Binder composition for electrochemical element, conductive material dispersion liquid for electrochemical element, slurry for electrochemical element electrode, electrode for electrochemical element, and electrochemical element

A binder composition with NMP and triphenylphosphine sulfide addresses dispersibility and adhesion issues in electrochemical elements, enhancing electrode performance by improving dispersibility and reducing gas generation.

CN119072803APending Publication Date: 2024-12-03ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380035917.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-27
Filing Date
2023-06-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Conventional electrochemical element binder compositions face challenges in improving the dispersibility of conductive materials, ensuring strong adhesion to the current collector, and reducing gas generation during charging and discharging.

Method used

A binder composition comprising N-methyl-2-pyrrolidone (NMP) and triphenylphosphine sulfide, with a specific content range and ratio of triphenylphosphine sulfide to hydrophilic group-containing monomer units, is used to enhance dispersibility and peel strength, and reduce gas generation.

Benefits of technology

The composition achieves high dispersibility of conductive materials, resulting in electrodes with excellent peel strength and reduced gas generation, thereby improving the performance of electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005098322230000241
    Figure BDA0005098322230000241
Patent Text Reader

Abstract

The present invention provides a binder composition for an electrochemical element, the binder composition comprising a polymer, N-methyl-2-pyrrolidone, and triphenylphosphine sulfide, the polymer comprising a nitrile group-containing monomer unit, an alkylene structural unit, and a hydrophilic group-containing monomer unit, the content of the triphenylphosphine sulfide is 2-100 ppm by mass (inclusive) with respect to the content of the polymer, and when the content of the triphenylphosphine sulfide with respect to the content of the polymer is (a) and the content of the hydrophilic group-containing monomer unit with respect to the content of the polymer is (b), the relational expression 0.004 (%) < = {(a) / (b)} * 100 (%) < = 0.150 (%) is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive composition for an electrochemical element, a conductive material dispersion for an electrochemical element, a slurry for an electrochemical element electrode, an electrode for an electrochemical element, and an electrochemical element. Background Art

[0002] Electrochemical devices such as lithium-ion secondary batteries, lithium-ion capacitors, and electric double layer capacitors are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and have been used in a wide range of applications. Therefore, in recent years, the improvement of battery components such as electrodes has been studied for the purpose of further improving the performance of electrochemical devices.

[0003] Here, the electrode for an electrochemical element generally has a current collector and an electrode composite material layer formed on the current collector. Moreover, the electrode composite material layer is formed, for example, by applying a slurry containing an electrode active material and a binder composition containing a binder material on the current collector and drying the applied slurry.

[0004] Therefore, in order to further improve the performance of electrochemical devices, attempts have been made to improve the binder composition used to form the electrode composite material layer.

[0005] For example, Patent Document 1 discloses a non-aqueous secondary battery positive electrode binder composition, which includes a first binder material, the non-aqueous secondary battery positive electrode binder composition includes iron, and at least one of ruthenium and rhodium, and the total content of iron, ruthenium and rhodium is 5×10 -3 According to Patent Document 1, by using the above-mentioned binder composition, a positive electrode of a non-aqueous secondary battery having excellent life characteristics can be produced even when an aging treatment is performed under low temperature and low charge depth conditions.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent document 1: International Publication No. 2016 / 103730. Summary of the invention

[0009] Problem that the invention aims to solve

[0010] Furthermore, in recent years, conductive materials are being used in forming electrode composite material layers. Here, when forming an electrode composite material layer using a conductive material, a conductive material dispersion obtained by mixing a conductive material and a binder composition is used.

[0011] However, from the viewpoint of improving the dispersibility of the conductive material, the above-mentioned conventional electrochemical element binder composition still has room for improvement. In addition, for the above-mentioned conventional electrochemical element binder composition, it is required that the electrode composite material layer formed using the binder composition is firmly adhered to the current collector (i.e., the electrode exerts excellent peel strength). Furthermore, the electrode made using the above-mentioned conventional electrochemical element binder composition also has room for improvement in reducing the amount of gas generated by repeated charging and discharging.

[0012] Therefore, an object of the present invention is to provide an adhesive composition for an electrochemical element that can prepare a conductive material dispersion having sufficiently high dispersibility of a conductive material and can produce an electrode having excellent peel strength and reduced gas generation.

[0013] Another object of the present invention is to provide a conductive material dispersion for an electrochemical device and a slurry for an electrochemical device electrode, which can produce an electrode having sufficiently high dispersibility of a conductive material, excellent peel strength and reduced gas generation.

[0014] Furthermore, an object of the present invention is to provide an electrode for an electrochemical device having excellent peel strength and reduced gas generation, and an electrochemical device having the electrode for an electrochemical device.

[0015] Solutions for solving problems

[0016] The present inventors have conducted in-depth research for the purpose of solving the above problems. Then, the present inventors have newly discovered that the dispersibility of the conductive material in the conductive material dispersion can be fully improved by using a binder composition comprising a polymer, N-methyl-2-pyrrolidone (hereinafter sometimes referred to as "NMP") and triphenylphosphine sulfide, wherein the polymer comprises a nitrile-containing monomer unit, an alkylene structural unit and a hydrophilic group-containing monomer unit, the content of triphenylphosphine sulfide is within a specified range, and the content of triphenylphosphine sulfide and the content of the hydrophilic group-containing monomer unit satisfy a specified relationship. In addition, it has been newly discovered that by using the binder composition, an electrode with excellent peel strength and reduced gas generation can be produced, thereby completing the present invention.

[0017] That is, the object of the present invention is to advantageously solve the above-mentioned problems. [1] The adhesive composition for electrochemical elements of the present invention is characterized in that it comprises a polymer, N-methyl-2-pyrrolidone and triphenylphosphine sulfide, wherein the polymer comprises a nitrile group-containing monomer unit, an alkylene structural unit and a hydrophilic group-containing monomer unit, and the content of the triphenylphosphine sulfide is greater than 2 mass ppm and less than 100 mass ppm relative to the content of the polymer. When the content of the triphenylphosphine sulfide relative to the content of the polymer is (a) and the content of the hydrophilic group-containing monomer unit relative to the content of the polymer is (b), the following relationship is satisfied: 0.004(%)≤{(a) / (b)}×100(%)≤0.150(%).

[0018] As described above, according to the electrochemical element binder composition containing a polymer having a specified composition, NMP, and triphenylphosphine sulfide, wherein the content of triphenylphosphine sulfide is within a specified range, and the content of triphenylphosphine sulfide and the content of hydrophilic group-containing monomer units satisfy a specified relationship, the dispersibility of the conductive material in the conductive material dispersion can be sufficiently improved. In addition, by using the electrochemical element binder composition, an electrode with excellent peel strength and reduced gas generation can be produced.

[0019] In the present invention, "containing a monomer unit" means "a polymer obtained by using the monomer contains a repeating unit derived from the monomer". In addition, the ratio of each monomer unit and / or structural unit contained in the polymer can be expressed as 1 H-NMR and 13 C-NMR and other nuclear magnetic resonance (NMR) methods.

[0020] In the present invention, "the content of triphenylphosphine sulfide" can be measured by gas chromatography.

[0021] Here, [2] the binder composition for electrochemical elements of the present invention preferably has a monovalent cation content of 100 ppm by mass or less relative to the content of the above-mentioned polymer. If the monovalent cation content is 100 ppm by mass or less relative to the content of the polymer, crosslinking of the hydrophilic group-containing monomer units in the polymer via the monovalent cation can be suppressed, thereby stabilizing the viscosity of the binder composition for electrochemical elements.

[0022] In the present invention, "the content of monovalent cations" can be measured using the method described in Examples.

[0023] In addition, the present invention aims to advantageously solve the above-mentioned problems. [3] The electrochemical element conductive material dispersion of the present invention is characterized in that it contains at least the electrochemical element binder composition described in [1] or [2] and a conductive material. As such, the conductive material of the electrochemical element conductive material dispersion containing at least the electrochemical element binder composition and the conductive material of the present invention has sufficiently high dispersibility. Furthermore, by using the electrochemical element conductive material dispersion, an electrode having excellent peel strength and reduced gas generation can be produced.

[0024] [4] In the electrochemical device conductive material dispersion of the present invention, the conductive material is preferably carbon nanotubes. If carbon nanotubes are used as the conductive material, the resistance of the electrode composite material layer can be reduced, thereby improving the device characteristics of the electrochemical device.

[0025] In addition, the present invention aims to advantageously solve the above-mentioned problems. [5] The slurry for electrochemical element electrodes of the present invention is characterized by comprising at least the electrochemical element conductive material dispersion liquid described in [3] or [4] and an electrode active material. If the slurry for electrochemical element electrodes comprising at least the electrochemical element conductive material dispersion liquid and the electrode active material is used, an electrode having excellent peel strength and reduced gas generation can be produced.

[0026] In addition, the present invention aims to advantageously solve the above-mentioned problems. [6] The electrode for electrochemical element of the present invention is characterized by having an electrode composite material layer formed using the above-mentioned slurry for electrochemical element electrode. The electrode having the electrode composite material layer formed using the above-mentioned slurry for electrochemical element electrode has excellent peel strength and reduced gas generation.

[0027] The present invention aims to advantageously solve the above-mentioned problems. [7] The electrochemical device of the present invention is characterized by comprising the above-mentioned electrode for electrochemical device. The electrochemical device comprising the above-mentioned electrode for electrochemical device has excellent device characteristics.

[0028] Effects of the Invention

[0029] According to the present invention, it is possible to provide an adhesive composition for an electrochemical element that can prepare a conductive material dispersion having sufficiently high dispersibility of a conductive material and can produce an electrode having excellent peel strength and reduced gas generation.

[0030] Furthermore, according to the present invention, it is possible to provide a conductive material dispersion for an electrochemical element and a slurry for an electrochemical element electrode, which can produce an electrode having sufficiently high dispersibility of a conductive material, excellent peel strength and reduced gas generation.

[0031] Furthermore, according to the present invention, it is possible to provide an electrode for an electrochemical device having excellent peel strength and reduced gas generation, and an electrochemical device having the electrode for an electrochemical device. DETAILED DESCRIPTION

[0032] Hereinafter, embodiments of the present invention will be described in detail.

[0033] Here, the binder composition for electrochemical devices of the present invention can be used to prepare a slurry for electrochemical device electrodes after being mixed with a conductive material to prepare a conductive material dispersion for electrochemical devices of the present invention containing the conductive material and the binder composition for electrochemical devices.

[0034] Furthermore, the slurry for electrochemical element electrodes of the present invention prepared using the electrochemical element conductive material dispersion can be used when producing electrodes for electrochemical elements such as lithium ion secondary batteries.

[0035] Furthermore, the electrochemical device of the present invention is characterized by having the electrochemical device electrode of the present invention produced using the electrochemical device electrode slurry.

[0036] (Adhesive composition for electrochemical device)

[0037] The adhesive composition for electrochemical elements of the present invention (hereinafter referred to as "adhesive composition") is characterized in that it contains a polymer and triphenylphosphine sulfide in N-methyl-2-pyrrolidone (NMP) as a solvent, the polymer contains a nitrile group-containing monomer unit, an alkylene structural unit and a hydrophilic group-containing monomer unit, the content of triphenylphosphine sulfide is greater than 2 mass ppm and less than 100 mass ppm relative to the content of the polymer, and when the content of triphenylphosphine sulfide relative to the content of the polymer is (a) and the content of the hydrophilic group-containing monomer unit relative to the content of the polymer is (b), the following relationship is satisfied: 0.004(%)≤{(a) / (b)}×100(%)≤0.150(%).

[0038] Furthermore, the adhesive composition of the present invention may further contain, as an optional component, components used in the field of electrochemical devices as other components in addition to the above-mentioned components.

[0039] Moreover, the binder composition of the present invention has a polymer containing a specified monomer unit and a structural unit, the content of triphenylphosphine sulfide is within a specified range, and the content of triphenylphosphine sulfide and the content of the hydrophilic group-containing monomer unit satisfy a specified relationship. Therefore, if the binder composition is used, the dispersibility of the conductive material in the conductive material dispersion can be fully improved. In addition, if the binder composition of the present invention is used, an electrode with excellent peel strength and reduced gas generation can be produced.

[0040] The reason why the use of the binder composition of the present invention can sufficiently improve the dispersibility of the conductive material in the conductive material dispersion and produce an electrode having excellent peel strength and reduced gas generation is not clear, but is presumed as follows.

[0041] The binder composition of the present invention contains triphenylphosphine sulfide in an amount of 2 mass ppm or more and 100 mass ppm or less relative to the content of the polymer, so that the contribution of triphenylphosphine sulfide suppresses the gelation caused by the thickening of the polymer when preparing the conductive material dispersion, resulting in an improvement in the dispersibility of the conductive material in the conductive material dispersion. In addition, the gelation of the polymer can also be suppressed in the electrochemical element electrode slurry containing the conductive material dispersion, so the electrode composite material layer formed using the electrochemical element electrode slurry can be firmly adhered to the current collector. Furthermore, by triphenylphosphine sulfide, the water retention of the polymer decreases, so the gas generation of the electrode is reduced.

[0042] <Polymer>

[0043] The polymer is a component that can retain components included in the electrode composite layer formed using the electrode slurry, without detaching from the electrode composite layer.

[0044] Furthermore, the polymer contains the nitrile group-containing monomer unit, the alkylene structural unit and the hydrophilic group-containing monomer unit as described above, and optionally further contains other monomer units.

[0045] [Nitrile-containing monomer unit]

[0046] The nitrile group-containing monomer unit is a repeating unit derived from a nitrile group-containing monomer. Even if it is a nitrile group-containing monomer unit, a unit that can be equivalent to a hydrophilic group-containing monomer unit, that is, a monomer unit containing a hydrophilic group such as an acidic group and a hydroxyl group is not included in the "nitrile group-containing monomer unit" as a constituent element of the polymer of the present invention.

[0047] Here, as the nitrile group-containing monomer capable of forming the nitrile group-containing monomer unit, an α,β-ethylenically unsaturated nitrile monomer can be cited. Specifically, as the α,β-ethylenically unsaturated nitrile monomer, there is no particular limitation as long as it is an α,β-ethylenically unsaturated compound having a nitrile group, and examples thereof include: acrylonitrile; α-halogenated acrylonitrile such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitrile such as methacrylonitrile and α-ethylacrylonitrile, etc.

[0048] Among these, from the viewpoint of improving the adhesive force of the polymer, as the nitrile group-containing monomer, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred.

[0049] The nitrile group-containing monomer may be used alone or in combination of two or more at any ratio.

[0050] And, when all repeating units (total of monomeric unit and structural unit) in polymer are 100 mass %, the containing ratio of the monomeric unit containing nitrile group in polymer is preferably more than 10 mass %, more preferably more than 30 mass %, preferably less than 55 mass %.If the containing ratio of the monomeric unit containing nitrile group in polymer is within the above range, the dispersibility of the conductive material in conductive material dispersion liquid, electrode slurry can be further improved.

[0051] [Alkylene structural unit]

[0052] The alkylene structural unit is composed only of the general formula: -C n H 2n -[wherein n is an integer greater than or equal to 2] is a repeating unit consisting of an alkylene structure represented by.

[0053] The alkylene structural unit may be linear or branched, preferably a linear alkylene structural unit, i.e. a linear alkylene structural unit. In addition, the number of carbon atoms in the alkylene structural unit is preferably 4 or more (i.e., n in the above general formula is an integer of 4 or more).

[0054] Here, the method for introducing the alkylene structural unit into the polymer is not particularly limited, and examples thereof include the following methods (1) and (2):

[0055] (1) A method of preparing a polymer from a monomer composition containing a conjugated diene monomer, and hydrogenating the polymer to convert the conjugated diene monomer units into alkylene structural units;

[0056] (2) A method for producing a polymer from a monomer composition comprising a 1-olefin monomer.

[0057] Among them, method (1) is preferred because it is easy to produce a polymer.

[0058] Examples of the conjugated diene monomer include conjugated diene compounds having 4 or more carbon atoms, such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, and 1,3-pentadiene. Among them, conjugated diene compounds having 4 or more carbon atoms are preferred, and 1,3-butadiene is more preferred.

[0059] That is, the alkylene structural unit is preferably a structural unit obtained by hydrogenating a conjugated diene monomer unit (a conjugated diene hydride unit), more preferably a structural unit obtained by hydrogenating a conjugated diene monomer unit having 4 or more carbon atoms (a conjugated diene hydride unit having 4 or more carbon atoms), and further preferably a structural unit obtained by hydrogenating a 1,3-butadiene monomer unit (a 1,3-butadiene hydride unit).

[0060] Examples of the 1-olefin monomer include ethylene, propylene, and 1-butene.

[0061] The conjugated diene monomer and the 1-olefin monomer may be used alone or in combination of two or more at any ratio.

[0062] Moreover, when all repeating units (total of monomeric units and structural units) in the polymer are 100% by mass, the content of the alkylene structural unit in the polymer is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 50% by mass or more, preferably 90% by mass or less, more preferably 85% by mass or less, further preferably 80% by mass or less. If the content of the alkylene structural unit in the polymer is within the above range, the dispersibility of the conductive material can be further improved in the conductive material dispersion and the electrode slurry.

[0063] [Hydrophilic group-containing monomer unit]

[0064] The hydrophilic group-containing monomer unit is a repeating unit derived from a hydrophilic group-containing monomer. Examples of the hydrophilic group-containing monomer that can form the hydrophilic group-containing monomer unit include carboxylic acid group-containing monomers, hydroxyl group-containing monomers, sulfonic acid group-containing monomers, and phosphoric acid group-containing monomers.

[0065] Examples of the carboxylic acid group-containing monomer include monocarboxylic acids and derivatives thereof, dicarboxylic acids and anhydrides thereof, and derivatives thereof.

[0066] Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid.

[0067] Examples of the monocarboxylic acid derivative include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, and β-diaminoacrylic acid.

[0068] Examples of the dicarboxylic acid include maleic acid, fumaric acid, and itaconic acid.

[0069] Examples of the dicarboxylic acid derivatives include maleic acid esters such as methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, methylallyl maleate, diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate.

[0070] Examples of the anhydride of dicarboxylic acid include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride.

[0071] Furthermore, as the monomer having a carboxylic acid group, an acid anhydride that generates a carboxyl group by hydrolysis can also be used.

[0072] Other examples include monoesters and diesters of α,β-ethylenically unsaturated polycarboxylic acids such as monoethyl maleate, diethyl maleate, monobutyl maleate, dibutyl maleate, monoethyl fumarate, diethyl fumarate, monobutyl fumarate, dibutyl fumarate, monocyclohexyl fumarate, dicyclohexyl fumarate, monoethyl itaconate, diethyl itaconate, monobutyl itaconate, and dibutyl itaconate.

[0073] Examples of the hydroxyl-containing monomer include: ethylenically unsaturated alcohols such as (meth)allyl alcohol, 3-butene-1-ol, and 5-hexene-1-ol; alkyl alcohol esters of ethylenically unsaturated carboxylic acids such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, di-2-hydroxyethyl maleate, di-4-hydroxybutyl maleate, and di-2-hydroxypropyl itaconate; and 2 =CR 1 -COO-(C q H 2q O) pH (wherein p represents an integer from 2 to 9, q represents an integer from 2 to 4, R 1Esters of polyalkylene glycol represented by methyl or hydrogen and (meth)acrylic acid; mono(meth)acrylates of dihydroxy esters of dicarboxylic acids such as 2-hydroxyethyl-2'-(meth)acryloyloxyphthalate and 2-hydroxyethyl-2'-(meth)acryloyloxysuccinate; vinyl ethers such as 2-hydroxyethyl vinyl ether and 2-hydroxypropyl vinyl ether; (meth)allyl-2-hydroxyethyl ether, (meth)allyl-2-hydroxypropyl ether, (meth)allyl-3-hydroxypropyl ether, (meth)allyl-2-hydroxybutyl ether, (meth)allyl-3-hydroxybutyl ether, (meth)allyl-4-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxybutyl ether, (meth)allyl-6-hydroxyethyl ether, (meth)allyl-2-hydroxyethyl ether, (meth)allyl-2-hydroxypropyl ether, (meth)allyl-3-hydroxypropyl ether, (meth)allyl-2 ... Mono(meth)allyl ethers of alkylene glycols such as -hydroxyhexyl ether; mono(meth)allyl ethers of polyoxyalkylene glycols such as diethylene glycol mono(meth)allyl ether and dipropylene glycol mono(meth)allyl ether; mono(meth)allyl ethers of halogen and hydroxyl-substituted (poly)alkylene glycols such as glycerol mono(meth)allyl ether, (meth)allyl-2-chloro-3-hydroxypropyl ether and (meth)allyl-2-hydroxy-3-chloropropyl ether; mono(meth)allyl ethers of polyphenols such as eugenol and isoeugenol and their halogen-substituted products; (meth)allyl sulfide ethers of alkylene glycols such as (meth)allyl-2-hydroxyethyl sulfide and (meth)allyl-2-hydroxypropyl sulfide, etc.

[0074] In the present invention, "(meth)allyl" means an allyl group and / or a methallyl group, and "(meth)acryloyl" means an acryloyl group and / or a methacryloyl group.

[0075] Examples of the sulfonic acid group-containing monomer include vinyl sulfonic acid, methylvinyl sulfonic acid, (meth)allyl sulfonic acid, styrene sulfonic acid, 2-sulfoethyl (meth)acrylate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid.

[0076] Examples of the phosphoric acid group-containing monomer include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate.

[0077] Among these, from the viewpoint of improving the dispersibility of the electrode active material while ensuring the dispersibility of the conductive material in the electrode slurry and improving the adhesion of the electrode composite material layer to the current collector, carboxylic acid group-containing monomers, hydroxyl group-containing monomers, and sulfonic acid group-containing monomers are preferred, and carboxylic acid group-containing monomers and hydroxyl group-containing monomers are more preferred.

[0078] The hydrophilic group-containing monomer may be used alone or in combination of two or more at any ratio.

[0079] Moreover, when all repeating units (total of monomeric units and structural units) in the polymer are 100% by mass, the content ratio of the hydrophilic group-containing monomeric unit in the polymer is preferably more than 5% by mass, more preferably more than 10% by mass, and preferably less than 30% by mass. If the content ratio of the hydrophilic group-containing monomeric unit is more than the above-mentioned lower limit, the electrode active material can be well dispersed while ensuring the dispersibility of the conductive material in the conductive electrode slurry. In addition, if the content ratio of the hydrophilic group-containing monomeric unit in the polymer is below the above-mentioned upper limit, the dispersibility of the conductive material is not excessively damaged, and the degradation caused by the concavo-convex and charge concentration of the electrode composite material layer can be suppressed.

[0080] [Other monomer units]

[0081] The other monomer units that may be contained in the polymer are not particularly limited, and examples thereof include (meth)acrylic acid ester monomer units and aromatic vinyl monomer units. As the other monomer units, (meth)acrylic acid ester monomer units are particularly preferred.

[0082] Examples of the (meth)acrylate monomer capable of forming the (meth)acrylate monomer unit include an alkyl (meth)acrylate monomer having one ethylenically unsaturated bond. Examples of the alkyl (meth)acrylate monomer include an alkyl (meth)acrylate monomer having a linear alkyl group and an alkyl (meth)acrylate monomer having a branched alkyl group. For example, as (meth) acrylic acid ester monomers, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, amyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, stearyl acrylate and other alkyl acrylates; methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate and other alkyl methacrylates, etc. Among these, from the viewpoint of imparting appropriate affinity with the electrolyte to the obtained electrode composite material layer, preferably the alkyl (meth) acrylic acid ester whose alkyl group is a linear alkyl group, more preferably butyl acrylate and methyl methacrylate.

[0083] As the aromatic vinyl monomer capable of forming the aromatic vinyl monomer unit, there can be mentioned, for example, styrene, styrene sulfonic acid and its salts, α-methylstyrene, p-tert-butylstyrene, butoxystyrene, vinyltoluene, chlorostyrene, and vinylnaphthalene, etc. Among them, styrene is preferred as the aromatic vinyl monomer from the viewpoint of further improving the dispersibility of the conductive material dispersion.

[0084] The monomers capable of forming other monomer units may be used alone or in combination of two or more at any ratio.

[0085] Moreover, when the amount of all repeating units in the polymer (the total of monomer units and structural units) is 100 mass%, the content ratio of other monomer units in the polymer is preferably 10 mass% or less, more preferably 5 mass% or less, and particularly preferably 0 mass% (that is, the polymer contains only nitrile group-containing monomer units, alkylene structural units and hydrophilic group-containing monomer units).

[0086] [Iodine value]

[0087] Moreover, the iodine value of the polymer is preferably 120 mg / 100 mg or less, more preferably 100 mg / 100 mg or less, and further preferably 60 mg / 100 mg or less. If the iodine value of the polymer is 120 mg / 100 mg or less, the element characteristics of the electrochemical element can be improved by using the binder composition of the present invention. In addition, the lower limit of the iodine value of the polymer is not particularly limited, for example, 1 mg / 100 mg or more.

[0088] In the present invention, the "iodine value" can be measured using the method described in the Examples.

[0089] [Weight average molecular weight]

[0090] The weight average molecular weight of the polymer is preferably 10000 or more, more preferably 15000 or more, preferably 100000 or less, more preferably 80000 or less, and further preferably 50000 or less. If the weight average molecular weight of the polymer is within the above range, the viscosity of the adhesive composition can be stabilized.

[0091] In addition, in the present invention, the "weight average molecular weight" can be measured using the method described in Examples.

[0092] [Polymer preparation method]

[0093] The method for producing the polymer is not particularly limited, and the polymer can be produced, for example, by polymerizing a monomer composition containing the monomers described above in the presence of a chain transfer agent such as tert-dodecyl mercaptan to obtain a polymer, and then hydrogenating the obtained polymer.

[0094] Here, the content ratio of each monomer in the monomer composition for preparing the polymer can be determined according to the content ratio of each repeating unit in the polymer.

[0095] The polymerization method is not particularly limited, and any method can be used, such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. In addition, as the polymerization reaction, any reaction such as ionic polymerization, radical polymerization, and living radical polymerization can be used.

[0096] Furthermore, the method for hydrogenating the polymer is not particularly limited, and an oil layer hydrogenation method, a water layer direct hydrogenation method, and a water layer indirect hydrogenation method (for example, see International Publication No. 2013 / 080989) which are general methods using a catalyst can be used.

[0097] <Triphenylphosphine sulfide>

[0098] In the binder composition of the present invention, the content of triphenylphosphine sulfide is 2 mass ppm or more relative to the content of the polymer, preferably 3 mass ppm or more, more preferably 5 mass ppm or more, 100 mass ppm or less, preferably 90 mass ppm or less, more preferably 60 mass ppm or less. If the content of triphenylphosphine sulfide is above the above lower limit relative to the content of the polymer, in the conductive material dispersion and electrode slurry using the binder composition, the gas generation in the electrode can be fully reduced while improving the dispersibility of the conductive material. In addition, if the content of triphenylphosphine sulfide is below the above upper limit relative to the content of the polymer, the peel strength of the electrode can be fully improved.

[0099] Here, when the adhesive composition of the present invention has the content of triphenylphosphine sulfide relative to the content of the polymer as described above and the content of the hydrophilic group-containing monomer unit relative to the content of the polymer as (a), the following relationship is satisfied: 0.004(%)≤{(a) / (b)}×100(%)≤0.150(%).

[0100] Moreover, in the above relationship, the value represented by {(a) / (b)}×100(%) is preferably 0.005(%) or more, more preferably 0.040(%) or more, preferably 0.130(%) or less, and more preferably 0.100(%) or less. If the value represented by {(a) / (b)}×100(%) is 0.004(%) or more, the dispersibility of the conductive material can be sufficiently improved in the conductive material dispersion using the binder composition. In addition, if the value represented by {(a) / (b)}×100(%) is 0.150(%) or less, the amount of gas generated can be sufficiently reduced in the electrode made using the binder composition.

[0101] <Other ingredients>

[0102] As the binder composition of the present invention, other components that can be included in addition to polymers, NMP and triphenylphosphine sulfide are not particularly limited. As other components, for example, binder materials (polyvinylidene fluoride, polyacrylate, etc.), reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives other than polymers can be cited. As long as they do not affect the battery reaction, they are not particularly limited, and known additives can be used, such as additives recorded in International Publication No. 2012 / 115096. In addition, the binder composition of the present invention may also include a solvent other than NMP.

[0103] These other components may be used alone or in combination of two or more at any ratio.

[0104] Furthermore, the adhesive composition of the present invention may contain monovalent cations. At this time, the content of the monovalent cations contained in the adhesive composition is preferably 100 mass ppm or less relative to the content of the polymer, more preferably 90 mass ppm or less, preferably 60 mass ppm or less. If the content of the monovalent cations contained in the adhesive composition is 100 mass ppm or less relative to the content of the polymer, the hydrophilic group-containing monomer units in the polymer can be suppressed from being cross-linked via monovalent cations, so that the viscosity of the adhesive composition can be stabilized.

[0105] The monovalent cation is derived from a component that can be used when preparing the polymer, for example. The monovalent cation is not particularly limited, and examples thereof include potassium (K) and sodium (Na).

[0106] <Method for preparing adhesive composition for electrochemical element>

[0107] The binder composition of the present invention is not particularly limited, and can be prepared, for example, by the following method: after preparing a polymer according to the above-mentioned method for preparing a polymer, triphenylphosphine sulfide and NMP are added and mixed, and then the solvent used in the preparation of the polymer is removed. In addition, when the above-mentioned other components are combined, mixing can be performed by a known method before or after the solvent is removed. The mixing method is not particularly limited, and mixing can be performed by a known method.

[0108] (Conductive material dispersion for electrochemical devices)

[0109] The conductive material dispersion for electrochemical devices of the present invention (hereinafter simply referred to as “conductive material dispersion”) contains at least the above-mentioned binder composition of the present invention and a conductive material, and may further contain other components as desired.

[0110] Moreover, the conductive material dispersion of the present invention contains the binder composition of the present invention, so the dispersibility of the conductive material is sufficiently high. In addition, the conductive material dispersion of the present invention contains the binder composition of the present invention, so if the conductive material dispersion is used, an electrode with excellent peel strength and reduced gas generation can be produced.

[0111] The conductive material dispersion of the present invention is an intermediate product for preparing the slurry for electrochemical element electrodes of the present invention described later, and generally does not contain an electrode active material.

[0112] Furthermore, the polymer and triphenylphosphine sulfide contained in the conductive material dispersion of the present invention are derived from the binder composition of the present invention, and their preferred existence ratio is the same as that of the binder composition of the present invention.

[0113] <Conductive Materials>

[0114] The conductive material is not particularly limited, and conductive carbon materials such as carbon black (e.g., acetylene black, Ketjen black (registered trademark), furnace black, etc.), single-walled or multi-walled carbon nanotubes (multi-walled carbon nanotubes include stacked cup-shaped ones), carbon nanohorns, vapor-grown carbon fibers, milled carbon fibers obtained by sintering and pulverizing polymer fibers, single-walled or multi-walled graphene, and carbon nonwoven fabric sheets obtained by sintering nonwoven fabrics composed of polymer fibers, as well as fibers or foils of various metals can be used. These materials can be used alone or in combination of two or more.

[0115] Among these, carbon nanotubes (hereinafter sometimes referred to as "CNTs") are preferred as the conductive material from the viewpoint of reducing the resistance of the electrode composite material layer and obtaining an electrochemical device with further improved device characteristics.

[0116] The CNTs are not particularly limited, and CNTs synthesized by a known CNT synthesis method such as an arc discharge method, a laser ablation method, or a chemical vapor deposition method (CVD method) can be used.

[0117] Here, the BET specific surface area of ​​CNT is preferably 100 m 2 / g or more, more preferably 150m 2 / g or more, more preferably 200m 2 / g or more, preferably 2500m 2 / g or less.

[0118] In the present invention, the "BET specific surface area" refers to a nitrogen adsorption specific surface area measured using the BET method, and can be measured in accordance with ASTM D3037-81.

[0119] <Other ingredients>

[0120] The other components that can be included in the conductive material dispersion are not particularly limited, and examples thereof include the same components as those that can be included in the adhesive composition of the present invention. In addition, the other components can be used alone or in combination of two or more in any ratio.

[0121] <Ratio of Binder Composition to Conductive Material in Conductive Material Dispersion>

[0122] Here, when the binder composition and the conductive material are mixed to obtain a conductive material dispersion, the amount ratio of the binder composition to the conductive material is not particularly limited. The conductive material and the binder composition can be mixed, for example, in the following amount ratio: the obtained conductive material dispersion preferably contains 10 parts by mass or more and 100 parts by mass or less of the polymer, preferably 15 parts by mass or more and 50 parts by mass or less of the polymer per 100 parts by mass of the conductive material.

[0123] <Method for preparing conductive material dispersion>

[0124] The conductive material dispersion of the present invention can be prepared by mixing the above-mentioned components by a known method.

[0125] Furthermore, mixing can be performed using a mixer such as a ball mill, a sand mill, a bead mill, a pigment disperser, an attritor, an ultrasonic disperser, a homogenizer, a planetary mixer, or a filmix.

[0126] The solid content concentration of the conductive material dispersion can be, for example, 1 mass % or more and 25 mass % or less.

[0127] (Slurry for electrochemical element electrodes)

[0128] The slurry for electrochemical element electrodes of the present invention (hereinafter, simply referred to as "slurry for electrodes") is a composition comprising the above-mentioned conductive material dispersion of the present invention and an electrode active material. That is, the slurry for electrodes of the present invention contains a polymer, triphenylphosphine sulfide, NMP, a conductive material and an electrode active material, and optionally contains the above-mentioned other components.

[0129] Furthermore, since the slurry composition for an electrode of the present invention contains the conductive material dispersion of the present invention, by using the slurry for an electrode, an electrode having excellent peel strength and reduced gas generation can be produced.

[0130] The polymer, triphenylphosphine sulfide and conductive material contained in the electrode slurry of the present invention are derived from the binder composition and conductive material dispersion of the present invention, and their preferred abundance ratio is the same as that of the binder composition and conductive material dispersion of the present invention.

[0131] In addition, the case where the slurry for electrodes of the present invention is a slurry for lithium ion secondary battery electrodes will be described below as an example, but the present invention is not limited to the following example.

[0132] <Electrode Active Material>

[0133] The electrode active material (positive electrode active material, negative electrode active material) to be blended in the electrode slurry is not particularly limited, and a known electrode active material can be used.

[0134] For example, as a positive electrode active material for a lithium ion secondary battery, there is no particular limitation, and metal oxides containing lithium (Li) can be cited. Moreover, as a positive electrode active material, it is preferred that in addition to lithium (Li), a positive electrode active material further contains at least one selected from cobalt (Co), nickel (Ni), manganese (Mn) and iron (Fe). As such a positive electrode active material, lithium cobalt oxide (LiCoO 2 ), lithium manganese oxide (LiMn 2 O 4 ), lithium nickel oxide (LiNiO 2 ), Co-Ni-Mn lithium-containing composite oxides, Ni-Mn-Al lithium-containing composite oxides, Ni-Co-Al lithium-containing composite oxides, olivine-type lithium manganese phosphate (LiMnPO 4 ), olivine lithium iron phosphate (LiFePO 4 )、Li 1+x Mn 2-x O 4 (0<X<2) represented by lithium excess spinel compound, Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 ]O 2 、LiNi 0.5 Mn 1.5 O 4 、Li[Ni 0.5 Co 0.2 Mn 0.3 ]O 2 wait.

[0135] The electrode active material may be used alone or in combination of two or more at any ratio.

[0136] In addition, the particle size of the electrode active material is not particularly limited and can be the same as that of conventionally used electrode active materials.

[0137] Furthermore, the amount of the electrode active material in the electrode slurry is not particularly limited and can be set within the range conventionally used.

[0138] <Method for preparing slurry for electrochemical element electrodes>

[0139] The method for preparing the electrode slurry of the present invention is not particularly limited. The electrode slurry can be prepared by mixing the conductive material dispersion of the present invention and an electrode active material.

[0140] The mixing method is not particularly limited, and the same method as the mixing method in the preparation of the conductive material dispersion of the present invention described above can be used.

[0141] (Electrode for electrochemical device)

[0142] The electrode for an electrochemical device of the present invention (hereinafter simply referred to as "electrode") has an electrode composite material layer formed using the above-mentioned electrode slurry of the present invention. More specifically, the electrode of the present invention generally has the above-mentioned electrode composite material layer on a current collector.

[0143] Furthermore, since the electrode composite material layer of the electrode of the present invention is formed of the above-mentioned slurry for an electrode of the present invention, it is excellent in peel strength and the amount of gas generated is reduced.

[0144] <Current collector>

[0145] The current collector is made of a material having electrical conductivity and electrochemical durability. There is no particular limitation on the current collector, and a known current collector can be used. For example, as the current collector of the positive electrode of the lithium ion secondary battery, a current collector made of aluminum or an aluminum alloy can be used. In this case, aluminum and aluminum alloys can be used in combination, or different types of aluminum alloys can be used in combination. Aluminum and aluminum alloys are heat-resistant and electrochemically stable, and therefore are excellent current collector materials.

[0146] <Method for producing an electrode for an electrochemical device>

[0147] The manufacturing method of the electrode of the present invention is not particularly limited. The electrode of the present invention can be manufactured by, for example, applying the above-mentioned electrode slurry of the present invention to at least one surface of the current collector and drying it to form an electrode composite material layer. In more detail, the manufacturing method includes: a step of applying the electrode slurry of the present invention to at least one surface of the current collector (coating step); and a step of drying the electrode slurry applied to at least one surface of the current collector to form an electrode composite material layer on the current collector (drying step).

[0148] [Coating process]

[0149] As a method for applying the electrode slurry of the present invention to the current collector, it is not particularly limited, and a known method can be used. Specifically, as a coating method, a notch wheel coating method, a scraper method, an immersion method, a reverse roll coating method, a direct roll coating method, a gravure method, an extrusion method, a brush coating method, etc. can be used. At this time, the electrode slurry can be applied only on one surface of the current collector, or it can be applied on both surfaces of the current collector. The thickness of the slurry film on the current collector after coating and before drying can be appropriately set according to the thickness of the electrode composite material layer obtained by drying.

[0150] [Drying process]

[0151] The method for drying the electrode slurry on the current collector is not particularly limited, and a known method can be used, for example: a drying method using warm air, hot air, or low-humidity air; a vacuum drying method; a drying method using irradiation of infrared rays, electron beams, etc. By drying the electrode slurry on the current collector in this way, an electrode composite material layer can be formed on the current collector, and an electrode for an electrochemical element having a current collector and an electrode composite material layer can be obtained.

[0152] In addition, after the drying step, the electrode composite material layer may be subjected to a press treatment using a metal mold press or a roll press, etc. The press treatment can further improve the adhesion between the electrode composite material layer and the current collector.

[0153] (Electrochemical Components)

[0154] The electrochemical element of the present invention has the above-mentioned electrode for electrochemical element of the present invention. Moreover, the electrochemical element of the present invention has the electrode for electrochemical element of the present invention, so the element characteristics are excellent. In addition, the electrochemical element of the present invention can be a non-aqueous secondary battery such as a double electric layer capacitor or a lithium ion secondary battery. Among them, the electrochemical element of the present invention is preferably a non-aqueous secondary battery, more preferably a lithium ion secondary battery.

[0155] Here, a lithium ion secondary battery as an example of the electrochemical element of the present invention is described below. The lithium ion secondary battery has a positive electrode, a negative electrode, an electrolyte, and a separator. Moreover, the electrode of the present invention is used as at least one of the positive electrode and the negative electrode.

[0156] <Electrode>

[0157] Electrodes other than the above-mentioned electrode of the present invention that can be used in the lithium ion secondary battery as the electrochemical element of the present invention are not particularly limited, and known electrodes can be used.

[0158] <Electrolyte>

[0159] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent is generally used. As the supporting electrolyte of a lithium ion secondary battery, for example, a lithium salt can be used. Examples of the lithium salt include LiPF 6 、LiAsF 6 , LiBF 4 、LiSbF 6 、LiAlCl 4 、LiClO 4 CF 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is preferred because it is easily soluble in solvents and exhibits a high degree of dissociation. 6 、LiClO 4 CF 3 SO 3 Li, particularly preferably LiPF 6 In addition, the electrolyte may be used alone or in combination of two or more in any ratio. Generally, the lithium ion conductivity tends to be higher when a supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted according to the type of supporting electrolyte.

[0160] As the organic solvent used for the electrolyte, as long as it can dissolve the supporting electrolyte, it is not particularly limited, and it is preferred to use, for example: carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, mixed solutions of these solvents can also be used. Among them, because the dielectric constant is high and the stable potential region is wide, carbonates are preferably used, and a mixture of ethylene carbonate and ethyl methyl carbonate is further preferably used.

[0161] The concentration of the electrolyte in the electrolytic solution can be adjusted appropriately. In addition, known additives such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and methyl ethyl sulfone may be added to the electrolytic solution.

[0162] <Spacer>

[0163] As a separator, there is no particular limitation, and for example, the separators described in Japanese Patent Publication No. 2012-204303 can be used. Among these, from the viewpoint of being able to make the overall film thickness of the separator thinner, thereby being able to increase the ratio of the electrode active material in the lithium ion secondary battery and increasing the capacity per unit volume, a microporous membrane composed of a polyolefin-based (polyethylene, polypropylene, polybutylene, polyvinyl chloride) resin is preferred.

[0164] <Method for producing lithium-ion secondary battery>

[0165] The lithium ion secondary battery as an electrochemical element can be manufactured by, for example, the following method: the positive electrode and the negative electrode are overlapped by a separator, and the battery is wound, folded, etc. according to the shape of the battery as needed, placed in a battery container, and the electrolyte is injected into the battery container and sealed. In order to prevent the internal pressure rise, overcharge and discharge, etc. of the lithium ion secondary battery, a fuse, a PTC element, an overcurrent protection element, a porous metal mesh, a guide plate, etc. can be provided as needed. The shape of the lithium ion secondary battery can be, for example, any one of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc.

[0166] Example

[0167] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%", "ppm" and "part" indicating an amount are based on mass unless otherwise specified.

[0168] Furthermore, unless otherwise stated, in a polymer produced by copolymerizing a plurality of monomers, the ratio of a monomer unit formed by polymerizing a certain monomer in the polymer generally corresponds to the ratio (feed ratio) of the certain monomer in all monomers used for polymerization of the polymer.

[0169] Furthermore, when the polymer is a hydrogenated polymer obtained by hydrogenating a polymer containing conjugated diene monomer units, the total content ratio of the unhydrogenated conjugated diene monomer units and the alkylene structural units which are the conjugated diene monomer units after hydrogenation in the hydrogenated polymer is consistent with the ratio (charging ratio) of the conjugated diene monomer in all monomers used for the polymerization of the polymer.

[0170] In the Examples and Comparative Examples, various measurements and evaluations were carried out according to the following methods.

[0171] [Iodine value]

[0172] The iodine value of the polymer is measured in accordance with JIS K6235.

[0173] <Weight Average Molecular Weight>

[0174] The weight average molecular weight (Mw) of the polymer was measured by gel permeation chromatography (GPC) under the following measurement conditions using a LiBr-DMF solution having a concentration of 10 mM.

[0175] Separation column: Shodex KD-806M (manufactured by Showa Denko K.K.)

[0176] Detector: Differential refractometer detector RID-10A (manufactured by Shimadzu Corporation)

[0177] Flow rate of eluent: 0.3 mL / min

[0178] Column temperature: 40°C

[0179] · Standard polymer: TSK standard polystyrene (manufactured by Tosoh Corporation)

[0180] <Value of {(a) / (b)}×100[%]>

[0181] Based on the contents of the polymer and triphenylphosphine sulfide in the adhesive composition prepared in the Examples and Comparative Examples, the content of triphenylphosphine sulfide relative to the content of the polymer (a) and the content of the hydrophilic group-containing monomer unit in the polymer relative to the content of the polymer (b) were calculated. Then, the value of {(a) / (b)}×100[%] was calculated.

[0182] <Content of Monovalent Cation>

[0183] Collect about 0.5g of the binder composition in terms of solid content conversion, dissolve it in about 7mL of concentrated sulfuric acid, and slowly add about 3mL of concentrated nitric acid for wet decomposition. After decomposition, the acid is concentrated, fixed to 10mL with ultrapure water, and the amount of potassium ions and sodium ions is determined by inductively coupled plasma atomic emission spectrometry (ICP-AES). Then, the total amount of potassium and sodium contained in the binder composition is calculated according to the measured value, and the total amount obtained is used as the amount of monovalent cations contained in the binder composition. Then, the content of monovalent cations relative to the content of polymer A in the binder composition is calculated.

[0184] <Adhesive Viscosity Change Rate>

[0185] For the adhesive compositions prepared in the examples and comparative examples, the viscosity of the adhesive composition one hour after the slurry was prepared was measured using a single-cylinder rotational viscometer (25°C, rotation speed = 60 rpm, rotor shape: 4) in accordance with JIS Z8803:1991, and the value one minute after the start of the measurement was obtained as the viscosity (η) of the adhesive composition. 0In addition, the viscosity of the adhesive composition one week after the adhesive composition was prepared was obtained and used as the viscosity of the adhesive composition (η 1 ).

[0186] The adhesive viscosity change rate was calculated according to the following formula and evaluated according to the following criteria: The lower the adhesive viscosity change rate, the better the viscosity stability of the adhesive composition.

[0187] Adhesive viscosity change rate (%) = {(η1 / η0)} × 100

[0188] A: The viscosity change rate of the adhesive is less than 10%

[0189] B: The viscosity change rate of the adhesive is more than 10% and less than 30%

[0190] C: The viscosity change rate of the adhesive is more than 30%

[0191] <Dispersibility of Conductive Material>

[0192] The conductive material dispersions prepared in the examples and comparative examples were subjected to rheometer (MCR302 manufactured by Anton Paar) at a temperature of 25° C. and a shear rate of 2.5 s -1 The viscosity is measured under the conditions of . Using this viscosity, the dispersibility of the conductive material dispersion is evaluated according to the following criteria. At the same solid content concentration (or a solid content concentration of a very close value), the lower the viscosity of the conductive material dispersion, the better the conductive material is dispersed.

[0193] A: Viscosity less than 1000mPa·s

[0194] B: Viscosity is 1000mPa·s or more and less than 3000mPa·s

[0195] C: Viscosity is 3000mPa·s or more and less than 10000mPa·s

[0196] D: Viscosity is 10000mPa·s or more

[0197] <Peel Strength>

[0198] The positive electrode for lithium ion secondary battery made in the embodiment and comparative example is cut into a rectangle with a length of 100mm and a width of 10mm as a test piece, and the surface with the positive electrode composite material layer is faced downward, and a transparent tape (according to the transparent tape of JIS Z1522) is pasted on the surface of the positive electrode composite material layer, and the stress when one end of the current collector is stretched and peeled off at a tensile speed of 100mm / minute in the vertical direction is measured (in addition, the transparent tape is fixed to the test bench). 3 measurements are carried out, and the average value is obtained as the peel strength, and it is evaluated according to the following benchmark. The larger the value of the peel strength, the more excellent the adhesion of the positive electrode composite material layer and the current collector.

[0199] A: Peel strength is 30N / m or more

[0200] B: Peel strength is 25 N / m or more and less than 30 N / m

[0201] C: Peel strength is 20 N / m or more and less than 25 N / m

[0202] D: Peel strength less than 20N / m

[0203] <Gas Generation from Electrodes>

[0204] The secondary batteries prepared in the embodiments and comparative examples were left to stand at 25°C for 24 hours. Then, at 25°C, the battery was charged to 4.35V at 0.1C and discharged to 2.75V at 0.1C. The battery cell of the battery was immersed in liquid paraffin, and the volume X0 of the battery cell was measured. Furthermore, the charging and discharging operation was repeated for 1000 cycles under the same conditions as above at 60°C. The battery cell of the battery after 1000 cycles was immersed in liquid paraffin, and the volume X1 of the battery cell was measured. The battery cell volume change rate ΔX before and after the high-temperature cycle test of repeated 1000 cycles of charge and discharge was calculated by the following formula, and evaluated according to the following criteria. The smaller the value of the battery cell volume change rate ΔX, the less gas is generated from the electrode, and the better the ability of the electrode to suppress gas generation.

[0205] Battery cell volume change rate ΔX (%) = (X1-X0) / X0×100

[0206] A: The battery cell volume change rate is less than 20%

[0207] B: The battery cell volume change rate is greater than 20% and less than 30%

[0208] C: The battery cell volume change rate is 30% or more and less than 40%

[0209] D: Battery cell volume change rate is more than 40%

[0210] (Example 1)

[0211] <Preparation of polymer>

[0212] 200 parts of ion exchange water, 25 parts of 10% sodium dodecylbenzene sulfonate aqueous solution, 30 parts of acrylonitrile as a nitrile group-containing monomer, 10 parts of methacrylic acid as a hydrophilic group-containing monomer, and 2.50 parts of tert-dodecyl mercaptan as a chain transfer agent were added to the reactor in sequence. Then, after replacing the internal gas with nitrogen three times, 60 parts of 1,3-butadiene as a conjugated diene monomer were added. Then, the reactor was kept at 10°C, 0.03 parts of cumene hydroperoxide as a polymerization initiator, appropriate amounts of a reducing agent and a chelating agent were added, and the polymerization reaction was continued while stirring. When the polymerization conversion rate reached 80%, 0.1 parts of a 10% hydroquinone aqueous solution as a polymerization terminator were added to terminate the polymerization reaction. Then, the residual monomers were removed at a water temperature of 80°C to obtain an aqueous dispersion of a polymer precursor.

[0213] A water dispersion and a palladium catalyst (a solution prepared by mixing a 1% palladium acetate acetone solution with an equal weight of ion exchange water) were added to an autoclave so that the palladium content was 3000ppm relative to the weight of the solid content contained in the water dispersion of the precursor of the obtained polymer, and a hydrogenation reaction was performed at a hydrogen pressure of 3Mpa and a temperature of 55°C for 3 hours to obtain a reaction solution. A strongly acidic cation exchange resin (manufactured by Purolite, "C100") in an amount equal to the weight of the solid content contained in the liquid was added to the obtained reaction solution, and the mixture was stirred for 2 hours with an oscillator at room temperature (25°C), and then filtered with a 200-mesh filter cloth to obtain a water dispersion of the target polymer (hydrogenated nitrile rubber). The mixture was then concentrated to a solid content concentration of 40% using an evaporator.

[0214] <Preparation of Adhesive Composition>

[0215] 50 parts of the aqueous dispersion of the above polymer (equivalent to 20 parts in terms of solid content), 0.0010 parts of triphenylphosphine sulfide (50 ppm relative to the amount of the polymer) and 300 parts of N-methyl-2-pyrrolidone (NMP) were added, and after all the water was evaporated under reduced pressure, NMP was evaporated to obtain an adhesive composition with a polymer concentration of 8%. The obtained adhesive composition was used to evaluate the iodine value, weight average molecular weight, {(a) / (b)}×100(%) value of the polymer, the content of monovalent cations and the adhesive viscosity change rate. The results are shown in Table 1.

[0216] <Preparation of Conductive Material Dispersion>

[0217] 4.0 parts of carbon nanotubes (specific surface area: 280 m 2 / g), 1.0 part (solid content conversion amount) of the above-obtained binder composition and the amount of NMP contained in the binder composition, which is a total of 100 parts of NMP, were stirred (3000rpm, 10 minutes), and then a thin film rotary high-speed mixer (Primex company, product name "FILMIX, 56-50 type") was used to perform dispersion treatment at a peripheral speed of 40m / second for 10 minutes to prepare a conductive material dispersion having a solid content concentration of 5.0%. Then, the obtained conductive material dispersion was used to evaluate the dispersibility of the conductive material. The results are shown in Table 1.

[0218] <Preparation of positive electrode slurry>

[0219] 98.0 parts of a ternary active material (LiNi 0.6 Co 0.2 Mn 0.2 O 2 ) (volume average particle size: 10 μm), 1.0 part of polyvinylidene fluoride as a binder, 1.0 part (solid content conversion amount) of the above-obtained conductive material dispersion, and NMP are mixed with a planetary mixer (60 rpm, 30 minutes) to prepare a positive electrode slurry. In addition, the amount of NMP added is adjusted so that the viscosity of the obtained positive electrode slurry (measured by a single-cylinder rotational viscometer according to JIS Z8803:1991. Temperature: 25°C, rotation speed: 60 rpm) is within the range of 4000 to 5000 mPa·s.

[0220] <Production of positive electrode>

[0221] A 20 μm thick aluminum foil was prepared as a current collector. The positive electrode slurry obtained as described above was coated with a notch wheel coater at a unit area weight of 20 mg / cm after drying. 2 The positive electrode raw material was rolled using a roller press to produce a positive electrode composite material layer (density: 3.2 g / cm 3 ) and aluminum foil. Then, the sheet-shaped positive electrode was cut into a width of 48.0 mm and a length of 47 cm to serve as a positive electrode for a lithium ion secondary battery. The peel strength of the positive electrode was evaluated. The results are shown in Table 1.

[0222] <Production of negative electrode>

[0223] 90 parts of spherical artificial graphite (volume average particle size: 12 μm) and 10 parts of SiO as the negative electrode active material were mixed using a planetary mixer. xA mixture of 1,2-dimethyl-1-nitropropene (volume average particle size: 10 μm), 1 part of styrene-butadiene polymer as a negative electrode binder, 1 part of carboxymethyl cellulose as a thickener, and an appropriate amount of water as a dispersion medium were stirred to prepare a negative electrode slurry.

[0224] Next, a copper foil with a thickness of 15 μm was prepared as a current collector. The negative electrode slurry obtained as described above was applied in an amount of 10 mg / cm after drying. 2 The negative electrode raw material was then rolled using a roller press to produce a negative electrode raw material having a density of 1.6 g / cm 3 The negative electrode sheet was formed by a negative electrode composite material layer and a copper foil. Then, the negative electrode sheet was cut into pieces with a width of 50.0 mm and a length of 52 cm to serve as a negative electrode for a lithium ion secondary battery.

[0225] <Manufacturing of lithium-ion secondary batteries>

[0226] The electrode composite material layers of the positive electrode and the negative electrode prepared as described above are opposite to each other through a separator (microporous film made of polyethylene) with a thickness of 15 μm, and a core with a diameter of 20 mm is used for winding to obtain a wound body. Then, the obtained wound body is compressed in one direction at a speed of 10 mm / second until the thickness becomes 4.5 mm. In addition, the compressed wound body is elliptical when viewed from above, and the ratio of its major diameter to minor diameter (major diameter / minor diameter) is 7.7.

[0227] In addition, prepare the electrolyte (1.0 M LiPF 6 Solution (the solvent is a mixed solution of 5% by mass of fluoroethylene carbonate added to a mixed solvent of ethylene carbonate / ethyl methyl carbonate = 3 / 7 (mass ratio), and 2% by volume of vinylene carbonate is added as an additive)).

[0228] Thereafter, the compressed winding body was stored in an aluminum laminate shell together with 3.2 g of electrolyte. Then, a nickel lead was connected to a predetermined position of the negative electrode of the lithium ion secondary battery, and an aluminum lead was connected to a predetermined position of the positive electrode of the lithium ion secondary battery, and the opening of the shell was sealed by heat to obtain a lithium ion secondary battery. The lithium ion secondary battery was in the shape of a bag with a width of 35 mm, a height of 60 mm, and a thickness of 5 mm, and the nominal capacity of the battery was 700 mAh.

[0229] The results are shown in Table 1.

[0230] (Example 2)

[0231] When preparing the binder composition, the amount of triphenylphosphine sulfide was changed to 0.0018 parts (90 ppm relative to the amount of the polymer), and the binder composition, conductive material dispersion, positive electrode slurry, positive electrode, negative electrode and lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0232] (Example 3)

[0233] When preparing the binder composition, the amount of triphenylphosphine sulfide was changed to 0.0001 part (5 ppm relative to the amount of the polymer), and the binder composition, conductive material dispersion, positive electrode slurry, positive electrode, negative electrode and lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0234] (Example 4)

[0235] When preparing the polymer, the amount of the strongly acidic cation exchange resin (manufactured by Purolite, "C100") was changed to 0.5 parts by mass. A binder composition, a conductive material dispersion, a positive electrode slurry, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0236] (Example 5)

[0237] When preparing the polymer, the amount of acrylonitrile was changed to 31 parts, the amount of methacrylic acid was changed to 7 parts, the amount of 1,3-butadiene was changed to 62 parts, and the amount of triphenylphosphine sulfide was changed to 0.0018 parts (90 ppm relative to the amount of the polymer). Otherwise, the binder composition, the conductive material dispersion, the positive electrode slurry, the positive electrode, the negative electrode, and the lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0238] (Example 6)

[0239] When preparing the polymer, the amount of the strongly acidic cation exchange resin (manufactured by Purolite, "C100") was changed to 0.2 parts by mass. A binder composition, a conductive material dispersion, a positive electrode slurry, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0240] (Comparative Example 1)

[0241] The binder composition, conductive material dispersion, positive electrode slurry, positive electrode, negative electrode and lithium ion secondary battery were prepared in the same manner as in Example 1 except that triphenylphosphine sulfide was not used in the preparation of the binder composition. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0242] (Comparative Example 2)

[0243] When preparing the binder composition, the amount of triphenylphosphine sulfide was changed to 0.0032 parts (160 ppm relative to the amount of the nitrile polymer), and the binder composition, conductive material dispersion, positive electrode slurry, positive electrode, negative electrode and lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0244] (Comparative Example 3)

[0245] When preparing the polymer, the amount of acrylonitrile was changed to 24 parts, the amount of methacrylic acid was changed to 30 parts, the amount of 1,3-butadiene was changed to 46 parts, and the amount of triphenylphosphine sulfide was changed to 0.0002 parts (relative to the amount of nitrile polymer is 10 ppm). In addition, the binder composition, the conductive material dispersion, the positive electrode slurry, the positive electrode, the negative electrode and the lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0246] (Comparative Example 4)

[0247] In the preparation of the polymer, except that the amount of acrylonitrile was changed to 40 parts and the amount of methacrylic acid was changed to 0 parts, a binder composition, a conductive material dispersion, a positive electrode slurry, a positive electrode, a negative electrode, and a lithium ion secondary battery were prepared in the same manner as in Example 1. Then, various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0248] [Table 1]

[0249]

[0250] As shown in Table 1, the adhesive compositions of Examples 1 to 6 can prepare conductive material dispersions having excellent dispersibility of conductive materials, and by using the conductive material dispersions, lithium ion secondary batteries having excellent peel strength and suppressed gas generation can be obtained.

[0251] On the other hand, as shown in Table 1, in Comparative Example 1 in which a binder composition not containing triphenylphosphine sulfide is used, the dispersibility of the conductive material is reduced, and the gas generation of the electrode is not suppressed. In addition, as shown in Comparative Example 2, when the amount of triphenylphosphine sulfide contained in the binder composition exceeds the prescribed amount, the dispersibility of the conductive material is reduced and the peel strength is also reduced. In addition, as shown in Comparative Example 3, when the amount of triphenylphosphine sulfide contained in the binder composition and the amount of the hydrophilic group-containing monomer unit do not satisfy the prescribed relationship, the gas generation of the electrode is not suppressed.

[0252] Furthermore, from Comparative Example 4, it is understood that when the adhesive composition does not contain a polymer having a predetermined composition, the dispersibility of the conductive material decreases.

[0253] Industrial Applicability

[0254] According to the present invention, it is possible to provide an adhesive composition for an electrochemical element that can prepare a conductive material dispersion having sufficiently high dispersibility of a conductive material and can produce an electrode having excellent peel strength and reduced gas generation.

[0255] Furthermore, according to the present invention, it is possible to provide a conductive material dispersion for an electrochemical element and a slurry for an electrochemical element electrode, which can produce an electrode having sufficiently high dispersibility of a conductive material, excellent peel strength and reduced gas generation.

[0256] Furthermore, according to the present invention, it is possible to provide an electrode for an electrochemical device having excellent peel strength and reduced gas generation, and an electrochemical device having the electrode for an electrochemical device.

Claims

1. An adhesive composition for an electrochemical element, comprising: A polymer comprising a nitrile group-containing monomer unit, an alkylene structural unit and a hydrophilic group-containing monomer unit; N-methyl-2-pyrrolidone; and Triphenylphosphine sulfide; The content of the triphenylphosphine sulfide is 2 mass ppm or more and 100 mass ppm or less relative to the content of the polymer, When the content of the triphenylphosphine sulfide relative to the content of the polymer is (a) and the content of the hydrophilic group-containing monomer unit relative to the content of the polymer is (b), the following relationship is satisfied: 0.004(%)≤{(a) / (b)}×100(%)≤0.150(%).

2. The adhesive composition for electrochemical elements according to claim 1, wherein The content of the monovalent cation is 100 ppm by mass or less relative to the content of the polymer. 3 . A conductive material dispersion for an electrochemical element, comprising at least the binder composition for an electrochemical element according to claim 1 and a conductive material.

4. The conductive material dispersion for electrochemical element according to claim 3, wherein The conductive material is carbon nanotube. 5 . A slurry for an electrochemical element electrode, comprising at least the conductive material dispersion for an electrochemical element according to claim 3 and an electrode active material. 6 . An electrochemical element electrode comprising an electrode composite material layer formed using the slurry for an electrochemical element electrode according to claim 5 . 7 . An electrochemical device comprising the electrode for an electrochemical device according to claim 6 .

Citation Information

Patent Citations

  • Electrode for secondary battery, binder for secondary battery electrode, manufacturing method and secondary battery

    JP2012204303A

  • Secondary cell negative electrode, secondary cell, slurry composition for negative electrode, and method of producing secondary cell negative electrode

    WO2012115096A1

  • Binder composition for secondary battery positive electrode, slurry composition for secondary battery positive electrode, secondary battery positive electrode, and secondary battery

    WO2013080989A1

  • Binder composition for non-aqueous secondary cell positive electrode, composition for non-aqueous secondary cell positive electrode, non-aqueous secondary cell positive electrode and non-aqueous secondary cell, and method for producing composition for non-aqueous secondary cell positive electrode, non-aqueous secondary cell positive electrode and non-aqueous secondary cell

    WO2016103730A1