Preparation method and application of thermally-induced rapid-hardening capsule
Sodium silicate capsules are prepared through fluidized bed technology and physical method of spray gun atomization wax liquid curing, which solves the complex and cost-effective preparation of existing thermogenic fast gel capsules, and realizes regular surface and efficient dispersion of the capsules, supporting Large-scale industrial production.
Patent Information
- Application Number
- CN202411183818.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The existing thermally induced rapid gel capsule preparation methods are complex and costly. The organic shells used are harmful to the human body, and the preparation devices are complex, making it difficult to achieve large-scale industrial production.
The physical method is used to prepare the paraffin-wrapped capsules of sodium silicate particles through fluidized bed technology, and the spray gun atomized wax liquid is used to cure it on the surface of the sodium silicate particles, combining vibration dispersion and automated processes to achieve uniform and dense preparation of the capsules.
简化了制备过程,降低了成本,实现了胶囊的规则表面和高效分散,避免了人体和环境污染,支持了大规模工业化生产。
Smart Images

Figure HDA0005012959960000011 
Figure HDA0005012959960000012 
Figure HDA0005012959960000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a preparation method of a thermal rapid gel capsule and application thereof. Background Art
[0002] Sodium silicate (Na2SiO3), commonly known as water glass, is a commonly used alkali activator that can promote the hydration reaction between components such as silicate in mineral powder and water, and promote the hydration reaction activity of cement, thereby accelerating the setting speed of concrete, improving the early and late strength of concrete, and improving the working performance of concrete. Currently, researchers are committed to continuously improving the preparation technology of sodium silicate capsules to repair cracks in concrete. When a temperature field is applied, the paraffin melts and releases the encapsulated sodium silicate, promoting the hydration reaction between components such as silicate in mineral powder and water, and promoting the hydration reaction activity of cement, which can effectively repair cracks in concrete and improve the density and durability of concrete.
[0003] Thermo-accelerated gel capsules are prepared by wrapping alkali activators with hot-melt materials. Common alkali activators include sodium hydroxide, sodium silicate, etc. By applying a temperature field to dissolve the shell material and release the internal alkali activator, the concrete can solidify quickly. This is a technology that effectively controls the concrete solidification process and has many applications in scenarios such as 3D printing concrete where cement solidification needs to be controlled.
[0004] The commonly used methods for preparing thermal rapid gel capsules are mostly chemical methods, which are complicated in preparation process and expensive to mass produce. At the same time, many organic shells used are usually harmful to the human body. In addition, the preparation equipment is too complicated, which wastes manpower and material resources and greatly increases the cost. Summary of the invention
[0005] To solve the above problems, the present invention provides a method for preparing a thermo-accelerated gel capsule and its application. The capsule is prepared by a physical method, the preparation process is easier to control, and an automated preparation process is realized with low cost and high efficiency, which is conducive to industrial expansion of production.
[0006] In order to achieve the above object, the technical solution provided by the present invention is:
[0007] A method for preparing a thermosensitive gel capsule is provided, and the specific steps are as follows:
[0008] 1) Preparation of wax solution: put the chopped wax into the heating pool to melt, and set the temperature to keep it warm after it is completely melted to prevent the wax from solidifying;
[0009] 2) Preparation of spraying device: directly transport the melted wax from the heating pool to the heatable spray gun through the delivery pipe, the heatable spray gun is connected to the bottom spray fluidized bed, and the delivery pipe is heated by the heating belt;
[0010] 3) Sodium silicate feeding: Add the sodium silicate granules into the feeding bin. The equipment uses the negative pressure airflow generated by the exhaust fan to directly press the material into the raw material container of the fluidized bed through the feeding pipe to achieve automatic feeding;
[0011] 4) Capsule preparation: Start the fluidized bed to suspend the sodium silicate particles in the device, start the heatable spray gun to atomize the liquid wax into small droplets that adhere evenly to the surface of the sodium silicate particles along the air flow direction, and adjust the air inlet temperature before spraying to solidify the wax and firmly adhere to the surface of the particles to obtain capsules;
[0012] 5) Particle dispersion: After the preparation is completed, the material is discharged and the capsules obtained in step 4) are placed on a conveyor belt. Solid lubricants are added during the conveying process. The conveyor belt is equipped with left and right vibration devices to improve the dispersion of particles and prevent the particles from sticking. The preparation process is completed to obtain the thermo-accelerated gel capsule.
[0013] According to the above scheme, in step 1), the wax selected is one of coconut wax and paraffin wax. Preferably, the melting point of the wax is 40-60°C, and the selected wax completely melts into liquid at above 60°C.
[0014] According to the above scheme, in step 1), the heating pool is directly connected to the spray gun through a delivery pipe and includes a temperature detection and control device, and the insulation temperature is 60-80°C.
[0015] According to the above scheme, in step 1), the wax selected is 10wt%-30wt% of the sodium silicate particles used in step 3).
[0016] According to the above scheme, in step 2), the temperature of the spray gun can be heated to 45-90°C, and the temperature of the heating belt can be 50-100°C; preferably, the caliber of the spray gun is 0.3-0.5mm.
[0017] According to the above scheme, in step 2), the average particle size of sodium silicate is 0.8-1 mm.
[0018] According to the above scheme, in step 4), the air inlet speed of the fluidized bed is 0.5-2 m / s, and the air inlet temperature is 40-60°C.
[0019] According to the above scheme, in step 5), the solid lubricant used is one of talcum powder or graphite.
[0020] According to the above scheme, in step 5), the vibration frequency of the vibration device is 10-50 Hz.
[0021] According to the above scheme, in step 5), the amount of solid lubricant used is 5wt%-15wt% of the sodium silicate particles.
[0022] According to the above scheme, in step 5), the obtained thermal rapid gel capsule has a regular surface and a thin wax shell with a thickness of 50-100 μm.
[0023] Provided is an application of the thermal rapid gel capsule prepared by the preparation method in concrete.
[0024] The beneficial effects of the present invention are as follows:
[0025] 1. The present invention prepares the sodium silicate capsules wrapped with paraffin by fluidized bed technology. When the paraffin liquid is sprayed out by atomization of a spray gun, the inlet air temperature is slightly lower than the wax solidification temperature. When the atomized liquid droplets adhere to the surface of the sodium silicate particles, they will solidify and form a thin wax shell layer on the surface of the sodium silicate particles. Since the movement of each sodium silicate particle in the fluidized bed is random, the shell structure is uniform and dense. At the same time, during the transmission process, the capsules are dispersed by a solid lubricant, and the gaps on the surface of the capsules can be filled, so that the particles are more regular. The present invention adopts a physical method to prepare the capsules, the preparation process is easier to control, and an automated preparation process is realized, which greatly saves manpower, material resources and financial resources, and can realize large-scale production. No substances harmful to the human body and the environment are generated in the preparation process, and the preparation process is green and environmentally friendly, and has important application prospects.
[0026] 2. The sodium silicate capsules coated with wax shells obtained by the present invention have uniform and dense shells, and the gaps are filled with lubricants, so that the particles are more regular. When used in concrete, the capsules can be prevented from being broken due to uneven stress and having an adverse effect on the strength of the concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the shell structure model obtained in the embodiment of the present invention.
[0028] Figure 2 The present invention provides a simplified preparation process flow chart of the sodium silicate capsules obtained in the present invention.
[0029] Figure 3 This is a sample picture of the sodium silicate capsule obtained in the embodiment of the present invention under a 150x optical microscope, wherein Figure 3 a is uncoated sodium silicate particles, Figure 3 b is the wax-coated sodium silicate capsule obtained in Example 2, and the scale bar is 500 μm. DETAILED DESCRIPTION
[0030] In order to better understand the present invention, the present invention will be further explained below in conjunction with specific examples. The specific examples are only for a better understanding of the present invention and are not limited to the following examples.
[0031] Example 1
[0032] A method for preparing sodium silicate capsules comprises the following steps:
[0033] 1. Usage of each medicine: paraffin 50.17g, sodium silicate 499.99g, talcum powder 25.53g.
[0034] 2. The specific implementation steps are as follows:
[0035] 1) Preparation of wax solution: put the chopped paraffin into the heating pool and heat it to melt, the temperature is set to 70°C;
[0036] 2) Preparation of spraying device: directly transport the melted wax from the heating pool to the heatable spray gun through the delivery pipe, the heatable spray gun is connected to the bottom spray fluidized bed, and the delivery pipe is heated by the heating belt. The diameter of the spray gun is 0.3mm, and the temperature of the heating belt is 70℃;
[0037] 3) Feeding device: Add the sodium silicate granules into the feeding bin, and the equipment uses the negative pressure airflow generated by the exhaust fan to directly press the materials into the raw material container of the fluidized bed through the feeding pipe to achieve automatic feeding. Among them, the particle size of the sodium silicate particles is 0.8-1.0mm;
[0038] 4) Capsule preparation: Start the fluidized bed to suspend the sodium silicate particles in the device, start the heatable spray gun to atomize the liquid wax into small droplets that adhere evenly to the surface of the sodium silicate particles along the air flow direction, and adjust the air inlet temperature before spraying to solidify the wax and firmly adhere to the surface of the particles to obtain capsules. Among them, the air inlet temperature is 55℃, the air inlet speed is 1m / s, and the spray gun temperature is 70℃;
[0039] 5) Particle dispersion: After preparation, the capsules are placed on a conveyor belt and the prepared talcum powder is added for vibration dispersion, and the capsules are prepared. The vibration frequency is 25 Hz.
[0040] Example 2
[0041] A method for preparing sodium silicate capsules comprises the following steps:
[0042] 1. Usage of each medicine: paraffin 100.10g, sodium silicate 499.95g, talcum powder 50g.
[0043] 2. The specific implementation steps are as follows:
[0044] Preparation of wax solution: put the chopped paraffin into the heating pool and heat it to melt. The temperature is set to 70℃.
[0045] 2) Preparation of spraying device: directly transport the melted wax from the heating pool to the heatable spray gun through the conveying pipe, the heatable spray gun is connected to the bottom spray fluidized bed, and the conveying pipe is heated by the heating belt. The diameter of the spray gun is 0.5mm, and the temperature of the heating belt is 80℃;
[0046] 3) Feeding device: Add the sodium silicate granules into the feeding bin. The equipment uses the negative pressure airflow generated by the exhaust fan to directly press the material into the raw material container of the fluidized bed through the feeding pipe to achieve automatic feeding. The particle size of the sodium silicate particles is 0.8-1.0mm;
[0047] 4) Capsule preparation: Start the fluidized bed to suspend the sodium silicate particles in the device, start the heatable spray gun to atomize the liquid wax into small droplets that adhere evenly to the surface of the sodium silicate particles along the air flow direction, and adjust the air inlet temperature before spraying to solidify the wax and firmly adhere to the surface of the particles to obtain capsules. Among them, the air inlet temperature is 55℃, the air inlet speed is 1m / s, and the spray gun temperature is 80℃;
[0048] 5) Particle dispersion: After preparation, the capsules are placed on a conveyor belt and the prepared talcum powder is added for vibration dispersion, and the capsules are prepared. The vibration frequency is 30 Hz.
[0049] Example 3
[0050] A method for preparing sodium silicate capsules comprises the following steps:
[0051] 1. Usage of each medicine: paraffin 50.05g, sodium silicate 500.02g, talcum powder 37.52g.
[0052] 2. The specific implementation steps are as follows:
[0053] 1) Preparation of wax solution: put the chopped paraffin into the heating pool and heat it to melt, the temperature is set to 70°C;
[0054] 2) Preparation of spraying device: directly transport the melted wax from the heating pool to the heatable spray gun through the delivery pipe, the heatable spray gun is connected to the bottom spray fluidized bed, and the delivery pipe is heated by the heating belt. The diameter of the spray gun is 0.3mm, and the temperature of the heating belt is 80℃;
[0055] 3) Feeding device: Add the sodium silicate granules into the feeding bin. The equipment uses the negative pressure airflow generated by the exhaust fan to directly press the material into the raw material container of the fluidized bed through the feeding pipe to achieve automatic feeding. The particle size of the sodium silicate particles is 0.8-1.0mm;
[0056] 4) Capsule preparation: Start the fluidized bed to suspend the sodium silicate particles in the device, start the heatable spray gun to atomize the liquid wax into small droplets that adhere evenly to the surface of the sodium silicate particles along the air flow direction, and adjust the air inlet temperature before spraying to solidify the wax and firmly adhere to the surface of the particles to obtain capsules. Among them, the air inlet temperature is 55℃, the air inlet speed is 1m / s, and the spray gun temperature is 70℃;
[0057] 5) Particle dispersion: After preparation, the capsules are placed on a conveyor belt and the prepared talcum powder is added for vibration dispersion, and the capsules are prepared. The vibration frequency is 20 Hz.
[0058] Example 4
[0059] A method for preparing sodium silicate capsules comprises the following steps:
[0060] 1. Usage of each medicine: Coconut wax 74.98g, sodium silicate 500.04g, talcum powder 50.02g.
[0061] 2. The specific implementation steps are as follows:
[0062] 1) Preparation of wax solution: put the chopped paraffin into the heating pool and heat it to melt, the temperature is set to 70°C;
[0063] 2) Preparation of spraying device: The melted wax is directly transported from the heating pool to the heatable spray gun through the conveying pipe, the heatable spray gun is connected to the bottom spray fluidized bed, and the conveying pipe is heated by the heating belt. The diameter of the spray gun is 0.5mm, and the temperature of the heating belt is 85℃;
[0064] 3) Feeding device: Add the sodium silicate granules into the feeding bin. The equipment uses the negative pressure airflow generated by the exhaust fan to directly press the material into the raw material container of the fluidized bed through the feeding pipe to achieve automatic feeding. The particle size of the sodium silicate particles is 0.8-1.0mm;
[0065] 4) Capsule preparation: Start the fluidized bed to suspend the sodium silicate particles in the device, start the heatable spray gun to atomize the liquid wax into small droplets that adhere evenly to the surface of the sodium silicate particles along the air flow direction, and adjust the air inlet temperature before spraying to solidify the wax and firmly adhere to the surface of the particles to obtain capsules. Among them, the air inlet temperature is 55℃, the air inlet speed is 1m / s, and the spray gun temperature is 70℃;
[0066] 5) Particle dispersion: After preparation, the capsules are placed on a conveyor belt and the prepared talcum powder is added for vibration dispersion, and the capsules are prepared. The vibration frequency is 25 Hz.
[0067] The talcum powder used in the above example is industrial grade 3000 mesh. The sodium silicate capsules are dispersed during the preparation process, and the conveyor belt is added with a vibration device to further disperse the capsules. The entire preparation process can be fully automated, and the entire production process will not cause pollution to the environment, which can greatly save manpower, material resources, and financial resources, and can realize large-scale production process.
[0068] The above examples are only for a better understanding of the present invention and are not intended to limit the present invention. Any modifications and substitutions based on the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a thermal rapid gel capsule, It is characterized in that The specific steps are as follows: 1) Preparation of wax solution: put the chopped wax into the heating pool to melt, and set the temperature to keep it warm after it is completely melted to prevent the wax from solidifying; 2) Preparation of spraying device: directly transport the melted wax from the heating pool to the heatable spray gun through the delivery pipe, the heatable spray gun is connected to the bottom spray fluidized bed, and the delivery pipe is heated by the heating belt; 3) Sodium silicate feeding: Add the sodium silicate granules into the feeding bin. The equipment uses the negative pressure airflow generated by the exhaust fan to directly press the material into the raw material container of the fluidized bed through the feeding pipe to achieve automatic feeding; 4) Capsule preparation: Start the fluidized bed to suspend the sodium silicate particles in the device, start the heatable spray gun to atomize the liquid wax into small droplets that adhere evenly to the surface of the sodium silicate particles along the air flow direction, and adjust the air inlet temperature before spraying to solidify the wax and firmly adhere to the surface of the particles to obtain capsules; 5) Particle dispersion: After the preparation is completed, the material is discharged and the capsules obtained in step 4) are placed on a conveyor belt. Solid lubricants are added during the conveying process. The conveyor belt is equipped with left and right vibration devices to improve the dispersion of particles and prevent the particles from sticking. The preparation process is completed to obtain the thermo-accelerated gel capsule.
2. The preparation method according to claim 1, It is characterized in that In the step 1), the wax selected is one of coconut wax and paraffin wax.
3. The preparation method according to claim 1, It is characterized in that In the step 1), the melting point of the wax selected is 40-60°C.
4. The preparation method according to claim 1, It is characterized in that In the step 1), the heating pool is directly connected to the spray gun by a delivery pipe and includes a temperature detection and control device, and the insulation temperature is 60-80°C.
5. The preparation method according to claim 1, It is characterized in that In the step 1), the wax selected is 10-30wt% of the sodium silicate particles used in the step 3).
6. The preparation method according to claim 1, It is characterized in that In the step 5), the amount of solid lubricant used is 5-15wt% of the sodium silicate particles.
7. The preparation method according to claim 1, It is characterized in that In the step 2), the temperature of the heated spray gun is 45-90°C, and the temperature of the heating zone is 50-100°C; in the step 4), the air inlet speed of the fluidized bed is 0.5-2m / s, and the air inlet temperature is 40-60°C.
8. The preparation method according to claim 1, It is characterized in that In the step 5), the solid lubricant used is talcum powder or graphite.
9. The preparation method according to claim 1, It is characterized in that In the step 5), the vibration frequency of the vibration device is 10-50 Hz.
10. Use of the thermal rapid gel capsule prepared by the preparation method according to any one of claims 1 to 9 in concrete.