Preparation method of atomic-scale dispersion (M1)-cluster (Mn) multi-scale site synergistic catalytic material
By modifying the carbon-containing gas on the industrial support, the controllable adjustment of atomic dispersion and cluster sites is achieved, which solves the problem that precious metal catalysts in the prior art are difficult to achieve multi-scale site loading in the industry, and improves the catalytic activity and selective, and avoid hazards and control problems under high temperature conditions.
Patent Information
- Application Number
- CN202411179189.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
It is difficult for existing precious metal catalysts to achieve simultaneous loading and regulation of atomic dispersion and cluster sites in the industry, resulting in limited catalytic activity and selectivity, and traditional methods have hazards and control difficulties under high temperature conditions.
By modifying commonly used industrial carriers, they are converted into active carriers with self-reduction functions, capturing and anchoring the reduction of precious metal ions in situ, achieving controllable proportional adjustment of atomic dispersion and cluster sites, avoiding additional energy The process of input and high-temperature hydrogen reduction.
It realizes the coordinated catalyst of atomic dispersion and cluster sites loading on industrial support, improves catalytic activity and selectivity, is suitable for tandem reactions, and the process is safe and controllable.
Smart Images

Figure HDA0005011599020000011 
Figure HDA0005011599020000021 
Figure HDA0005011599020000031
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalysts, and specifically relates to an atomic-level dispersed (M1)-cluster (M n ) A method for preparing multi-scale site synergistic catalytic materials, which is mainly used for tandem reactions. Background Art
[0002] Precious metal heterogeneous catalysts are widely used in the fields of petrochemicals, fine chemicals, environmental protection, energy production and conversion, etc. With the advancement of global industrialization, the demand for precious metal catalysts will continue to increase, and it is urgent to develop high-performance precious metal catalysts. Dispersing nanoparticles to clusters or even atomic-level dispersion scales is conducive to maximizing the exposure of metal atoms, improving catalytic performance and atomic utilization efficiency, and has become a hot area of research in recent years. However, most chemical reactions in industry involve multiple reactant molecules or contain multiple tandem steps, and the related adsorption activation is affected by structural sensitivity, especially some molecules show strong size dependence on active sites. For example, in tandem reductive amination reactions, NH3 molecules tend to be on cluster / nanoparticle sites, while H2 tends to be adsorbed on atomic-level dispersed sites (Coupling Cross-Dimensional Ru1-Run Sites in Confined Nanoislands to Overcomethe Limitation of Coadsorption and Diffusion in Tandem Reactions[J].ACSCatal.2024,14,1584-1594). Obviously, whether it is atomic-level dispersed sites, clusters or NPs, they can only provide one type of active center for catalytic reactions, and it is difficult to provide multiple structures to match the adsorption and activation of all reactants / intermediates, and the scope of application is extremely limited. Atomic-level dispersed sites and clusters can meet the needs of molecules adsorbed in independent active centers and aggregated active centers, respectively. Therefore, decoupling an active metal into two scales (atomic-level dispersed sites and clusters / nanoparticles) provides a prospect for solving the above difficulties.
[0003] In the patent "A single-component multi-center catalyst with spatial confinement in a metal nano-island and its preparation method", we introduced a method of anchoring different scales M1-M2 on the surface of reducible non-precious metal nanoparticles by atomic dilution method. nThe method of removing the defect sites, however, is difficult to implement in industrial carriers (silicon dioxide, alumina, zeolite, graphene oxide, diatomaceous earth, layered double hydroxides (LDH), etc.), and is not suitable for large-scale industrial expansion. In addition, the abundance of defect sites on the surface of industrial carriers is low, making it difficult to form covalent bonds with metal atoms, while the surface energy and chemical activity of atomic-level dispersion and cluster sites are high, and it is a natural trend for them to aggregate into particles. The traditional method of inducing the migration of metal atoms in nanoparticles by inputting external energy to achieve "top-down" redispersion is difficult to control the reaction process, making the regulation of the degree of dispersion of multi-scale sites a great challenge. Therefore, it is necessary to find a simple and controllable method for preparing an efficient catalyst that can simultaneously load multiple scale sites on the same carrier surface in large quantities. In this patent, we use carbon-containing gas to modify the surface of the oxide carrier to transform it into an active carrier with self-reduction function to capture and in-situ anchor and reduce precious metal ions, thereby achieving atomic-level dispersion (M1) and cluster (M2). n )Controllable regulation of site ratios. Summary of the invention
[0004] The purpose of the present invention is to provide a kind of atomic-level dispersed (M1)-cluster (M n ) Preparation method of synergistic catalytic materials with multi-scale sites and their application in tandem reactions.
[0005] The present invention provides a noble metal catalyst, wherein the noble metal is dispersed at the atomic level (M1) and clustered (M n ) exist on the surface of the oxide support in the form of M1-M n / X, M represents the active component precious metal, M1 and M n are atomic-level dispersion and cluster sites, respectively; X represents the oxide support.
[0006] In the above catalyst, the noble metal M may be Rh, Pd, Ru, Ir, Au, Ag, or Pt. In terms of mass percentage, the content of the noble metal in the catalyst may be 0.1% to 5%.
[0007] In the above catalyst, the carrier is silicon dioxide, aluminum oxide, zeolite, graphene oxide, diatomaceous earth, layered double metal hydroxide LDH carrier widely used in industry. After the carrier is treated with carbon-containing mixed gas G, an active carrier with self-reduction function is obtained.
[0008] The specific preparation steps of the catalyst provided by the present invention are as follows:
[0009] A: Place the carrier in a reactor, seal it, first let the protective gas enter the reactor through a deoxygenator, then let the carbon-containing atmosphere G and the protective gas enter the reactor, and control the flow rate of the G gas and the protective gas by a mass flow meter to adjust the ratio of the reaction gas; use a programmed temperature to heat the reactor, the heating rate is 2-15°C / min, the reaction temperature is 200-700°C, and the reaction time is 1-10h; the reaction gas flow rate is 10mL / min-100mL / min; after the reaction, an active carrier X is obtained;
[0010] The reaction gas is composed of carbon-containing gas G and protective gas, wherein the volume content of G is 5%-60%;
[0011] The protective gas is an inert gas, such as nitrogen, argon or helium;
[0012] The deoxidizing device is a drying tube to which a 401 manganese-based deoxidizer is added;
[0013] The G is one or more of C2H6, C2H4, C2H2, CH4, CO2, and CO.
[0014] B: Dissolve the noble metal M salt in the corresponding solvent in B to prepare a solution with a concentration of 10 to 50 mmol / L;
[0015] The M salt is present in the form of at least one of nitrate, sulfate, hydrochloride, acetylacetonate and acetate;
[0016] The solvent is at least one of ethanol, methanol, acetone, carbon tetrachloride and water;
[0017] C: The active carrier X prepared in step A is uniformly dispersed in the solvent described in step B to obtain a suspension with a solid content of 0.05-0.5 g / mL; the noble metal M salt solution prepared in step B is added to make the loading amount of M 0.1-5 wt%, and the mixture is stirred continuously and heated to 30-80°C until the solvent is completely evaporated. The obtained solid is placed in an oven at 40-80°C and dried for 1 hour to obtain M1-M n / X catalyst.
[0018] Beneficial effects of the present invention:
[0019] In the preparation process of the catalyst preparation method provided by the present invention, the surface of the carrier X widely used in industry is first modified by a carbon-containing gas to transform it into an active carrier with a self-reducing function, which can capture and in-situ anchor and reduce precious metal ions. By adjusting one or more factors of the carrier treatment atmosphere, temperature, and time, the number of reducing active species modified on the carrier surface can be adjusted to achieve atomic-level dispersion (M1) and clustering (M2). n) site ratio can be controlled. This process avoids the process of additional energy input-induced redispersion when preparing highly dispersed catalysts with inert industrial carriers, and also avoids the danger of reducing precious metals with hydrogen under traditional high-temperature conditions. This multi-scale site catalyst is used in cascade reactions and has excellent catalytic activity and selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The CO infrared characterization of the multi-scale catalyst prepared in Example 1 shows obvious CO linear adsorption peaks and bridge adsorption peaks, which are respectively attributed to the CO at the atomically dispersed Pt1 sites and the aggregated cluster Pt n The adsorption of Pt sites indicates that Pt exists on the SiO2 surface in both atomic-level dispersion and cluster forms in the catalyst.
[0021] Figure 2 This is a spherical aberration electron microscope photograph of the catalyst prepared in Example 3. It can be seen that the metal Ru is uniformly dispersed on the surface of the alumina carrier in the form of atomic-level dispersion and clusters.
[0022] Figure 3 The results are shown for evaluating the catalyst in the reductive amination cascade reaction in the application example. DETAILED DESCRIPTION
[0023] Example 1
[0024] A. Weigh 2g of silica sample and place it in the reactor, seal it, first let the protective gas enter the reactor through the deoxygenator, select methane and acetylene as G gas, and let it enter the reactor after passing through the deoxygenator. The mass flow meter controls the flow rate ratio of methane, acetylene and protective gas to be 4:1:5, so that the gas ratio flowing through the reactor is 40% CH4 / 10% C2H2 / 50% N2 (protective gas). Use programmed heating, heat to 500℃ at a heating rate of 10℃ / min, adjust the gas flow rate to 35mL / min, and the reaction time is 2h. After the reaction is completed, cool to room temperature, take out the sample, and obtain a silica carrier with self-reduction activity.
[0025] B: Dissolve H2PtCl6 in ethanol to make 17.60mmol / L Pt 4+ Impregnation fluid.
[0026] C: The silica carrier prepared in step A was evenly dispersed in 5 mL of ethanol to obtain a suspension with a solid content of 0.4 g / mL; the Pt salt solution prepared in step B was added to make the Pt loading amount 0.5 wt%, and the mixture was stirred continuously and heated to 40°C until the ethanol was completely evaporated. The obtained solid was placed in a 40°C oven and dried for 1 h to obtain Pt1-Pt n / SiO2 catalyst.
[0027] Example 2
[0028] A. Weigh 2g of silica sample and place it in the reactor, seal it, first let the protective gas enter the reactor through the deoxygenator, select methane and acetylene as G gas, and let it enter the reactor after passing through the deoxygenator. The mass flow meter controls the flow rate ratio of methane, acetylene and protective gas to be 1:2:7, so that the gas ratio flowing through the reactor is 10% CH4 / 20% C2H2 / 70% N2 (protective gas). Use programmed heating, heat to 500℃ at a heating rate of 5℃ / min, adjust the gas flow rate to 35mL / min, and the reaction time is 4h. After the reaction is completed, cool to room temperature, take out the sample, and obtain a silica carrier with self-reduction activity.
[0029] B: Dissolve H2PtCl6 in ethanol to make 17.60mmol / L Pt 4+ Impregnation fluid.
[0030] C: The silica carrier prepared in step A was evenly dispersed in 5 mL of ethanol to obtain a suspension with a solid content of 0.4 g / mL; the Pt salt solution prepared in step B was added to make the Pt loading amount 0.8 wt %, and the mixture was stirred continuously and heated to 40°C until the ethanol was completely evaporated. The obtained solid was placed in a 40°C oven and dried for 1 h to obtain Pt1-Pt n / SiO2 catalyst.
[0031] Example 3
[0032] A. Weigh 2g of alumina sample and place it in a reactor, seal it, first let the protective gas enter the reactor through the deoxygenator, select methane and carbon monoxide as G gas, and let it enter the reactor after passing through the deoxygenator. Use a mass flow meter to control the flow rate ratio of methane, carbon monoxide and protective gas to be 1:5:4, so that the gas ratio flowing through the reactor is 10% CH4 / 50% CO / 40% N2 (protective gas). Use programmed heating, raise the temperature to 400℃ at a heating rate of 5℃ / min, adjust the gas flow rate to 50mL / min, and the reaction time is 3h. After the reaction is completed, cool to room temperature, take out the sample, and obtain an alumina carrier with self-reduction activity.
[0033] B: Dissolve RuCl3·3H2O in deionized water to make 37.65mmol / L Ru 3+ Impregnation fluid.
[0034] C: The alumina carrier prepared in step A was uniformly dispersed in 4 mL of deionized water to obtain a suspension with a solid content of 0.5 g / mL; the Ru prepared in step B was added 3+ Salt solution, Ru 3+The loading amount was 1.5 wt %, and the mixture was stirred continuously and heated to 60 ° C until the deionized water was completely evaporated. The obtained solid was placed in an oven at 40 ° C and dried for 1 h to obtain Ru1-Ru n / Al2O3 catalyst.
[0035] Example 4
[0036] A. Weigh 2g of alumina sample and place it in a reactor, seal it, first let the protective gas enter the reactor through the deoxygenator, select methane and carbon monoxide as G gas, and let it enter the reactor after passing through the deoxygenator. Use a mass flow meter to control the flow rate ratio of methane, carbon monoxide and protective gas to be 5:1:4, so that the gas ratio flowing through the reactor is 50% CH4 / 10% CO / 40% N2 (protective gas). Use programmed heating, raise the temperature to 400℃ at a heating rate of 10℃ / min, adjust the gas flow rate to 50mL / min, and the reaction time is 4h. After the reaction is completed, cool to room temperature, take out the sample, and obtain an alumina carrier with self-reduction activity.
[0037] B: Dissolve HAuCl4·3H2O in deionized water to prepare 19.35mmol / L Au 3+ Impregnation fluid.
[0038] C: The alumina carrier prepared in step A was uniformly dispersed in 4 mL of deionized water to obtain a suspension with a solid content of 0.5 g / mL; the Au prepared in step B was added 3+ Salt solution, Au 3+ The loading amount was 1 wt%, and the mixture was stirred continuously and heated to 60 °C until the deionized water was completely evaporated. The obtained solid was placed in an oven at 40 °C and dried for 1 h to obtain Au1-Au n / Al2O3 catalyst.
[0039] Example 5
[0040] A. Weigh 2g of layered double metal hydroxide LDH sample and place it in a reactor, seal it, first let the protective gas enter the reactor through the deoxygenation device, select methane and carbon monoxide as G gas, and let it enter the reactor after passing through the deoxygenation device. The flow rate ratio of methane, carbon monoxide and protective gas is controlled by a mass flow meter to be 1:5:4, so that the gas ratio flowing through the reactor is 10% CH4 / 50% CO / 40% N2 (protective gas). Use programmed heating, heat to 300℃ at a heating rate of 10℃ / min, adjust the gas flow rate to 50mL / min, and the reaction time is 4h. After the reaction is completed, cool to room temperature, take out the sample, and obtain an LDH carrier with self-reduction activity.
[0041] B: Dissolve RuCl3·3H2O in deionized water to make 37.65mmol / L Ru 3+ Impregnation fluid.
[0042] C: The layered double hydroxide LDH carrier prepared in step A was uniformly dispersed in 4 mL of deionized water to obtain a suspension with a solid content of 0.5 g / mL; the Ru prepared in step B was added 3+ Salt solution, Ru 3+ The loading amount was 1.5 wt %, and the mixture was stirred continuously and heated to 60 ° C until the deionized water was completely evaporated. The obtained solid was placed in an oven at 40 ° C and dried for 1 h to obtain Ru1-Ru n / LDH catalyst.
[0043] Comparative Example
[0044] A. The comparative carriers were prepared according to step A in Examples 1-5, except that the gas used was not treated with a carbon-containing mixed gas.
[0045] B. Weigh 2 g of carrier sample and disperse it evenly in 4 mL of corresponding solvent to obtain a suspension with a solid content of 0.5 g / mL; add the prepared corresponding salt solution to make the metal loading at 1%, continue stirring and heat to 60°C until the solvent is completely evaporated, place the obtained solid in a 60°C oven and dry it for 1 hour to obtain a catalyst precursor.
[0046] C. Place the catalyst precursor obtained in step B in a tubular furnace, set the reaction temperature to 350° C., and calcine for 4 hours in an atmosphere of 10% H2 / N2 to obtain the corresponding noble metal catalyst M / X.
[0047] Application Examples
[0048] The Ru1-Ru prepared in Example 3 was subjected to a probe reaction using a tandem reductive amination reaction to prepare a primary amine. n / Al2O3 catalyst was used for performance evaluation, and Ru / Al2O3 was selected as comparison sample.
[0049] The evaluation device is a high-pressure reactor, and the operating steps are as follows:
[0050] Weigh 1mmol 5-hydroxymethylfurfural, 100mg catalyst, 0.5mL NH3·MeOH solution, and 15mL methanol solution into a 50mL autoclave, and seal the autoclave. Pass 99.9% H2 into the autoclave to replace the air in the autoclave, then raise the temperature of the autoclave to 100℃, pass 99.9% H2 and keep the pressure at 2MPa, take samples and analyze every 1h, and react for a total of 10h. Use Agilent gas chromatography to detect the product, and use the internal standard method for data processing. The results are shown in Figure 3 It can be clearly seen from the figure that the Ru1-Ru n / Al2O3 multi-scale site catalyst has good catalytic activity in tandem reductive amination reaction.
Claims
1. An atomically dispersed (M1)-cluster (M n ) A multi-scale site synergistic catalyst, characterized in that: M1-M n / X, noble metal M in the form of single atoms (M1) and clusters (M n ) are anchored on the oxide carrier X in the form of coexistence; the mass percentage of M in the overall catalyst is 0.1% to 5%.
2. Preparation of the atomically dispersed (M1)-cluster (M1) as claimed in claim 1 n ) A method for multi-scale site synergistic catalyst, characterized in that Prepared by the following steps: A: Place the carrier in a reactor and seal it. First, allow the protective gas to enter the reactor through a deoxygenation device, then pass the carbon-containing atmosphere G and the protective gas into the reactor, and control the flow rates of the G gas and the protective gas by a mass flow meter to adjust the ratio of the reaction gas; use a programmed temperature to heat the reactor, the heating rate is 2-15°C / min, the reaction temperature is 200-700°C, and the reaction time is 1-10h; the reaction gas flow rate is 10mL / min-100mL / min; after the reaction, an active oxide carrier X is obtained; The reaction gas is composed of carbon-containing gas G and protective gas, wherein the volume content of G is 5%-60%; The protective gas is an inert gas, such as nitrogen, argon or helium; The deoxidizing device is a drying tube to which a 401 manganese-based deoxidizer is added; G is one or more of C2H6, C2H4, C2H2, CH4, CO2, CO B: Dissolve the noble metal M salt in the corresponding solvent in B to prepare a solution with a concentration of 10 to 50 mmol / L; The M salt is present in the form of at least one of nitrate, sulfate, hydrochloride, acetylacetonate and acetate; The solvent is at least one of ethanol, methanol, acetone, carbon tetrachloride and water; C: The carrier X prepared in step A is uniformly dispersed in the solvent described in step B to obtain a suspension with a solid content of 0.05-0.5 g / mL; the noble metal M salt solution prepared in step B is added to make the loading amount of M 0.1-5 wt%, and the mixture is continuously stirred and heated to 30-80°C until the solvent is completely evaporated, and the obtained solid is placed in an oven at 40-80°C and dried for 1 h to obtain M1-M n / X catalyst.
3. The method according to claim 2, characterized in that: By adjusting one or more of the carrier treatment atmosphere, temperature, and time, the number of reducing active species modified on the carrier surface can be adjusted to achieve atomic-level dispersion (M1) and clustering (M n )Controllable regulation of site ratios.
Citation Information
Patent Citations
Systems and methods for high temperature synthesis of monatomic and polyatomic dispersions
CN114502276A
Single-component multi-center catalyst for space confinement in metal nano island and preparation method of single-component multi-center catalyst
CN117732482A
Method and device for preparing alumina carrier and catalyst with reduction function by using carbon-containing mixed gas
CN118105962A
Highly active metal oxide supported atomically dispersed platinum group metal catalysts
US20200391185A1