Modified ruthenium-based composite catalytic material as well as preparation method and application thereof
By modifying the ruthenium-based composite catalytic material, using cesium salt and barium salt to modify the ruthenium-based catalyst and structured cordierite support, the problems of high-temperature energy consumption and catalyst stability in ammonia decomposition and hydrogen production technology are solved, and low-temperature and high-efficiency ammonia decomposition are achieved. The ammonia decomposition conversion rate reaches more than 90%.
Patent Information
- Application Number
- CN202411220755.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The existing ammonia decomposition hydrogen production technology has problems such as high-temperature energy consumption, low thermal conductivity of the catalyst, and the stability and powdering of the catalyst under high aerial speed conditions, which cannot achieve low-temperature and high-efficiency ammonia decomposition.
Modified ruthenium-based composite catalytic material composed of a ruthenium-based catalyst co-modified by cesium salt and barium salt and structured cordierite support is modified by electronic additives and structural additives, and combined with high thermal conductivity support to improve the catalyst. low temperature activity and high airspeed stability.
Under conditions of 400-500°C and 0.6MPa, the ammonia decomposition conversion rate reaches more than 90%, which significantly improves the thermal stability and mechanical stability of the catalyst, and avoids the reduction of activity and powdering problems caused by too low catalyst surface temperature.
Smart Images

Figure CN119075980A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a modified ruthenium-based composite catalytic material and a preparation method and application thereof. Background Art
[0002] As a secondary energy source with abundant sources, green and low carbon, and wide applications, hydrogen energy can help to absorb renewable energy on a large scale, achieve large-scale peak load regulation of power grids and cross-seasonal and cross-regional energy storage, and accelerate the low-carbonization of industries, construction, transportation and other fields. It is an important energy source for achieving low-carbon energy transformation. However, strict storage and transportation requirements limit the widespread application of hydrogen energy.
[0003] Ammonia (NH3) is a common chemical hydrogen storage material with a hydrogen storage content of up to 17.7wt.%, and ammonia can be easily stored in liquid form at room temperature and low pressure. Ammonia decomposition hydrogen production technology is a highly valuable, clean, and efficient in-situ hydrogen production technology that can effectively solve the problem of traditional high-pressure hydrogen storage. However, in reality, there are three major bottlenecks in ammonia decomposition hydrogen production:
[0004] First, ammonia decomposition to produce hydrogen usually needs to be carried out at a high temperature of 600-800℃, and this high temperature environment will cause serious energy consumption; second, the ammonia decomposition reaction is a strongly endothermic reaction, and the thermal conductivity of general catalyst carriers is low. For example, the thermal conductivity of activated carbon is 0.17-0.28W / mK, which leads to a low local temperature on the catalyst surface during the reaction, resulting in a decrease in reaction activity; third, existing commercial granular catalysts also have the problem of easy pulverization and increased resistance under long-term use, low stability of ammonia decomposition under high space velocity conditions, and high mass transfer cost and energy consumption.
[0005] At present, ruthenium-based catalysts are considered to be the most active ammonia decomposition catalysts at low temperatures. However, the high ruthenium content in existing catalysts leads to high catalyst costs and cannot be put into commercial use. In addition, the active temperature range of ammonia decomposition is still relatively high (>450°C). The doping of alkali metal additives can also help improve the activity of the ammonia decomposition reaction. However, the interaction and activity of the active sites of ruthenium modified by different alkali metal types are far from the optimal effect. How to improve the low-temperature ammonia decomposition activity, thermal stability and high-space velocity mechanical stability of the catalyst is a new idea for building a new ammonia decomposition catalyst. Summary of the invention
[0006] Based on the above problems, the present invention provides a modified ruthenium-based composite catalytic material and a preparation method and application thereof to improve the low catalyst temperature ammonia decomposition activity, thermal stability and high space velocity mechanical stability. The specific invention content is as follows:
[0007] In the first aspect, the present invention provides a modified ruthenium-based composite catalytic material, which is composed of a ruthenium-based catalyst co-modified with a cesium salt and a barium salt, and a structured cordierite carrier thereof, and the molecular formula of the modified ruthenium-based composite catalytic material is: [(Cs a -Ba b )-Ru c / C] d -[MgAlSi]; where
[0008] [(Cs a -Ba b )-Ru c / C] represents a ruthenium-based catalyst co-modified with cesium salt and barium salt supported on activated carbon;
[0009] [MgAlSi] represents the structured cordierite support;
[0010] a represents the molar percentage of cesium salt to metallic ruthenium, and a is between 1 and 15;
[0011] b represents the molar percentage of barium salt to metallic ruthenium, and b is between 0.5 and 5;
[0012] c represents the mass percentage of metallic ruthenium to activated carbon, and c is between 0.5-10;
[0013] d represents the mass percentage of the activated carbon-supported ruthenium-based catalyst co-modified with cesium salt and barium salt to the structured cordierite support, and d is between 1-35.
[0014] Optionally, a is 5-10;
[0015] b is 1-2;
[0016] The c is 1-5;
[0017] The d is 20-30.
[0018] In a second aspect, the present invention provides a method for preparing the modified ruthenium-based composite catalytic material according to the first aspect, the preparation method comprising the following steps:
[0019] S1, according to the molecular formula of the ruthenium-based catalyst co-modified with cesium salt and barium salt supported on activated carbon [(Cs a -Ba b )-Ru c / C] composition, weighing a preset mass of ruthenium trichloride and barium nitrate and dissolving them in deionized water to form a mixed solution, then adding a preset mass of activated carbon, and impregnating them under magnetic stirring at room temperature for 5-15 hours to form a first suspension;
[0020] S2. After vacuum drying the first suspension at 25-90° C. for 2-12 h, the obtained black solid powder is transferred to a tube furnace, and reduced in a reducing atmosphere at 500-600° C. for 2-5 h to obtain a reduced product;
[0021] S3, dissolving a preset mass of cesium nitrate in deionized water to obtain a cesium nitrate solution, and then placing the reduction product in the cesium nitrate solution, and immersing under magnetic stirring at room temperature for 6-12 hours to form a second suspension;
[0022] S4, vacuum drying the second suspension at 25-90° C. for 2-12 h to obtain an activated carbon-supported cesium salt and barium salt co-modified ruthenium-based catalyst [(Cs a -Ba b )-Ru c / C];
[0023] S5. According to the molecular formula of the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi] composition, the [(Cs a -Ba b )-Ru c / C], magnesium oxide and a binder are added to deionized water in a preset ratio and mixed, and magnetically stirred at room temperature for 2-12 hours to form a colloidal solution, and then the structured cordierite is impregnated in the colloidal solution and vacuum impregnated at room temperature for 2-10 hours. The impregnated structured cordierite is transferred to a tube furnace, calcined at 500-600° C. for 2-5 hours in an inert atmosphere, and taken out after cooling to obtain the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi].
[0024] Optionally, in the mixed solution, the concentration of ruthenium ions is 5-10 mg / mL, and the concentration of barium ions is 5-50 mg / mL;
[0025] In the cesium nitrate solution, the cesium ion concentration is 5-50 mg / mL.
[0026] Optionally, the binder is polyethylene glycol, hydroxymethyl cellulose or hydroxyethyl cellulose.
[0027] Optionally, the magnesium oxide accounts for 10-20% of the mass of the colloidal solution;
[0028] The binder accounts for 1-2% of the mass of the colloidal solution;
[0029] The [(Cs a -Ba b )-Ru c / C] accounts for 5-10% of the mass of the colloidal solution.
[0030] Optionally, the pore size of the structured cordierite is between 0.5-2 mm, the radial size is between 10-200 mm, and the height is between 20-300 mm.
[0031] In a third aspect, the present invention provides an application of the modified ruthenium-based composite catalytic material described in the first aspect, wherein the modified ruthenium-based composite catalytic material is used for decomposing ammonia to produce hydrogen.
[0032] Optionally, the use of the modified ruthenium-based composite catalytic material for ammonia decomposition to produce hydrogen comprises: after the modified ruthenium-based composite catalytic material is loaded into a fixed bed reactor, ammonia gas is introduced to carry out ammonia decomposition to produce hydrogen reaction;
[0033] The reaction space velocity of ammonia is 1000-20000h -1 , the reaction temperature is 300-500°C, and the reaction pressure is 0.1-5MPa.
[0034] Optionally, the concentration of ammonia participating in the ammonia decomposition hydrogen production reaction is 10-100 vol.%.
[0035] Compared with the prior art, the modified ruthenium-based composite catalytic material and its preparation method and application provided by the present invention have the following advantages:
[0036] The present invention provides a modified ruthenium-based composite catalytic material, which is composed of a ruthenium-based catalyst co-modified with a cesium salt and a barium salt, and a structured cordierite carrier thereof. The molecular formula of the modified ruthenium-based composite catalytic material is: [(Cs a -Ba b )-Ru c / C] d -[MgAlSi]; where [(Cs a -Ba b )-Ru c / C] represents activated carbon-supported ruthenium-based catalyst co-modified with cesium salt and barium salt; [MgAlSi] represents structured cordierite support.
[0037] In the modified ruthenium-based composite catalytic material provided by the present invention, ruthenium carbon is modified by means of an electronic auxiliary agent, alkali metal cesium, and a structural auxiliary agent, alkaline earth metal barium, so that it can efficiently catalyze and promote the decomposition of ammonia to produce hydrogen under low temperature conditions, and structured cordierite is used as a carrier material, which has the advantages of high thermal conductivity and good stability, and can effectively avoid the defects of reduced activity due to low catalyst surface temperature, as well as the problem of catalyst pulverization under high space velocity. The catalyst has high catalytic activity, and under the reaction conditions of a temperature of 400-500°C and a pressure of 0.6MPa, the ammonia decomposition conversion rate is not less than 90%. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 The flowchart of the preparation method of the modified ruthenium-based composite catalytic material provided by the embodiment of the present invention is shown;
[0040] Figure 2 A physical picture of a modified ruthenium-based composite catalytic material provided in an embodiment of the present invention is shown;
[0041] Figure 3 The transmission electron microscope image of [(Cs5-Ba2)-Ru5 / C] provided by the embodiment of the present invention is shown;
[0042] Figure 4 The figure shows the change of ammonia decomposition efficiency of the modified ruthenium-based composite catalytic material provided in Example 1 of the present invention at different temperatures;
[0043] Figure 5 The figure shows the change of ammonia decomposition efficiency of the modified ruthenium-based composite catalytic material provided in Example 1 of the present invention under different pressures;
[0044] Figure 6 The ammonia conversion rate of the modified ruthenium-based composite catalytic material provided in Examples 1-5 of the present invention is shown;
[0045] Figure 7 The figure shows the ammonia conversion rate of the ammonia decomposition hydrogen production catalytic material provided in the comparative example of the present invention. DETAILED DESCRIPTION
[0046] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0047] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the prior art can be used. The reagents and other instruments used without specifying the manufacturer are all conventional reagent products that can be purchased commercially.
[0048] Currently, ruthenium-based catalysts are considered to be the most active ammonia decomposition catalysts at low temperatures. However, the high ruthenium content of this type of catalyst leads to a high catalyst preparation cost, and the active temperature range for catalytic ammonia decomposition is still relatively high (>450°C), which causes energy consumption and a short catalyst life. In view of this, the present invention modifies the ruthenium-based catalyst with the help of alkali metals and alkaline earth metals, and combines it with a structured cordierite carrier to obtain a new ammonia decomposition hydrogen production catalyst material; the present invention further explores the performance of the modified ruthenium-based ammonia decomposition catalytic material to verify that the catalyst has good low-temperature ammonia decomposition activity, thermal stability and high space velocity mechanical stability. The specific implementation method is as follows:
[0049] In the first aspect, the present invention provides a modified ruthenium-based composite catalytic material, which is composed of a ruthenium-based catalyst co-modified with a cesium salt and a barium salt, and a structured cordierite carrier thereof, and the molecular formula of the modified ruthenium-based composite catalytic material is: [(Cs a -Ba b )-Ru c / C] d -[MgAlSi]; where
[0050] [(Cs a -Ba b )-Ru c / C] represents a ruthenium-based catalyst co-modified with cesium salt and barium salt supported on activated carbon;
[0051] [MgAlSi] represents the structured cordierite support;
[0052] a represents the molar percentage of cesium salt to metallic ruthenium, and a is between 1 and 15;
[0053] b represents the molar percentage of barium salt to metallic ruthenium, and b is between 0.5 and 5;
[0054] c represents the mass percentage of metallic ruthenium to activated carbon, and c is between 0.5-10;
[0055] d represents the mass percentage of the activated carbon-supported ruthenium-based catalyst co-modified with cesium salt and barium salt to the structured cordierite support, and d is between 1-35.
[0056] In specific implementation, in the modified ruthenium-based composite catalytic material provided by the present invention, the ruthenium-carbon catalyst is modified by means of the electronic auxiliary agent alkali metal cesium and the structural auxiliary agent alkaline earth metal barium. The electronic auxiliary agent cesium can effectively provide electrons to the metal ruthenium particles, thereby facilitating the breaking of the nitrogen-hydrogen bond of ammonia; and the structural auxiliary agent barium helps to form more B5 active sites of the metal ruthenium particles, which is beneficial to the adsorption of ammonia on the metal ruthenium, thereby achieving efficient catalytic promotion of ammonia decomposition and hydrogen production under low temperature conditions. The present invention uses structured cordierite as a carrier material to carry a modified ruthenium-based catalyst, which has the advantages of high thermal conductivity and good stability, and can effectively avoid the defect of reduced activity due to the low surface temperature of the catalyst, as well as the problem of catalyst pulverization at high space velocity. The catalyst has high catalytic activity, and the ammonia decomposition conversion rate can reach 99.1% under the reaction conditions of 450°C and 0.6MPa.
[0057] In some embodiments, a may be 5-10; b may be 1-2; c may be 1-5; and d may be 20-30.
[0058] In a second aspect, the present invention provides a method for preparing the modified ruthenium-based composite catalytic material described in the first aspect. Figure 1 The flowchart of the preparation method of the modified ruthenium-based composite catalytic material provided in the embodiment of the present invention is shown as follows: Figure 1 As shown, the preparation method comprises the following steps:
[0059] S1, according to the molecular formula of the ruthenium-based catalyst co-modified with cesium salt and barium salt supported on activated carbon [(Cs a -Ba b )-Ru c / C] composition, weighing a preset mass of ruthenium trichloride and barium nitrate and dissolving them in deionized water to form a mixed solution, then adding a preset mass of activated carbon, and impregnating them under magnetic stirring at room temperature for 5-15 hours to form a first suspension;
[0060] S2. After vacuum drying the first suspension at 25-90° C. for 2-12 h, the obtained black solid powder is transferred to a tube furnace, and reduced in a reducing atmosphere at 500-600° C. for 2-5 h to obtain a reduced product;
[0061] S3, dissolving a preset mass of cesium nitrate in deionized water to obtain a cesium nitrate solution, and then placing the reduction product in the cesium nitrate solution, and immersing under magnetic stirring at room temperature for 6-12 hours to form a second suspension;
[0062] S4, vacuum drying the second suspension at 25-90° C. for 2-12 h to obtain an activated carbon-supported cesium salt and barium salt co-modified ruthenium-based catalyst [(Cs a -Ba b )-Ru c / C];
[0063] S5. According to the molecular formula of the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi] composition, the [(Cs a -Ba b )-Ru c / C], magnesium oxide and a binder are added to deionized water in a preset ratio and mixed, and magnetically stirred at room temperature for 2-12 hours to form a colloidal solution, and then the structured cordierite is impregnated in the colloidal solution and vacuum impregnated at room temperature for 2-10 hours. The impregnated structured cordierite is transferred to a tube furnace, calcined at 500-600° C. for 2-5 hours in an inert atmosphere, and taken out after cooling to obtain the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi].
[0064] In specific implementation, the preset mass refers to the molecular formula of the modified ruthenium-based composite catalyst material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi], the value ranges of a, b, c, and d determine the specific amounts of each raw material; as an example, in step S1, a preset mass of ruthenium trichloride and barium nitrate are weighed and dissolved in a mixed solution formed by deionized water, and the ruthenium ion concentration is 5-10 mg / mL, and the barium ion concentration is 5-50 mg / mL; in step S3, a preset mass of cesium nitrate is dissolved in a cesium nitrate solution obtained in deionized water, and the cesium ion concentration is 5-50 mg / mL.
[0065] In a third aspect, the present invention provides an application of the modified ruthenium-based composite catalytic material described in the first aspect, wherein the modified ruthenium-based composite catalytic material is used for hydrogen production by decomposing ammonia. Specifically, the process comprises: after the modified ruthenium-based composite catalytic material is loaded into a fixed bed reactor, ammonia gas is introduced to carry out ammonia decomposition hydrogen production reaction; the reaction space velocity of the ammonia gas is 1000-20000h -1 , the reaction temperature is 300-500°C, and the reaction pressure is 0.1-5MPa.
[0066] In order to enable those skilled in the art to understand the present application more clearly, a modified ruthenium-based composite catalytic material described in the present application, a preparation method and an application thereof are now described in detail through the following examples.
[0067] The structured cordierite carriers used in the following examples and comparative examples were all purchased from Suzhou Guohongtai Environmental Protection Technology Co., Ltd.
[0068] Example 1
[0069] Weigh 0.102g of ruthenium trichloride and 0.258g of barium nitrate respectively, dissolve them in 10mL of deionized water to form a mixed solution, wherein the ruthenium ion concentration is 5mg / mL and the barium ion concentration is 13.5mg / mL. Add 1.0g of activated carbon to the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The first suspension obtained is vacuum dried at 80°C for 12 hours, and the resulting black solid powder is placed in a porcelain boat. Reduce it at 600°C in a tube furnace for 5 hours, and the atmosphere used is a hydrogen-argon mixture (hydrogen content 10%), and the heating rate is 5°C / min. Weigh 0.482g of cesium nitrate and dissolve it in 30mL of deionized water, wherein the cesium ion concentration is 10.9mg / mL. Place the solid obtained by reduction in the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The second suspension obtained is vacuum dried at 80°C for 12 hours, and the [(Cs5-Ba2)-Ru5 / C] catalyst is obtained after taking it out.
[0070] Weigh 1.0g [(Cs5-Ba2)-Ru5 / C], 1.0g magnesium oxide and 0.1g polyethylene glycol PEG-300, add 5mL deionized water, and stir magnetically at room temperature for 12 hours to form a colloidal solution. Take a structured cordierite carrier with a diameter of 10mm, a height of 50mm, and a pore size of 1mm, and its mass is 3.70g. Weigh 0.74g of the colloidal solution, place the cordierite carrier in the colloidal solution, and after vacuum impregnation for 2 hours at room temperature, turn the cordierite upside down and continue vacuum impregnation for 2 hours. After impregnation, the cordierite is calcined at 600℃ in a tubular furnace for 2 hours. The atmosphere used is argon gas, and the heating rate is 5℃ / min. After cooling, take it out to obtain [(Cs5-Ba2)-Ru5 / C] 20 -[MgAlSi].
[0071] Figure 2 The physical picture of the modified ruthenium-based composite catalytic material provided by the embodiment of the present invention is shown. Figure 3 A transmission electron microscope image of [(Cs5-Ba2)-Ru5 / C] provided in an embodiment of the present invention is shown.
[0072] Loading [(Cs5-Ba2)-Ru5 / C] in a fixed bed tubular reactor 20-[MgAlSi] catalyst was used for ammonia decomposition hydrogen production reaction. 50 mL / min of nitrogen was introduced at room temperature and the temperature was raised to 500°C at 5°C / min. After stabilization at 500°C for 1 hour, the reaction gas was introduced to test the ammonia decomposition performance. The ammonia in the product gas was absorbed by dilute sulfuric acid and detected by ion chromatography. The reaction space velocity was 1500 h -1 , the reaction temperature range is 350-500°C, the reaction pressure range is 0.1-2MPa, and the ammonia concentration range is 10-100vol.%.
[0073] Figure 4 The modified ruthenium-based composite catalytic material provided in Example 1 of the present invention shows the change in ammonia decomposition efficiency at different temperatures (reaction conditions: reaction temperature is 375, 400, 425, 450, 475, 500 ° C, reaction pressure is 0.6 MPa, ammonia concentration is 10 vol.%, reaction space velocity is 1500 h -1 ),like Figure 4 As shown, when the ammonia decomposition reaction temperature is 375, 400, 425, 450, 475, 500°C, the corresponding ammonia conversion rates are 77.6, 93.0, 97.9, 99.1, 99.7, 99.8% respectively; the corresponding hydrogen production rates are 19.4, 23.3, 24.5, 24.9, 25.0, 25.1 mmol / h respectively; it can be seen that the modified ruthenium-based composite catalytic material provided in Example 1 has an ammonia decomposition conversion rate of not less than 90% under the reaction conditions of a temperature of 400-500°C and a pressure of 0.6 MPa. And the modified ruthenium-based composite catalytic material provided in Example 1 has an ammonia decomposition conversion rate of up to 99.1% under the reaction conditions of a temperature of 450°C and a pressure of 0.6 MPa.
[0074] Figure 5 The modified ruthenium-based composite catalytic material provided in Example 1 of the present invention shows the change in ammonia decomposition efficiency under different pressures (reaction conditions: reaction temperature is 450°C, reaction pressures are 0.1, 0.5, 1.0, 1.5, 2.0 MPa, ammonia concentration is 10 vol.%, reaction space velocity is 1500 h -1 ),like Figure 5 As shown, when the ammonia decomposition reaction pressure is 0.1, 0.5, 1.0, 1.5, and 2.0 MPa, the corresponding ammonia conversion rates are 99.5, 99.3, 97.9, 96.9, and 96.3%, respectively; the corresponding hydrogen production rates are 25.0, 24.9, 24.5, 24.2, and 24.0 mmol / h, respectively.
[0075] Example 2
[0076] Weigh 0.102g of ruthenium trichloride and 0.129g of barium nitrate respectively, dissolve them in 10mL of deionized water to form a mixed solution, wherein the ruthenium ion concentration is 5mg / mL and the barium ion concentration is 6.8mg / mL. Add 1.0g of activated carbon to the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The first suspension obtained is vacuum dried at 80°C for 12 hours, and the resulting black solid powder is placed in a porcelain boat. Reduce it at 600°C in a tube furnace for 5 hours, and the atmosphere used is a hydrogen-argon mixture (hydrogen content 10%), and the heating rate is 5°C / min. Weigh 0.482g of cesium nitrate and dissolve it in 30mL of deionized water, wherein the cesium ion concentration is 10.9mg / mL. Place the solid obtained by reduction in the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The second suspension obtained is vacuum dried at 80°C for 12 hours, and the [(Cs5-Ba1)-Ru5 / C] catalyst is obtained after taking it out.
[0077] Weigh 1.0g [(Cs5-Ba1)-Ru5 / C], 1.0g magnesium oxide and 0.1g polyethylene glycol PEG-300, add 5mL deionized water, and stir magnetically at room temperature for 12 hours to form a colloidal solution. Take a structured cordierite carrier with a diameter of 10mm, a height of 50mm, and a pore size of 1mm, and its mass is 3.70g. Weigh 0.74g of the colloidal solution, place the cordierite carrier in the colloidal solution, and after vacuum impregnation for 2 hours at room temperature, turn the cordierite upside down and continue vacuum impregnation for 2 hours. After impregnation, the cordierite is calcined at 600℃ in a tubular furnace for 2 hours. The atmosphere used is argon, and the heating rate is 5℃ / min. After cooling, take it out to obtain [(Cs5-Ba1)-Ru5 / C] 20 -[MgAlSi].
[0078] Loading [(Cs5-Ba1)-Ru5 / C] in a fixed bed tubular reactor 20 -[MgAlSi] catalyst for ammonia decomposition to produce hydrogen, with a reaction space velocity of 1500h -1 , the reaction temperature is 450°C, the reaction pressure is 0.6MPa, and the ammonia concentration is 10vol.%.
[0079] Example 3
[0080] Weigh 0.102g of ruthenium trichloride and 0.258g of barium nitrate respectively, dissolve them in 10mL of deionized water to form a mixed solution, wherein the ruthenium ion concentration is 5mg / mL and the barium ion concentration is 13.5mg / mL. Add 1.0g of activated carbon to the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The obtained first suspension is vacuum dried at 80°C for 12 hours, and the obtained black solid powder is placed in a porcelain boat. Reduce it at 600°C in a tube furnace for 5 hours, and the atmosphere used is a hydrogen-argon mixture (hydrogen content 10%), and the heating rate is 5°C / min. Weigh 0.964g of cesium nitrate and dissolve it in 50mL of deionized water, wherein the cesium ion concentration is 13.1mg / mL. The solid obtained by reduction is placed in the solution and impregnated with magnetic stirring at room temperature for 12 hours. The obtained second suspension is vacuum dried at 80°C for 12 hours, and [(Cs 10 -Ba2)-Ru5 / C] catalyst.
[0081] Weigh 1.0g[(Cs 10 -Ba2)-Ru5 / C], 1.0g magnesium oxide and 0.1g polyethylene glycol PEG-300, add 5mL deionized water, and stir magnetically at room temperature for 12 hours to form a colloidal solution. Take a cordierite carrier with a diameter of 10mm, a height of 50mm, and a pore size of 1mm, and its mass is 3.70g. Weigh 0.74g of the colloidal solution, place the cordierite carrier in the colloidal solution, and vacuum impregnate it at room temperature for 2 hours. After vacuum impregnation, turn the cordierite upside down and continue vacuum impregnation for 2 hours. After impregnation, the cordierite is calcined at 600℃ in a tube furnace for 2 hours. The atmosphere used is argon gas, and the heating rate is 5℃ / min. After cooling, take it out to obtain [(Cs 10 -Ba2)-Ru5 / C] 20 -[MgAlSi].
[0082] In a fixed bed tubular reactor, [(Cs 10 -Ba2)-Ru5 / C] 20 -[MgAlSi] catalyst for ammonia decomposition to produce hydrogen, with a reaction space velocity of 1500h -1 , the reaction temperature is 450°C, the reaction pressure is 0.6MPa, and the ammonia concentration is 10vol.%.
[0083] Example 4
[0084] Weigh 0.041g of ruthenium trichloride and 0.258g of barium nitrate respectively, dissolve them in 4mL of deionized water to form a mixed solution, wherein the ruthenium ion concentration is 5mg / mL and the barium ion concentration is 33.8mg / mL. Add 1.0g of activated carbon to the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The first suspension obtained is vacuum dried at 80°C for 12 hours, and the resulting black solid powder is placed in a porcelain boat. Reduce it at 600°C in a tube furnace for 5 hours, and the atmosphere used is a hydrogen-argon mixture (hydrogen content 10%), and the heating rate is 5°C / min. Weigh 0.482g of cesium nitrate and dissolve it in 30mL of deionized water, wherein the cesium ion concentration is 10.9mg / mL. Place the reduced solid in the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The second suspension obtained is vacuum dried at 80°C for 12 hours, and the [(Cs5-Ba2)-Ru2 / C] catalyst is obtained after taking it out.
[0085] Weigh 1.0g [(Cs5-Ba2)-Ru2 / C], 1.0g magnesium oxide and 0.1g polyethylene glycol PEG-300, add 5mL deionized water, and stir magnetically at room temperature for 12 hours to form a colloidal solution. Take a structured cordierite carrier with a diameter of 10mm, a height of 50mm, and a pore size of 1mm, and its mass is 3.70g. Weigh 0.74g of the colloidal solution, place the cordierite carrier in the colloidal solution, and after vacuum impregnation for 2 hours at room temperature, turn the cordierite upside down and continue vacuum impregnation for 2 hours. After impregnation, the cordierite is calcined at 600℃ in a tubular furnace for 2 hours. The atmosphere used is argon, and the heating rate is 5℃ / min. After cooling, take it out to obtain [(Cs5-Ba2)-Ru2 / C] 20 -[MgAlSi].
[0086] Loading [(Cs5-Ba2)-Ru2 / C] in a fixed bed tubular reactor 20 -[MgAlSi] catalyst for ammonia decomposition to produce hydrogen, with a reaction space velocity of 1500h -1 , the reaction temperature is 450°C, the reaction pressure is 0.6MPa, and the ammonia concentration is 10vol.%.
[0087] Example 5
[0088] Weigh 0.102g of ruthenium trichloride and 0.258g of barium nitrate respectively, dissolve them in 10mL of deionized water to form a mixed solution, wherein the ruthenium ion concentration is 5mg / mL and the barium ion concentration is 13.5mg / mL. Add 1.0g of activated carbon to the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The first suspension obtained is vacuum dried at 80°C for 12 hours, and the resulting black solid powder is placed in a porcelain boat. Reduce it at 600°C in a tube furnace for 5 hours, and the atmosphere used is a hydrogen-argon mixture (hydrogen content 10%), and the heating rate is 5°C / min. Weigh 0.482g of cesium nitrate and dissolve it in 30mL of deionized water, wherein the cesium ion concentration is 10.9mg / mL. Place the solid obtained by reduction in the solution and impregnate it with magnetic stirring at room temperature for 12 hours. The second suspension obtained is vacuum dried at 80°C for 12 hours, and the [(Cs5-Ba2)-Ru5 / C] catalyst is obtained after taking it out.
[0089] Weigh 1.0g [(Cs5-Ba2)-Ru5 / C], 1.0g magnesium oxide and 0.1g polyethylene glycol PEG-300, add 5mL deionized water, and stir magnetically at room temperature for 12 hours to form a colloidal solution. Take a structured cordierite carrier with a diameter of 25mm, a height of 50mm, and a pore size of 1mm, the mass of which is 22.30g, weigh 6.69g of the colloidal solution, place the cordierite carrier in the colloidal solution, and after vacuum impregnation for 2 hours at room temperature, turn the cordierite upside down and continue vacuum impregnation for 2 hours. After impregnation, the cordierite is calcined at 600℃ in a tubular furnace for 2 hours. The atmosphere used is argon, and the heating rate is 5℃ / min. After cooling, take it out to obtain [(Cs5-Ba2)-Ru2 / C] 30 -[MgAlSi].
[0090] Loading [(Cs5-Ba2)-Ru2 / C] in a fixed bed tubular reactor 30 -[MgAlSi] catalyst for ammonia decomposition to produce hydrogen, with a reaction space velocity of 1500h -1 , the reaction temperature is 450°C, the reaction pressure is 0.6MPa, and the ammonia concentration is 10vol.%.
[0091] Figure 6 The ammonia conversion rate of the modified ruthenium-based composite catalytic material provided in Examples 1-5 of the present invention is shown. Figure 6 As shown, at a reaction space velocity of 1500 h -1 Under the conditions of reaction temperature of 450°C, reaction pressure of 0.6 MPa and ammonia concentration of 10 vol.%, the ammonia conversion rates of the modified ruthenium-based composite catalytic materials provided in Examples 1-5 were not less than 95%.
[0092] Comparative Example 1
[0093] Weigh 0.102g of ruthenium trichloride and dissolve it in 10mL of deionized water to form a mixed solution in which the ruthenium ion concentration is 5mg / mL. Add 1.0g of activated carbon to the solution and impregnate it for 12 hours under magnetic stirring at room temperature. The obtained suspension is vacuum dried at 80°C for 12 hours, and the obtained black solid powder is placed in a porcelain boat. Reduce it at 600°C in a tubular furnace for 5 hours. The atmosphere used is a hydrogen-argon mixed gas (hydrogen content 10%), and the heating rate is 5°C / min. After taking it out, the [Ru5 / C] catalyst is obtained.
[0094] Weigh 1.0g [Ru5 / C], 1.0g magnesium oxide and 0.1g polyethylene glycol PEG-300, add 5mL deionized water, and stir magnetically at room temperature for 12 hours to form a colloidal solution. Take a structured cordierite carrier with a diameter of 10mm, a height of 50mm, and a pore size of 1mm, and its mass is 3.70g. Weigh 0.74g of the colloidal solution, place the cordierite carrier in the colloidal solution, and vacuum impregnate it at room temperature for 2 hours. After turning the cordierite upside down, continue vacuum impregnation for 2 hours. After impregnation, the cordierite is calcined at 600℃ in a tubular furnace for 2 hours. The atmosphere used is argon gas, and the heating rate is 5℃ / min. After cooling, take it out to obtain [Ru5 / C] 20 -[MgAlSi].
[0095] Loading [Ru5 / C] in a fixed bed tubular reactor 20 -[MgAlSi] for ammonia decomposition to produce hydrogen, with a reaction space velocity of 1500h -1 , the reaction temperature is 450°C, the reaction pressure is 0.6MPa, and the ammonia concentration range is 10vol.%.
[0096] Comparative Example 2
[0097] The structured cordierite support [MgAlSi] used in Comparative Example 1 was loaded into a fixed bed tubular reactor to carry out ammonia decomposition hydrogen production reaction at a reaction space velocity of 1500 h -1 , the reaction temperature is 450°C, the reaction pressure is 0.6MPa, and the ammonia concentration range is 10vol.%.
[0098] Figure 7 The ammonia conversion rate of the ammonia decomposition hydrogen production catalytic material provided in the comparative example of the present invention is shown as follows: Figure 7As shown, by comparing Example 1 and Comparative Example 1, it can be seen that the modification of the ruthenium-based catalyst by alkali metal cesium and alkaline earth metal barium can effectively improve the ammonia decomposition activity. This is mainly because the electronic auxiliary agent cesium can effectively provide electrons to the metal ruthenium particles, thereby facilitating the breaking of the nitrogen-hydrogen bond of ammonia; and the structural auxiliary agent barium helps to form more B5 active sites of the metal ruthenium particles, which is beneficial to the adsorption of ammonia on the metal ruthenium. It can be seen that the modified ruthenium-based composite catalytic material based on structured cordierite proposed in the present invention has good catalytic activity and stability, and can be used to decompose ammonia to produce hydrogen under milder conditions (temperature 400-500°C, pressure 0.1-2MPa), showing broad practical application prospects.
[0099] In summary, the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi] has good ammonia decomposition activity and can achieve an ammonia conversion rate of more than 90% at a temperature of 400-500°C and a pressure of 0.1-2MPa.
[0100] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0101] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0102] The above is a detailed introduction to a modified ruthenium-based composite catalytic material, a preparation method and an application thereof provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technical personnel in the field, according to the idea of the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A modified ruthenium-based composite catalytic material, characterized in that: The modified ruthenium-based composite catalytic material is composed of a ruthenium-based catalyst co-modified with a cesium salt and a barium salt, and a structured cordierite carrier thereof. The molecular formula of the modified ruthenium-based composite catalytic material is: [(Cs a -Ba b )-Ru c / C] d -[MgAlSi]; among them, [(Cs a -Ba b )-Ru c / C] represents a ruthenium-based catalyst co-modified with cesium salt and barium salt supported on activated carbon; [MgAlSi] represents the structured cordierite support; a represents the molar percentage of cesium salt to metallic ruthenium, and a ranges from 1 to 15; b represents the molar percentage of barium salt to metallic ruthenium, and b is between 0.5 and 5; c represents the mass percentage of metallic ruthenium to activated carbon, and c ranges from 0.5 to 10; d represents the mass percentage of the activated carbon-supported cesium salt and barium salt co-modified ruthenium-based catalyst and the structured cordierite support, and d ranges from 1 to 35.
2. The modified ruthenium-based composite catalytic material according to claim 1, characterized in that: Said a is 5-10; b is 1-2; Said c is 1-5; The d is 20-30.
3. A method for preparing the modified ruthenium-based composite catalytic material according to any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: S1, according to the molecular formula of the ruthenium-based catalyst composed of activated carbon supported cesium salt and barium salt co-modified [(Cs a -Ba b )-Ru c / C] composition, weighing a preset mass of ruthenium trichloride and barium nitrate and dissolving them in deionized water to form a mixed solution, then adding a preset mass of activated carbon, and impregnating them under magnetic stirring at room temperature for 5-15 hours to form a first suspension; S2. After vacuum drying the first suspension at 25-90° C. for 2-12 hours, the resulting black solid powder is transferred to a tube furnace and reduced in a reducing atmosphere at 500-600° C. for 2-5 hours to obtain a reduced product; S3, dissolving a preset mass of cesium nitrate in deionized water to obtain a cesium nitrate solution, then placing the reduction product in the cesium nitrate solution, and immersing under magnetic stirring at room temperature for 6-12 hours to form a second suspension; S4, vacuum drying the second suspension at 25-90 ° C for 2-12 hours to obtain an activated carbon-supported cesium salt and barium salt co-modified ruthenium-based catalyst [(Cs a -Ba b )-Ru c / C]; S5. According to the molecular formula of the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi] composition, the [(Cs a -Ba b )-Ru c / C], magnesium oxide and a binder are added to deionized water in a preset ratio and mixed, and magnetically stirred at room temperature for 2-12 hours to form a colloidal solution, and then the structured cordierite is impregnated in the colloidal solution and vacuum impregnated at room temperature for 2-10 hours. The impregnated structured cordierite is transferred to a tube furnace and calcined at 500-600° C. for 2-5 hours in an inert atmosphere, and then taken out after cooling to obtain the modified ruthenium-based composite catalytic material [(Cs a -Ba b )-Ru c / C] d -[MgAlSi].
4. The preparation method according to claim 3, characterized in that In the mixed solution, the concentration of ruthenium ions is 5-10 mg / mL, and the concentration of barium ions is 5-50 mg / mL; In the cesium nitrate solution, the cesium ion concentration is 5-50 mg / mL.
5. The preparation method according to claim 3, characterized in that: The binder is polyethylene glycol, hydroxymethyl cellulose or hydroxyethyl cellulose.
6. The preparation method according to claim 3, characterized in that: The magnesium oxide accounts for 10-20% of the mass of the colloidal solution; The binder accounts for 1-2% of the mass of the colloidal solution; The [(Cs a -Ba b )-Ru c / C] accounts for 5-10% of the mass of the colloidal solution.
7. The preparation method according to claim 3, characterized in that: The pore size of the structured cordierite is between 0.5-2 mm, the radial size is between 10-200 mm, and the height is between 20-300 mm.
8. An application of the modified ruthenium-based composite catalytic material according to any one of claims 1 to 2, characterized in that: The modified ruthenium-based composite catalytic material is used for decomposing ammonia to produce hydrogen.
9. The application according to claim 8, characterized in that: The modified ruthenium-based composite catalytic material is used for ammonia decomposition to produce hydrogen, comprising: after the modified ruthenium-based composite catalytic material is loaded into a fixed bed reactor, ammonia is introduced to carry out an ammonia decomposition reaction to produce hydrogen; The reaction space velocity of the ammonia is 1000-20000h -1 , the reaction temperature is 300-500℃, and the reaction pressure is 0.1-5MPa.
10. The use according to claim 8 or 9, characterized in that: The concentration of ammonia gas involved in the ammonia decomposition hydrogen production reaction is 10-100 vol.%.
Citation Information
Patent Citations
Ammonia decomposition reaction device and ammonia decomposition method
CN112742310A
Ammonia synthesis catalyst, method for producing ammonia synthesis catalyst, and method for synthesizing ammonia
CN114377673A
Coating-containing integral structural formula ammonia decomposition catalyst and preparation method thereof
CN117816233A
Ammonia synthesis ruthenium based catalyst and preparing process thereof
CN1401426A
Combustion engine exhaust gas treatment multifonctional catalyst which contains uranium, at least one uranium promoter and at least one precious metal and process for its production