. In addition, defects such as vacancies of cations or anions may also be included. Strictly speaking, a layered rock salt type crystal structure is sometimes a structure formed by deformation of the lattice of a rock salt type crystal.

[0046] In this specification, etc., "rock salt type crystal structure" refers to a structure in which cations and anions are arranged alternately. In addition, vacancies of cations or anions may also be included.

[0047] In this specification, "homogeneous" refers to a phenomenon in which a certain element (e.g., A) in a solid containing multiple elements (e.g., A, B, C) has the same characteristics and is distributed in a specific region. Specifically, the element concentrations between specific regions can be substantially the same. For example, the difference in element concentrations in specific regions is within 10%. The specific region can be, for example, a surface portion, a surface, a convex portion, a concave portion, an interior, etc.

[0048] In this specification, "segregation" refers to a phenomenon in which a certain element (e.g., B) is spatially non-uniformly distributed in a solid containing multiple elements (e.g., A, B, C). Alternatively, it means that the concentration of a certain element is different from the concentration of other elements. Segregation is synonymous with uneven distribution, precipitation, unevenness, deviation, and mixing of high-concentration areas or low-concentration areas.

[0049] In this specification, etc., the "surface part" of a particle of an active material, etc., for example, refers to an area within 50nm from the surface to the inside, more preferably within 35nm, further preferably within 20nm, and most preferably within 10nm. In addition, the surface caused by a crack or a crack can be regarded as a surface. In addition, in this specification, etc., an area deeper than the surface part is sometimes referred to as "inside". In addition, in this specification, etc., "grain boundary" refers to, for example, the following parts: the part where the particles are bonded together; the part where the crystal orientation changes inside the particle (including the central part); the part containing more defects; the part with a disordered crystal structure; etc. In addition, the grain boundary can also be said to be a kind of surface defect. In addition, "near the grain boundary" refers to an area within 20nm, preferably within 10nm from the grain boundary. In this specification, etc., "particles" are not limited to spheres (circular in cross section), and the cross-sectional shape of each particle may also be an ellipse, a rectangle, a trapezoid, a triangle, a quadrilateral with an arc at the corner, an asymmetric shape, etc., and each particle may also be amorphous.

[0050] In addition, when describing the characteristics of a single particle of a positive electrode active material in the following embodiments, it is not necessary for all particles to have the characteristics. For example, as long as 50% or more, preferably 70% or more, and more preferably 90% or more of three or more positive electrode active material particles selected irregularly have the characteristics, it can be said that the characteristics of the positive electrode active material and the secondary battery including the positive electrode active material are fully improved.

[0051] (Implementation Method 1) In this embodiment, a lithium ion battery having good charging and discharging characteristics even in a low temperature environment will be described.

[0052] [Lithium-ion battery] A lithium ion battery according to one embodiment of the present invention includes a positive electrode, a negative electrode, and an electrolyte. When the electrolyte includes an electrolyte solution, a separator is included between the positive electrode and the negative electrode. In addition, an outer packaging body covering at least a portion of the periphery of the positive electrode, the negative electrode, and the electrolyte may also be included.

[0053] In this embodiment, the structure of the lithium-ion battery is focused on for description, and this structure is required for realizing a lithium-ion battery having good discharge characteristics even in a low temperature environment (e.g., below 0°C, below -10°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and most preferably below -60°C) and / or a lithium-ion battery having good charging characteristics even in a low temperature environment. Specifically, the description is centered on the positive electrode active material and the electrolyte contained in the positive electrode. In Embodiment 2, a method for manufacturing the positive electrode active material contained in the lithium-ion battery is described, and in Embodiment 3, details of other structures of a lithium-ion battery of one embodiment of the present invention are described.

[0054] Figure 1A 1 is a cross-sectional schematic diagram illustrating the internal structure of a lithium-ion battery 10. The lithium-ion battery 10 includes a positive electrode 11, a negative electrode 12, and a separator 13. The positive electrode 11 includes a positive electrode current collector 21 and a positive electrode active material layer 22 on the positive electrode current collector 21, and the negative electrode 12 includes a negative electrode current collector 31 and a negative electrode active material layer 32. As shown in the figure, the positive electrode active material layer 22 and the negative electrode active material layer 32 are opposite to each other through the separator 13. In addition, although Figure 1A Although not shown in the figure, the lithium ion battery 10 contains an electrolyte in the gaps included in the positive electrode active material layer 22 , the gaps included in the separator 13 , and the gaps included in the negative electrode active material layer 32 .

[0055] Note that although Figure 1A Although one positive electrode 11, one negative electrode 12, and one separator 13 are shown, the lithium ion battery of one embodiment of the present invention is not limited to this structure. A structure including two positive electrodes 11, two negative electrodes 12, and two separators 13 may be adopted, or two or more positive electrodes 11, two or more negative electrodes 12, and two or more separators 13 may be stacked. In addition, a winding structure may be adopted instead of using Figure 1A The laminated structure shown.

[0056] Figure 1B yes Figure 1A An enlarged view of portion A surrounded by a dotted line in FIG.

[0057] The positive electrode active material layer 22 includes a positive electrode active material 100 and a conductive material 41. Although not shown in the figure, a binder may be included in addition to the positive electrode active material 100 and the conductive material 41.

[0058] In addition, as shown in the figure, the gaps included in the positive electrode active material layer 22 are preferably filled with the electrolyte 51. For example, preferably more than 60% of the gaps included in the positive electrode active material layer 22 are filled with the electrolyte 51, more preferably more than 70% of the gaps are filled, more preferably more than 80% of the gaps are filled, more preferably more than 90% of the gaps are filled, more preferably more than 95% of the gaps are filled, and most preferably more than 99% of the gaps are filled. Note that the gaps included in the positive electrode active material layer 22 refer to the area other than the solid components (positive electrode active material, conductive material, etc.) in the positive electrode active material layer 22.

[0059] Although detailed description is omitted, similar to the description of the positive electrode active material layer 22, preferably, the voids included in the negative electrode active material layer 32 are also filled with the electrolyte 51. For example, preferably, more than 60% of the voids included in the negative electrode active material layer 32 are filled with the electrolyte 51, more preferably, more than 70% of the voids are filled, more preferably, more than 80% of the voids are filled, more preferably, more than 90% of the voids are filled, more preferably, more than 95% of the voids are filled, and most preferably, more than 99% of the voids are filled. Note that the voids included in the negative electrode active material layer 32 refer to the region other than the solid components (negative electrode active material, conductive material, etc.) in the negative electrode active material layer 32.

[0060] Thus, by filling the positive electrode active material layer 22 and the negative electrode active material layer 32 with the electrolyte 51, the area where the positive electrode active material and the negative electrode active material are in contact with the electrolyte can be expanded. That is, a lithium ion battery with good charging and discharging characteristics in a low temperature environment can be realized.

[0061] In addition, during charging in a low temperature environment, the potential barrier when lithium ions are separated from the positive electrode active material tends to become higher. That is, it can be said that the lower the temperature of the charging environment, the greater the overvoltage required to separate lithium ions from the positive electrode active material. In other words, during charging in a low temperature environment, the positive electrode active material may be exposed to a high voltage (a high potential relative to the lithium potential). In other words, during charging in a low temperature environment, the charging capacity may decrease when the positive electrode active material is not exposed to a high voltage.

[0062] Therefore, as a positive electrode active material included in a lithium ion battery having excellent charging and discharging characteristics even in a low temperature environment, it is preferable to use a positive electrode active material that can withstand a high voltage and obtain a high charge capacity during charging in a low temperature environment.

[0063] In addition, as an electrolyte contained in a lithium ion battery having excellent charging and discharging characteristics even in a low temperature environment, it is preferred to use a material that has excellent lithium ion conductivity when charging and / or discharging (charging and discharging) is performed in a low temperature environment (for example, 0°C, -10°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C, and most preferably -60°C).

[0064] A positive electrode active material and an electrolyte that are preferred as a lithium ion battery having excellent charging and discharging characteristics even in a low-temperature environment are described in detail below.

[0065] [positive electrode] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer contains a positive electrode active material and may further contain at least one of a conductive material and a binder.

[0066] <Positive Electrode Active Material> The positive electrode active material has the function of absorbing lithium ions and releasing lithium ions accompanying charging and discharging. As a positive electrode active material used in one embodiment of the present invention, a material (or a material with little resistance increase) that deteriorates less with charging and / or discharging in a low temperature environment even at a high charging voltage (hereinafter also referred to as "high charging voltage") can be used. Specifically, a positive electrode active material (composite oxide) having a particle size (to be precise, a median particle size (D50)) of 12 μm or less (preferably 10.5 μm or less, more preferably 8 μm or less) described later can be used. The positive electrode active material contains any one or more of the added element X, the added element Y and the added element Z. The added element X, the added element Y and the added element Z will be described in detail in <Containing Elements>.

[0067] When the particle size of the positive electrode active material is too small, it is sometimes difficult to carry out coating when manufacturing the positive electrode. In addition, when the particle size of the positive electrode active material is too small, the surface area may be too large and the surface of the positive electrode active material may over-react with the electrolyte. Alternatively, when the particle size of the positive electrode active material is too small, a large amount of conductive material used as a conductive path between particles needs to be mixed, which may lead to a decrease in capacity. Therefore, the particle size (median particle size (D50)) of the positive electrode active material is preferably greater than 1 μm. In addition, as the particle size of the positive electrode active material, even the smallest particle is preferably greater than 100 nm. In addition, when the particle size of the positive electrode active material is greater than the thickness of the active material layer described later, the particle density of the active material layer cannot be increased, so even the largest particle is preferably less than 50 μm in particle size.

[0068] The particle size can be measured using a particle size distribution analyzer that utilizes laser diffraction and scattering methods, etc. D50 refers to the particle size at which the cumulative amount of the particle size distribution curve accounts for 50% in the particle size distribution measurement result. The measurement of the particle size is not limited to laser diffraction type particle size distribution measurement, and the major axis of the particle cross-section can also be measured through analysis using SEM (Scanning Electron Microscope) or TEM (Transmission Electron Microscope), etc. Additionally, as a method for measuring D50 through analysis using SEM or TEM, etc., for example, more than 20 particles are measured and a cumulative particle amount curve is created, and the particle size at which the cumulative amount accounts for 50% is defined as D50.

[0069] In this specification, etc., unless otherwise specified, the "charging voltage" is expressed based on the potential of lithium metal. In this specification, etc., a "high charging voltage" refers to, for example, a charging voltage of 4.5 V or more, preferably 4.55 V or more, more preferably a high voltage charge of 4.6 V or more, 4.65 V or more, or 4.7 V or more, whereby Li x CoO2 is in a state where x is small, for example, 0.1 < x ≤ 0.24. Additionally, as long as the positive electrode active material is a material with less deterioration during charge and discharge even when using a high charging voltage, two or more materials with different particle sizes and / or compositions can be used. In this specification, etc., "different compositions" includes not only cases where the structures of the elements contained in the material are different, but also cases where although the structures of the elements contained in the material are the same, the proportions of the elements contained are different.

[0070] Note that, as described above, in this specification, etc., when the negative electrode is lithium metal as a reference, a "high charging voltage" refers to a potential of 4.5 V or more, but when the negative electrode is a carbon material (such as graphite), a potential of 4.4 V or more is referred to as a "high charging voltage". Specifically, in the case of a half-cell using lithium metal as the negative electrode, a charging voltage of 4.5 V or more is referred to as a high charging voltage, while in the case of a full-cell using a carbon material (such as graphite) as the negative electrode, a charging voltage of 4.4 V or more is referred to as a high charging voltage.

[0071] Even at a high charging voltage, by using a material that deteriorates less with charge and discharge in a low temperature environment (e.g., 0°C, -10°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C, and most preferably -60°C) as a positive electrode active material, a lithium ion battery having a large discharge capacity even at a low temperature environment can be realized. In addition, a lithium ion battery having a discharge capacity value in a low temperature environment (e.g., 0°C, -10°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C, and most preferably -60°C) that is 50% or more (preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and most preferably 90% or more) compared to the discharge capacity value at 20°C can be realized. Note that the above numerical values ​​are numerical values ​​when both charge and discharge are performed in a low temperature environment, and the measurement conditions of charge and discharge in a low temperature environment and charge and discharge at 20°C are the same except for the temperature (hereinafter sometimes referred to as "charge and discharge temperature" in this specification, etc.).

[0072] More specifically, the discharge capacity when charged and discharged at 0°C is preferably 85% or more, more preferably 90% or more, further preferably 95% or more, and further preferably 98% or more, relative to the discharge capacity when charged and discharged at 20°C. In addition, the discharge capacity when charged and discharged at -10°C is preferably 80% or more, more preferably 85% or more, further preferably 90% or more, and further preferably 95% or more, relative to the discharge capacity when charged and discharged at 20°C. In addition, the discharge capacity when charged and discharged at -20°C is preferably 75% or more, more preferably 80% or more, further preferably 85% or more, and further preferably 90% or more, relative to the discharge capacity when charged and discharged at 20°C. In addition, the discharge capacity when charged and discharged at -30°C is preferably 70% or more, more preferably 75% or more, further preferably 80% or more, and further preferably 85% or more, relative to the discharge capacity when charged and discharged at 20°C. In addition, the discharge capacity when charged and discharged at -40°C is preferably 60% or more, more preferably 65% ​​or more, further preferably 70% or more, and further preferably 75% or more relative to the discharge capacity when charged and discharged at 20°C. In addition, as the above-mentioned discharge condition, for example, discharge can be performed at a current rate of 0.1C (note, 1C = 200mA / g).

[0073] In addition, a lithium ion battery having a large discharge energy density under a low temperature environment (e.g., 0°C, -10°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C, and most preferably -60°C) can be realized. In addition, a lithium ion battery having a discharge energy density value under a low temperature environment (e.g., 0°C, -10°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C, and most preferably -60°C) of 50% or more (preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and most preferably 90% or more) compared to the discharge energy density value at 20°C can be realized. In addition, the charging and discharging under the low temperature environment are the same as the charging and discharging under 20°C except for the temperature.

[0074] The temperature during charging or discharging described in this specification and the like refers to the temperature of the lithium-ion battery. In the measurement of battery characteristics at various temperatures, for example, the following method can be used for measurement: a thermostatic bath that is stable at a desired temperature is used, and after the battery to be measured (e.g., a test battery or a half-cell) is placed in the thermostatic bath, the measurement is started after a sufficient time (e.g., more than 1 hour) has passed until the temperature of the test battery becomes the same as the temperature of the thermostatic bath, but the method is not limited thereto.

[0075] 2 and 3 , a description will be given of a positive electrode active material 100 that is less degraded by repeated charge and discharge at a high charge voltage.

[0076] Figure 2A and Figure 2B This is a cross-sectional view of a positive electrode active material 100 according to one embodiment of the present invention. FIG. 3A to FIG. 3C Show enlarged Figure 2B The figure near AB in . In addition, Figures 3D to 3F Show enlarged Figure 2B Figure near the CD in .

[0077] like Figure 2A As shown, the positive electrode active material 100 includes a surface portion 100a and an inner portion 100b. In the above drawings, the boundary between the surface portion 100a and the inner portion 100b is indicated by a dotted line.

[0078] The surface portion 100a of the positive electrode active material 100 refers to, for example, within 50nm from the surface to the inside, preferably within 35nm from the surface to the inside, more preferably within 20nm from the surface to the inside, and most preferably within 10nm from the surface in a vertical or approximately vertical direction to the inside. Approximately vertical means 80° or more and 100° or less. The surface generated by cracks and / or fissures can also be referred to as the surface. The surface portion 100a is synonymous with the vicinity of the surface, the area near the surface, or the shell.

[0079] In addition, a region deeper than the surface layer portion 100a in the positive electrode active material is referred to as an inner portion 100b. The inner portion 100b is synonymous with an inner region or a core.

[0080] In addition, when the positive electrode active material 100 has a layered rock salt type crystal structure of the space group R-3m, as Figure 2B As shown, the surface layer portion 100a includes an end region 100a1 and a base region 100a2. Figure 2A and Figure 2B , the straight line with (001) represents the (001) plane. Here, the end region 100a1 has a surface exposed in a direction intersecting the (001) plane, and the region within 50 nm from the surface to the inside, more preferably within 35 nm from the surface to the inside, further preferably within 20 nm from the surface to the inside, and most preferably within 10 nm vertically or substantially vertically from the surface to the inside is called the end region 100a1. Note that here, "intersection" means that the angle formed by the perpendicular line of the first plane ((001) plane and the normal line of the second plane (the surface of the positive electrode active material 100) is greater than 10 degrees and less than 90 degrees, and more preferably greater than 30 degrees and less than 90 degrees.

[0081] In addition, the base region 100a2 has a surface parallel to the (001) plane, and the area within 50 nm from the surface to the inside, more preferably within 35 nm from the surface to the inside, further preferably within 20 nm from the surface to the inside, and most preferably within 10 nm from the surface to the inside is called the base region 100a2. Note that here, "parallel" means that the angle formed by the perpendicular line of the first surface ((001) plane) and the normal line of the second surface (the surface of the positive electrode active material 100) is greater than 0 degrees and less than 10 degrees, preferably greater than 0 degrees and less than 5 degrees, and more preferably greater than 0 degrees and less than 2.5 degrees.

[0082] In addition, the surface of the positive electrode active material 100 refers to the surface of the composite oxide including the surface layer 100a and the inner part 100b. Therefore, the positive electrode active material 100 does not include: a material attached with a metal oxide such as aluminum oxide (Al2O3) that does not contain a lithium position that contributes to charging and discharging; carbonates, hydroxyl groups, etc. that are chemically adsorbed after the positive electrode active material is manufactured. In addition, the attached metal oxide refers to, for example, a metal oxide whose crystal orientation is different from the crystal structure of the inner part 100b.

[0083] TEM (Transmission Electron Microscope: Transmission Electron Microscope) images, STEM (Scanning Transmission Electron Microscope: Scanning Transmission Electron Microscope) images, HAADF-STEM (High-angle Annular Dark Field Scanning TEM: High-angle annular dark field) images, ABF-STEM (Annular Bright-Field Scanning Transmission Electron Microscope: Annular Bright Field Scanning Transmission Electron Microscope) images, electron diffraction patterns, etc. can be used to determine whether the crystal orientation of the two regions is roughly the same. In addition, it can also be determined by the FFT pattern of the TEM image and the FFT pattern of the STEM image. In addition, X-ray diffraction (XRD: X-ray Diffraction), neutron diffraction, etc. can be used as a basis for judgment.

[0084] In addition, the electrolyte adhering to the positive electrode active material 100 , decomposed products of the electrolyte, the organic solvent, the binder, the conductive agent, or compounds derived from these are also not included.

[0085] The positive electrode active material 100 is a compound containing transition metals and oxygen into which lithium can be inserted and removed, so the interface between the region where there is a transition metal M (e.g., Co, Ni, Mn, Fe, etc.) and oxygen that is oxidized and reduced with the insertion and removal of lithium and the region where there is no transition metal M and oxygen is called the surface of the positive electrode active material. In addition, the surface generated by sliding and / or cracks may also be referred to as the surface of the positive electrode active material. When analyzing the positive electrode active material, the surface is sometimes covered with a protective film, but the protective film is not included in the positive electrode active material. As a protective film, a single layer or multilayer film of carbon, metal, oxide, resin, etc. is sometimes used.

[0086] <Contains elements> The positive electrode active material 100 includes lithium, cobalt, oxygen, and an additive element. Alternatively, the positive electrode active material 100 may include lithium cobalt oxide (LiCoO2) to which the additive element is added. Note that the positive electrode active material 100 of one embodiment of the present invention may have a crystal structure described later. Therefore, the composition of lithium cobalt oxide is not strictly limited to Li:Co:O=1:1:2.

[0087] In order to keep the charge neutral during the insertion and removal of lithium ions, the positive electrode active material of the lithium ion secondary battery preferably contains a transition metal that can be oxidized and reduced. Preferably, the positive electrode active material 100 of one embodiment of the present invention mainly uses cobalt as a transition metal for redox reaction. In addition to cobalt, one or two selected from nickel and manganese can also be used. Among the transition metals contained in the positive electrode active material 100, cobalt preferably accounts for more than 75 atomic%, preferably more than 90 atomic%, and more preferably more than 95 atomic%. At this time, there are many advantages such as: it can be synthesized more easily: easy to handle: has good cycle characteristics; etc.

[0088] In addition, compared with composite oxides such as lithium nickelate (LiNiO2) in which nickel accounts for more than half of the transition metal, when cobalt accounts for more than 75 atomic%, preferably more than 90 atomic%, and more preferably more than 95 atomic% of the transition metal in the positive electrode active material 100, Li x The smaller the x in CoO2, the better the stability. This is because cobalt is less affected by the distortion caused by the Jan-Taylor effect than nickel. The strength of the Jan-Taylor effect in transition metal compounds varies according to the number of electrons in the d orbital of the transition metal. Layered rock salt-type composite oxides such as lithium nickelate, in which octahedrally coordinated low-spin nickel (III) accounts for more than half of the transition metal, are greatly affected by the Jan-Taylor effect, and the layers composed of nickel and oxygen octahedra are prone to distortion. Therefore, concerns about the collapse of the crystal structure during the charge and discharge cycle increase. In addition, nickel ions are larger than cobalt ions and are close to the size of lithium ions. Therefore, in layered rock salt-type composite oxides such as lithium nickelate, in which nickel accounts for more than half of the transition metal, there is a problem of easy mixing of nickel and lithium cations.

[0089] As the additive element contained in the positive electrode active material 100, one or more selected from magnesium, fluorine, nickel, aluminum, titanium, zirconium, vanadium, iron, manganese, chromium, niobium, arsenic, zinc, silicon, sulfur, phosphorus, boron, barium, bromine and beryllium are preferably used. In addition, the sum of transition metals in the additive element is preferably less than 25 atomic%, more preferably less than 10 atomic%, and further preferably less than 5 atomic%.

[0090] That is to say, as the positive electrode active material 100, any one or more of lithium cobalt oxide containing magnesium, lithium cobalt oxide containing magnesium and aluminum, lithium cobalt oxide containing magnesium, aluminum and titanium, lithium cobalt oxide containing magnesium and nickel, lithium cobalt oxide containing magnesium, aluminum and nickel, lithium cobalt oxide containing magnesium and fluorine, lithium cobalt oxide containing magnesium, fluorine and titanium, lithium cobalt oxide containing magnesium, fluorine and aluminum, lithium cobalt oxide containing magnesium, fluorine, titanium and aluminum, lithium cobalt oxide containing magnesium, fluorine and nickel, and lithium cobalt oxide containing magnesium, fluorine, nickel and aluminum can be used.

[0091] In addition, it can also be said that any one or more of a positive electrode active material comprising cobalt, oxygen and magnesium, a positive electrode active material comprising cobalt, oxygen, magnesium and aluminum, a positive electrode active material comprising cobalt, oxygen, magnesium, aluminum and titanium, a positive electrode active material comprising cobalt, oxygen, magnesium and nickel, a positive electrode active material comprising cobalt, oxygen, magnesium, aluminum and nickel, a positive electrode active material comprising cobalt, oxygen, magnesium, aluminum and nickel, a positive electrode active material comprising cobalt, oxygen, magnesium and fluorine, a positive electrode active material comprising cobalt, oxygen, magnesium, fluorine and titanium, a positive electrode active material comprising cobalt, oxygen, magnesium, fluorine and aluminum, a positive electrode active material comprising cobalt, oxygen, magnesium, fluorine, titanium and aluminum, a positive electrode active material comprising cobalt, oxygen, magnesium, fluorine and nickel, and a positive electrode active material comprising cobalt, oxygen, magnesium, fluorine, nickel and aluminum can be used as the positive electrode active material 100 for lithium ion batteries.

[0092] The additive element is preferably dissolved in the positive electrode active material 100. For example, in STEM-EDX line analysis, the depth at which the amount of the additive element increases is preferably deeper than the depth at which the amount of the transition metal M increases, that is, inside the positive electrode active material 100.

[0093] As described below, the above-mentioned added element further stabilizes the crystal structure of the positive electrode active material 100. Note that in this specification and the like, the added element is synonymous with a mixture or a part of a raw material.

[0094] As the additive element, it is not necessary to contain magnesium, fluorine, nickel, aluminum, titanium, zirconium, vanadium, iron, manganese, chromium, niobium, arsenic, zinc, silicon, sulfur, phosphorus, boron, barium, bromine or beryllium.

[0095] For example, by manufacturing a positive electrode active material 100 that does not substantially contain manganese, the above advantages such as easier synthesis, easier handling, and good cycle characteristics can be improved. The weight of manganese contained in the positive electrode active material 100 is preferably 600 ppm or less, and more preferably 100 ppm or less.

[0096] The surface part 100a is the area where lithium ions are first separated during charging, and is also the area where the lithium concentration is likely to be lower than that of the inner part 100b. In addition, it can also be said that some of the bonds in the atoms on the surface of the particles of the positive electrode active material 100 contained in the surface part 100a are cut. Therefore, the surface part 100a is likely to become unstable and the crystal structure is likely to deteriorate. On the other hand, as long as the surface part 100a can be sufficiently stabilized, the Li x When x in CoO2 is small, for example, when x is 0.24 or less, the layered structure composed of cobalt and oxygen octahedra in the inner 100b can be prevented from being easily collapsed. Furthermore, the deviation of the layer composed of cobalt and oxygen octahedra in the inner 100b can be suppressed.

[0097] In order to make the surface part 100a have a stable composition and crystal structure, the surface part 100a preferably contains an added element, and more preferably contains a plurality of added elements. In addition, the concentration of one or more of the added elements selected from the surface part 100a is preferably higher than that of the inner part 100b. In addition, one or more of the added elements selected from the positive electrode active material 100 preferably have a concentration gradient. In addition, it is more preferred that the distribution of the added elements in the positive electrode active material 100 is different. For example, it is more preferred that the depth of the added element concentration peak from the surface is different. Here, the concentration peak refers to the maximum value of the concentration in the surface part 100a or the range below 50nm from the surface.

[0098] Describe the distribution of added elements. FIG. 3A to FIG. 3C Is magnification Figure 2B The figure near AB in FIG. 1 is a figure for explaining the end region 100a1 of the positive electrode active material 100. Figures 3D to 3F Is magnification Figure 2B The diagram near CD in FIG. 1 is a diagram for explaining the base region 100 a 2 of the positive electrode active material 100 .

[0099] For example, Figure 3A and Figure 3D In the example shown in the figure, some of the additive elements such as magnesium, fluorine, titanium, silicon, phosphorus, boron, calcium, etc. preferably have a concentration gradient increasing from the inner part 100b to the surface. The additive element having such a concentration gradient is called additive element X.

[0100] like Figure 3B and Figure 3E It is preferably indicated by shading that other added elements such as aluminum, manganese, etc. have a concentration gradient and are in the ratio Figure 3A and Figure 3D The deeper region of the additive element X shown has a concentration peak. The concentration peak may exist in the surface portion 100a or in a region deeper than the surface portion 100a. For example, it is preferred that a region of 5 nm or more and 30 nm or less from the surface to the inside has a peak. The additive element having such a concentration gradient is referred to as additive element Y.

[0101] like Figure 3C and Figure 3F In the figure, as shown by the presence or absence of shadows and the concentration of shadows, sometimes other added elements such as nickel and barium are clearly present in the end region 100a1, but are not actually present in the base region 100a2. Note that here, "clearly present" means that the characteristic X-ray energy spectrum of the element is detected in the cross-sectional STEM-EDX analysis of the positive electrode active material 100.

[0102] In addition, "substantially absent" means that the characteristic X-ray spectrum of the element cannot be detected in the cross-sectional STEM-EDX analysis of the positive electrode active material 100. In this case, it is also referred to as the element being below the detection limit in the STEM-EDX analysis. The added element having the above distribution is referred to as the added element Z.

[0103] Magnesium, which is one of the added elements X, is divalent. In the layered rock salt type crystal structure, magnesium ions are more stable in the lithium position than in the cobalt position in the layered rock salt type crystal structure, and thus easily enter the lithium position. When magnesium is present at an appropriate concentration at the lithium position of the surface portion 100a, the layered rock salt type crystal structure can be easily maintained. This is because magnesium present at the lithium position is used as a support between the CoO2 layers. In addition, when magnesium is present, for example, in the Li x When x in CoO2 is 0.24 or less, the oxygen around magnesium can be suppressed from being released. In addition, it can be expected that the density of the positive electrode active material 100 is improved when magnesium is present. In addition, when the magnesium concentration of the surface portion 100a is high, it can be expected that the corrosion resistance to hydrofluoric acid generated by the decomposition of the electrolyte can be improved.

[0104] If magnesium has an appropriate concentration, it has no negative effect on the insertion and removal of lithium accompanying charge and discharge, so the above advantages can be obtained. However, excess magnesium may have a negative effect on the insertion and removal of lithium. In addition, the effect of contributing to the stabilization of the crystal structure is sometimes reduced. This is because magnesium not only enters the lithium position but also the cobalt position. In addition, there is also the following concern: excessive magnesium compounds (for example, oxides or fluorides, etc.) that are not substituted at the lithium position or the cobalt position are segregated on the surface of the positive electrode active material and become the resistance component of the secondary battery. In addition, the increase in the magnesium concentration of the positive electrode active material sometimes reduces the discharge capacity of the positive electrode active material. This is because the excess magnesium enters the lithium position and the amount of lithium contributing to charge and discharge is reduced.

[0105] Therefore, it is preferred that an appropriate amount of magnesium is included in the positive electrode active material 100 as a whole. For example, the number of magnesium atoms is preferably greater than 0.001 times and less than 0.1 times the number of cobalt atoms, more preferably greater than 0.01 times and less than 0.04 times, and further preferably about 0.02 times. Here, the amount of magnesium in the positive electrode active material 100 as a whole can be, for example, a value obtained by analyzing all elements of the positive electrode active material 100 using GD-MS, ICP-MS, etc., or a value based on the coordination value of the raw materials in the manufacturing process of the positive electrode active material 100.

[0106] In addition, aluminum, one of the added elements Y, may exist in the cobalt position in the layered rock salt type crystal structure. Aluminum is a typical trivalent element and its valence does not change, so the lithium around aluminum is not easy to move during charge and discharge. Therefore, aluminum and the lithium around it are used as pillars to suppress changes in the crystal structure. In addition, aluminum has the effect of suppressing the dissolution of surrounding cobalt and improving continuous charging tolerance. In addition, the Al-O bond is stronger than the Co-O bond, so the oxygen around aluminum can be suppressed from detaching. Through the above effects, thermal stability is improved. Therefore, when aluminum is included as an added element, the safety of the positive electrode active material 100 when used in a secondary battery can be improved. In addition, a positive electrode active material 100 that is not prone to crystal structure collapse even after repeated charge and discharge can be achieved.

[0107] On the other hand, when the amount of aluminum is too large, there is a possibility that the insertion and extraction of lithium may be adversely affected.

[0108] Therefore, it is preferred that an appropriate amount of aluminum is included in the positive electrode active material 100 as a whole. For example, the number of aluminum atoms in the positive electrode active material 100 as a whole is preferably greater than 0.05% and less than 4% of the number of cobalt atoms, more preferably greater than 0.1% and less than 2%, and further preferably greater than 0.3% and less than 1.5%. Alternatively, it is preferably greater than 0.05% and less than 2%. Alternatively, it is preferably greater than 0.1% and less than 4%. The amount in the positive electrode active material 100 as a whole shown here can be, for example, a value obtained by elemental analysis of the positive electrode active material 100 as a whole using GD-MS, ICP-MS, etc., or a value obtained based on the mixing of raw materials in the manufacturing process of the positive electrode active material 100.

[0109] In addition, nickel, which is one of the added elements Z, may be present at the cobalt site or the lithium site. When nickel is present at the cobalt site, the redox potential is lower than that of cobalt, and the discharge capacity is increased, which is preferable.

[0110] In addition, when nickel is present at the lithium position, the deviation of the layered structure composed of octahedrons of cobalt and oxygen is suppressed. In addition, the volume change caused by charging and discharging is also suppressed. In addition, the elastic modulus is improved, that is, it becomes hard. This is because the nickel present at the lithium position is also used as a support between the CoO2 layers. Therefore, it can be expected that the crystal structure is more stable, especially when charged at a high temperature of 45°C or above, so it is preferred.

[0111] On the other hand, when the amount of nickel is too large, the influence of distortion due to the Jan-Teller effect increases, which is not preferable. In addition, when the amount of nickel is too large, it may have a negative impact on the insertion and extraction of lithium.

[0112] Therefore, it is preferred that an appropriate amount of nickel is included in the positive electrode active material 100 as a whole. For example, the number of nickel atoms contained in the positive electrode active material 100 is preferably greater than 0% of the number of cobalt atoms and less than 7.5%, more preferably greater than 0.05% and less than 4%, further preferably greater than 0.1% and less than 2%, and further preferably greater than 0.2% and less than 1%. Alternatively, it is preferably greater than 0% and less than 4%. Alternatively, it is preferably greater than 0% and less than 2%. Alternatively, it is preferably greater than 0.05% and less than 7.5%. Alternatively, it is preferably greater than 0.05% and less than 2%. Alternatively, it is preferably greater than 0.1% and less than 7.5%. Alternatively, it is preferably greater than 0.1% and less than 4%. The amount of nickel shown here can be, for example, a value obtained by elemental analysis of the positive electrode active material as a whole using GD-MS, ICP-MS, etc., or a value obtained by mixing raw materials in the manufacturing process of the positive electrode active material.

[0113] In addition, fluorine, one of the added elements X, is a monovalent anion, and when part of the oxygen in the surface portion 100a is replaced by fluorine, the lithium detachment energy is reduced. This is because the valence change of the cobalt ion accompanying the detachment of lithium varies according to the presence or absence of fluorine, for example, from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine, and the redox potential is different. Therefore, when part of the oxygen in the surface portion 100a of the positive electrode active material 100 is replaced by fluorine, it can be said that the detachment and insertion of lithium ions near fluorine occur smoothly. Therefore, when the positive electrode active material 100 is used in a secondary battery, the charge and discharge characteristics, high current characteristics, etc. can be improved. In addition, by having fluorine in the surface portion 100a of the surface including the portion in contact with the electrolyte, the corrosion resistance to hydrofluoric acid can be effectively improved. In addition, as shown in the following embodiment, when the melting point of fluorides such as lithium fluoride is lower than the melting point of other added element sources, it can be used as a flux (also known as a solubility aid) to reduce the melting point of other added element sources.

[0114] In addition, it is known that titanium oxide, one of the added elements X, has super hydrophilicity. Therefore, by manufacturing the positive electrode active material 100 containing titanium oxide in the surface layer 100a, it sometimes has good wettability to solvents with high polarity. When manufacturing a secondary battery, the positive electrode active material 100 has good contact with the interface of the electrolyte with high polarity, and sometimes the increase of internal resistance can be suppressed.

[0115] In addition, if Figure 3A and Figure 3C As shown, when the surface layer 100a contains both magnesium and nickel, it is possible that divalent nickel exists more stably near divalent magnesium. x When x in CoO 2 is small, the dissolution of magnesium is also suppressed. Thus, magnesium and nickel contribute to the stabilization of the surface layer portion 100 a.

[0116] In addition, when different additive elements such as additive element X, additive element Y and additive element Z are simultaneously included, the crystal structure of a wider area can be stabilized, so it is preferred. For example, when the positive electrode active material 100 simultaneously includes magnesium, one of the additive elements X, aluminum, one of the additive elements Y, and nickel, the crystal structure of a wider area can be stabilized compared to the case where only one or two of the additive elements X, Y and Z are included. In this way, when the positive electrode active material 100 simultaneously includes additive elements X, Y and Z, additive elements X such as magnesium and additive elements Z such as nickel can fully stabilize the surface, so additive elements Y such as aluminum are not required on the surface. On the contrary, aluminum is preferably widely distributed in a deeper area. Aluminum is preferably detected continuously in an area with a depth of more than 1nm and less than 25nm from the surface. In an area widely distributed in a depth of more than 0nm and less than 50nm from the surface, preferably in an area with a depth of more than 1nm and less than 50nm from the surface, the crystal structure of a wider area can be stabilized, so it is preferred.

[0117] In addition, if Figure 3C and Figure 3F As shown, when a large amount of the additive element Z is included in the end region 100a1 (also referred to as preferential inclusion, selective inclusion, etc.), the stability of the crystal structure of the end region 100a1 of the positive electrode active material 100 is improved when lithium ions enter and exit during charging and discharging of the lithium ion battery. Therefore, it is preferred. In addition, when the additive element Z has the above distribution, for example, when the positive electrode active material 100 is lithium cobalt oxide, the effects of the decrease in discharge voltage or the decrease in discharge capacity caused by the addition of the additive element Z can be suppressed as much as possible, so it is preferred.

[0118] When multiple additive elements are included as described above, each additive element plays a synergistic role and contributes to further stabilization of the surface portion 100a. In particular, when magnesium, nickel and aluminum are included, the effect of achieving a stable composition and crystal structure is high, so it is preferred. Among them, in the surface portion 100a of the positive electrode active material 100, it is preferred to have a region where magnesium is distributed closer to the surface than aluminum. In addition, it is most preferred that, in addition to the above-mentioned magnesium and aluminum distribution areas, there is also an area where nickel distribution and magnesium distribution overlap in the end area 100a1 in the surface portion 100a of the positive electrode active material 100.

[0119] <Crystal Structure> <Li x When x in CoO2 is 1> Preferably, the positive electrode active material 100 of one embodiment of the present invention is in a discharged state, that is, in a Li xWhen x=1 in CoO2, it has a layered rock salt type crystal structure belonging to the space group R-3m. The layered rock salt type composite oxide has a high discharge capacity and a two-dimensional diffusion path for lithium ions, which is suitable for the insertion / extraction reaction of lithium ions and is excellent as a positive electrode active material for secondary batteries. Therefore, the inner part 100b, which occupies most of the volume of the positive electrode active material 100, preferably has a layered rock salt type crystal structure.

[0120] On the other hand, the surface portion 100a of the positive electrode active material 100 of one embodiment of the present invention preferably strengthens the layered structure composed of the octahedron of the transition metal M and oxygen in the interior 100b to prevent the layered structure from collapsing even if lithium is separated from the positive electrode active material 100 due to charging. Alternatively, the surface portion 100a is preferably used as a barrier film of the positive electrode active material 100. Alternatively, the surface portion 100a of the outer peripheral portion of the positive electrode active material 100 preferably strengthens the positive electrode active material 100. Here, strengthening refers to suppressing the structural changes of the surface portion 100a and the interior 100b of the positive electrode active material 100 such as the separation of oxygen and / or suppressing the oxidative decomposition of the electrolyte on the surface of the positive electrode active material 100.

[0121] Therefore, the surface portion 100a preferably has a crystal structure different from that of the interior 100b. In addition, the composition and crystal structure of the surface portion 100a at room temperature (25°C) are preferably more stable than those of the interior 100b. For example, at least a portion of the surface portion 100a of the positive electrode active material 100 of one embodiment of the present invention preferably has a rock salt type crystal structure. Alternatively, the surface portion 100a preferably has both a layered rock salt type crystal structure and a rock salt type crystal structure. Alternatively, the surface portion 100a preferably has the characteristics of both a layered rock salt type and a rock salt type crystal structure.

[0122] In addition, the concentration of a part of the added element A, especially magnesium, nickel and aluminum in the surface part 100a is preferably higher than the concentration in the inner part 100b, but they are preferably also present irregularly and in small amounts in the inner part 100b. When magnesium and aluminum are present in the lithium position of the inner part 100b at an appropriate concentration, it has the effect of easily maintaining the layered rock salt type crystal structure as described above. In addition, when nickel is present in the inner part 100b at an appropriate concentration, the deviation of the layered structure composed of the octahedron of the transition metal M and oxygen is suppressed as described above. In addition, in the case of simultaneously containing magnesium and nickel, divalent magnesium is also likely to be more stably present near divalent nickel, so a synergistic effect of suppressing the dissolution of magnesium can be expected.

[0123] In addition, it is preferable that the crystal structure changes continuously from the inner portion 100 b toward the surface due to the concentration gradient of the added element A. Alternatively, it is preferable that the crystal orientations of the surface portion 100 a and the inner portion 100 b are substantially identical.

[0124] For example, it is preferred that the crystal structure changes continuously from the inner part 100b of the layered rock salt type to the surface and the surface layer part 100a of the rock salt type or having both characteristics of the rock salt type and the layered rock salt type. Alternatively, it is preferred that the crystal orientation of the surface layer part 100a of the rock salt type or having both characteristics of the rock salt type and the layered rock salt type is roughly consistent with that of the inner part 100b of the layered rock salt type.

[0125] In addition, in this specification, etc., the layered rock salt type crystal structure belonging to the space group R-3m possessed by the composite oxide containing transition metal M such as lithium and cobalt refers to the following crystal structure: a rock salt type ion arrangement having alternating arrangements of cations and anions, and transition metal M and lithium are regularly arranged to form a two-dimensional plane, so that lithium can diffuse in two dimensions. In addition, defects such as vacancies of cations or anions may also be included. Strictly speaking, the layered rock salt type crystal structure is sometimes a structure formed by deformation of the lattice of rock salt type crystals.

[0126] In addition, the rock salt type crystal structure has a cubic crystal structure such as space group Fm-3m, in which cations and anions are arranged alternately. In addition, vacancies of cations or anions may also be included.

[0127] In addition, it can be determined whether the crystal has the characteristics of both the layered rock salt type crystal structure and the rock salt type crystal structure by electron diffraction, TEM images, cross-sectional STEM images, and the like.

[0128] There is no difference in the position of cations in the rock salt type crystal structure, but in the layered rock salt type crystal structure, there are two types of cation positions, one is the position where lithium occupies most of the position and the other is the position where the transition metal M occupies. Both the rock salt type and the layered rock salt type have a stacked structure in which the two-dimensional planes of cations and the two-dimensional planes of anions are arranged alternately. In the bright spots of the electron diffraction image of the crystal plane forming the above-mentioned two-dimensional plane, when the central spot (transmitted spot) is taken as the origin 000, the bright spot closest to the central spot is, for example: the bright spot of the (111) plane of the ideal rock salt type crystal structure or the bright spot of the (003) plane of the ideal layered rock salt type crystal structure. For example, when comparing the electron diffraction images of rock salt type MgO and layered rock salt type LiCoO2, the bright spot of the (003) plane of LiCoO2 is observed at a distance of about half the distance of the bright spot of the (111) plane of MgO. Therefore, for example, when the analysis area includes two phases of rock salt type MgO and layered rock salt type LiCoO2, there are plane orientations in which bright spots of stronger brightness and bright spots of weaker brightness are arranged alternately in the electron diffraction image. Bright spots common to the rock salt type and the layered rock salt type have high brightness, while bright spots occurring only in the layered rock salt type have low brightness.

[0129] In addition, in a cross-sectional STEM image or the like, when observing a layered rock-salt type crystal structure from a direction perpendicular to the c-axis, layers with higher brightness and layers with lower brightness are alternately observed. Since there is no difference in the positions of the cations in the rock-salt type, the above-mentioned characteristics are not observed. When adopting a crystal structure having the characteristics of both the rock-salt type and the layered rock-salt type, when observing from a specific crystal orientation, layers with higher brightness and layers with lower brightness are alternately observed in a cross-sectional STEM image or the like, and in the layer with lower brightness, that is, in a part of the lithium layer, there is a metal whose atomic number is greater than that of lithium.

[0130] The anions of the layered rock-salt type crystal and the rock-salt type crystal respectively form a cubic closest-packed structure (face-centered cubic lattice structure). It can be considered that the anions of the O3'-type crystal described later also form a cubic closest-packed structure. Thus, when the layered rock-salt type crystal comes into contact with the rock-salt type crystal, there is a crystal plane where the cubic closest-packed structures formed by the anions are oriented in the same direction.

[0131] In addition, it can be explained as follows. The anions on the {111} plane of the crystal structure of the cubic crystal have a triangular lattice. The layered rock-salt type has a rhombohedral structure belonging to the space group R-3m, but for easy understanding of the structure, it is usually represented by a composite hexagonal lattice, and the (0001) plane of the layered rock-salt type has a hexagonal lattice. The triangular lattice of the {111} plane of the cubic crystal has the same atomic arrangement as the hexagonal lattice of the (0001) plane of the layered rock-salt type. The state where the lattices of the two are integrated can be said to be the state where the cubic closest-packed structures are oriented in the same direction.

[0132] Note that the space groups of the layered rock-salt type crystal and the O3'-type crystal are R-3m, which is different from the space group Fm-3m of the rock-salt type crystal (the space group of a general rock-salt type crystal), so the Miller indices of the crystal planes satisfying the above conditions are different between the layered rock-salt type crystal and the O3'-type crystal and the rock-salt type crystal. In this specification, sometimes the state where the cubic closest-packed structures formed by the anions in the layered rock-salt type crystal, the O3'-type, and the rock-salt type crystal are oriented in the same direction means the state where the crystal orientations are substantially the same.

[0133] <Li x State where x in <LiCoO2 is small> The positive electrode active material 100 of one embodiment of the present invention has the above-mentioned distribution of the additive element A and / or crystal structure in the discharged state, so the crystal structure of <Li x CoO2 in the state where x is small is different from that of the existing positive electrode active material. Note that here, x being small means the case where 0.1 < x ≤ 0.24.

[0134] Use Figures 4 to 7 To compare the existing positive electrode active material with the positive electrode active material 100 of one embodiment of the present invention to illustrate the change accompanied by <Lix The change of x in CoO2 changes the crystal structure.

[0135] Figure 5 Shows changes in the crystal structure of conventional positive electrode active materials. Figure 5 The conventional positive electrode active material shown is lithium cobalt oxide (LiCoO 2 ) which does not contain the added element A.

[0136] exist Figure 5 In the case of Li, R-3m O3 is attached x The crystal structure of lithium cobalt oxide with x=1 in CoO2. In this crystal structure, lithium occupies an octahedral position and includes three CoO2 layers in the unit cell. Therefore, this crystal structure is sometimes called an O3 type structure. Note that the CoO2 layer refers to a structure in which the octahedral structure of cobalt coordinated to six oxygens is continuous on one plane in a state of edge sharing. Sometimes this structure is called a layer composed of octahedrons of cobalt and oxygen.

[0137] In addition, it is known that the symmetry of lithium in existing cobalt oxide increases when x=0.5, and the cobalt oxide has a monoclinic crystal structure belonging to the space group P2 / m. In this structure, the unit cell includes one CoO2 layer. Therefore, it is sometimes called an O1-type structure or a monoclinic O1-type structure.

[0138] The positive electrode active material when x=0 has a trigonal crystal structure belonging to the space group P-3m1, and the unit cell also includes a CoO2 layer. Therefore, this crystal structure is sometimes called an O1-type structure or a trigonal O1-type structure. In addition, the trigonal system is sometimes converted into a composite hexagonal lattice and called a hexagonal O1-type.

[0139] In addition, the existing lithium cobalt oxide has a crystal structure belonging to the space group R-3m when x=0.12. It can also be said that this structure is a structure in which CoO2 structures such as the trigonal O1 type structure and LiCoO2 structures such as those belonging to R-3m O3 are alternately stacked. Therefore, this crystal structure is sometimes called the H1-3 type structure. In addition, in fact, the number of cobalt atoms in each unit cell of the H1-3 type structure is twice that of other structures. However, in Figure 5 In this specification, in order to facilitate comparison with other crystal structures, the c-axis of the H1-3 type structure is 1 / 2 of the unit cell.

[0140] As an example of an H1-3 type structure, the coordinates of cobalt and oxygen in the unit cell can be represented by Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), and O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are both oxygen atoms. For example, Rietveld analysis using an XRD pattern can determine which unit cell is used to represent the crystal structure of the positive electrode active material. At this time, a unit cell with a small GOF (goodness of fit) value can be used.

[0141] When repeated Li x When x in CoO2 is 0.24 or less, the crystal structure of conventional lithium cobalt oxide changes repeatedly between the H1-3 type structure and the structure belonging to R-3m O3 in the discharge state (ie, non-equilibrium phase transition) during charging and discharging.

[0142] However, the CoO2 layers of the above two crystal structures deviate greatly. Figure 5 As shown by the dotted line and arrows, in the H1-3 type structure, the CoO2 layer deviates significantly from the R-3m O3 structure in the discharge state. Such dynamic structural changes will have an adverse effect on the stability of the crystal structure.

[0143] Furthermore, the volume difference between the two crystal structures is also large. When comparing the same number of cobalt atoms, the volume difference between the H1-3 structure and the R-3m O3 structure in the discharged state exceeds 3.5%, typically 3.9% or more.

[0144] In addition to the above, the structure of the H1-3 type structure having a continuous CoO2 layer like that of the trigonal O1 type is likely to be unstable.

[0145] Therefore, when charging and discharging are repeated until x becomes less than 0.24, the crystal structure of the existing lithium cobalt oxide collapses. The collapse of the crystal structure will cause the deterioration of the cycle characteristics. This is because the collapse of the crystal structure reduces the number of locations where lithium can exist stably, and the insertion and removal of lithium become difficult.

[0146] On the other hand, Figure 4 In the positive electrode active material 100 of one embodiment of the present invention shown in FIG. xThe change in the crystal structure between the discharge state where x is 1 and the state where x is less than 0.24 in CoO2 is less than that of the existing positive electrode active materials. More specifically, the deviation of the CoO2 layer between the state where x is 1 and the state where x is less than 0.24 can be reduced. In addition, the volume change when comparing each cobalt atom can be reduced. Therefore, even if the positive electrode active material 100 of one embodiment of the present invention is repeatedly charged and discharged with x being less than 0.24, it is not easy to cause the crystal structure to collapse and good cycle characteristics can be achieved. In addition, the positive electrode active material 100 of one embodiment of the present invention is not easy to cause the crystal structure to collapse and good cycle characteristics can be achieved. x When x in CoO2 is 0.24 or less, it can have a more stable crystal structure than the existing positive electrode active material. x When x in CoO2 is 0.24 or less, short circuit is less likely to occur. In this case, the safety of the secondary battery is further improved, which is preferred.

[0147] Figure 4 Shown in Li x The crystal structure of the inner portion 100b of the positive electrode active material 100 when x in CoO2 is about 1 and about 0.2. The inner portion 100b occupies most of the volume of the positive electrode active material 100 and has a great influence on charge and discharge, so it can be said that it is the part with the greatest influence caused by the deviation of the CoO2 layer and the change in volume.

[0148] When x=1, the positive electrode active material 100 has the same R-3m O3 type structure as that of conventional lithium cobalt oxide.

[0149] However, when the conventional lithium cobalt oxide has an H1-3 type structure and x is 0.24 or less, for example, about 0.2 or about 0.12, the positive electrode active material 100 has crystals with a structure different from the above structure.

[0150] When x=0.2, the positive electrode active material 100 of one embodiment of the present invention has a crystal structure belonging to the space group R-3m belonging to the trigonal system. The symmetry of the CoO2 layer of this structure is the same as that of O3. Therefore, this crystal structure is called O3' type structure. Figure 4 The crystal structure is indicated by R-3mO3'.

[0151] The coordinates of cobalt and oxygen in the unit cell of the O3' structure can be represented by Co(0, 0, 0.5) and O(0, 0, x) (0.20≤x≤0.25), respectively. In addition, the lattice constant of the unit cell is as follows: the a-axis is preferably 2.797≤a≤2.837(×10 -1 nm), more preferably 2.807≤a≤2.827(×10-1 nm), typically a=2.817(×10 -1 The c-axis is preferably 13.681≤c≤13.881(×10 -1 nm), more preferably 13.751≤c≤13.811, typically c=13.781(×10 -1 nm).

[0152] In the O3' type structure, ions of cobalt, nickel, magnesium, etc. occupy the positions coordinated to six oxygen atoms. In addition, light elements such as lithium sometimes occupy the positions coordinated to four oxygen atoms.

[0153] like Figure 4 The dotted line in the figure shows that there is almost no deviation between the CoO2 layers of the R-3m(O3) and O3' structures in the discharged state.

[0154] In addition, the difference in volume of the same number of cobalt atoms between the R-3m (O3) type structure and the O3' type structure in the discharged state is 2.5% or less, more specifically 2.2% or less, and typically 1.8%.

[0155] Thus, in the positive electrode active material 100 of one embodiment of the present invention, Li x When x in CoO2 is smaller, that is, when more lithium is detached, the change in the crystal structure is suppressed compared with the existing positive electrode active material. In addition, the change in volume when compared by the same number of cobalt atoms is also suppressed. Therefore, the crystal structure of the positive electrode active material 100 is not easy to collapse even if x is repeatedly charged and discharged to be less than 0.24. Therefore, the decrease in the charge and discharge capacity of the positive electrode active material 100 caused by the charge and discharge cycle is suppressed. In addition, a larger amount of lithium can be stably used than the existing positive electrode active material, so the discharge capacity per unit weight and unit volume of the positive electrode active material 100 is larger. Therefore, by using the positive electrode active material 100, a secondary battery with a higher discharge capacity per unit weight and unit volume can be manufactured.

[0156] In addition, it was confirmed that the positive electrode active material 100 x When x in CoO2 is 0.15 or more and 0.24 or less, it sometimes has an O3' structure, and it is also considered to have an O3' structure when x exceeds 0.24 and is 0.27 or less. x In addition to x in CoO2, it is also affected by the number of charge and discharge cycles, charge and discharge current, temperature, electrolyte, etc., and is therefore not limited to the above range of x.

[0157] Therefore, the positive electrode active material 100 in Li xWhen x in CoO2 is greater than 0.1 and less than 0.24, the entire interior 100b of the positive electrode active material 100 does not need to have an O3' type structure, but may have other crystal structures or may be partially amorphous.

[0158] The positive electrode active material 100 sometimes has an H1-3 type structure only when the charging voltage is further increased. In addition, as described above, the crystal structure is affected by the number of charge and discharge cycles, charge and discharge current, temperature, electrolyte, etc., so when the charging voltage is lower, for example, even at 25°C and the charging voltage is 4.5V or more and less than 4.6V, the positive electrode active material 100 of one embodiment of the present invention sometimes has an O3' type structure.

[0159] In addition, Figure 4 In the O3'-type structure, lithium exists at all lithium positions with equal probability, but the positive electrode active material 100 of one embodiment of the present invention is not limited to this. It can also exist in a concentrated manner at a part of the lithium positions. For example, it can also have a structure like Figure 5 The monoclinic O1 structure (Li 0.5 The distribution of lithium can be analyzed, for example, by neutron diffraction.

[0160] In addition, although the O3' type structure contains lithium irregularly between the layers, it can also have a crystal structure similar to the CdCl2 type crystal structure. This crystal structure similar to the CdCl2 type crystal structure is similar to the crystal structure of lithium nickel oxide charged to become Li 0.06 However, pure lithium cobalt oxide or layered rock salt-type positive electrode active materials containing a large amount of cobalt generally do not have a CdCl2-type crystal structure.

[0161] In addition, the concentration gradient of the added element A preferably has the same gradient in multiple regions of the surface portion 100a of the positive electrode active material 100. In other words, the reinforcing element derived from the added element A preferably exists homogeneously in the surface portion 100a. Even if a portion of the surface portion 100a is reinforced, if there is a portion that is not reinforced, stress may be concentrated in this portion. When stress is concentrated in a portion of the positive electrode active material 100, defects such as cracks may occur from this portion, thereby causing the collapse of the positive electrode active material and a decrease in discharge capacity.

[0162] Note that the added element A in the surface layer portion 100 a of the positive electrode active material 100 does not necessarily have the same concentration gradient.

[0163] Here, the CD vicinity has a layered rock salt type crystal structure belonging to R-3m, and the surface is (001) oriented. The distribution of the additive element A on the (001) oriented surface may also be different from other surfaces. For example, compared with surfaces other than the (001) orientation, the distribution of one or more concentration peaks selected from the additive element X and the additive element Y in the (001) oriented surface and its surface portion 100a may also be limited to a portion closer to the surface. Alternatively, compared with other orientations, the concentration of one or more selected from the additive element X and the additive element Y in the (001) oriented surface and its surface portion 100a may also be lower. Alternatively, in the (001) oriented surface and its surface portion 100a, one or more elements selected from the additive element X and the additive element Y may also be below the detection limit.

[0164] In the layered rock salt type crystal structure belonging to R-3m, cations are arranged parallel to the (001) plane. It can be said that this is a structure in which CoO2 layers and lithium layers are stacked alternately parallel to the (001) plane. Therefore, the diffusion path of lithium ions is also parallel to the (001) plane.

[0165] The CoO2 layer is relatively stable, and therefore relatively stable when the surface of the positive electrode active material 100 is oriented in the (001) direction. The main diffusion path of lithium ions during charge and discharge is not exposed on the (001) surface.

[0166] On the other hand, on the surface other than the (001) orientation, the diffusion path of lithium ions is exposed. Therefore, the surface other than the (001) orientation and the surface layer 100a are important areas for maintaining the diffusion path of lithium ions, and are the areas where lithium ions first leave, so they tend to be unstable. Therefore, in order to maintain the overall crystal structure of the positive electrode active material 100, it is very important to strengthen the surface other than the (001) orientation and the surface layer 100a.

[0167] Therefore, in the positive electrode active material 100 of another embodiment of the present invention, it is important that the distribution of the added element A in the plane other than (001) and the surface layer portion 100a thereof is as follows: Figure 3A and Figure 3C On the other hand, in the (001) plane and its surface layer portion 100a, the concentration of the additive element A may be relatively low as described above, or the additive element A may not be contained.

[0168] In the manufacturing method of heating after manufacturing high-purity LiCoO2 and mixing the additive element A, the additive element A mainly diffuses through the diffusion path of lithium ions, as shown in the following embodiment. Therefore, it is easy to set the distribution of the additive element A in the surface other than (001) and its surface part 100a to a preferred range.

[0169] <Grain Boundary> Preferably, in addition to the distribution described above, at least a portion of the additional element A in the positive electrode active material 100 according to one embodiment of the present invention is non-uniformly distributed at the grain boundary and its vicinity.

[0170] In this specification, etc., "non-uniformly distributed" means that the concentration of an element in an arbitrary region is different from that in other regions. "Non-uniformly distributed" is synonymous with "segregation", "precipitation", "non-uniform", "deviation" and "mixture of high-concentration regions and low-concentration regions".

[0171] For example, the magnesium concentration at the grain boundary and its vicinity of the positive electrode active material 100 is preferably higher than that in other regions of the interior 100b. In addition, the fluorine concentration at the grain boundary and its vicinity is preferably higher than that in other regions of the interior 100b. In addition, the nickel concentration at the grain boundary and its vicinity is also preferably higher than that in other regions of the interior 100b. In addition, the aluminum concentration at the grain boundary and its vicinity is preferably higher than that in other regions of the interior 100b.

[0172] Grain boundaries are a type of surface defect. Therefore, like the surface, they tend to be unstable and are prone to changes in crystal structure. Therefore, the higher the concentration of the additive element A at the grain boundary and its vicinity, the more effectively the changes in crystal structure can be suppressed.

[0173] In addition, when the concentrations of magnesium and fluorine are high at the grain boundary and its vicinity, even when cracks are generated along the grain boundary of the positive electrode active material 100 of one embodiment of the present invention, the concentrations of magnesium and fluorine are high near the surface generated by the cracks. Therefore, the corrosion resistance of the positive electrode active material to hydrofluoric acid can also be improved after the cracks are generated.

[0174] <Analysis Method> In order to determine whether a positive electrode active material is in Li x The positive electrode active material 100 of one embodiment of the present invention, which has an O3'-type structure when x in CoO2 is small, can contain Li x The positive electrode of the positive electrode active material having a smaller x in CoO2 is determined by analysis using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), or the like.

[0175] In particular, XRD is preferred because of the following advantages: the symmetry of transition metals such as cobalt in the positive electrode active material can be analyzed with high resolution; the height of crystallinity and the orientation of crystallinity can be compared; the periodic distortion of the lattice and the grain size can be analyzed; sufficient accuracy can be obtained when directly measuring the positive electrode obtained by disassembling a secondary battery, etc. Through XRD, especially powder XRD, a diffraction peak reflecting the crystal structure of the positive electrode active material 100b inside 100 that occupies most of the volume of the positive electrode active material 100 can be obtained.

[0176] When analyzing the crystal size by powder XRD, it is preferable to perform the measurement without affecting the orientation due to pressure, etc. For example, it is preferable to take out the positive electrode active material from the positive electrode obtained by disassembling the secondary battery as a powder sample for measurement.

[0177] As described above, the positive electrode active material 100 according to one embodiment of the present invention is characterized in that: x When x in CoO2 is 1 or 0.24 or less, the crystal structure changes less. When charged at a high voltage, materials with a crystal structure that changes greatly by more than 50% cannot withstand repeated high-voltage charging and discharging, so they are not preferred.

[0178] Note that sometimes the O3' type structure cannot be obtained by simply adding additive elements. For example, even under the same conditions such as lithium cobalt oxide containing magnesium and fluorine or lithium cobalt oxide containing magnesium and aluminum, the concentration and distribution of the additive elements in Li x When x in CoO2 is 0.24 or less, the O3' type structure may account for 60% or more, or the H1-3 type structure may account for 50% or more.

[0179] In addition, when x is too small such as 0.1 or less or when the charging voltage exceeds 4.9 V, an H1-3 type or trigonal O1 type structure is also generated in the positive electrode active material 100 of one embodiment of the present invention. Therefore, in order to determine whether it is a positive electrode active material 100 of one embodiment of the present invention, analysis of the crystal structure such as XRD and information such as the charging capacity or the charging voltage are required.

[0180] However, the positive electrode active material in a state where x is small may change its crystal structure when exposed to air. For example, it may change from an O3'-type structure to an H1-3-type structure. Therefore, all samples used in analyzing the crystal structure are preferably treated in an inert atmosphere such as an argon atmosphere.

[0181] In addition, whether the distribution of the additive element contained in the positive electrode active material is in the above-mentioned state can be determined by analyzing by XPS, Energy Dispersive X-ray Spectroscopy (EDX), Electron Probe Microanalysis (EPMA), or the like.

[0182] The crystal structure of the surface layer portion 100 a , grain boundaries, and the like can be analyzed by performing electron diffraction or the like on a cross section of the positive electrode active material 100 .

[0183] <<Charging Method>> As charging for determining whether the composite oxide is the positive electrode active material 100 of one embodiment of the present invention, for example, a coin battery (CR2032 type, 20 mm in diameter, 3.2 mm in height) of a lithium counter electrode can be manufactured and charged.

[0184] More specifically, as the positive electrode, a positive electrode obtained by applying a slurry obtained by mixing a positive electrode active material, a conductive material, and a binder to a positive electrode current collector of an aluminum foil can be used.

[0185] Lithium metal can be used as the counter electrode. Note that the potential of the positive electrode when a material other than lithium metal is used as the counter electrode is different from that of the secondary battery. Unless otherwise specified, the voltage and potential in this specification and the like refer to the potential of the positive electrode.

[0186] As the electrolyte contained in the electrolytic solution, 1 mol / L lithium hexafluorophosphate (LiPF6) is used. As the electrolytic solution, a solution obtained by mixing ethylene carbonate (EC) and diethyl carbonate (DEC) at a volume ratio of EC:DEC=3:7 and 2 wt% vinylene carbonate (VC) can be used.

[0187] As the separator, a polypropylene porous film having a thickness of 25 μm can be used.

[0188] The positive electrode can and the negative electrode can may be formed of stainless steel (SUS).

[0189] The coin cell manufactured under the above conditions is charged at any voltage (for example, 4.5V, 4.55V, 4.6V, 4.65V, 4.7V, 4.75V or 4.8V). There is no limitation on the charging method as long as it can be charged at any voltage and for a sufficient time. For example, when charging with CCCV, the current in CC charging can be set to be greater than 20mA / g and less than 100mA / g. CV charging can be performed until it is greater than 2mA / g and less than 10mA / g. In order to observe the phase change of the positive electrode active material, it is preferred to charge at the above-mentioned smaller current value. The temperature is set to 25°C or 45°C. After charging in this manner, the coin cell is disassembled in a glove box in an argon atmosphere and the positive electrode is taken out, thereby obtaining a positive electrode active material of any charging capacity. When various analyses are performed later, it is preferably sealed under an argon atmosphere to prevent reaction with external components. For example, XRD can be performed under the condition of a sealed container sealed in an argon atmosphere. At this time, the sealed container needs to be tightly sealed, and an argon atmosphere needs to be maintained during measurement. In addition, it is preferred to take out the positive electrode for analysis immediately after charging. Specifically, it is preferably performed within 1 hour after charging, and more preferably within 30 minutes after charging. Furthermore, the time from taking out the positive electrode from the glove box in the argon atmosphere to starting the XRD analysis is preferably within 5 minutes, and more preferably within 2 minutes.

[0190] In addition, when analyzing the crystal structure of the charged state after multiple charge and discharge, the multiple charge and discharge conditions may also be different from the above-mentioned charging conditions. For example, charging can be performed at a current value of 20 mA / g or more and 100 mA / g or less to perform constant current charging to any voltage (for example, 4.6 V, 4.65 V, 4.7 V, 4.75 V or 4.8 V), and then constant voltage charging can be performed at a current value of 2 mA / g or more and 10 mA / g or less, and discharging can be performed at a constant current discharge to 2.5 V at a current value of 20 mA / g or more and 100 mA / g or less.

[0191] Furthermore, when analyzing the crystal structure in a discharged state after multiple charge and discharge, for example, constant current discharge to 2.5 V may be performed at a current value of 20 mA / g or more and 100 mA / g or less.

[0192] <xrd> There is no limitation on the apparatus and conditions for XRD measurement. For example, the measurement can be performed with the following apparatus and conditions. XRD device: D8 ADVANCE manufactured by Bruker AXS X-ray source: CuKα1 ray Output: 40KV, 40mA Slit width: Div.Slit, 0.5° Detector: LynxEye Scanning mode: 2θ / θ continuous scanning Measuring range (2θ): 15° to 90° (100 minutes) Step width (2θ): set to 0.01° Counting time: 1 second / step Sample stage rotation: 15rpm

[0193] When the sample to be measured is a powder sample, the sample can be installed by placing it in a glass sample holder; or sprinkling the sample on a silicon non-reflective plate coated with grease; etc. When the sample to be measured is a positive electrode, the positive electrode active material layer can be installed according to the measurement surface required by the device by attaching the positive electrode to the substrate with double-sided tape.

[0194] Figure 6 and Figure 7 The ideal powder XRD patterns calculated by CuKα1 radiation from the O3' type structure and H1-3 type structure models are shown. In addition, for comparison, the XRD patterns calculated from Li x Ideal XRD patterns calculated for the crystal structures of LiCoO2 O3 where x is 1 and trigonal O1 where x is 0 in CoO2. The patterns of LiCoO2(O3) and CoO2(O1) were made using Reflex Powder Diffraction, one of the modules of Materials Studio (BIOVIA), based on the crystal structure information obtained from ICSD (Inorganic Crystal Structure Database). The range of 2θ was set to 15° to 75°, Step size = 0.01, and wavelength λ1 = 1.540562×10 -10 m, λ2 are not set, and Monochromator is set to single. The XRD pattern of H1-3 type structure is based on Figure 5 The information of the H1-3 type structure shown was prepared in the same manner as described above. The XRD pattern of the O3' type structure was prepared by the following method: the crystal structure was inferred from the XRD pattern of the positive electrode active material of one embodiment of the present invention and fitted using TOPAS ver.3 (crystal structure analysis software manufactured by Bruker), and the XRD pattern was prepared in the same manner as other structures.

[0195] like Figure 6 As shown, in the O3'-type structure, diffraction peaks appear at 2θ of 19.25±0.12° (19.13° or more and 19.37° or less) and 2θ of 45.47±0.10° (45.37° or more and 45.57° or less).

[0196] However, if Figure 7 As shown, in the H1-3 type structure and the trigonal O1 type structure, the peak does not appear at the above position. x The appearance of diffraction peaks at 2θ=19.25±0.12° (above 19.13° and below 19.37°) and 2θ=45.47±0.10° (above 45.37° and below 45.57°) when x in CoO2 is small is a characteristic of the positive electrode active material 100 of one embodiment of the present invention.

[0197] This also indicates that: the position of the XRD diffraction peak appearing in the crystal structure when x=1 is close to the position of the XRD diffraction peak appearing in the crystal structure when x≤0.24; more specifically, regarding the peaks in the main diffraction peaks of the crystal structure when x=1 and the crystal structure when x≤0.24, the 2θ difference between the peaks appearing at 42° or more and 46° or less is less than 0.7°, preferably less than 0.5°.

[0198] In addition, the positive electrode active material 100 of one embodiment of the present invention is Li x When x in CoO2 is small, it has an O3' type structure, but it is not necessary to have an O3' type structure as a whole. It can have other crystal structures, and it can also be partially amorphous. Note that when performing Rietveld analysis on the XRD pattern, the O3' type structure is preferably 50% or more, more preferably 60% or more, and further preferably 66% or more. When the O3' type structure is 50% or more, more preferably 60% or more, and further preferably 66% or more, a positive electrode active material with sufficiently excellent cycle characteristics can be achieved.

[0199] Furthermore, the O3'-type structure measured by Rietveld analysis after 100 or more charge and discharge cycles from the start of measurement is preferably 35% or more, more preferably 40% or more, and even more preferably 43% or more.

[0200] In addition, the sharpness of the diffraction peak in the XRD pattern indicates the height of crystallinity. Therefore, each diffraction peak after charging is preferably sharp, that is, the half-width is preferably narrow. The half-width of the peak of the same crystalline phase varies according to the measurement conditions of XRD and / or the value of 2θ. When the above-mentioned measurement conditions are adopted, for example, the half-width of the peak observed at 2θ of 43° or more and 46° or less is preferably 0.2° or less, more preferably 0.15° or less, and further preferably 0.12° or less. Note that it is not necessary for all peaks to meet the above conditions. As long as a part of the peaks meet the above conditions, it can be said that the crystallinity of its crystalline phase is higher. The above-mentioned higher crystallinity fully contributes to the stabilization of the crystal structure after charging.

[0201] In addition, the grain size of the O3' type structure of the positive electrode active material 100 is reduced to only about 1 / 20 of that of LiCoO2(O3) in the discharged state. Therefore, even under the same XRD measurement conditions as the positive electrode before charge and discharge, the Li x When x in CoO2 is small, a clear peak of O3' type structure is confirmed. On the other hand, even if a part of the existing LiCoO2 can have a structure similar to O3' type structure, the grain size will become smaller and its peak will become wider and smaller. The grain size can be obtained from the half width of the XRD peak.

[0202] <xps> X-ray photoelectron spectroscopy (XPS) can analyze the depth range of about 2nm to 8nm (generally less than 5nm) from the surface when analyzing inorganic oxides and using monochromated aluminum Kα line as the X-ray source, so the concentration of each element in about half of the depth direction of the surface part 100a can be quantitatively analyzed. In addition, by performing narrow scan analysis, the bonding state of the elements can be analyzed. The measurement accuracy of XPS is about ±1 atomic% in many cases. Although it depends on the element, the detection limit is about 1 atomic%.

[0203] In the positive electrode active material 100 of one embodiment of the present invention, the concentration of one or more selected from the added elements in the surface part 100a is preferably higher than the concentration in the inner part 100b. That is, the concentration of one or more selected from the added elements in the surface part 100a is preferably higher than the average concentration of the entire positive electrode active material 100. Therefore, for example, it can be said that the concentration of one or more selected from the added elements in the surface part 100a measured by XPS or the like is preferably higher than the average concentration of the entire positive electrode active material 100 measured by ICP-MS (inductively coupled plasma mass spectrometry) or GD-MS (glow discharge mass spectrometry analysis). For example, the concentration of magnesium in at least a portion of the surface part 100a measured by XPS or the like is preferably higher than the magnesium concentration of the entire positive electrode active material 100. In addition, the concentration of nickel in at least a portion of the surface part 100a is preferably higher than the nickel concentration of the entire positive electrode active material 100. In addition, the concentration of aluminum in at least a portion of the surface part 100a is preferably higher than the aluminum concentration of the entire positive electrode active material 100. In addition, the fluorine concentration in at least a portion of the surface layer portion 100 a is preferably higher than the fluorine concentration in the entire positive electrode active material 100 .

[0204] Note that the surface and surface layer 100a of the positive electrode active material 100 of one embodiment of the present invention do not include carbonates, hydroxyls, etc. chemically adsorbed after the positive electrode active material 100 is manufactured. In addition, it does not include electrolytes, adhesives, conductive materials, or compounds derived from them attached to the surface of the positive electrode active material 100. Therefore, when quantifying the elements contained in the positive electrode active material, the following correction can also be performed, that is, removing carbon, hydrogen, excess oxygen, excess fluorine, etc. that may be detected by surface analysis such as XPS. For example, XPS can identify the type of bonding by analysis, and can also perform corrections to remove CF bonds derived from the adhesive.

[0205] In addition, the samples of the positive electrode active material and the positive electrode active material layer can be washed before various analyses to remove the electrolyte, adhesive, conductive material or compounds derived from them attached to the surface of the positive electrode active material. At this time, sometimes lithium is dissolved in the solvent used for washing, but the added element is not easy to dissolve, so it has no effect on the atomic ratio of the added element.

[0206] In addition, the concentration of the added element can also be compared with the ratio of cobalt. By using the ratio with cobalt, the influence of carbonates chemically adsorbed after manufacturing the positive electrode active material can be reduced for comparison, so it is preferred. For example, the ratio of the number of atoms of magnesium to cobalt obtained by XPS analysis Mg / Co is preferably 0.400 or more, more preferably 0.500 or more, more preferably 0.600 or more, more preferably 0.700 or more, more preferably 0.800 or more, more preferably 0.900 or more, and more preferably 1.000 or more. In addition, Mg / Co is preferably less than 2.000, preferably less than 1.500, preferably less than 1.400, preferably less than 1.300, or preferably less than 1.200.

[0207] In addition, for example, the ratio of the number of atoms of nickel and cobalt obtained by XPS analysis, Ni / Co, is preferably 0.05 or more, more preferably 0.06 or more, more preferably 0.07 or more, more preferably 0.08 or more, and more preferably 0.09 or more. In addition, Ni / Co is preferably 0.200 or less, preferably 0.150 or less, preferably 0.140 or less, preferably 0.130 or less, preferably 0.120 or less, or preferably 0.110 or less.

[0208] In addition, for example, the ratio of the number of fluorine atoms to the number of cobalt atoms F / Co obtained by XPS analysis is preferably 0.100 or more, more preferably 0.200 or more, more preferably 0.300 or more, more preferably 0.400 or more, more preferably 0.500 or more, more preferably 0.600 or more, and more preferably 0.700 or more. In addition, F / Co is preferably 1.500 or less, preferably 1.200 or less, preferably 1.100 or less, preferably 1.000 or less, and preferably 0.900 or less.

[0209] It can also be said that the above range means that the above added element is not attached to a narrow range on the surface of the positive electrode active material 100, but is widely distributed in the surface layer 100a of the positive electrode active material 100 at a preferred concentration. In other words, the result of the XPS analysis of the positive electrode active material 100 in the above range indicates that even if charging and discharging are repeated with x being less than 0.24, the crystal structure is not easily collapsed, and excellent cycle characteristics can be achieved.

[0210] When performing XPS analysis, for example, monochromatized aluminum Kα rays are used as an X-ray source. In addition, for example, the extraction angle is 45°. For example, the measurement can be performed with the following apparatus and conditions. Measuring device: Quantera II manufactured by PHI X-ray source: monochromated aluminum Kα (1486.6 eV) Detection area: Detection depth: about 4nm to 5nm (extraction angle is 45°) Measurement spectrum: wide scan, narrow scan for each detected element

[0211] In addition, when the positive electrode active material 100 of one embodiment of the present invention is analyzed by XPS, it is preferred that the peak of the bonding energy between fluorine and other elements is 682eV or more and less than 685eV, more preferably about 684.3eV. This value is different from the 685eV of the bonding energy of lithium fluoride and the 686eV of the bonding energy of magnesium fluoride. In other words, when the positive electrode active material 100 of one embodiment of the present invention includes fluorine, it is preferably a bond other than lithium fluoride and magnesium fluoride.

[0212] In addition, when the positive electrode active material 100 of one embodiment of the present invention is analyzed by XPS, it is preferred that the peak of the bonding energy between magnesium and other elements is 1302eV or more and less than 1304eV, more preferably about 1303eV. This value is different from the 1305eV of the bonding energy of magnesium fluoride, and is close to the value of the bonding energy of magnesium oxide. In other words, when the positive electrode active material 100 of one embodiment of the present invention includes magnesium, it is preferably a bond other than magnesium fluoride.

[0213] <edx> One or two of the selected additive elements contained in the positive electrode active material 100 preferably have a concentration gradient. In addition, the positive electrode active material 100 is more preferably different in depth from the surface according to the concentration peak of the additive element. The concentration gradient of the additive element can be evaluated by, for example, exposing a cross section of the positive electrode active material 100 by FIB or the like and analyzing the cross section by EDX, EPMA, or the like.

[0214] In EDX measurement, the method of measuring while scanning in the region for two-dimensional evaluation is called EDX surface analysis. In addition, the method of evaluating the atomic concentration distribution in the positive electrode active material by linear scanning and measurement is called EDX line analysis. Sometimes the method of extracting the data of the linear region from the surface analysis of EDX is called EDX line analysis. In addition, the method of measuring without scanning is called EDX point analysis.

[0215] By EDX surface analysis (e.g., element mapping), the concentration of added elements in the surface layer 100a, the interior 100b, and the vicinity of the grain boundary of the positive electrode active material 100 can be quantitatively analyzed. In addition, by EDX line analysis, the concentration distribution and maximum value of the added element can be analyzed. In addition, in the analysis of thinning the sample such as STEM-EDX, the concentration distribution in the depth direction from the surface of the positive electrode active material in a specific area to the center can be analyzed without being affected by the distribution in the depth direction, so it is preferred.

[0216] Therefore, when EDX surface analysis or EDX point analysis is performed on the positive electrode active material 100 of one embodiment of the present invention, the concentration of each additional element, especially the additional element X, is preferably higher in the surface layer portion 100 a than in the inner portion 100 b .

[0217] The surface of the positive electrode active material in STEM-EDX analysis or the like refers to the average value M of the detected amount of characteristic X-rays originating from cobalt in the interior. AVE and the background average M BG The point where 50% of the total or the characteristic X-ray from oxygen becomes the average value of the internal detection amount O AVE and the background average O BG In addition, it is considered that the difference between the points where the total of 50% of the total of the cobalt and oxygen inside and the background is due to the influence of metal oxides and carbonates containing oxygen attached to the surface, so the average value M of the detected amount inside the cobalt can be used. AVE and the background average M BG The sum of 50% of the points.

[0218] The average value of the cobalt background above M BG For example, it can be obtained by averaging the outside of the portion where the amount of cobalt detected begins to increase, that is, the range of 2 nm or more, preferably 3 nm or more. AVE The average value of the background value of oxygen can be obtained by averaging a range of 2 nm or more, preferably 3 nm or more, in a region where the counts of cobalt and oxygen are saturated and stable, such as from a region where the amount of cobalt detected begins to increase to a depth of 30 nm or more, preferably to a depth of 50 nm or more. BG and the average value of the amount of oxygen detected inside AVE It can also be found in the same way.

[0219] In addition, the surface of the positive electrode active material 100 in the cross-sectional STEM (scanning transmission electron microscope) image or the like refers to: the boundary of the region where the image of the crystal structure derived from the positive electrode active material is observed and the region where the image is not observed, and refers to the outermost side of the region where the atomic column derived from the nucleus of the metal element having an atomic number greater than lithium in the metal element constituting the positive electrode active material is confirmed. The surface in the STEM image or the like can also be judged by referring to an analysis with a higher spatial resolution.

[0220] The peak in STEM-EDX line analysis refers to the maximum value in a graph with the intensity of the characteristic X-ray of each element as the vertical axis and the analysis position as the horizontal axis, and can also refer to the maximum value of the detected intensity or the characteristic X-ray of each element. As noise in STEM-EDX line analysis, the measured value of the half width below the spatial resolution (R), for example, below R / 2, is considered.

[0221] For example, when performing EDX surface analysis or EDX point analysis on a positive electrode active material 100 containing magnesium as an added element, the magnesium concentration of the surface portion 100a is preferably higher than the magnesium concentration of the internal portion 100b. In addition, when performing EDX line analysis, the magnesium concentration peak of the surface portion 100a preferably appears within a depth range of 3nm from the surface of the positive electrode active material 100 to the center, more preferably within a depth range of 1nm, and further preferably within a depth range of 0.5nm. Alternatively, preferably within ±1nm from the surface. In addition, the concentration of magnesium is preferably reduced to less than 60% of the peak concentration at a point from the peak top to a depth of 1nm. In addition, it is preferably reduced to less than 30% of the peak concentration at a point from the peak top to a depth of 2nm. The concentration peak described here is the maximum value of the concentration. In addition, due to the influence of the spatial resolution in EDX line analysis, the position of the magnesium concentration peak sometimes takes a negative value as a depth from the surface to the inside.

[0222] In the positive electrode active material 100 containing magnesium and fluorine as additive elements, the distribution of fluorine preferably overlaps with the distribution of magnesium. For example, the difference in the depth direction between the fluorine concentration peak and the magnesium concentration peak is preferably within 10 nm, more preferably within 3 nm, and further preferably within 1 nm.

[0223] In addition, when performing EDX line analysis, the fluorine concentration peak of the surface portion 100a preferably appears within a depth range of 3nm from the surface of the positive electrode active material 100 to the center, more preferably within a depth range of 1nm, and further preferably within a depth range of 0.5nm. Alternatively, preferably within ±1nm from the surface. In addition, the fluorine concentration peak is preferably slightly closer to the surface side than the magnesium concentration peak, and the resistance to fluorine is improved at this time, so it is preferred. For example, the fluorine concentration peak is preferably closer to the surface side by more than 0.5nm than the magnesium concentration peak, and more preferably closer to the surface side by more than 1.5nm than the magnesium concentration peak.

[0224] In addition, in the positive electrode active material 100 containing nickel as an added element, the nickel concentration peak of the surface portion 100a preferably appears within a depth range of 3nm from the surface of the positive electrode active material 100 to the center, more preferably within a depth range of 1nm, and further preferably within a depth range of 0.5nm. Alternatively, preferably within ±1nm from the surface. In addition, in the positive electrode active material 100 containing magnesium and nickel, the distribution of nickel preferably overlaps with the distribution of magnesium. For example, the difference in the depth direction of the nickel concentration peak and the magnesium concentration peak is preferably within 10nm, more preferably within 3nm, and further preferably within 1nm.

[0225] In addition, when the positive electrode active material 100 includes aluminum as an additive element, when performing EDX line analysis, the concentration peaks of magnesium, nickel or fluorine are closer to the surface than the aluminum concentration peak of the surface portion 100a. For example, the aluminum concentration peak preferably appears in the range of a depth of 0.5 nm or more and 50 nm or less from the surface of the positive electrode active material 100 to the center, and more preferably appears in the range of a depth of 3 nm or more and 30 nm or less.

[0226] In addition, when the positive electrode active material 100 is subjected to EDX line analysis, surface analysis or point analysis, the ratio of the number of atoms of magnesium Mg to cobalt Co in the magnesium concentration peak (Mg / Co) is preferably 0.05 or more and 0.6 or less, more preferably 0.1 or more and 0.4 or less. The ratio of the number of atoms of aluminum Al to cobalt Co in the aluminum concentration peak (Al / Co) is preferably 0.01 or more and 0.6 or less, more preferably 0.05 or more and 0.45 or less. The ratio of the number of atoms of nickel Ni to cobalt Co in the nickel concentration peak (Ni / Co) is preferably 0 or more and 0.2 or less, more preferably 0.01 or more and 0.1 or less, more preferably 0.05 or more and 0.1 or less. The ratio of the number of atoms of fluorine F to cobalt Co in the fluorine concentration peak (F / Co) is preferably 0 or more and 1.6 or less, more preferably 0.1 or more and 1.4 or less.

[0227] In addition, the grain boundary refers to, for example: the part where the particles of the positive electrode active material 100 are bonded together; the part where the crystal orientation changes inside the positive electrode active material 100, such as the repeated discontinuous part of the bright line and the dark line in the STEM image, the part containing multiple crystal defects, the part with a disordered crystal structure, etc. In addition, the crystal defect refers to the defect observable by the cross-sectional TEM (transmission electron microscope), cross-sectional STEM image, etc., that is, the structure and voids where other atoms enter the lattice. The grain boundary can be said to be a kind of surface defect. In addition, the vicinity of the grain boundary refers to the area within 10nm from the grain boundary.

[0228] When the positive electrode active material 100 is subjected to line analysis or surface analysis, the ratio of the number of atoms of the added element A to the cobalt Co near the grain boundary (A / Co) is preferably greater than 0.020 and less than 0.50. More preferably, it is greater than 0.025 and less than 0.30. Further preferably, it is greater than 0.030 and less than 0.20. Alternatively, it is preferably greater than 0.020 and less than 0.30. Alternatively, it is preferably greater than 0.020 and less than 0.20. Alternatively, it is preferably greater than 0.025 and less than 0.50. Alternatively, it is preferably greater than 0.025 and less than 0.20. Alternatively, it is preferably greater than 0.030 and less than 0.50. Alternatively, it is preferably greater than 0.030 and less than 0.30.

[0229] For example, when the added element is magnesium, when performing line analysis or surface analysis on the positive electrode active material 100, the atomic number ratio of magnesium to cobalt (Mg / Co) near the grain boundary is preferably 0.020 or more and 0.50 or less. More preferably, it is 0.025 or more and 0.30 or less. Further preferably, it is 0.030 or more and 0.20 or less. Or, it is preferably 0.020 or more and 0.30 or less. Or, it is preferably 0.020 or more and 0.20 or less. Or, it is preferably 0.025 or more and 0.50 or less. Or, it is preferably 0.025 or more and 0.20 or less. Or, it is preferably 0.030 or more and 0.50 or less. Or, it is preferably 0.030 or more and 0.30 or less. In addition, when multiple parts of the positive electrode active material 100, for example, three or more parts, are within the above range, it can be said that the added element is not distributed in a narrow range attached to the surface of the positive electrode active material 100, but is widely distributed in the surface layer portion 100a of the positive electrode active material 100 at an appropriate concentration.

[0230] <Raman spectroscopy> As described above, at least a part of the surface layer portion 100a of the positive electrode active material 100 of one aspect of the present invention preferably has a rock salt-type crystal structure. Therefore, when analyzing the positive electrode active material 100 and the positive electrode including the positive electrode active material 100 by Raman spectroscopy, a crystal structure of a cubic crystal system such as a rock salt-type crystal structure is preferably observed in addition to the layered rock salt-type crystal structure. In the STEM images and nano-beam electron diffraction patterns described later, unless cobalt substituting for the lithium position and cobalt present at the oxygen tetracoordination position exist at a certain frequency in the depth direction during observation, bright spots cannot be detected in the STEM images and nano-beam electron diffraction patterns. On the other hand, Raman spectroscopy is an analysis for detecting the vibration mode of bonds such as Co-O, so sometimes a peak of the wave number of the corresponding vibration mode is observed even when the amount of the corresponding Co-O bond present is small. And Raman spectroscopy can measure a range of about several μm² in area and about 1 μm in depth of the surface layer portion, so it is possible to detect with high sensitivity the state where the Co-O bond exists only on the particle surface. 2 That is, it can measure a range with an area of several μm² and a depth of about 1 μm of the surface layer portion, so it can detect with high sensitivity the state where the Co-O bond exists only on the particle surface.

[0231] For example, when the laser wavelength is 532 nm, in layered rock salt-type LiCoO₂, peaks are observed at 470 cm -1 to 490 cm -1 , 580 cm -1 to 600 cm -1 (vibration mode: E g , A 1g ). On the other hand, in cubic crystal system CoO x (0 < x < 1) (rock salt-type Co 1-y O(0 < y < 1) or spinel-type Co₃O₄), at 665 cm -1 Up to 685cm -1 A peak was observed at (vibration mode: A 1g ).

[0232] Therefore, when 470cm -1 Up to 490cm -1 The peak in the range of 580cm -1 Up to 600cm -1 The peaks in the range of 665cm -1 Up to 685cm -1 When the integrated intensities of the peaks in the range of are respectively represented as I1, I2 and I3, I3 / I2 is preferably 1% or more and 10% or less, and more preferably 3% or more and 9% or less.

[0233] When a cubic crystal structure such as a rock salt type is observed within the above range, it can be said that the surface layer portion 100 a of the positive electrode active material 100 has a rock salt type crystal structure within a suitable range.

[0234] <Nanobeam electron diffraction pattern> As with Raman spectroscopy, it is preferred that the characteristics of the layered rock salt type crystal structure and the rock salt type crystal structure are also observed from the nanobeam electron diffraction image. Note that in the STEM image and the nanobeam electron diffraction pattern, in view of the above-mentioned difference in sensitivity, it is preferred that the characteristics of the rock salt type crystal structure on the surface portion 100a, especially on the outermost surface (for example, from the surface to a depth of 1nm) are not too obvious. This is because compared with the case where the outermost surface is covered with a rock salt type crystal structure, the diffusion path of lithium can be further ensured and the function of stabilizing the crystal structure can be stronger when the layered rock salt type crystal structure is maintained and the lithium layer has added elements such as magnesium.

[0235] Therefore, for example, when obtaining a nanobeam electron diffraction pattern of a region at a depth of 1 nm or less from the surface and a nanobeam electron diffraction pattern of a region at a depth of 3 nm to 10 nm, the smaller the difference in lattice constant that can be calculated therefrom is, the better.

[0236] For example, the difference in lattice constants calculated between the measured portion at a depth of 1 nm or less from the surface and the measured portion at a depth of 3 nm or more and 10 nm or less is preferably: 0.1 (×10 -1 nm) and the c-axis is 1.0 (×10 -1 In addition, it is more preferable that the a-axis is 0.03 (×10 -1 nm) and the c-axis is 0.6 (×10 -1 In addition, it is more preferable that the a-axis is 0.04 (×10 -1 nm) and the c-axis is 0.3 (×10 -1 nm) or less.

[0237] <Electrolytes> As a mode of the electrolyte, an electrolyte comprising a solvent and being dissolved in an electrolyte can be used. As the solvent of the electrolyte, it is preferred to use an aprotic organic solvent, for example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, vinyl chloride carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, ethylene glycol dimethyl ether (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme (methyl diglyme), acetonitrile, benzonitrile, tetrahydrofuran, cyclopentane sulfone, one of sultones, etc., or two or more of the above can be used in any combination and ratio.

[0238] By using one or more ionic liquids (room temperature molten salts) with flame retardancy and low volatility as solvents for the electrolyte, even if the internal temperature rises due to internal short circuit or overcharge of the storage device, the rupture and ignition of the storage device can be prevented. The ionic liquid is composed of cations and anions, including organic cations and anions. As organic cations for the electrolyte, aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations and quaternary phosphonium cations or aromatic cations such as imidazolium cations and pyridinium cations can be cited. In addition, as anions for the electrolyte, monovalent amide anions, monovalent methylated anions, fluorosulfonic acid anions, perfluoroalkyl sulfonic acid anions, tetrafluoroborate anions, perfluoroalkyl borate anions, hexafluorophosphate anions or perfluoroalkyl phosphate anions can be cited.

[0239] In addition, as the electrolyte dissolved in the above solvent, for example, LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10 、Li2B 12 Cl 12 , one or more of the following lithium salts: LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2, lithium bis(oxalate borate) (Li(C2O4)2, abbreviated as: LiBOB), etc.

[0240] In addition, additives such as vinylene carbonate, propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate borate) (LiBOB) or dinitrile compounds such as succinonitrile and adiponitrile may be added to the electrolyte. The concentration of the additive may be set to, for example, 0.1 wt% or more and 5 wt% or less in the entire solvent in which the electrolyte is dissolved.

[0241] Alternatively, a polymer gel electrolyte in which a polymer is swollen with an electrolyte solution may be used.

[0242] In addition, by using a polymer gel electrolyte, safety against leakage is improved, and the secondary battery can be made thinner and lighter.

[0243] As gelled polymer, silicone gel, acrylic acid gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, fluorine polymer gel etc. can be used. As gelled polymer, for example, polymers with polyoxyalkylene structures such as polyethylene oxide (PEO), PVDF and polyacrylonitrile etc. and copolymers comprising these etc. can be used. For example, PVDF-HFP as a copolymer of PVDF and hexafluoropropylene (HFP) can be used. In addition, the formed polymer can also have a porous shape.

[0244] <Example 1 of Electrolyte> As one embodiment of the present invention, the electrolyte used may be a material having good lithium ion conductivity even when charged and / or discharged (charge and discharge) in a low temperature environment (e.g., 0°C, -10°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C, and most preferably -60°C).

[0245] An example of an electrolyte is described below. Note that, as an example, the electrolyte described in this embodiment is an electrolyte formed by dissolving a lithium salt in an organic solvent, which can also be called an electrolyte solution, but the electrolyte is not limited to a liquid electrolyte (electrolyte solution) that is liquid at room temperature, and a solid electrolyte can also be used. Alternatively, an electrolyte (semi-solid electrolyte) that includes both a liquid electrolyte that is liquid at room temperature and a solid electrolyte that is solid at room temperature can also be used.

[0246] As an example of the organic solvent described in this embodiment, when ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are included, the above ethylene carbonate, the above ethyl methyl carbonate, and the above dimethyl carbonate can be used in a state where the total content is 100 vol%, and the volume ratio of the above ethylene carbonate, the above ethyl methyl carbonate, and the above dimethyl carbonate is x:y:100 - x - y (note that 5 ≤ x ≤ 35 and 0 < y < 65). More specifically, an organic solvent containing EC, EMC, and DMC in a volume ratio of EC:EMC:DMC = 30:35:35 (volume ratio) can be used. Note that the above volume ratio can also be the volume ratio before mixing the organic solvents, and the external air during mixing of the organic solvents can also be at room temperature (typically 25°C). The proportion of the compounds contained in the organic solvent can be analyzed, for example, by nuclear magnetic resonance (NMR), gas chromatography (GC / MS), high performance liquid chromatography (HPLC), etc.

[0247] EC is a cyclic carbonate and has the effect of promoting the dissociation of lithium salts because of its high relative dielectric constant. On the other hand, EC has a high viscosity and a high freezing point (melting point) of 38°C. Therefore, when only EC is used as the organic solvent, it is difficult to use it in a low-temperature environment. Thus, the organic solvent specifically described as one mode of the present invention contains not only EC but also EMC and DMC. EMC is a chain carbonate and has the effect of reducing the viscosity of the electrolyte, and its freezing point is -54°C. In addition, DMC is also a chain carbonate and has the effect of reducing the viscosity of the electrolyte, and its freezing point is -43°C. The organic solvents are mixed in such a way that the total content of the three organic solvents of EC, EMC, and DMC having the above physical properties is 100 vol% and the volume ratio is x:y:100 - x - y (note that 5 ≤ x ≤ 35, 0 < y < 65), and the electrolyte manufactured using the above organic solvent has a characteristic that the freezing point is -40°C or lower.

[0248] The lowest freezing point of a general electrolyte for a lithium-ion battery is about -20°C. Therefore, it is difficult to manufacture a battery that can be charged and discharged at -40°C. The freezing point of the electrolyte described as an example in this embodiment is -40°C or lower, and thus a lithium-ion battery capable of being charged and discharged in an extremely low-temperature environment of -40°C can be realized.

[0249] In addition, as the electrolyte dissolved in the above solvent, a lithium salt can be used. For example, LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10 、Li2B 12 Cl 12 , at least one lithium salt selected from LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2, and lithium bis(oxalato)borate (LiBOB). The volume of the electrolyte dissolved in the above solvent can be 0.5 mol / L or more and 1.5 mol / L or less, preferably 0.7 mol / L or more and 1.3 mol / L or less, more preferably 0.8 mol / L or more and 1.2 mol / L or less. As a specific example of use, LiPF6 can be 0.5 mol / L or more and 1.5 mol / L or less with respect to the volume of the above solvent, preferably 0.7 mol / L or more and 1.3 mol / L or less, more preferably 0.8 mol / L or more and 1.2 mol / L or less.

[0250] In addition, as the electrolytic solution, preferably, the content of granular dust or elements other than the constituent elements of the electrolytic solution (hereinafter simply referred to as "impurities") is small and highly purified. Specifically, the ratio of impurities in the weight of the electrolytic solution is preferably 1% or less, more preferably 0.1% or less, and further preferably 0.01% or less.

[0251] Furthermore, for the purpose of improving safety, etc., a coating film (Solid Electrolyte Interphase Film) is formed at the interface between the electrode (active material layer) and the electrolytic solution, and additives such as vinylene carbonate (VC), propanesultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalato)borate (LiBOB), or dinitrile compounds such as succinonitrile or adiponitrile can also be added to the electrolytic solution. The concentration of the additive can be set, for example, to be 0.1 wt% or more and 5 wt% or less in the whole solvent.

[0252] <Example 2 of electrolyte> As the organic solvent of the electrolyte according to one aspect of the present invention, it preferably contains two or more selected from fluorinated cyclic carbonates and fluorinated chain carbonates. For example, the organic solvent described in this embodiment preferably contains fluoroethylene carbonate (FEC) and methyl 3,3,3-trifluoropropionate (MTFP). The reasons are described below.

[0253] <FEC and MTFP> FEC is one of the cyclic carbonates, and because it has a high relative dielectric constant, it has the effect of promoting the dissociation of lithium salts when used in an organic solvent. In addition, FEC has a substituent that exhibits electron-withdrawing properties, so it is easy to bond with lithium ions through Coulomb force. Specifically, it can be said that the solvation energy of FEC is smaller than that of ethylene carbonate (abbreviated as "EC") that does not have a substituent that exhibits electron-withdrawing properties, so it is easy to generate solvation with lithium ions. Furthermore, the HOMO of FEC is considered to be deep, and it is not easy to oxidize when the HOMO is deep, and the oxidation resistance is improved. On the other hand, the viscosity of FEC is high, and when only FEC is used as an organic solvent, it is difficult to use below the freezing point. Therefore, the organic solvent specifically described as one embodiment of the present invention includes not only FEC, but also MTFP. MTFP is one of the chain carbonates, and has the effect of reducing or maintaining the viscosity of the electrolyte. Of course, the solvation energy of MTFP is also smaller than that of methyl propionate (abbreviated as "MP") that does not have a substituent that exhibits electron-withdrawing properties, so it can sometimes generate solvation with lithium ions.

[0254] It is preferred that the total content of the two organic solvents FEC and MTFP having such physical properties is 100 vol%, and they are mixed in a volume ratio of x:100-x (note, 5≤x≤30, preferably 10≤x≤20). It is preferred that the organic solvent is mixed in a manner such that there is more MTFP than FEC. Note that the above volume ratio may also be the volume ratio measured before the mixing of the organic solvents, and the outside air when the organic solvents are mixed may also be room temperature (typically 25°C). The organic solvent mixed with FEC and MTFP has a viscosity that allows it to work as a lithium-ion battery, and maintains an appropriate viscosity even below freezing, so it is preferred.

[0255] The general organic solvent used for lithium-ion batteries solidifies at about -20°C, so it is difficult to manufacture a lithium-ion battery that can be charged and discharged at -40°C, preferably -50°C. However, the organic solvent described as an example in this embodiment can achieve a solidification point of below -40°C, preferably below -50°C, so that a lithium-ion battery that can be charged and discharged in an environment below the freezing point can be realized. As a result, a lithium-ion battery that can be charged and discharged in a wide temperature range including at least below the freezing point can be realized.

[0256] In the above description, FEC is used as a representative for description, but it can be said that any organic compound described as a fluorinated cyclic carbonate has the effect of promoting the dissociation of lithium salts; the solvation energy is small and it is easy to generate solvation with lithium ions; the viscosity is high, and it is difficult to use below the freezing point when only the organic compound is used. In addition, although MTFP is used as a representative for description in the above description, it can be said that any organic compound described as a fluorinated chain carbonate has the effect of reducing or maintaining the viscosity of the electrolyte of one embodiment of the present invention. Therefore, as long as the organic solvent of one embodiment of the present invention includes a fluorinated cyclic carbonate and a fluorinated chain carbonate, a lithium ion battery that can be charged and discharged in a wide temperature range at least including below the freezing point can be provided.

[0257] In Electrolyte Example 2, the material described in Electrolyte Example 1 can be used as the lithium salt. In addition, the material described in Electrolyte Example 1 can also be used as the additive.

[0258] An example of an electrolyte that can be used in a lithium ion battery according to one embodiment of the present invention is described above, but the electrolyte that can be used in a lithium ion battery according to one embodiment of the present invention is not limited to this example. Other materials can also be used as long as they have excellent lithium ion conductivity when charged and discharged in a low temperature environment.

[0259] A lithium ion battery of one embodiment of the present invention includes at least the above-mentioned positive electrode active material and electrolyte, so that a lithium ion battery having good discharge characteristics even in a low temperature environment and / or a lithium ion battery having good charging characteristics even in a low temperature environment can be realized. More specifically, when a test battery is manufactured by including at least the above-mentioned positive electrode active material and electrolyte and using lithium metal as a negative electrode, the following lithium ion battery can be realized: relative to the discharge capacity when the test battery is charged and discharged at 20°C, the discharge capacity when the test battery is charged and discharged at -40°C is 70% or more. In addition, as a condition for the above-mentioned discharge, for example, discharge can be performed at a current rate of 0.1C (note, 1C = 200mA / g). In this specification, etc., when a discharge capacity of 50% or more compared to the discharge capacity under a 20°C environment can be achieved under a T°C environment (T is an arbitrary temperature (°C)), it is recorded that the lithium ion battery can operate at T°C.

[0260] The contents of this embodiment mode can be freely combined with the contents of other embodiment modes.

[0261] (Implementation Method 2) In this embodiment, a method for producing a positive electrode active material that can be used for a lithium ion battery having good discharge characteristics even in a low temperature environment is described with reference to FIGS. 8 to 10 .

[0262] <Example 1 of Method for Producing Positive Electrode Active Material> Reference FIG. 8A to FIG. 8D An example of a method for producing a positive electrode active material that can be used in one embodiment of the present invention (Example 1 of a method for producing a positive electrode active material) is described. Note that in <Example 1 of a method for producing a positive electrode active material>, the additional elements described as additional element X, additional element Y, and additional element Z in Embodiment 1 are collectively referred to as additional element A.

[0263] First, as step S10, lithium cobalt oxide used as a starting material is prepared. As the starting material, lithium cobalt oxide having a particle size (strictly speaking, a median particle size (D50)) of 10 μm or less (preferably 8 μm or less) can be used. As the lithium cobalt oxide having a median particle size (D50) of 10 μm or less, either known or publicly available (in short, commercially available) lithium cobalt oxide can be used, or lithium cobalt oxide obtained by Figure 8B The lithium cobalt oxide is manufactured by the steps S11 to S14 shown. As a typical example of commercially available lithium cobalt oxide with a median particle size (D50) of less than 10 μm, lithium cobalt oxide manufactured by Nippon Chemical Industry Co., Ltd. (trade name "CELLSEED C-5H") can be cited. The median particle size (D50) of the lithium cobalt oxide manufactured by Nippon Chemical Industry Co., Ltd. (trade name "CELLSEED C-5H") is approximately 7 μm. In addition, the following describes a method for manufacturing lithium cobalt oxide having a median particle size (D50) of less than 10 μm obtained by steps S11 to S14.

[0264] <Step S11> exist Figure 8B In step S11 shown in the figure, a lithium source (Li source) and a cobalt source (Co source) are prepared as starting materials of lithium and transition metal, respectively.

[0265] As the lithium source, a compound containing lithium is preferably used, for example, lithium carbonate, lithium hydroxide, lithium nitrate, lithium fluoride, etc. The purity of the lithium source is preferably high, for example, a material with a purity of 99.99% or more is preferably used.

[0266] As the cobalt source, a compound containing cobalt is preferably used, for example, cobalt tetraoxide, cobalt hydroxide, etc. The purity of the cobalt source is preferably high, for example, it is preferred to use a material with a purity of 3N (99.9%) or more, preferably 4N (99.99%) or more, more preferably 4N5 (99.995%) or more, and further preferably 5N (99.999%) or more. By using a high-purity material, impurities in the positive electrode active material can be controlled. As a result, the capacity of the secondary battery is improved and the reliability of the secondary battery is improved.

[0267] In addition, the crystallinity of the cobalt source is preferably high, for example, it preferably has single crystal particles. As a method for evaluating the crystallinity of the transition metal source, there can be cited: evaluation using TEM (transmission electron microscope) images, STEM (scanning transmission electron microscope) images, HAADF-STEM (high angle annular dark field-scanning transmission electron microscopy) images, ABF-STEM (annular bright field scanning transmission electron microscope) images, etc.; or evaluation using X-ray diffraction (XRD), electron diffraction, neutron diffraction, etc. The above-mentioned method for evaluating crystallinity can also evaluate other crystallinities in addition to the transition metal source.

[0268] <Step S12> Then, as Figure 8B In step S12 shown, the lithium source and the cobalt source are crushed and mixed to produce a mixed material. The crushing and mixing can be performed by a dry method or a wet method. When the crushing and mixing are performed by a wet method, the powder can be ground smaller, so in order to obtain lithium cobalt oxide with a median particle size (D50) of less than 10 μm as a starting material, a wet method is preferred. When the crushing and mixing are performed by a wet method, a solvent is prepared. As a solvent, ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. can be used. It is preferred to use a non-protonic solvent that is not easy to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or more is used. Preferably, the dehydrated acetone with a moisture content suppressed to less than 10 ppm and a purity of more than 99.5% is mixed with a lithium source and a transition metal source for crushing and mixing. By using dehydrated acetone of the above purity, impurities that may be mixed can be reduced.

[0269] As a method for pulverizing and mixing, a ball mill or a sand mill can be used. When a ball mill is used, alumina balls or zirconia balls are preferably used as pulverizing media. Zirconia balls are preferred because they emit less impurities. In addition, when a ball mill or a sand mill is used, the peripheral speed is preferably set to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the medium.

[0270] <Step S13> Then, as Figure 8B In step S13 shown, the mixed material is heated. The heating temperature is preferably 800°C to 1100°C, more preferably 900°C to 1000°C, and further preferably about 950°C to 1000°C. When the temperature is too low, there is a concern that the decomposition and melting of the lithium source and the transition metal source are insufficient. On the other hand, when the temperature is too high, defects may occur due to the following reasons: lithium evaporates from the lithium source; and / or cobalt is excessively reduced; etc. For example, cobalt changes from trivalent to divalent, causing oxygen defects, etc.

[0271] When the heating time is too short, lithium cobalt oxide is not synthesized, but when the heating time is too long, the productivity decreases. Therefore, the heating time can be from 1 hour to 100 hours, preferably from 2 hours to 20 hours, and more preferably from 2 hours to 10 hours.

[0272] Although it varies depending on the temperature to be reached during heating, the heating rate is preferably 80° C. / h or more and 250° C. / h or less. For example, when heating at 1000° C. for 10 hours, the heating rate is preferably 200° C. / h.

[0273] The heating is preferably performed in an atmosphere with less water such as dry air, for example, preferably in an atmosphere with a dew point of -50°C or less, more preferably in an atmosphere with a dew point of -80°C or less. In the present embodiment, the heating is performed in an atmosphere with a dew point of -93°C. In addition, in order to suppress impurities that may be mixed into the material, the impurity concentrations of CH4, CO, CO2, H2, etc. in the heating atmosphere are preferably all below 5 ppb (parts per billion).

[0274] The heating atmosphere is preferably an oxygen-containing atmosphere. For example, a method of continuously introducing dry air into the reaction chamber can be cited. In this case, the flow rate of the dry air is preferably 10 L / min. A method of continuously introducing oxygen into the reaction chamber so that the oxygen flows through the reaction chamber is called "flowing".

[0275] When an oxygen-containing atmosphere is used as the heating atmosphere, a non-flowing method may also be used. For example, a method of first depressurizing the reaction chamber and then filling it with oxygen to prevent the oxygen from entering or leaving the reaction chamber may be used. This method is called purging. For example, the reaction chamber may be depressurized to -970 hPa, and then continued to be filled with oxygen until the pressure reaches 50 hPa.

[0276] After heating, the mixture may be cooled naturally, and the cooling time from the specified temperature to room temperature is preferably in the range of 10 hours to 50 hours. Note that it is not necessarily necessary to cool to room temperature, but only to a temperature allowed by the next step.

[0277] The heating in this step can be performed using a rotary kiln or a roller hearth kiln. Heating using a continuous or batch-type rotary kiln can be performed while stirring.

[0278] The container used for heating is preferably an alumina crucible or an alumina sagger. The alumina crucible is a material that is almost free of impurities. In this embodiment, an alumina sagger with a purity of 99.9% is used. In addition, heating the crucible or sagger after covering it with a lid can prevent the volatilization of the material, so it is preferred.

[0279] After heating, the material may be ground and screened as needed. When the heated material is recovered, it may be moved from the crucible to the mortar first, and then the heated material may be recovered. In addition, the mortar is preferably made of zirconium oxide or agate. In addition, the same heating conditions as those in step S13 may be used in the heating process described later other than step S13.

[0280] <Step S14> Through the above steps, it is possible to synthesize Figure 8B The lithium cobalt oxide (LiCoO2) shown in step S14 is an oxide containing multiple metal elements in its structure, so it can be called a composite oxide. In this specification, "composite oxide" refers to an oxide containing multiple metal elements in its structure. In addition, a grinding process and a classification process can be performed after step S13 to adjust the particle size distribution, and then the lithium cobalt oxide (LiCoO2) shown in step S14 can be obtained.

[0281] As shown in steps S11 to S14, an example of producing the composite oxide by a solid phase method is shown, but the composite oxide may also be produced by a coprecipitation method. Alternatively, the composite oxide may also be produced by a hydrothermal method.

[0282] After step S11 to step S14, lithium cobalt oxide can be obtained, which is a starting material for obtaining a positive electrode active material for a lithium ion battery having good discharge characteristics even in a low temperature environment. Specifically, the lithium cobalt oxide used as a starting material can obtain lithium cobalt oxide with a median particle size of less than 10 μm.

[0283] <Step S15> Then, as Fig. 8A In step S15 shown, lithium cobalt oxide, which is a starting material, is heated. The heating in step S15 is the first heating of lithium cobalt oxide, so it is sometimes referred to as initial heating in this specification, etc. In addition, this heating is also performed before step S31 shown below, so it is sometimes referred to as preheating treatment or pretreatment.

[0284] The lithium compounds and the like that unintentionally remain on the surface of the lithium cobalt oxide are detached due to the initial heating. In addition, the effect of improving the internal crystallinity can be expected. In addition, the lithium source and / or the cobalt source prepared in step S11 and the like are sometimes mixed with impurities, but by performing the initial heating, the impurities in the lithium cobalt oxide that is the starting material can be reduced. In addition, the effect of improving the internal crystallinity refers to, for example, the effect of alleviating the skewness, deviation, etc. caused by the difference in shrinkage of the lithium cobalt oxide manufactured in step S14.

[0285] After the initial heating, the surface of the lithium cobalt oxide is smoothed. In addition, after the initial heating, the cracks and crystal defects of the lithium cobalt oxide are also alleviated. In this specification, the surface "smooth" means: there are fewer bumps and the composite oxide is curved as a whole, and the corners are curved. Alternatively, the state with fewer foreign matter attached to the surface is also called "smooth". It can be considered that foreign matter is the cause of bumps and bumps, and it is preferred that foreign matter is not attached to the surface.

[0286] Note that when performing this initial heating, it is not necessary to separately prepare materials used as a lithium compound source, an additional element source, or a flux.

[0287] When the heating time of this step is too short, a sufficient effect cannot be obtained, but when the heating time is too long, the productivity decreases. The range of appropriate heating time can be selected from the heating conditions described in step S13 and implemented. In addition, in order to maintain the crystal structure of the composite oxide, the heating temperature of step S15 is preferably lower than the temperature of step S13. In addition, in order to maintain the crystal structure of the composite oxide, the heating time of step S15 is preferably shorter than the heating time of step S13. For example, it is preferred to heat at a temperature of 700°C or more and 1000°C or less (more preferably 800°C or more and 900°C or less) for more than 1 hour and less than 20 hours (more preferably 1 hour or more and less than 5 hours).

[0288] In lithium cobalt oxide, a temperature difference sometimes occurs between the surface and the inside of the lithium cobalt oxide after the heating in step S13. Sometimes the temperature difference causes a shrinkage difference. It can also be considered that the shrinkage difference occurs because the fluidity between the surface and the inside is different according to the temperature difference. Due to the energy related to the shrinkage difference, a difference in internal stress occurs in the lithium cobalt oxide. The difference in internal stress is also called distortion, and this energy is sometimes called distortion energy. It can be considered that the internal stress is removed after the initial heating in step S15, in other words, the distortion energy is uniformized after the initial heating in step S15. When the distortion energy is uniformized, the distortion of the lithium cobalt oxide is alleviated. Therefore, the surface of the lithium cobalt oxide becomes smooth. It can also be said that the surface is improved. In other words, it can be considered that after step S15, the shrinkage difference generated in the lithium cobalt oxide is alleviated, so that the surface of the composite oxide can be smoothed.

[0289] In addition, the shrinkage difference sometimes leads to the generation of small deviations in the lithium cobalt oxide, such as the generation of crystal deviations. In order to reduce the deviation, step S15 is preferably performed. After step S15, the deviation of the composite oxide can be uniformed (relaxing the deviation of crystals etc. generated in the composite oxide or arranging the grains). As a result, the surface of the composite oxide may become smooth.

[0290] By using lithium cobalt oxide having a smooth surface as a positive electrode active material, deterioration during charge and discharge as a secondary battery is reduced, and cracking of the positive electrode active material can be prevented.

[0291] In addition, as described above, pre-synthesized lithium cobalt oxide having a median particle size of 10 μm or less may be used in step S10. In this case, steps S11 to S13 may be omitted. By performing step S15 on the pre-synthesized lithium cobalt oxide, lithium cobalt oxide having a smooth surface may be obtained.

[0292] Note that step S15 is not a structure that must exist in one embodiment of the present invention, so an embodiment in which step S15 is omitted is also included in one embodiment of the present invention.

[0293] <Step S20> Next, refer to Figure 8C and Fig.8D The details of step S20 of preparing to add element A as an A source will be described.

[0294] <Step S21> Figure 8C The step S20 shown includes steps S21 to S23. In step S21, an additive element A is prepared. As specific examples of the additive element A, one or more selected from magnesium, fluorine, nickel, aluminum, titanium, zirconium, vanadium, iron, manganese, chromium, niobium, arsenic, zinc, silicon, sulfur, phosphorus, and boron can be used. In addition, one or more selected from bromine and beryllium can also be used. Figure 8C An example is shown in which a magnesium source (Mg source) and a fluorine source (F source) are prepared. Note that in step S21, in addition to adding the element A, a lithium source may be prepared separately.

[0295] When magnesium is selected as the additive element A, the source of the additive element A may be referred to as a magnesium source. As the magnesium source, magnesium fluoride (MgF2), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), or magnesium carbonate (MgCO3) may be used. A plurality of magnesium sources may also be used.

[0296] When fluorine is selected as the additive element A, the source of the additive element A may be referred to as a fluorine source. As the fluorine source, for example, lithium fluoride (LiF), magnesium fluoride (MgF2), aluminum fluoride (AlF3), titanium fluoride (TiF4), cobalt fluoride (CoF2, CoF3), nickel fluoride (NiF2), zirconium fluoride (ZrF4), vanadium fluoride (VF5), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF2), calcium fluoride (CaF2), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF2), cerium fluoride (CeF3, CeF4), lanthanum fluoride (LaF3) or sodium aluminum hexafluoride (Na3AlF6) may be used. Among them, lithium fluoride has a relatively low melting point of 848°C and is easily melted in the heating step described later, so it is preferred.

[0297] Magnesium fluoride can be used as both a fluorine source and a magnesium source. In addition, lithium fluoride can also be used as a lithium source. As another lithium source used in step S21, lithium carbonate can be cited.

[0298] Alternatively, the fluorine source may be a gas, and fluorine (F2), carbon fluoride, sulfur fluoride, or oxyfluoride (OF2, O2F2, O3F2, O4F2, O5F2, O6F2, O2F) or the like may be mixed in the atmosphere in the heating step described later.

[0299] In the present embodiment, lithium fluoride (LiF) is prepared as a fluorine source, and magnesium fluoride (MgF2) is prepared as a fluorine source and a magnesium source. When lithium fluoride and magnesium fluoride are mixed at a molar ratio of about LiF:MgF2=65:35, it is most effective in lowering the melting point. In addition, when the ratio of lithium fluoride is too large, lithium becomes excessive and may cause deterioration of the cycle characteristics. For this reason, the molar ratio of lithium fluoride and magnesium fluoride is preferably LiF:MgF2=x:1 (0≤x≤1.9), more preferably LiF:MgF2=x:1 (0.1≤x≤0.5), and further preferably LiF:MgF2=x:1 (x=0.33 or its vicinity). Note that when not specifically stated in this specification, etc., a certain value or its vicinity refers to a value greater than 0.9 times and less than 1.1 times the value.

[0300] <Step S22> Then, in Figure 8C In step S22 shown in the figure, the magnesium source and the fluorine source are pulverized and mixed. This step can be carried out by selecting the conditions for pulverization and mixing described in step S12.

[0301] <Step S23> Then, in Figure 8C In step S23, the pulverized and mixed materials are collected to obtain a source of the additive element A (source A). The source of the additive element A shown in step S23 includes a plurality of starting materials and can also be called a mixture.

[0302] The median particle size (D50) of the particle size of the above mixture is preferably 100 nm or more and 10 μm or less, more preferably 300 nm or more and 5 μm or less. The median particle size (D50) when using one material as the source of the added element A is also preferably 100 nm or more and 10 μm or less, more preferably 300 nm or more and 5 μm or less.

[0303] When the mixture (including the case where there is only one additive element) that has been micronized in step S22 is mixed with lithium cobalt oxide in a subsequent step, the mixture can be easily uniformly attached to the surface of the lithium cobalt oxide. When the mixture is uniformly attached to the surface of the lithium cobalt oxide, it is easy to uniformly distribute or diffuse the additive element in the surface layer portion 100a of the composite oxide after heating, which is preferred.

[0304] <Step S21> use Fig.8D Description and Figure 8C Different processes. Fig.8D The illustrated step S20 includes steps S21 to S23.

[0305] exist Fig.8D In step S21 shown, four sources of additive elements A are prepared to be added to lithium cobalt oxide. That is, Fig.8D The type of source of added element A and Figure 8C In addition, a lithium source may be prepared separately in addition to the element A source.

[0306] As four sources of additive elements A, a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source) and an aluminum source (Al source) are prepared. The magnesium source and the fluorine source can be obtained from Figure 8C As the nickel source, nickel oxide, nickel hydroxide, etc. can be used. As the aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.

[0307] <Step S22> and <Step S23> then, Fig.8D The steps S22 and S23 shown in FIG. Figure 8C The same applies to step S22 and step S23 described in .

[0308] <Step S31> Then, in Fig. 8A In step S31, the lithium cobalt oxide and the additive element A source (A source) that have passed step S15 (initial heating) are mixed. Here, the ratio of the number of atoms Co of cobalt in the lithium cobalt oxide that has passed step S15 to the number of atoms Mg of magnesium in the additive element A is preferably Co:Mg=100:y (0.1≤y≤6), and more preferably Co:Mg=100:y (0.3≤y≤3). When the additive element A is added to the lithium cobalt oxide that has passed the initial heating, the additive element A can be added uniformly. Therefore, it is preferred that the order is not to perform initial heating (step S15) after adding the additive element A, but to add the additive element A after the initial heating (step S15).

[0309] In addition, when nickel is selected as the additive element A, the mixing in step S31 is preferably performed in such a manner that the number of nickel atoms in the nickel source is 0.05% or more and 4% or less of the number of cobalt atoms in the lithium cobalt oxide after step S15. In addition, when aluminum is selected as the additive element A, the mixing in step S31 is preferably performed in such a manner that the number of aluminum atoms in the aluminum source is 0.05% or more and 4% or less of the number of cobalt atoms in the lithium cobalt oxide after step S15.

[0310] In order not to damage the shape of the lithium cobalt oxide particles, the mixing of step S31 is preferably performed under milder conditions than the crushing-mixing of step S12. For example, it is preferred to adopt conditions with fewer rotations or shorter time than the mixing of step S12. In addition, it can be said that the dry method is a milder condition than the wet method. Mixing can be performed using, for example, a ball mill, a sand mill, etc. When a ball mill is used, it is preferred to use, for example, zirconia balls as the medium.

[0311] In the present embodiment, the mixing is performed by a dry method at 150 rpm for 1 hour using a ball mill using zirconia balls having a diameter of 1 mm. The mixing is performed in a dry room having a dew point of -100°C or higher and -10°C or lower.

[0312] <Step S32> Then, in Fig. 8A In step S32, the mixed materials are recovered to obtain a mixture 903. When recovered, the materials may be screened after being crushed as needed.

[0313] <Step S33> Then, in Fig. 8A In step S33 shown, the mixture 903 is heated. The heating of step S33 is preferably performed at a temperature of 800°C to 1100°C, more preferably 800°C to 950°C, and further preferably 850°C to 900°C. In addition, the heating time of step S33 may be 1 hour to 100 hours, preferably 1 hour to 10 hours. The lower limit of the heating temperature of step S33 needs to be above the temperature at which the reaction of lithium cobalt oxide and the source of the additive element A progresses. The temperature at which the reaction progresses may be set to the temperature at which mutual diffusion of the elements contained in the source of the additive element A occurs, and may also be lower than the melting point of the above-mentioned material. Taking the oxide as an example, from the melting point T m 0.757 times (Taman temperature T d ) solid phase diffusion begins to occur, so the heating temperature in step S33 can be set above 500°C.

[0314] Of course, the reaction is more likely to proceed when the temperature is set above the temperature at which one or more of the materials selected from the mixture 903 are melted. For example, when LiF and MgF2 are included as the source of the additive element A, the eutectic point of LiF and MgF2 is around 742°C, so the lower limit of the heating temperature in step S33 is preferably set to 742°C or above.

[0315] In differential scanning calorimetry (DSC measurement), an endothermic peak of a mixture 903 obtained by mixing LiCoO2:LiF:MgF2=100:0.33:1 (molar ratio) was observed at around 830° C. Therefore, the lower limit of the heating temperature is more preferably set to 830° C. or more.

[0316] A higher heating temperature is preferred because the reaction proceeds more easily, the heating time is shortened, and the productivity is improved.

[0317] The upper limit of the heating temperature is set to be lower than the decomposition temperature of lithium cobalt oxide (1130°C). At a temperature near the decomposition temperature, slight decomposition of lithium cobalt oxide may occur. Therefore, the heating temperature is preferably 1000°C or lower, more preferably 950°C or lower, and further preferably 900°C or lower.

[0318] When the mixture 903 is heated, the partial pressure of fluorine or fluoride derived from the fluorine source or the like is preferably controlled within an appropriate range.

[0319] In the manufacturing method described in this embodiment, some materials such as LiF as a fluorine source are sometimes used as a flux. Through the above function, the heating temperature can be reduced to a temperature lower than the decomposition temperature of lithium cobalt oxide, for example, above 742°C and below 950°C, and additive elements such as magnesium can be distributed in the surface layer, thereby manufacturing a positive electrode active material with good characteristics.

[0320] However, the specific gravity of LiF in the gas state is lighter than that of oxygen, so it is possible that LiF volatilizes or sublimates by heating, and when LiF volatilizes or sublimates, the LiF in the mixture 903 decreases. At this time, the function of LiF as a flux is reduced. Therefore, it is preferred to heat while suppressing the volatilization of LiF. In addition, even if LiF is not used as a fluorine source, it is possible that Li on the surface of LiCoO2 reacts with F as a fluorine source to generate LiF and the LiF volatilizes. Therefore, even if a fluoride having a melting point higher than LiF is used, it is also necessary to suppress volatilization.

[0321] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF in the heating furnace is high. By heating as described above, volatilization of LiF in the mixture 903 can be suppressed.

[0322] The heating in this step is preferably performed in a manner that does not cause the particles of the mixture 903 to adhere together. When the particles of the mixture 903 adhere together during heating, the area of ​​the particles in contact with oxygen in the atmosphere is reduced, and the diffusion path of the added element (such as fluorine) is blocked, so that the added element (such as magnesium and fluorine) may not be easily distributed in the surface layer.

[0323] In addition, when the added element (such as fluorine) is evenly distributed in the surface layer, a smooth and less uneven positive electrode active material can be obtained. Therefore, in order to maintain the smooth state of the heated surface through step S15 or further smoothen it in this process, it is preferred that the particles of the mixture 903 are not bonded together.

[0324] In addition, when heating is performed using a rotary kiln, it is preferred to control the flow rate of the oxygen-containing atmosphere in the kiln for heating. For example, it is preferred to reduce the flow rate of the oxygen-containing atmosphere; first purge the atmosphere to introduce the oxygen atmosphere into the kiln, and then stop the atmosphere from flowing; etc. When the oxygen is flowing, the fluorine source may evaporate, which is not preferred in order to maintain the smoothness of the surface.

[0325] When heating is performed using a roller kiln, for example, by covering the container containing the mixture 903 with a lid, the mixture 903 can be heated in a LiF-containing atmosphere.

[0326] <Step S34> Then, in Fig. 8A In step S34 shown, the heated material is recovered and ground as needed to obtain the positive electrode active material 100. At this time, it is preferred that the recovered positive electrode active material 100 is also screened. Through the above process, a positive electrode active material 100 (composite oxide) with a median particle size of 12 μm or less (preferably 10.5 μm or less, more preferably 8 μm or less) can be manufactured. Note that the positive electrode active material 100 contains the added element A.

[0327] <Example 2 of Method for Producing Positive Electrode Active Material> Reference Fig. 9 FIG. 10 illustrates another example of a method for producing a positive electrode active material that can be used as one embodiment of the present invention (Example 2 of the method for producing a positive electrode active material). In Example 2 of the method for producing a positive electrode active material, the number of times the additional element is added and the mixing method are different from those in Example 1 of the method for producing a positive electrode active material, but other records can refer to the records in Example 1 of the method for producing a positive electrode active material. Note that in <Example 2 of the method for producing a positive electrode active material>, the additional element X described in Implementation Example 1 is represented as additional element A1. In addition, the additional element Y and the additional element Z described in Implementation Example 1 are collectively referred to as additional element A2.

[0328] exist Fig. 9 In, with Fig. 8A Similarly, step S10 and step S15 are performed to prepare lithium cobalt oxide that has been initially heated. Note that step S15 is not an essential structure in one embodiment of the present invention, so an embodiment in which step S15 is omitted is also included in one embodiment of the present invention.

[0329] <Step S20a> Next, as shown in step S20a, a first additional element A1 source (A1 source) is prepared. Fig. 10A The details of step S20a will be described.

[0330] <Step S21> exist Fig. 10A Step S21 shown in the figure is to prepare a first added element A1 source (A1 source). As the A1 source, it can be obtained from Figure 8C The additive element A1 is selected from the additive element A1 described in step S21. For example, any one or more selected from magnesium, fluorine and calcium can be used as the additive element A1. Fig. 10A An example is shown in which a magnesium source (Mg source) and a fluorine source (F source) are used as the additive element A1.

[0331] exist Fig. 10A Steps S21 to S23 shown in FIG. 1 can be performed by Figure 8C The production is performed under the same conditions as steps S21 to S23 shown in the figure. As a result, the added element A1 source (A1 source) can be obtained in step S23.

[0332] in addition, Fig. 9 Steps S31 to S33 shown can be performed by Fig. 8A The same conditions are used to manufacture the steps S31 to S33 shown.

[0333] <Step S34a> Next, the material heated in step S33 is recovered to obtain lithium cobalt oxide containing the additive element A1. Here, in order to distinguish it from the lithium cobalt oxide (first composite oxide) after step S15, it is also referred to as a second composite oxide.

[0334] <Step S40> exist Fig. 9 In step S40, a second source of the added element A2 (A2 source) is prepared. Fig. 10B and Fig. 10C Step S40 is described.

[0335] <Step S41> exist Fig. 10B Step S40 shown in the figure is to prepare a second added element A2 source (A2 source). As the A2 source, it can be obtained from Figure 8C The additive element A2 is selected from the additive element A described in step S20. For example, any one or more selected from nickel, titanium, boron, zirconium and aluminum can be suitably used as the additive element A2. Fig. 10B An example is shown in which a nickel source (Ni source) and an aluminum source (Al source) are used as the additive element A2.

[0336] Fig. 10B Steps S41 to S43 shown in FIG. Figure 8C The same conditions are applied to steps S21 to S23 as shown. As a result, the added element A2 source (A2 source) can be obtained in step S43.

[0337] Fig. 10C Steps S41 to S43 shown are Fig. 10B An example of a deformation of . Fig. 10C In step S41, a nickel source (Ni source) and an aluminum source (Al source) are prepared, and they are crushed independently in step S42a. As a result, a plurality of second additional element A2 sources (A2 sources) are prepared in step S43. Fig. 10C Step S40 and Fig. 10B The difference of step S40 is that the additional element source is pulverized independently in step S42a.

[0338] <Step S51 to Step S53> then, Fig. 9 Steps S51 to S53 shown in FIG. Fig. 8A The conditions of step S53 of the heating process are preferably the same as those of step S31 to step S34. Fig. 9 The temperature of step S33 is lower or / and the time is shorter than that shown in FIG. Specifically, the heating is preferably 800° C. to 950° C., more preferably 820° C. to 870° C., and further preferably 850° C.±10° C. The heating time is, for example, preferably 0.5 hours to 8 hours, more preferably 1 hour to 5 hours.

[0339] Note that when nickel is selected as the additive element A2, the mixing in step S51 is preferably performed in such a manner that the number of nickel atoms in the nickel source is 0.05% or more and 4% or less of the number of cobalt atoms in the lithium cobalt oxide after step S15. In addition, when aluminum is selected as the additive element A2, the mixing in step S51 is preferably performed in such a manner that the number of aluminum atoms in the aluminum source is 0.05% or more and 4% or less of the number of cobalt atoms in the lithium cobalt oxide after step S15.

[0340] <Step S54> Then, in Fig. 9 In step S54 shown, the heated material is recovered and ground as needed to obtain a positive electrode active material 100. Through the above process, a positive electrode active material 100 (composite oxide) having a median particle size of 12 μm or less (preferably 10.5 μm or less, more preferably 8 μm or less) can be manufactured. In addition, a positive electrode active material 100 that can be used for a lithium ion battery having good discharge characteristics even in a low temperature environment can be manufactured. The positive electrode active material 100 contains an additive element A1 and an additive element A2.

[0341] In the manufacturing method example 2 described above, as Fig. 9 As shown in FIG10 , the additive elements are divided into a first additive element A1 and a second additive element A2 and introduced into the lithium cobalt oxide. By introducing the additive elements separately, the distribution of each additive element along the depth direction can be changed. For example, the first additive element can be distributed in a manner that the concentration in the surface portion is higher than that in the interior, and the second additive element can be distributed in a manner that the concentration in the interior portion is higher than that in the surface portion. Fig. 8A and Fig.8D The positive electrode active material 100 manufactured by the steps of adding multiple additive elements A sources together has the advantage of being able to be manufactured at low cost. Fig. 9 10 manufactures the positive electrode active material 100 by adding a plurality of sources of the additive element A in a plurality of steps, so the manufacturing cost is relatively high, but the distribution of each additive element A in the depth direction can be more accurately controlled, so it is preferred.

[0342] This embodiment mode can be used in combination with other embodiment modes as desired.

[0343] (Implementation 3) In this embodiment, elements constituting a lithium ion battery are described.

[0344] [positive electrode] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer contains a positive electrode active material and may further contain at least one of a conductive material and a binder. As the positive electrode active material, the material described in Embodiment 1 may also be used.

[0345] Fig.11A An example of a schematic diagram showing a cross section of a positive electrode is shown.

[0346] The positive electrode current collector 21 may be, for example, a metal foil. The positive electrode may be formed by applying a slurry on a metal foil and drying it. Alternatively, the slurry may be pressed after drying. In the positive electrode, an active material layer is formed on the positive electrode current collector 21.

[0347] The slurry is a material liquid used to form an active material layer on the positive electrode current collector 21, and contains an active material, a binder and a solvent, and preferably also contains a conductive material. The slurry is sometimes referred to as an electrode slurry or an active material slurry. Sometimes, the positive electrode slurry is used when forming a positive electrode active material layer, and sometimes, the negative electrode slurry is used when forming a negative electrode active material layer.

[0348] The positive electrode active material 100 has the function of absorbing lithium ions and releasing lithium ions accompanying charge and discharge. As a positive electrode active material 100 used in one embodiment of the present invention, a material with little degradation accompanying charge and discharge even when a high charging voltage is used. In this specification, etc., unless otherwise specified, the charging voltage is expressed based on the potential of lithium metal.

[0349] As the positive electrode active material 100 used in one embodiment of the present invention, any material can be used as long as it is a material that has little deterioration accompanying charge and discharge even when a high charging voltage is used, and the materials described in Embodiment 1 or Embodiment 2 can be used. In addition, as long as the positive electrode active material 100 is a material that has little deterioration accompanying charge and discharge even when a high charging voltage is used, two or more materials with different particle sizes can be used.

[0350] FIG. 11A to FIG. 11D Show Figure 1B The deformation example of the positive electrode active material layer is shown.

[0351] Fig.11A Carbon black 43 as an example of a conductive material and an electrolyte 51 contained in gaps between particles of the positive electrode active material 100 are shown. The electrolyte 51 includes a second positive electrode active material 110 in addition to the positive electrode active material 100 .

[0352] In order to fix the positive electrode current collector 21 and the active material such as metal foil, the positive electrode of the secondary battery can also be mixed with an adhesive (resin). Adhesive is also called a binder. Adhesive is a polymer material. When a large amount of adhesive is included, the ratio of the active material in the positive electrode is reduced and the discharge capacity of the secondary battery is reduced. Therefore, it is preferred to mix the amount of adhesive to a minimum.

[0353] Fig.11A The example in which the positive electrode active material 100 is spherical is shown, but there is no particular limitation on the shape. The cross-sectional shape of the positive electrode active material 100 may be, for example, an ellipse, a rectangle, a trapezoid, a triangle, a polygon with an arcuate corner, or an asymmetric shape. For example, Fig. 11B An example is shown in which the positive electrode active material 100 has a polygonal shape with rounded corners.

[0354] In addition, Fig. 11B In the positive electrode, graphene 42 is used as a carbon material used as a conductive material. Fig. 11B In the embodiment, a positive electrode active material layer including a positive electrode active material 100 , graphene 42 , and carbon black 43 is formed on the positive electrode current collector 21 .

[0355] Note that in the step of mixing the graphene 42 and the carbon black 43 to obtain the electrode slurry, the weight of the mixed carbon black is preferably 1.5 times or more and 20 times or less, and preferably 2 times or more and 9.5 times or less, that of the graphene.

[0356] When the mixing of graphene 42 and carbon black 43 is set within the above range, the dispersion stability of carbon black 43 is excellent when adjusting the slurry, and it is not easy to generate an aggregation part. In addition, when the mixing of graphene 42 and carbon black 43 is set within the above range, a high electrode density can be achieved compared to a positive electrode using only carbon black 43 as a conductive material. By increasing the electrode density, the capacity per unit weight can be increased. Specifically, the density of the positive electrode active material layer measured by weight can be 3.5 g / cc or more.

[0357] Compared with a positive electrode using only graphene as a conductive material, the electrode density is low, but the mixing of the first carbon material (graphene) and the second carbon material (acetylene black) is within the above range, thereby enabling correspondingly fast charging. Therefore, this is particularly effective when used for a vehicle-mounted secondary battery.

[0358] exist Fig. 11C , an example of a positive electrode using carbon fibers 44 instead of graphene is shown. Fig. 11C Shown with Fig. 11B Different example: By using carbon fiber 44, aggregation of carbon black 43 can be prevented and dispersibility can be improved.

[0359] Note that Fig. 11C In the figure, the region not filled with the positive electrode active material 100, the carbon fiber 44, and the carbon black 43 refers to a void or a binder.

[0360] Fig.11D Other examples of positive electrodes are shown. Fig. 11C An example is shown in which carbon fibers 44 are used instead of graphene 42. By using both graphene 42 and carbon fibers 44, aggregation of carbon black such as carbon black 43 can be prevented, and thus dispersibility can be improved.

[0361] Note that Fig.11D In the figure, the region not filled with the positive electrode active material 100, the carbon fiber 44, the graphene 42, and the carbon black 43 refers to a void or a binder.

[0362] The secondary battery can be manufactured by the following steps: FIG. 11A to FIG. 11D Any positive electrode in the above is stacked with a separator on the positive electrode, and the stacked body in which the negative electrode is stacked on the separator is placed in a container (an outer packaging body, a metal can, etc.) and the container is filled with an electrolyte.

[0363] <Adhesive> As the adhesive, for example, preferably used are rubber materials such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Fluorine rubber can also be used as the adhesive.

[0364] In addition, as the binder, for example, a water-soluble polymer is preferably used. As the water-soluble polymer, for example, polysaccharides can also be used. As the polysaccharides, cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, regenerated cellulose, starch, etc. can be used. It is more preferred to use these water-soluble polymers and the above-mentioned rubber material in combination.

[0365] Alternatively, as an adhesive, it is preferred to use materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose.

[0366] As the binder, a plurality of the above-mentioned materials may be used in combination.

[0367] For example, materials with particularly good viscosity regulating effects can also be used in combination with other materials. For example, although rubber materials and the like have high cohesive force and high elasticity, it is sometimes difficult to regulate viscosity when mixed in a solvent. In such a case, for example, it is preferably mixed with materials with particularly good viscosity regulating effects. As materials with particularly good viscosity regulating effects, for example, water-soluble polymers can be used. In addition, as water-soluble polymers with particularly good viscosity regulating functions, the above-mentioned polysaccharides can be used, for example, cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, or starch can be used.

[0368] Note that cellulose derivatives such as carboxymethyl cellulose, for example, can be easily used as viscosity modifiers by being converted into salts such as sodium salts and ammonium salts of carboxymethyl cellulose to improve their solubility. Due to the increased solubility, the dispersibility of active materials or other components can be improved when forming a slurry for an electrode. In this specification, etc., cellulose and cellulose derivatives used as binders for electrodes include their salts.

[0369] By dissolving a water-soluble polymer in water to stabilize its viscosity, the active material and other materials used as a binder combination, such as styrene-butadiene rubber, can be stably dispersed in an aqueous solution. Since the water-soluble polymer has a functional group, it is expected to be easily and stably attached to the surface of the active material. Most cellulose derivatives such as carboxymethyl cellulose have functional groups such as hydroxyl groups or carboxyl groups. Since they have functional groups, the polymer is expected to interact with each other and widely cover the surface of the active material.

[0370] When the binder covering or contacting the surface of the active material forms a film, it is also expected to be used as a passivation film to exert an effect of inhibiting the decomposition of the electrolyte. Here, the "passivation film" is a film that has no conductivity or very low conductivity. For example, when the passivation film is formed on the surface of the active material, it inhibits the decomposition of the electrolyte at the battery reaction potential. More preferably, the passivation film can transmit lithium ions while inhibiting the conductivity.

[0371] <Conductive Materials> Conductive materials are also called conductive agents or conductive aids, and carbon materials are used. By attaching conductive materials between multiple active materials, multiple active materials are electrically connected to each other and the conductivity is improved. Note that "attachment" does not mean that the active material and the conductive material are physically in close contact, but refers to the concept that includes the following situations: when covalent bonds occur; when bonded by van der Waals forces; when the conductive material covers part of the surface of the active material; when the conductive material is inserted into the surface unevenness of the active material; when they are electrically connected without contact, etc.

[0372] The active material layer such as the positive electrode active material layer and the negative electrode active material layer preferably contains a conductive material.

[0373] As the conductive material, for example, any one or two or more of carbon black such as acetylene black and furnace black, graphite such as artificial graphite and natural graphite, carbon fibers such as carbon nanofibers and carbon nanotubes, and graphene compounds can be used.

[0374] As the carbon fiber, for example, mesophase pitch carbon fiber, isotropic pitch carbon fiber, etc. can be used. In addition, as the carbon fiber, carbon nanofiber or carbon nanotube can be used. For example, carbon nanotube can be produced by vapor phase growth or the like.

[0375] The graphene compounds in this specification, etc. include graphene, multilayer graphene, multigraphene, graphene oxide, multilayer graphene oxide, multigraphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multigraphene oxide, graphene quantum dots, etc. Graphene compounds refer to compounds containing carbon and having a two-dimensional structure formed by a six-membered ring composed of carbon atoms in a flat plate, sheet, etc. shape. In addition, the two-dimensional structure formed by the six-membered ring composed of carbon atoms can be called a carbon sheet. Graphene compounds may also have functional groups. In addition, graphene compounds preferably have a curved shape. In addition, graphene compounds may also be curled up like carbon nanofibers.

[0376] The content of the conductive material in the total amount of the active material layer is preferably 1 wt % to 10 wt %, more preferably 1 wt % to 5 wt %.

[0377] Unlike granular conductive materials such as carbon black that form point contact with the active material, the graphene compound can form a surface contact with low contact resistance, so the conductivity of the granular active material and the graphene compound can be improved with a smaller amount than that of a general conductive material. Therefore, the ratio of the active material in the active material layer can be increased. As a result, the discharge capacity of the battery can be increased.

[0378] Carbon compounds in the form of particles such as carbon black and graphite or fibrous carbon compounds such as carbon nanotubes can easily enter microspaces. Microspaces refer to, for example, regions between multiple active materials. By combining carbon compounds that can easily enter microspaces and sheet-like carbon compounds such as graphene that can impart conductivity to multiple particles, the density of the electrode can be increased and a good conductive path can be formed. The battery obtained by the manufacturing method of one embodiment of the present invention can have high capacity density and stability, so it is very effective as a vehicle-mounted battery.

[0379] <Positive Electrode Current Collector> As the positive electrode current collector, materials with high conductivity such as stainless steel, gold, platinum, aluminum, titanium and their alloys can be used. In addition, the material used for the positive electrode current collector is preferably not dissolved due to the potential of the positive electrode. In addition, aluminum alloys to which elements such as silicon, titanium, neodymium, scandium, molybdenum, etc. that improve heat resistance are added can be used. In addition, metal elements that react with silicon to form silicides can also be used. As metal elements that react with silicon to form silicides, there are zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, nickel, etc. As the current collector, shapes such as foil, plate, sheet, mesh, punched metal mesh, and drawn metal mesh can be appropriately used. The thickness of the current collector is preferably 5 μm or more and 30 μm or less.

[0380] [negative electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. In addition, the negative electrode active material layer may also include a negative electrode active material and further include a conductive material and a binder.

[0381] <Negative Electrode Active Material> As the negative electrode active material, for example, an alloy material or a carbon material can be used.

[0382] As the negative electrode active material, an element that can perform a charge and discharge reaction by alloying / de-alloying reaction with lithium can be used. For example, a material containing at least one selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium and indium can be used. The capacity of such an element is higher than that of carbon, and in particular, the theoretical capacity of silicon is high, which is 4200mAh / g. Therefore, silicon is preferably used for the negative electrode active material. In addition, compounds containing these elements can also be used. For example, SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb and SbSn can be cited. Here, an element capable of performing a charge-discharge reaction through an alloying / de-alloying reaction with lithium, a compound containing the element, and the like are sometimes referred to as an alloy-based material.

[0383] In this specification, "SiO" refers to silicon monoxide, for example. Alternatively, SiO may also be represented as SiO x Here, x preferably represents a value of 1 or a value close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.

[0384] As the carbon material, graphite, easily graphitizable carbon (soft carbon), hardly graphitizable carbon (hard carbon), carbon fiber (carbon nanotube), graphene, carbon black, or the like can be used.

[0385] As graphite, artificial graphite or natural graphite can be cited. As artificial graphite, for example, mesocarbon microbeads (MCMB), coke-based artificial graphite, pitch-based artificial graphite, etc. can be cited. Here, spherical graphite with a spherical shape can be used as artificial graphite. For example, MCMB sometimes has a spherical shape, so it is preferred. In addition, MCMB is relatively easy to reduce its surface area, so it is sometimes preferred. As natural graphite, for example, flaky graphite, spheroidized natural graphite, etc. can be cited.

[0386] When lithium ions are inserted into graphite (when lithium-graphite intercalation compounds are generated), graphite shows a potential as low as that of lithium metal (0.05 V or more and 0.3 V or less vs. Li / Li + ). As a result, lithium-ion batteries using graphite can show high operating voltages. Graphite also has the following advantages: large capacity per unit volume; relatively small volume expansion; relatively cheap; and higher safety than lithium metal, so it is preferred.

[0387] In addition, as the negative electrode active material, oxides such as titanium dioxide (TiO2), lithium titanium oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5), tungsten dioxide (WO2), molybdenum dioxide (MoO2), etc.

[0388] In addition, as the negative electrode active material, Li 3N type structure containing lithium and transition metal nitride can be used. 3-x M x N (M = Co, Ni, Cu). For example, Li 2.6 Co 0.4 N3 shows a large charge and discharge capacity (900 mAh / g, 1890 mAh / cm 3 ), so it is preferred.

[0389] When a nitride containing lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so it can be combined with a material that does not contain lithium ions, such as V2O5 and Cr3O8, which is used as a positive electrode active material, and is therefore preferred. Note that when a material containing lithium ions is used as a positive electrode active material, a nitride containing lithium and a transition metal can also be used as a negative electrode active material by previously removing the lithium ions contained in the positive electrode active material.

[0390] In addition, materials that cause conversion reactions can also be used as negative electrode active materials. For example, transition metal oxides that do not form alloys with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can be used as negative electrode active materials. Materials that cause conversion reactions can also include oxides such as Fe2O3, CuO, Cu2O, RuO2, and Cr2O3, CoS 0.89 , sulfides such as NiS, CuS, nitrides such as Zn3N2, Cu3N, Ge3N4, phosphides such as NiP2, FeP2, CoP3, fluorine compounds such as FeF3, BiF3.

[0391] In addition, as another form of the negative electrode, it can also be a negative electrode that does not contain a negative electrode active material at the end of battery manufacturing. As a negative electrode that does not contain a negative electrode active material, for example, the following negative electrode can be used, which only contains a negative electrode collector at the end of forming the battery manufacturing, and the lithium ions separated from the positive electrode active material due to the charging of the battery are precipitated in the form of lithium metal on the negative electrode collector, thereby forming a negative electrode active material layer. The battery using this negative electrode is sometimes called a negative electrode-free (anode-free) battery, etc.

[0392] When using a negative electrode that does not contain a negative electrode active material, a film for homogenizing the precipitation of lithium may also be included on the negative electrode current collector. As a film for homogenizing the precipitation of lithium, for example, a solid electrolyte with lithium ion conductivity can be used. As a solid electrolyte, a sulfide solid electrolyte, an oxide solid electrolyte, and a polymer solid electrolyte can be used. Among them, the film of the polymer solid electrolyte is relatively easy to form evenly on the negative electrode current collector, so it is suitable for a film for homogenizing the precipitation of lithium. In addition, as a film for homogenizing the precipitation of lithium, for example, a metal film that forms an alloy with lithium can be used. As a metal film that forms an alloy with lithium, for example, a magnesium metal film can be used. Since lithium and magnesium form a solid solution in a wider composition range, it is suitable for a film for uniformly precipitating lithium.

[0393] In addition, when using a negative electrode that does not contain a negative electrode active material, a negative electrode current collector having concave and convex portions can be used. When using a negative electrode current collector having concave and convex portions, the concave portions of the negative electrode current collector are cavities that are easy to precipitate lithium contained in the negative electrode current collector, thereby preventing the shape of lithium from becoming dendritic when it precipitates.

[0394] As the conductive material and the binder which may be contained in the negative electrode active material layer, the same conductive material and the binder which may be contained in the positive electrode active material layer may be used.

[0395] <Negative Electrode Current Collector> As the negative electrode current collector, in addition to the same materials as the positive electrode current collector, copper foil, copper medal, etc. can also be used. In addition, as the negative electrode current collector, it is preferable to use a material that does not alloy with carrier ions such as lithium.

[0396] [Electrolytes] As the electrolyte, the membrane described in Embodiment 1 can be used as appropriate.

[0397] [Isolated Body] When the electrolyte includes an electrolyte solution, a separator is disposed between the positive electrode and the negative electrode. As the separator, for example, the following materials can be used: a material formed of a fiber having cellulose such as paper, a nonwoven fabric, a glass fiber, a ceramic, or a synthetic fiber such as nylon (polyamide), vinylon (polyvinyl alcohol-based fiber), polyester, acrylic resin, polyolefin, or polyurethane. The separator is preferably processed into a bag shape and disposed so as to surround either the positive electrode or the negative electrode.

[0398] The separator may have a multilayer structure. For example, a ceramic material, a fluorine material, a polyamide material or a mixture thereof may be coated on a thin film of an organic material such as polypropylene or polyethylene. As a ceramic material, for example, aluminum oxide particles or silicon oxide particles may be used. As a fluorine material, for example, PVDF or polytetrafluoroethylene may be used. As a polyamide material, for example, nylon or aromatic polyamide (meta-aramid or para-aramid) may be used.

[0399] By coating ceramic materials, the oxidation resistance is improved, thereby suppressing the degradation of the separator during high voltage charging, thereby improving the reliability of the secondary battery. By coating fluorine materials, it is easy to make the separator close to the electrode, which can improve the output characteristics. By coating polyamide materials (especially aromatic polyamide), the heat resistance is improved, thereby improving the safety of the secondary battery.

[0400] For example, a mixture of aluminum oxide and aramid may be applied to both sides of a polypropylene film. Alternatively, a mixture of aluminum oxide and aramid may be applied to the surface of the polypropylene film in contact with the positive electrode and a fluorine-based material may be applied to the surface in contact with the negative electrode.

[0401] By adopting a separator with a multi-layer structure, the safety of the secondary battery can be ensured even if the total thickness of the separator is small, and thus the capacity per unit volume of the secondary battery can be increased.

[0402] [Outer packaging] As the outer packaging body included in the secondary battery, for example, a metal material such as aluminum or a resin material can be used. In addition, a film-shaped outer packaging body can also be used. As the film, for example, a three-layer film can be used: a metal film with excellent flexibility such as aluminum, stainless steel, copper, nickel, etc. is arranged on a film composed of materials such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and an insulating synthetic resin film such as polyamide resin, polyester resin, etc. can also be arranged on the metal film as the outer surface of the outer packaging body.

[0403] This embodiment mode can be used in combination with other embodiment modes.

[0404] (Implementation 4) In this embodiment, an example of the shape of a secondary battery including a positive electrode manufactured by the manufacturing method described in the above embodiment will be described.

[0405] [Coin-type secondary battery] An example of a coin-type secondary battery will be described. Fig. 12A This is an exploded perspective view of a coin-type (single-layer flat) secondary battery. Fig. 12B This is its appearance picture. Fig. 12C Coin-type secondary batteries are mainly used in small electronic devices.

[0406] In order to easily understand the overlapping relationship (upper and lower relationship and position relationship) of components, Fig. 12A A schematic diagram is used. Therefore, Fig. 12A Not with Fig. 12B Exactly the same picture.

[0407] exist Fig. 12A In the embodiment, the positive electrode 304, the separator 310, the negative electrode 307, the spacer 322, and the gasket 312 are stacked. Then, the negative electrode can 302, the positive electrode can 301, and the gasket are used to seal the above components. Fig. 12A The gasket used for sealing is not shown. The spacer 322 and the gasket 312 are used to protect the inside or fix the position in the tank when the positive electrode tank 301 and the negative electrode tank 302 are pressed together. The spacer 322 and the gasket 312 are made of stainless steel or insulating material.

[0408] A stacked structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 is referred to as a positive electrode 304 .

[0409] Fig. 12B It is a perspective view of the manufactured coin-type secondary battery.

[0410] In the coin-type secondary battery 300, a positive electrode can 301 also serving as a positive terminal and a negative electrode can 302 also serving as a negative terminal are insulated and sealed by a gasket 303 formed of polypropylene or the like. The positive electrode 304 is formed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. In addition, the negative electrode 307 is formed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. In addition, the negative electrode 307 is not limited to a laminated structure, and a lithium metal foil or an alloy foil of lithium and aluminum may be used.

[0411] In the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 , the active material layer may be formed on one surface of the positive electrode and the negative electrode, respectively.

[0412] As the positive electrode can 301 and the negative electrode can 302, metals such as nickel, aluminum, and titanium, alloys thereof, and alloys of these and other metals (such as stainless steel, etc.) that are resistant to corrosion by the electrolyte can be used. In addition, in order to prevent corrosion caused by the electrolyte, etc., the positive electrode can 301 and the negative electrode can 302 are preferably covered with nickel, aluminum, etc. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.

[0413] By immersing the negative electrode 307, the positive electrode 304 and the separator 310 in an electrolyte, Fig. 12C As shown, the positive electrode can 301 is placed at the bottom, the positive electrode 304, the separator 310, the negative electrode 307 and the negative electrode can 302 are stacked in order, and the positive electrode can 301 and the negative electrode can 302 are pressed with the gasket 303 interposed therebetween to manufacture the coin-type secondary battery 300.

[0414] By adopting the above structure, it is possible to manufacture the coin-type secondary battery 300 having a high discharge capacity and excellent cycle characteristics.

[0415] [Cylindrical secondary battery] Next, refer to Fig.13A An example of a cylindrical secondary battery will be described. Fig.13A As shown, the top surface of the cylindrical secondary battery 616 includes a positive electrode cover (battery cover) 601, and the side and bottom surfaces thereof include a battery can (outer can) 602. The positive electrode cover 601 and the battery can (outer can) 602 are insulated by a gasket (insulating gasket) 610.

[0416] Fig. 13B It is a diagram schematically showing a cross section of a cylindrical secondary battery. Fig. 13B The cylindrical secondary battery shown has a positive electrode cover (battery cover) 601 on the top surface and a battery can (outer can) 602 on the side and bottom surfaces. The positive electrode cover and the battery can (outer can) 602 are insulated by a gasket (insulating gasket) 610.

[0417] A battery element is provided inside the hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a strip-shaped negative electrode 606 are wound around a separator 605. Although not shown, the battery element is wound around the central axis. One end of the battery can 602 is closed and the other end is open. As the battery can 602, metals such as nickel, aluminum, titanium, their alloys, and alloys of them and other metals (such as stainless steel, etc.) that are resistant to corrosion by the electrolyte can be used. In addition, in order to prevent corrosion caused by the electrolyte, the battery can 602 is preferably covered with nickel, aluminum, etc. On the inside of the battery can 602, the battery element in which the positive electrode, the negative electrode, and the separator are wound is sandwiched by a pair of opposing insulating plates 608 and insulating plates 609. In addition, a non-aqueous electrolyte (not shown) is injected into the interior of the battery can 602 in which the battery element is provided. As a non-aqueous electrolyte, the same electrolyte as a coin-type secondary battery can be used.

[0418] Since the positive electrode and the negative electrode used for the cylindrical storage battery are wound, the active material is preferably formed on both surfaces of the current collector.

[0419] By using the positive electrode active material 100 obtained in Embodiments 1 and 2, etc., for the positive electrode 604, a cylindrical secondary battery 616 having a high capacity, a high discharge capacity, and excellent cycle characteristics can be manufactured.

[0420] The positive electrode 604 is connected to the positive terminal (positive electrode current collecting wire) 603, and the negative electrode 606 is connected to the negative terminal (negative electrode current collecting wire) 607. Metal materials such as aluminum can be used for both the positive terminal 603 and the negative terminal 607. The positive terminal 603 is resistance-welded to the safety valve mechanism 613, and the negative terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cover 601 through a PTC (Positive Temperature Coefficient) element 611. When the internal pressure of the battery rises to exceed a specified threshold, the safety valve mechanism 613 cuts off the electrical connection between the positive electrode cover 601 and the positive electrode 604. In addition, the PTC element 611 is a thermally sensitive resistance element whose resistance increases when the temperature rises, and limits the current by increasing the resistance to prevent abnormal heating. As a PTC element, barium titanate (BaTiO3)-based semiconductor ceramics, etc. can be used.

[0421] Fig. 13C An example of a power storage system 615 is shown. The power storage system 615 includes a plurality of secondary batteries 616. The positive electrode of each secondary battery contacts a conductor 624 separated by an insulator 625, and the positive electrodes are electrically connected to each other. The conductor 624 is electrically connected to a control circuit 620 via a wiring 623. In addition, the negative electrode of each secondary battery is electrically connected to the control circuit 620 via a wiring 626. As the control circuit 620, a charge and discharge control circuit for performing charge and discharge, a protection circuit for preventing overcharge and / or overdischarge, etc. can be used.

[0422] Fig.13D An example of a power storage system 615 is shown. The power storage system 615 includes a plurality of secondary batteries 616, and the plurality of secondary batteries 616 are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of secondary batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 through a wiring 627. The plurality of secondary batteries 616 may be connected in parallel or in series, or may be connected in parallel and then in series. By configuring the power storage system 615 including the plurality of secondary batteries 616, a large amount of electric power can be obtained.

[0423] Alternatively, a plurality of secondary batteries 616 may be connected in parallel and then connected in series.

[0424] In addition, a temperature control device may be included between the plurality of secondary batteries 616. When the secondary battery 616 is overheated, it can be cooled by the temperature control device, and when the secondary battery 616 is overcooled, it can be heated by the temperature control device. Therefore, the performance of the power storage system 615 is not easily affected by the external temperature.

[0425] In addition, Fig.13D In FIG. 6 , the power storage system 615 is electrically connected to the control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of secondary batteries 616 via the conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of secondary batteries 616 via the conductive plate 614.

[0426] [Other structural examples of secondary batteries] An example of the structure of a secondary battery will be described using FIG. 14 and FIG. 15 .

[0427] Fig.14A The secondary battery 913 shown includes a winding body 950 provided with a terminal 951 and a terminal 952 inside a frame 930. The winding body 950 is impregnated with an electrolyte inside the frame 930. The terminal 952 is in contact with the frame 930, and the terminal 951 is prevented from contacting the frame 930 by an insulating material. Note that for convenience, although Fig.14A Frame 930 is shown separately in the figure, but in reality, winding body 950 is covered by frame 930, and terminals 951 and 952 extend outside frame 930. Frame 930 can be made of a metal material (such as aluminum) or a resin material.

[0428] In addition, if Fig. 14B As shown, multiple materials can also be used to form Fig.14A For example, in the frame 930 shown in FIG. Fig. 14B In the secondary battery 913 shown, a frame body 930 a and a frame body 930 b are bonded together, and a wound body 950 is provided in a region surrounded by the frame bodies 930 a and 930 b.

[0429] As the frame 930a, an insulating material such as an organic resin can be used. In particular, by using a material such as an organic resin to form the surface of the antenna, it is possible to suppress the shielding of the electric field by the secondary battery 913. In addition, if the electric field shielding caused by the frame 930a is small, the antenna can also be provided inside the frame 930a. As the frame 930b, for example, a metal material can be used.

[0430] Furthermore, Fig. 14C The structure of the wound body 950 is shown. The wound body 950 includes a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is formed by overlapping the negative electrode 931 and the positive electrode 932 with the separator 933 interposed therebetween to form a laminated sheet, and then winding the laminated sheet. In addition, a plurality of layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.

[0431] Alternatively, a secondary battery 913 including a wound body 950 a as shown in FIG. 15 may be used. Fig.15A The wound body 950a shown includes a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 includes a negative electrode active material layer 931a. The positive electrode 932 includes a positive electrode active material layer 932a.

[0432] By using the positive electrode active material 100 that can be obtained in Embodiments 1 and 2 for the positive electrode 932 , a secondary battery 913 having a high capacity, a high discharge capacity, and excellent cycle characteristics can be manufactured.

[0433] The separator 933 is wider than the negative electrode active material layer 931a and the positive electrode active material layer 932a, and is wound so as to overlap the negative electrode active material layer 931a and the positive electrode active material layer 932a. In addition, from the viewpoint of safety, it is preferable that the negative electrode active material layer 931a is wider than the positive electrode active material layer 932a. In addition, the winding body 950a of the above shape is preferable because of its good safety and productivity.

[0434] like Fig. 15B As shown, the negative electrode 931 is electrically connected to the terminal 951 by ultrasonic bonding, welding or pressing. The terminal 951 is electrically connected to the terminal 911a. In addition, the positive electrode 932 is electrically connected to the terminal 952 by ultrasonic bonding, welding or pressing. The terminal 952 is electrically connected to the terminal 911b.

[0435] like Fig. 15C As shown, the wound body 950a and the electrolyte are covered by the frame 930 to form a secondary battery 913. The frame 930 is preferably provided with a safety valve, an overcurrent protection element, etc. The safety valve is a valve that is opened at a specified internal pressure in the frame 930 to prevent battery rupture.

[0436] like Fig. 15B As shown, the secondary battery 913 may also include a plurality of winding bodies 950a. By using a plurality of winding bodies 950a, a secondary battery 913 with a larger discharge capacity can be realized. Fig.15A and Fig. 15B The other components of the secondary battery 913 shown can be referred to FIG. 14A to FIG. 14C The secondary battery 913 is shown.

[0437] <Laminated secondary battery> then, Fig.16A and Fig. 16B 1 is an external view showing an example of a laminated secondary battery. Fig.16A and Fig. 16B A positive electrode 503 , a negative electrode 506 , a separator 507 , an outer package 509 , a positive electrode lead electrode 510 , and a negative electrode lead electrode 511 are all shown.

[0438] Fig.17A It is an appearance diagram of a positive electrode 503 and a negative electrode 506. The positive electrode 503 includes a positive electrode current collector 501, and a positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. In addition, the positive electrode 503 has an area where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab area). The negative electrode 506 includes a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. In addition, the negative electrode 506 has an area where the negative electrode current collector 504 is partially exposed, namely, the tab area. The area or shape of the tab area of ​​the positive electrode and the negative electrode is not limited to Fig.17A Example shown.

[0439] <Method for manufacturing laminated secondary battery> Here, refer to Fig. 17B and Fig. 17C Yes Fig.16A An example of a method for producing a laminated secondary battery whose appearance is shown in FIG. 1 is described below.

[0440] First, the negative electrode 506, the separator 507, and the positive electrode 503 are stacked. Fig. 17B The stacked negative electrode 506, separator 507 and positive electrode 503 are shown. Here, an example using 5 sets of negative electrodes and 4 sets of positive electrodes is shown. In addition, it can also be said that it is a stacked body composed of negative electrodes, separators, and positive electrodes. Next, the tab regions of the positive electrode 503 are joined to each other, and the positive electrode lead electrode 510 is joined to the tab region of the outermost positive electrode. As the joining, ultrasonic welding or the like can be used, for example. Similarly, the tab regions of the negative electrode 506 are joined to each other, and the negative electrode lead electrode 511 is joined to the tab region of the outermost negative electrode.

[0441] Next, the negative electrode 506 , the separator 507 , and the positive electrode 503 are arranged on the outer packaging body 509 .

[0442] Below, as Fig. 17C As shown, the outer package 509 is folded along the portion indicated by the dotted line. Then, the outer periphery of the outer package 509 is joined. As the joining method, for example, heat pressing or the like can be used. At this time, in order to inject the electrolyte later, a non-joined area (hereinafter referred to as the introduction port) is provided on a part (or one side) of the outer package 509.

[0443] Next, the electrolyte is introduced into the inner side of the outer packaging body 509 from the introduction port provided in the outer packaging body 509. The electrolyte is preferably introduced under a reduced pressure atmosphere or an inert gas atmosphere. Finally, the introduction port is joined. In this way, the laminated secondary battery 500 can be manufactured.

[0444] By using the positive electrode active material 100 that can be obtained in Embodiments 1 and 2, etc., for the positive electrode 503, a secondary battery 500 having a high capacity, a high discharge capacity, and excellent cycle characteristics can be manufactured.

[0445] [Battery pack example] An example of a secondary battery pack according to one embodiment of the present invention that can be wirelessly charged using an antenna will be described with reference to FIG. 18 .

[0446] Fig.18A 1 is a diagram showing the appearance of a secondary battery pack 531 , which has a thin rectangular parallelepiped shape (or a relatively thick flat plate shape). Fig.18B 5 is a diagram for explaining the structure of a secondary battery pack 531. The secondary battery pack 531 includes a circuit board 540 and a secondary battery 513. A label 529 is attached to the secondary battery 513. The circuit board 540 is fixed by a sealing tape 515. The secondary battery pack 531 also includes an antenna 517.

[0447] The interior of the secondary battery 513 may have a structure including a wound body or a structure including a stacked body.

[0448] like Fig.18B As shown, in the secondary battery pack 531, for example, a control circuit 590 is provided on a circuit board 540. In addition, the circuit board 540 is electrically connected to the terminal 514. In addition, the circuit board 540 is electrically connected to the antenna 517, one of the positive and negative wires 551 of the secondary battery 513, and the other of the positive and negative wires 552.

[0449] In addition, if Fig. 18C As shown, it may also include a circuit system 590 a disposed on the circuit board 540 and a circuit system 590 b electrically connected to the circuit board 540 through the terminal 514 .

[0450] In addition, the shape of antenna 517 is not limited to a coil shape, for example, it can be a linear or plate shape. In addition, antennas such as a planar antenna, an aperture antenna, a traveling wave antenna, an EH antenna, a magnetic field antenna, or a dielectric antenna can also be used. Alternatively, antenna 517 can also be a flat conductor. The flat conductor can also be used as one of the conductors for electric field coupling. In other words, antenna 517 can also be used as one of the two conductors possessed by a capacitor. Thus, not only electromagnetic and magnetic fields are utilized, but also electric fields can be utilized to exchange electric power.

[0451] The secondary battery pack 531 includes a layer 519 between the antenna 517 and the secondary battery 513. The layer 519 has a function of shielding the electromagnetic field from the secondary battery 513, for example. As the layer 519, a magnetic body can be used, for example.

[0452] This embodiment mode can be used in combination with other embodiment modes.

[0453] (Implementation 5) In this embodiment, an example of a vehicle equipped with a secondary battery according to one embodiment of the present invention is described.

[0454] As a vehicle, a secondary battery can typically be used in a car. As a car, a new generation of clean energy vehicles such as a hybrid electric vehicle (HV), an electric vehicle (EV) or a plug-in hybrid electric vehicle (also referred to as PHEV or PHV) can be cited, and a secondary battery can be used as one of the power sources installed in the car. Vehicles are not limited to cars. For example, as a vehicle, a tram, a monorail, a ship, a submarine (submersible, unmanned submarine), a flying object (helicopter, unmanned aircraft (drone), airplane, rocket, satellite), an electric bicycle, an electric motorcycle, etc. can be cited, and a secondary battery including one embodiment of the present invention can be applied to these vehicles.

[0455] In the electric vehicle, there are provided first batteries 1301a and 1301b as secondary batteries for main driving, and a second battery 1311 for supplying power to an inverter 1312 for starting an engine 1304. The second battery 1311 is also called a cranking battery (also called a starting battery). The second battery 1311 only needs to have a high output and does not need to have a high capacity. In addition, the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.

[0456] The internal structure of the first battery 1301a can be either Fig. 14C or Fig.15A The winding type shown can also be used Fig.16A or Fig. 16B The laminated type shown.

[0457] In this embodiment, an example of connecting the first battery 1301a and 1301b in parallel is shown, but more than three batteries may be connected in parallel. In addition, as long as sufficient power can be stored in the first battery 1301a, the first battery 1301b may not be provided. By forming a battery pack with multiple secondary batteries, a larger amount of power can be taken out. Multiple secondary batteries may be connected in parallel, in series, or in series after being connected in parallel. Sometimes multiple secondary batteries are referred to as battery packs.

[0458] In order to cut off the power from the plurality of secondary batteries, the vehicle-mounted secondary battery includes a charging plug or a circuit breaker that can cut off the high voltage without using a tool, which is provided in the first battery 1301a.

[0459] In addition, the power of the first battery 1301a, 1301b is mainly used to rotate the engine 1304, and the power is also supplied to the 42V series vehicle-mounted components (electric power steering system 1307, heater 1308, defogger 1309, etc.) through the DCDC circuit 1306. In the case where the rear wheel includes a rear engine 1317, the first battery 1301a is used to rotate the rear engine 1317.

[0460] Furthermore, the second battery 1311 supplies power to 14V series vehicle-mounted components (audio 1313 , power windows 1314 , lights 1315 , etc.) via the DCDC circuit 1310 .

[0461] Next, use Fig.19A The first battery 1301a is described.

[0462] Fig.19A An example of using nine rectangular secondary batteries 1300 as a battery pack 1415 is shown. In addition, the nine rectangular secondary batteries 1300 are connected in series and one electrode is fixed using a fixing portion 1413 formed of an insulator and the other electrode is fixed using a fixing portion 1414 formed of an insulator. In this embodiment, an example of fixing using fixing portions 1413 and 1414 is shown, but it can also be stored in a battery storage box (also referred to as a frame). Assuming that the vehicle is vibrated or shaken from the outside (road surface, etc.), it is preferable to use fixing portions 1413, 1414 and a battery storage box to fix multiple secondary batteries. In addition, one electrode is electrically connected to the control circuit unit 1320 via wiring 1421. In addition, the other electrode is electrically connected to the control circuit unit 1320 via wiring 1422.

[0463] Alternatively, a memory circuit including a transistor using an oxide semiconductor may be used as the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor is sometimes referred to as a BTOS (Battery operating system or Battery oxide semiconductor).

[0464] It is preferred to use a metal oxide used as an oxide semiconductor. For example, as a metal oxide, it is preferred to use an In-M-Zn oxide (the element M is selected from one or more of aluminum, gallium, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium). In particular, the In-M-Zn oxide that can be applied to the metal oxide is preferably CAAC-OS (C-Axis Aligned Crystal Oxide Semiconductor) or CAC-OS (Cloud-Aligned Composite Oxide Semiconductor). In addition, In-Ga oxide and In-Zn oxide can also be used as metal oxides. CAAC-OS is an oxide semiconductor including a plurality of crystalline regions, and the c-axis of the plurality of crystalline regions is oriented in a specific direction. In addition, the specific direction refers to the thickness direction of the CAAC-OS film, the normal direction of the formed surface of the CAAC-OS film, or the normal direction of the surface of the CAAC-OS film. In addition, the crystalline region is a region having a periodicity of atomic arrangement. Note that when the atomic arrangement is viewed as a lattice arrangement, the crystalline region is also a region where the lattice arrangement is consistent.

[0465] In addition, "CAC-OS" refers to a structure in which the material is separated into a first region and a second region to form a mosaic shape, and the first region is distributed in the film (hereinafter also referred to as a cloud shape). That is, CAC-OS refers to a composite metal oxide having a structure in which the first region and the second region are mixed. Note that it is sometimes difficult to observe a clear boundary between the first region and the second region.

[0466] For example, in the CAC-OS of In-Ga-Zn oxide, based on the EDX mapping image obtained by energy dispersive X-ray spectroscopy (EDX), it can be confirmed that the structure has a region with In as the main component (first region) and a region with Ga as the main component (second region) that are unevenly distributed and mixed.

[0467] When CAC-OS is used for transistors, the complementary effect of the conductivity of the first region and the insulation of the second region can give CAC-OS a switch function (a function of controlling on / off). In other words, a portion of the CAC-OS material has a conductive function and another portion has an insulating function, and the entire material has a semiconductor function. By separating the conductive function and the insulating function, each function can be maximized. Therefore, by using CAC-OS for transistors, a high on-state current (I on ), high field effect mobility (μ) and good switching performance.

[0468] Oxide semiconductors have various structures and various characteristics. The oxide semiconductor of one embodiment of the present invention may include two or more of an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, a-like OS, CAC-OS, nc-OS, and CAAC-OS.

[0469] In addition, the control circuit unit 1320 preferably uses a transistor containing an oxide semiconductor because the transistor can be used in a high temperature environment. In order to simplify the process, the control circuit unit 1320 can also be formed using a unipolar transistor. The operating ambient temperature range of the transistor containing an oxide semiconductor in the semiconductor layer is larger than that of the single-crystalline Si transistor, that is, above -40°C and below 150°C, and the characteristic change of the secondary battery when overheated is smaller than that of the single-crystalline Si transistor. The off-state current of the transistor containing an oxide semiconductor is also below the lower limit of the measurement at 150°C, but the temperature dependence of the off-state current characteristics of the single-crystalline Si transistor is large. For example, at 150°C, the off-state current of the single-crystalline Si transistor increases, and the switching ratio of the current does not become sufficiently large. The control circuit unit 1320 can improve safety. In addition, by combining with a secondary battery in which the positive electrode active material 100 that can be obtained in embodiments 1, 2, etc. is used for the positive electrode, a synergistic effect of safety can be obtained. The secondary battery and the control circuit unit 1320 using the positive electrode active material 100 obtained in the first and second embodiments, etc., for the positive electrode greatly contribute to reducing accidents such as fires caused by the secondary battery.

[0470] The control circuit unit 1320 using a storage circuit including a transistor using an oxide semiconductor can also be used as an automatic control device for a secondary battery for instability such as micro short circuits. As functions for solving the instability of secondary batteries, there can be cited prevention of overcharging, prevention of overcurrent, control of overheating during charging, cell balancing in a battery pack, prevention of overdischarge, a capacity meter, automatic control of charging voltage and current according to temperature, control of charging current according to the degree of degradation, detection of abnormal behavior of micro short circuits, prediction of abnormalities regarding micro short circuits, etc. The control circuit unit 1320 has at least one of the above functions. In addition, ultra-miniaturization of the automatic control device for secondary batteries can be achieved.

[0471] In addition, "micro short circuit" refers to a very small short circuit inside the secondary battery. It is not a state where the positive and negative electrodes of the secondary battery cannot be charged or discharged due to a short circuit, but a phenomenon in which a short circuit current flows slightly in a very small short circuit portion. Since a large voltage change occurs even in a short and very small portion, this abnormal voltage value will affect subsequent speculation.

[0472] One of the reasons for micro short circuits is believed to be that due to repeated charging and discharging, uneven distribution of positive electrode active materials occurs, local current concentration occurs in part of the positive electrode and part of the negative electrode, and part of the separator becomes inoperative, or side reactions produce side reactants, leading to micro short circuits.

[0473] In addition to micro short circuits, the control circuit unit 1320 detects the terminal voltage of the secondary battery and manages the charge and discharge state of the secondary battery. For example, to prevent overcharging, both the output transistor of the charging circuit and the blocking switch can be turned off at almost the same time.

[0474] then, Fig.19B Show Fig.19A An example of a block diagram of a battery pack 1415 is shown.

[0475] The control circuit unit 1320 includes: a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging; a control circuit 1322 for controlling the switch unit 1324; and a voltage measuring unit of the first battery 1301a. In the control circuit unit 1320, the upper limit voltage and the lower limit voltage of the secondary battery used are set to control the upper limit of the current flowing from the outside or the upper limit of the output current flowing to the outside. The range above the lower limit voltage and below the upper limit voltage of the secondary battery is the recommended voltage range. When the voltage is outside this range, the switch unit 1324 functions and serves as a protection circuit. In addition, the control circuit unit 1320 controls the switch unit 1324 to prevent overdischarge and / or overcharge, so it can also be called a protection circuit. For example, when the control circuit 1322 detects a voltage that will become overcharge, the current is shielded by closing the switch of the switch unit 1324. In addition, the function of shielding the current according to the increase in temperature can also be set by setting a PTC element in the charge and discharge path. In addition, the control circuit unit 1320 includes an external terminal 1325 (+IN) and an external terminal 1326 (−IN).

[0476] The switch section 1324 can be formed by combining n-channel transistors or p-channel transistors. In addition to switches including Si transistors using single crystal silicon, power transistors such as Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaOx (gallium oxide; x is a real number greater than 0) can also be used to form the switch section 1324. In addition, the storage element using the OS transistor can be freely configured by stacking it on a circuit using the Si transistor, so it is easy to achieve integration. In addition, the OS transistor can be manufactured using the same manufacturing device as the Si transistor, so it can be manufactured at a low cost. That is, by stacking the control circuit section 1320 using the OS transistor on the switch section 1324 for integration, the switch section 1324 and the control circuit section 1320 can be integrated into one chip. The volume occupied by the control circuit section 1320 can be reduced, so miniaturization can be achieved.

[0477] The first battery 1301a and 1301b mainly supply power to the 42V series (high voltage series HV) vehicle-mounted equipment, while the second battery 1311 supplies power to the 14V series (low voltage series LV) vehicle-mounted equipment. In many cases, the second battery 1311 adopts a lead-acid battery because of cost advantages. However, the lead-acid battery has the disadvantages of large self-discharge compared with the lithium-ion battery and easy deterioration due to a phenomenon called sulfation. Although there is an advantage of no need for maintenance when a lithium-ion battery is used as the second battery 1311, an abnormality that is difficult to distinguish during manufacturing may occur when it is used for a long period of time, such as more than three years. In particular, in order to prevent the situation that the second battery 1311 of the starter inverter cannot work, even if the first battery 1301a and 1301b have residual capacity, the second battery 1311 is charged in a manner that is always kept fully charged by supplying power from the first battery to the second battery.

[0478] This embodiment shows an example in which lithium ion batteries are used for both the first battery 1301a and the second battery 1311. Fig.19C ) The second battery 1311 may also use a lead acid battery, an all-solid battery, or an electric double layer capacitor.

[0479] In addition, the regenerative energy caused by the rotation of the tire 1316 is transmitted to the engine 1304 through the transmission 1305, and is charged to the second battery 1311 from the engine controller 1303 and the battery controller 1302 through the control circuit unit 1321. In addition, the first battery 1301a is charged from the battery controller 1302 through the control circuit unit 1320. In addition, the first battery 1301b is charged from the battery controller 1302 through the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is preferable that the first batteries 1301a and 1301b can be charged at a high speed.

[0480] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b, etc. The battery controller 1302 sets the charging conditions according to the charging characteristics of the secondary battery to be used and performs high-speed charging.

[0481] In addition, although not shown in the figure, when the electric vehicle is connected to an external charger, the socket of the charger or the connecting cable of the charger is electrically connected to the battery controller 1302. The power supplied from the external charger is charged to the first battery 1301a, 1301b through the battery controller 1302. In addition, some chargers are provided with a control circuit without using the function of the battery controller 1302, but in order to prevent overcharging, it is preferred to charge the first battery 1301a, 1301b through the control circuit unit 1320. In addition, sometimes the socket of the charger or the connecting cable of the charger is provided with a control circuit. The control circuit unit 1320 is sometimes referred to as an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. In addition, the ECU includes a microcomputer. In addition, the ECU uses a CPU or a GPU.

[0482] As an external charger installed in a charging station, there are 100V outlet-200V outlet or three-phase 200V and 50kW outlet, etc. In addition, it is also possible to charge by supplying power from an external charging device through a contactless power supply method.

[0483] In order to charge the battery in a short time during high-speed charging, a secondary battery that can withstand charging at a high voltage is desired.

[0484] In addition, when graphene is used as a conductive material and the capacity can be suppressed from decreasing and maintained at a high capacity even if the thickness of the electrode layer is increased and the load is increased, a synergistic effect can be achieved to realize a secondary battery with greatly improved electrical characteristics. In particular, it is very effective for secondary batteries used in vehicles, and a longer driving distance can be achieved without increasing the weight ratio of the secondary battery relative to the total weight of the vehicle, specifically, a vehicle that can travel a distance of more than 500 km per charge.

[0485] In particular, the secondary battery of the present embodiment described above can increase the operating voltage of the secondary battery by using the positive electrode active material 100 described in Embodiments 1 and 2, thereby increasing the available capacity as the charging voltage increases. In addition, by using the positive electrode active material 100 described in Embodiments 1 and 2 for the positive electrode, a secondary battery for a vehicle with good cycle characteristics can be provided.

[0486] Next, an example in which a secondary battery as one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.

[0487] In addition, when Fig.13D , Fig. 15C , Fig.19A When any of the secondary batteries shown in is installed in a vehicle, a new generation of clean energy vehicles such as hybrid electric vehicles (HV), electric vehicles (EV) or plug-in hybrid electric vehicles (PHV) can be realized. In addition, the secondary battery can also be installed in agricultural machinery, electric bicycles including electric-assisted bicycles, motorcycles, electric wheelchairs, electric karts, ships, submarines, airplanes, rockets, artificial satellites, space probes, planetary probes or spacecraft. The secondary battery of one embodiment of the present invention can be a high-capacity secondary battery. Therefore, the secondary battery of one embodiment of the present invention is suitable for miniaturization and lightweight, and can be suitable for use in transportation vehicles.

[0488] FIG. 20A to FIG. 20D A transport vehicle using one embodiment of the present invention is shown. Fig. 20A The car 2001 shown is an electric car using an electric motor as a power source for running. Alternatively, the car 2001 is a hybrid car that can use an electric motor and an engine as a power source for running. When the secondary battery is installed in the vehicle, the example of the secondary battery shown in the embodiment 4 can be set in one or more parts. Fig. 20A The illustrated automobile 2001 includes a battery pack 2200 including a secondary battery module in which a plurality of secondary batteries are connected, and preferably also includes a charge control device electrically connected to the secondary battery module.

[0489] In addition, in the automobile 2001, the secondary battery of the automobile 2001 can be charged by supplying power from an external charging device using a plug-in method or a contactless power supply method. When charging, the charging method or the specifications of the connector can be appropriately performed according to the methods specified by CHAdeMO (a registered trademark in Japan) or the combined charging system "Combined Charging System". As a charging device, a charging station set up in a commercial facility or a home power supply can also be used. For example, by supplying power from the outside using plug-in technology, the power storage device installed in the automobile 2001 can be charged. Charging can be performed by converting AC power into DC power using a conversion device such as an AC / DC converter.

[0490] In addition, although not shown in the figure, the power receiving device can also be installed in the vehicle and the power can be supplied non-contactly from the power transmission device on the ground for charging. When the non-contact power supply method is used, by assembling the power transmission device in the road or the outer wall, charging can be performed not only when the vehicle is parked but also when it is driving. In addition, the non-contact power supply method can also be used to send and receive power between two vehicles. Furthermore, a solar cell can be set on the outside of the vehicle to charge the secondary battery when it is parked or driving. Such non-contact power supply can be achieved using electromagnetic induction or magnetic field resonance.

[0491] exist Fig. 20B In the diagram, a large transport vehicle 2002 including an electrically controlled engine is shown as an example of a transport vehicle. The secondary battery module of the transport vehicle 2002 is, for example, a secondary battery module having a maximum voltage of 170V, in which four secondary batteries with a nominal voltage of 3.0V or more and 5.0V or less are connected in series and 48 cells are connected. The battery pack 2201 has the same characteristics as the battery pack 2201 except for the number of secondary batteries constituting the secondary battery module. Fig. 20A The functions are the same, so the description is omitted.

[0492] exist Fig. 20C In the figure, a large transport vehicle 2003 including an electrically controlled engine is shown as an example. The secondary battery module of the transport vehicle 2203 is, for example, a secondary battery module having a maximum voltage of 600V in which more than 100 secondary batteries having a nominal voltage of 3.0V or more and 5.0V or less are connected in series. Therefore, a secondary battery having less uneven characteristics is required. By using a secondary battery in which the positive electrode active material 100 described in embodiments 1 and 2, etc. is used for the positive electrode, a secondary battery having stable battery characteristics can be manufactured, and mass production can be performed at low cost from the perspective of yield. In addition, in addition to the difference in the number of secondary batteries constituting the secondary battery module, the battery pack 2202 has the same Fig.23A The functions are the same, so the description is omitted.

[0493] exist Fig.20D , an aircraft 2004 equipped with an engine burning fuel is shown as an example. Fig.20D The aircraft 2004 shown includes wheels for taking off and landing, so it can be said that the aircraft 2004 is a type of transportation vehicle. In the aircraft 2004, multiple secondary batteries are connected to form a secondary battery module and include a battery pack 2203 having a secondary battery module and a charging control device.

[0494] The secondary battery module of the aircraft 2004 has, for example, eight 4V secondary batteries connected in series and a maximum voltage of 32V. In addition to the number of secondary batteries constituting the secondary battery module of the battery pack 2203, the Fig. 20A The functions are the same, so the description is omitted.

[0495] Fig.20E As an example, an artificial satellite 2005 using a secondary battery 2204 is shown. Since the artificial satellite 2005 is used in the extremely low temperature space, it is preferable to include a secondary battery 2204 of one embodiment of the present invention having good low temperature resistance. In addition, the secondary battery 2204 is preferably installed inside the artificial satellite 2005 in a state covered with a heat-insulating member.

[0496] This embodiment mode can be used in combination with other embodiment modes.

[0497] (Implementation method 6) In this embodiment, using Fig.21A and Fig.21B An example in which the secondary battery of one embodiment of the present invention is installed in a building will be described.

[0498] Fig.21A The house shown includes a storage device 2612 having a secondary battery module of one embodiment of the present invention and a solar panel 2610. The storage device 2612 is electrically connected to the solar panel 2610 through wiring 2611 or the like. In addition, the storage device 2612 can be electrically connected to a ground-mounted charging device 2604. The power obtained by the solar panel 2610 can be charged into the storage device 2612. In addition, the power stored in the storage device 2612 can be charged into a secondary battery included in the vehicle 2603 through the charging device 2604. The storage device 2612 is preferably arranged in the underfloor space portion. By being arranged in the underfloor space portion, the space on the floor can be effectively utilized. Alternatively, the storage device 2612 can also be arranged on the floor.

[0499] The power stored in the power storage device 2612 can also be supplied to other electronic devices in the house. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the electronic devices can be used by using the power storage device 2612 of one embodiment of the present invention as an uninterruptible power supply.

[0500] Fig.21B An example of a power storage device according to one embodiment of the present invention is shown below. Fig.21B As shown, a power storage device 791 according to one embodiment of the present invention is provided in an underfloor space 796 of a building 799. In addition, the control circuit described in Embodiment 5 may be provided in the power storage device 791, and a secondary battery using the positive electrode active material 100 obtained in Embodiments 1 and 2, etc., as the positive electrode, may be used in the power storage device 791, thereby obtaining a synergistic effect of safety. The control circuit described in Embodiment 5 and the secondary battery using the positive electrode active material 100 described in Embodiments 1 and 2, etc., as the positive electrode greatly contribute to reducing accidents such as fires caused by the power storage device 791 including the secondary battery.

[0501] The power storage device 791 is provided with a control device 790 , and the control device 790 is electrically connected to the switchboard 703 , the power storage controller 705 (also referred to as a control device), the display 706 , and the router 709 through wiring.

[0502] Electric power is supplied from the commercial power supply 701 to the switchboard 703 through the lead-in installation portion 710. In addition, both the electric power from the power storage device 791 and the electric power from the commercial power supply 701 are supplied to the switchboard 703, and the switchboard 703 supplies the supplied electric power to the general load 707 and the storage load 708 through the socket (not shown).

[0503] Examples of the general load 707 include electric appliances such as a television and a personal computer, and examples of the power storage load 708 include electric appliances such as a microwave oven, a refrigerator, and an air conditioner.

[0504] The power storage controller 705 has a measuring unit 711, a predicting unit 712, and a planning unit 713. The measuring unit 711 has a function of measuring the power consumption of the general load 707 and the power storage load 708 in a day (e.g., from 0:00 to 24:00). In addition, the measuring unit 711 may also have a function of measuring the power of the power storage device 791 and the power supplied from the commercial power supply 701. In addition, the predicting unit 712 has a function of predicting the required power consumed by the general load 707 and the power storage load 708 in the next day based on the power consumption of the general load 707 and the power storage load 708 in a day. In addition, the planning unit 713 has a function of determining the charging and discharging plan of the power storage device 791 based on the required power predicted by the predicting unit 712.

[0505] The amount of power consumed by the general load 707 and the power storage load 708 measured by the measuring unit 711 can be confirmed using the display 706. Alternatively, it can be confirmed using an electrical appliance such as a television or a personal computer through the router 709. Furthermore, it can be confirmed using a portable electronic terminal such as a smartphone or a tablet terminal through the router 709. In addition, the required power for each time period (or each hour) predicted by the prediction unit 712 can be confirmed using the display 706, an electrical appliance, or a portable electronic terminal.

[0506] This embodiment mode can be used in combination with other embodiment modes.

[0507] (Implementation 7) In the present embodiment, as an example of a vehicle equipped with a secondary battery, an example in which a lithium ion battery according to one embodiment of the present invention is installed in a motorcycle or a bicycle is described.

[0508] Fig.22A An example of an electric bicycle using the power storage device according to one embodiment of the present invention will be described. Fig.22A The electric bicycle 8700 shown can use the power storage device of one embodiment of the present invention. For example, the power storage device of one embodiment of the present invention includes a plurality of storage batteries and a protection circuit.

[0509] The electric bicycle 8700 includes a power storage device 8702. The power storage device 8702 supplies power to a motor that assists the rider. In addition, the power storage device 8702 is portable. Fig. 22B The power storage device 8702 taken out of the bicycle is shown. The power storage device 8702 has a plurality of storage batteries 8701 included in the power storage device of one embodiment of the present invention built in, and the remaining power, etc. can be displayed by the display unit 8703. In addition, the power storage device 8702 includes a control circuit 8704 shown in Embodiment 5 that can perform charging control or abnormality detection of the secondary battery. The control circuit 8704 is electrically connected to the positive electrode and the negative electrode of the storage battery 8701. In addition, by combining with a secondary battery using the positive electrode active material 100 that can be obtained in Embodiments 1, 2, etc. for the positive electrode, a synergistic effect of safety can be obtained. The secondary battery using the positive electrode active material 100 that can be obtained in Embodiments 1, 2, etc. for the positive electrode and the control circuit 8704 have made a great contribution to reducing accidents such as fires caused by secondary batteries.

[0510] Fig. 22C This is an example of a two-wheeled vehicle using the power storage device of one embodiment of the present invention. Fig. 22C The illustrated scooter 8600 includes a power storage device 8602, a side mirror 8601, and a turn signal lamp 8603. The power storage device 8602 can supply power to the turn signal lamp 8603. In addition, the power storage device 8602 equipped with a plurality of secondary batteries using the positive electrode active material 100 obtained in Embodiments 1 and 2 as a positive electrode can have a high capacity and contribute to miniaturization.

[0511] In addition, Fig. 22C In the illustrated scooter 8600, the power storage device 8602 can be stored in the under-seat storage section 8604. Even if the under-seat storage section 8604 is small, the power storage device 8602 can be stored in the under-seat storage section 8604.

[0512] This embodiment mode can be used in combination with other embodiment modes.

[0513] (Implementation 8) In this embodiment, an example of installing a secondary battery of one embodiment of the present invention in an electronic device is described. As an electronic device equipped with a secondary battery, for example, a television device (also referred to as a television or a television receiver), a display for a computer, a digital camera, a digital video camera, a digital photo frame, a mobile phone (also referred to as a mobile phone, a mobile phone device), a portable game console, a portable information terminal, a sound reproduction device, a large game console such as a pinball machine, etc. can be cited. As a portable information terminal, a notebook personal computer, a tablet terminal, an e-book terminal, a mobile phone, etc. can be cited.

[0514] Fig.23A An example of a mobile phone is shown. The mobile phone 2100 includes an operation button 2103, an external connection port 2104, a speaker 2105, a microphone 2106, etc. in addition to a display unit 2102 mounted on a housing 2101. In addition, the mobile phone 2100 includes a secondary battery 2107. By including the secondary battery 2107 using the positive electrode active material 100 described in Embodiments 1 and 2 as a positive electrode, a high capacity can be achieved, and a structure that can cope with the space saving required for miniaturization of the housing can be achieved.

[0515] The mobile phone 2100 can execute various application programs such as mobile phone, e-mail, article reading and writing, music playing, network communication, computer games, etc.

[0516] In addition to time setting, the operation button 2103 may have various functions such as power switch, wireless communication switch, silent mode setting and cancellation, power saving mode setting and cancellation, etc. For example, by using the operating system incorporated in the mobile phone 2100, the function of the operation button 2103 can be freely set.

[0517] In addition, the mobile phone 2100 can perform short-range wireless communication standardized by the communication system. For example, by communicating with a headset capable of wireless communication, a hands-free call can be made.

[0518] In addition, the mobile phone 2100 has an external connection port 2104, and data can be directly sent to or received from other information terminals through a connector. In addition, charging can also be performed through the external connection port 2104. In addition, the charging operation can also be performed using wireless power supply without using the external connection port 2104.

[0519] The mobile phone 2100 preferably includes a sensor. For example, a fingerprint sensor, a pulse sensor, a body sensor such as a temperature sensor, a touch sensor, a pressure sensor, or an acceleration sensor may be preferably installed as the sensor.

[0520] Fig. 23B An unmanned aerial vehicle 2300 including a plurality of rotors 2302 is shown. The unmanned aerial vehicle 2300 is also referred to as a drone. The unmanned aerial vehicle 2300 includes a secondary battery 2301 of one embodiment of the present invention, a camera 2303, and an antenna (not shown). The unmanned aerial vehicle 2300 can be remotely operated via the antenna. The secondary battery using the positive electrode active material 100 obtained in embodiments 1, 2, etc. for the positive electrode has a high energy density and high safety, so it can be used safely for a long period of time, so it is suitable as a secondary battery installed in the unmanned aerial vehicle 2300.

[0521] Fig.23C An example of a robot is shown. Fig.23C The robot 6400 shown includes a secondary battery 6409, an illumination sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a moving mechanism 6408, a computing device, and the like.

[0522] The microphone 6402 has a function of detecting the user's voice and surrounding sounds, etc. In addition, the speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user through the microphone 6402 and the speaker 6404.

[0523] The display unit 6405 has the function of displaying various information. The robot 6400 can display the information required by the user on the display unit 6405. The display unit 6405 can also be equipped with a touch panel. In addition, the display unit 6405 can be a detachable information terminal, and by setting it at a fixed position of the robot 6400, it can be charged and send and receive data.

[0524] The upper camera 6403 and the lower camera 6406 have the function of photographing the surrounding environment of the robot 6400. In addition, the obstacle sensor 6407 can detect whether there is an obstacle in the direction of the robot 6400 when it moves forward using the moving mechanism 6408. The robot 6400 can confirm the surrounding environment using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407 and move safely.

[0525] The robot 6400 is provided with a secondary battery 6409 and a semiconductor device or an electronic component according to one embodiment of the present invention. The secondary battery using the positive electrode active material 100 obtained in the first and second embodiments, etc., for the positive electrode has high energy density and high safety, so it can be used safely for a long period of time, and is therefore suitable as the secondary battery 6409 installed in the robot 6400.

[0526] Fig.23D An example of a sweeping robot is shown. The sweeping robot 6300 includes a display unit 6302 disposed on the surface of a frame 6301, a plurality of cameras 6303 disposed on the side, a brush 6304, an operation button 6305, a secondary battery 6306, various sensors, etc. Although not shown in the figure, the sweeping robot 6300 also has wheels, a suction port, etc. The sweeping robot 6300 can walk by itself and can detect garbage 6310 and suck the garbage into the suction port set below.

[0527] The sweeping robot 6300 can determine whether there are obstacles such as walls, furniture, or steps by analyzing the image taken by the camera 6303. In addition, when an object such as a wire that may be entangled with the brush 6304 is found through image analysis, the rotation of the brush 6304 can be stopped. The internal area of ​​the sweeping robot 6300 is equipped with a secondary battery 6306 and a semiconductor device or an electronic component according to one embodiment of the present invention. The secondary battery using the positive electrode active material 100 obtained in embodiments 1, 2, etc. for the positive electrode has high energy density and high safety, so it can be used safely for a long time for a long time, so it is suitable as a secondary battery 6306 installed in the sweeping robot 6300.

[0528] Fig.24A An example of a wearable device is shown. A secondary battery is used as a power source of the wearable device. In addition, in order to improve the splash-proof, waterproof or dust-proof performance when the user uses the wearable device in daily life or outdoors, the user not only wants the wearable device to be able to be charged by wire with the connector part exposed for connection, but also wants to be able to be charged wirelessly.

[0529] For example, the secondary battery of one embodiment of the present invention can be installed in Fig.24A The eyeglass-type device 4000 is shown. The eyeglass-type device 4000 includes a frame 4000a and a display unit 4000b. By installing a secondary battery on the temple portion of the curved frame 4000a, a light-weight eyeglass-type device 4000 with good weight balance and a long continuous use time can be realized. The secondary battery using the positive electrode active material 100 obtained in Embodiments 1 and 2 as the positive electrode has a high energy density, and a space-saving structure that can cope with the miniaturization of the frame can be realized.

[0530] In addition, the secondary battery of one embodiment of the present invention can be mounted on an earphone type device 4001. The earphone type device 4001 includes at least a microphone portion 4001a, a flexible tube 4001b, and an earphone portion 4001c. In addition, a secondary battery can be provided in the flexible tube 4001b or in the earphone portion 4001c. The secondary battery using the positive electrode active material 100 obtained in Embodiments 1 and 2 as a positive electrode has a high energy density and can realize a structure capable of coping with the space saving required for miniaturization of the frame.

[0531] In addition, the secondary battery of one embodiment of the present invention can be mounted on a device 4002 that can be directly mounted on the body. In addition, the secondary battery 4002b can be set in the thin frame 4002a of the device 4002. The secondary battery using the positive electrode active material 100 obtained in Embodiments 1 and 2, etc. for the positive electrode has a high energy density and can realize a space-saving structure that can cope with the miniaturization of the frame.

[0532] In addition, the secondary battery of one embodiment of the present invention can be installed in the device 4003 that can be mounted on clothes. In addition, the secondary battery 4003b can be set in the thin frame 4003a of the device 4003. The secondary battery using the positive electrode active material 100 obtained in the first and second embodiments, etc. for the positive electrode has a high energy density and can realize a space-saving structure that can cope with the miniaturization of the frame.

[0533] In addition, the secondary battery of one embodiment of the present invention can be mounted on a belt-type device 4006. The belt-type device 4006 includes a belt portion 4006a and a wireless power supply and receiving portion 4006b, and the secondary battery can be mounted in the inner area of ​​the belt portion 4006a. The secondary battery using the positive electrode active material 100 obtained in Embodiments 1 and 2 as the positive electrode has a high energy density and can realize a space-saving structure that can cope with the miniaturization of the frame.

[0534] In addition, the secondary battery of one embodiment of the present invention can be mounted on a watch-type device 4005. The watch-type device 4005 includes a display portion 4005a and a strap portion 4005b, and the secondary battery can be set on the display portion 4005a or the strap portion 4005b. The secondary battery using the positive electrode active material 100 obtained in the first and second embodiments, etc. for the positive electrode has a high energy density, and can realize a space-saving structure that can cope with the miniaturization of the frame.

[0535] The display unit 4005a can display various information such as e-mails and incoming phone calls in addition to the time.

[0536] In addition, since the watch-type device 4005 is a wearable device that is directly wrapped around the wrist, it can also be equipped with sensors for measuring the user's pulse, blood pressure, etc. Thus, the user's exercise volume and health-related data can be stored for health management.

[0537] Fig. 24B is a perspective view showing the watch-type device 4005 taken off from the wrist.

[0538] in addition, Fig.24C It is a side view. Fig.24C The internal region includes a secondary battery 913. The secondary battery 913 is the secondary battery described in Embodiment Mode 4. The secondary battery 913 is provided at a position overlapping the display portion 4005a, so that the wristwatch type device 4005 can be compact and lightweight with high density and high capacity.

[0539] The wristwatch-type device 4005 needs to be small and lightweight, so by using the positive electrode active material 100 obtained in Embodiments 1 and 2, etc. for the positive electrode of the secondary battery 913, a high energy density and small secondary battery 913 can be realized.

[0540] This embodiment mode can be used in combination with other embodiment modes. [Example 1]

[0541] <Method for producing sample 1> In this embodiment, the description of the first embodiment and Fig. 9 As shown in FIG. 10 and the like, a positive electrode active material 100 (sample 1) having a median particle size of 12 μm or less can be obtained.

[0542] As Fig. 9 As the starting material of step S10, lithium cobalt oxide (LiCoO2) containing no added elements is prepared from commercially available lithium cobalt oxide (manufactured by Nippon Chemical Industry Co., Ltd., CELLSEED C-5H). It is simply referred to as "C-5H" in the following specification, etc. The median particle size of C-5H is about 7.0 μm, which satisfies the condition that the median particle size is less than 10 μm.

[0543] Next, as heating in step S15, C-5H is placed in a sagger (container), covered with a lid, and then heated in a muffle furnace at 850°C for 2 hours. After the atmosphere in the muffle furnace becomes an oxygen atmosphere, no flow (O2 purge) is performed. In addition, when C-5H is placed in the sagger, the height (also called bulkiness) of the powder is placed in the sagger in a flat manner of less than 10 mm.

[0544] Next, according to Fig. 10A Step S20a shown in the figure is to prepare a source of the added element A1. First, lithium fluoride (LiF) is prepared as a F source, and magnesium fluoride (MgF2) is prepared as a Mg source. LiF and MgF2 are weighed in a ratio of LiF:MgF2 of 1:3 (molar ratio). Next, LiF and MgF2 are mixed in dehydrated acetone and stirred at a rotation speed of 500 rpm for 20 hours. A ball mill is used for mixing, and zirconia balls are used as a pulverizing medium. 20 mL of dehydrated acetone, zirconia balls, and 20 mL of slurry are added. 22 g of the Mg source (MgF2) and the F source (LiF) (about 9 g in total) were put into a mixing ball mill with a container capacity of 45 mL and mixed. Then, the mixture was sieved with a sieve with a mesh size of 300 μm to obtain the added element A1.

[0545] Next, according to Fig. 9 The step S31 shown is to mix the lithium cobalt oxide obtained by heating in step S15 (lithium cobalt oxide after initial heating) and the source of the additive element A1 obtained by step S20a. Specifically, the lithium cobalt oxide after initial heating and the source of the additive element A1 are weighed in a manner such that the number of atoms of magnesium relative to the number of atoms of cobalt in the lithium cobalt oxide is 1 atomic %, and then the lithium cobalt oxide and the source of the additive element A1 after initial heating are mixed by a dry method. At this time, stirring is performed at a rotation speed of 150 rpm for 1 hour. Then, sieving is performed using a sieve with a mesh size of 300 μm, thereby obtaining a mixture 903 (step S32).

[0546] Next, as step S33, the mixture 903 is heated. The heating conditions are 900° C. and 5 hours. During heating, the sagger containing the mixture 903 is covered with a lid. The atmosphere in the sagger is made to contain oxygen, and the ingress and egress of the oxygen are shielded (purged). A composite oxide containing Mg and F (lithium cobalt oxide containing Mg and F) is obtained by heating (step S34a).

[0547] Next, according to Fig. 10C Step S40 shown in the figure is to prepare the source of the additive element A2. First, nickel hydroxide (Ni(OH)2) is prepared as a Ni source, and aluminum hydroxide (Al(OH)3) is prepared as an Al source. Then, the nickel hydroxide and aluminum hydroxide are stirred in dehydrated acetone at a rotation speed of 500 rpm for 20 hours. A ball mill is used for mixing, and zirconium oxide balls are used as a grinding medium. 20 mL of dehydrated acetone, zirconium oxide balls, and 20 mL of acetone are mixed. 22 g and a total of about 10 g of nickel hydroxide and aluminum hydroxide were placed in separate containers of 45 mL of a mixing ball mill and mixed, and then sieved using a sieve with a mesh size of 300 μm to obtain an additive element A2 source.

[0548] Next, as step S51, the composite oxide containing Mg and F and the additive element A2 source are mixed by dry method. Specifically, the mixture is stirred at a rotation speed of 150 rpm for 1 hour. The mixing ratio is set so that the number of atoms of nickel hydroxide and aluminum hydroxide in the additive element A2 source is 0.5 atomic % relative to the number of atoms of cobalt in lithium cobalt oxide. The mixture is mixed using a ball mill, and zirconium oxide balls are used as a pulverizing medium. The zirconium oxide balls are mixed with the mixture of nickel hydroxide and aluminum hydroxide. 22g, a total of about 7.5g of Ni source, Al source and the composite oxide (lithium cobalt oxide containing Mg and F) obtained in step S34 were put into a mixing ball mill with a container capacity of 45mL for mixing. Finally, they were sieved using a 300μm sieve to obtain a mixture 904 (step S52).

[0549] Next, as step S53, the mixture 904 is heated. The heating conditions are 850°C and 2 hours. During heating, the sagger containing the mixture 904 is covered with a lid and heated in a muffle furnace. After the atmosphere in the muffle furnace becomes an oxygen atmosphere, no flow (O2 purge) is performed. By heating, lithium cobalt oxide (composite oxide) containing Mg, F, Ni and Al is obtained (step S54). Thus, a sample 1 of the positive electrode active material is obtained.

[0550] <Method for producing sample 2> Sample 2 was manufactured under conditions different from those of Sample 1. As a manufacturing method for Sample 2, the heating conditions when heating the mixture 903 in step S33 were set to 900° C. and 20 hours, and the heating conditions when heating the mixture 904 in step S53 were set to 850° C. and 10 hours. Except for the above-mentioned heating temperature, the same method as Sample 1 was used for manufacturing. Thus, Sample 2 of the positive electrode active material was obtained.

[0551] <Comparative Sample 1> As Comparative Sample 1, commercially available lithium cobalt oxide (CELLSEED C-5H, manufactured by Nippon Chemical Industry Co., Ltd.) containing no additive element was prepared.

[0552] <Particle size distribution measurement> Fig.25A The particle size distribution measurement results of sample 1 are shown. Fig.25B The particle size distribution measurement results of sample 2 are shown. Fig.25A and Fig.25B In FIG. 1 , the measurement data of Sample 1 and Sample 2 are shown by solid lines, and the measurement data of Comparative Sample 1 is shown by dotted lines.

[0553] The median particle size (D50) of sample 1 is about 9.7 μm, and the median particle size (D50) of sample 2 is about 9.5 μm. It can be confirmed that the median particle size (D50) of sample 1 and sample 2 both meet 12 μm or less (10.5 μm or less). The median particle size (D50) of comparative sample 1 is about 7.0 μm. In addition, the median particle size (D50) can be measured, for example, by observation using a SEM (scanning electron microscope) or TEM or by a particle size distribution analyzer using a laser diffraction and scattering method. In this embodiment, the laser diffraction particle size distribution measuring instrument SALD-2200 manufactured by Shimadzu Corporation is used for measurement.

[0554] <Ion Chromatography> The elements contained in the sample 1 and the comparative sample 1 were analyzed by ion chromatography. As the ion chromatograph, an ion chromatograph system Dionex ICS-2100 manufactured by Thermo Fisher Scientific Inc. was used.

[0555] The pretreatment of the analysis is described below. Prepare 250 mg of sample 1 and 2 ml of 0.05 M H2SO4 aqueous solution, put them into a glass container with a lid and mix them, thereby obtaining a first mixed solution. In addition, ultrasonic waves are applied for 1 hour as a mixture. Then, the container is left to...

Claims

1. A positive electrode active material, comprising: cobalt; oxygen; magnesium; aluminum; as well as nickel; The particle size of the positive electrode active material has a median particle size of 1 μm or more and 12 μm or less. The positive electrode active material includes the magnesium and the aluminum in the surface layer portion. The surface layer portion is a region within 50 nm from the surface of the positive electrode active material. Furthermore, when EDX line analysis in a depth direction is performed, the positive electrode active material includes a region where the magnesium is distributed closer to the surface of the positive electrode active material than the aluminum.

2. The positive electrode active material according to claim 1, wherein the positive electrode active material has a layered rock salt type crystal structure belonging to space group R-3m, The surface layer portion includes a base region having a surface parallel to the (001) plane of the crystal structure and an end region having a surface in a direction intersecting the (001) plane. Furthermore, when EDX line analysis in the depth direction is performed, the positive electrode active material includes a region in the end region where the distribution of the magnesium overlaps with the distribution of the nickel.

3. The positive electrode active material according to claim 2, The base region does not substantially contain nickel.

4. The positive electrode active material according to claim 1, wherein when the positive electrode active material is subjected to XPS analysis, the number of atoms of the magnesium relative to the number of atoms of the cobalt (Mg / Co) is greater than or equal to 0.400 and less than or equal to 1.500, Furthermore, the number of atoms of the nickel relative to the number of atoms of the cobalt (Ni / Co) is greater than or equal to 0.050 and less than or equal to 0.

150.

5. The positive electrode active material according to claim 4, wherein the positive electrode active material contains fluorine, Furthermore, when the positive electrode active material is subjected to XPS analysis, the number of fluorine atoms relative to the number of cobalt atoms (F / Co) is greater than or equal to 0.100 and less than or equal to 1.

000.

6. A lithium ion battery comprising: A positive electrode comprising the positive electrode active material according to any one of claims 1 to 5; as well as Electrolytes, The electrolyte includes lithium hexafluorophosphate, ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate.

7. The lithium ion battery according to claim 6, When the total volume of the ethylene carbonate, the ethyl methyl carbonate and the dimethyl carbonate in the electrolyte is 100 vol%, the volume ratio of the ethylene carbonate, the ethyl methyl carbonate and the dimethyl carbonate is x:y:100-xy (note that 5≤x≤35 and 0 <y<65)。 8. The lithium ion battery according to claim 7, The electrolyte includes the lithium hexafluorophosphate in an amount of 0.5 mol / L or more and 1.5 mol / L or less relative to the total volume of the ethylene carbonate, the ethyl methyl carbonate, and the dimethyl carbonate.

9. An electronic device comprising the lithium ion battery according to claim 6.

10. A vehicle comprising the lithium-ion battery of claim 6.