Method for secondary extraction of lithium from iron slag after magnetic separation of lepidolite
Through cyclone concentration and flotation technology, the problem of lithium mica being difficult to recover in iron slag after magnetic separation of lithium mica is solved, and efficient improvement of lithium mica concentrate grade and recovery rate is achieved, the process flow is simplified, and lithium resources are avoided. waste.
Patent Information
- Application Number
- CN202411009504.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The iron slag after magnetic separation of lithium mica contains a higher proportion of lithium mica, which makes it difficult to sell it on the market, resulting in waste of lithium resources and corporate cost pressure.
Using the steps of cyclone concentration, slurry adjustment, rough selection, primary sweep selection and secondary flotation machine selection, the concentration and recovery of lithium mica are improved through the cyclone classifier grading dehydration and flotation technology, and avoid the use of Ball mill, simplify process flow.
Effectively improve the concentrate grade and recovery rate of lithium mica, reduce the influence of fine-grained mud materials on the selectivity of collectors, and provide a new lithium extract of lithium mica magnetic separation iron slag method.
Smart Images

Figure CN119076193A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lepidolite beneficiation, and in particular to a method for secondary lithium extraction from iron slag after magnetic separation of lepidolite. Background Art
[0002] As an important component of lithium resources, the efficient utilization of lithium mica has become a research hotspot. The "flotation-gravity-magnetic" combined process is a common beneficiation process in lithium mica concentrators. Flotation recovers lithium mica minerals, gravity recovers tantalum-niobium minerals, and magnetic separation separates iron minerals to obtain lithium mica, tantalum-niobium and feldspar concentrates. However, the iron slag after magnetic separation also contains a certain amount of lithium mica, in which the Li2O grade can usually reach more than 0.3%. This part of the iron slag is usually directly returned to the ball mill to increase the comprehensive recovery rate of the concentrator by about 1%. However, after the iron slag enters the closed-loop system, the whiteness of the feldspar produced will be reduced, and the lithium mica concentrate in it is difficult to fully recover.
[0003] At present, this type of iron slag is difficult to sell in the market, which not only brings cost pressure to enterprises, but also causes waste of lithium resources. Optimizing the iron slag treatment process to efficiently recover lithium mica from iron slag is an urgent problem to be solved. Summary of the invention
[0004] In order to solve the technical problems existing in the background technology, the present invention provides a method for secondary lithium extraction from iron slag after lepidolite magnetic separation.
[0005] The present invention provides a method for secondary lithium extraction from iron slag after magnetic separation of lepidolite, comprising the following steps:
[0006] S1, cyclone concentration: after magnetic separation, the iron slag is re-selected and the tailings of the chute are sent to the cyclone thickener and classifier to obtain the thickener and classifier overflow and thickener and classifier underflow;
[0007] S2, slurry adjustment, roughing: the underflow of the thickening and classifying machine obtained in S1 is sent to the 1# stirring barrel, soda ash is added to the 1# stirring barrel to adjust the pH to 7.0-8.0, and then inhibitors and collectors are added to stir and adjust the slurry. After the slurry adjustment is completed, it is sent to the roughing flotation machine, and the foam is scraped under the conditions of mechanical stirring and air introduction to obtain roughing flotation foam and roughing flotation pulp;
[0008] S3, one-time scavenging: the roughing flotation pulp in S2 is used as roughing tailings, and the collector is added and stirred, and then sent to the flotation machine for scavenging to obtain flotation foam and flotation pulp after one-time scavenging;
[0009] S4, secondary flotation machine selection: the primary roughing flotation foam obtained in S2 is fed into the 2# mixing barrel as the primary selection feed, after adding inhibitor and stirring, it is fed into the flotation machine for primary selection to obtain primary selection flotation foam and flotation slurry. The primary selection flotation foam enters the secondary selection to obtain the secondary selection foam, which is the lithium mica concentrate product.
[0010] S5, filtration and dehydration: The overflow of S1 thickener and classifier is pumped into the belt filter to obtain return water and iron slag products after dehydration.
[0011] Preferably, the lithium mica iron slag is the tailings of the conventional lithium mica beneficiation plant, and its technical parameters are as follows: Li2O grade ≥ 0.3%, -200 mesh particle size ratio ≥ 30%, slurry concentration 5-7%, wherein -200 mesh means the fineness is less than 200 mesh.
[0012] In the present invention, in step S1, a cyclone classifier is used to remove moisture from the ore pulp, and the material is concentrated to a mass concentration of 20-60%.
[0013] Preferably, in S2, based on the mass of the material in the 1# stirring barrel, the amount of the inhibitor added is 100-300 g / t, and the amount of the collector added is 300-600 g / t.
[0014] Preferably, in S2, the slurry adjustment step includes: adding an inhibitor, stirring for 5-10 minutes, and then adding a collector, stirring for 5-10 minutes.
[0015] Preferably, the method for extracting lithium from iron slag containing lithium mica concentrate also includes: sending the flotation machine pulp obtained in S2 into a scavenging flotation machine, adding a collector to carry out a scavenging and scraping foam, sending the scraped foam to the roughing flotation machine of step S2, and sending the tailings to the belt filter, that is, the foam obtained in step S3 is sent to the roughing flotation machine of step S2, and the tailings are sent to the belt filter.
[0016] Preferably, in step S3, the amount of collector added is 300-500 g / t based on the mass of the material in the flotation machine after one sweep.
[0017] Preferably, in S3, the time for adding the collector and stirring is 5-10 min.
[0018] Preferably, in S3, the bubbles obtained by one scavenging are sent to the roughing flotation machine in step S2.
[0019] Preferably, in S4, the amount of inhibitor added is 50-100 g / t.
[0020] Preferably, in S4, the time for stirring after adding the inhibitor is 5-10 min.
[0021] Preferably, in S4, the underflow obtained from the primary and secondary selection is sent to the 1# mixing barrel of the rough selection in step S2.
[0022] Preferably, the inhibitor is sodium hexametaphosphate.
[0023] Preferably, the collector is YM8-1 collector produced by Shandong Jinjuyuan Industry and Trade Co., Ltd.
[0024] Preferably, multiple concentrating and classifying machines in S1 are connected in parallel, and one, two or more concentrating and classifying machines are started according to the changes in the materials.
[0025] In winter when the temperature is low, heating can be carried out in the 1# mixing barrel to keep the slurry temperature at 10°C or above, which is beneficial to the improvement of flotation indicators.
[0026] In the present invention, the method for secondary lithium extraction from iron slag after lepidolite magnetic separation is proposed, and the beneficial effects are as follows:
[0027] (1) The present invention uses a cyclone classifier for graded dehydration and simultaneously concentrates to an optimal flotation concentration of 20-60%, effectively reducing the influence of fine-grained muddy materials on the selectivity of the collector and improving the flotation environment for lithium extraction from iron slag;
[0028] (2) The present invention uses the entire process without using a ball mill, and provides a new method for iron slag beneficiation after magnetic separation of lithium mica ore that is efficient, simple, stable, and has high recovery rate and grade index, which can be used for popularization and application.
[0029] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0031] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar symbols throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0032] Example 1
[0033] A method for secondary lithium extraction from iron slag after magnetic separation of lithium-containing mica, comprising the following steps:
[0034] S1. Cyclone concentration: The lithium mica iron slag (grade 0.3%, particle size -200 mesh accounting for 30%, mass concentration 5%) provided by a lithium mica concentrator in Yifeng County, Jiangxi Province is sent to the cyclone for concentration to obtain the overflow of the concentrator and the underflow of the concentrator with a mass concentration of 20%;
[0035] S2, slurry adjustment, roughing: the thickening and classifying machine bottom flow obtained in S1 is sent to the 1# stirring barrel, soda ash is added to the 1# stirring barrel to adjust the pH to 8.0, and then sodium hexametaphosphate is added, stirred for 5 minutes, and the collector YM8-1 produced by Shandong Jinjuyuan Industry and Trade Co., Ltd. is added, and stirred for 5 minutes. After the slurry adjustment is completed, it is sent to the self-priming roughing flotation machine, and the foam is scraped under the conditions of mechanical stirring and air introduction to obtain roughing flotation foam and roughing flotation pulp, wherein, based on the mass of the material in the 1# stirring barrel, the amount of sodium hexametaphosphate added is 100g / t, and the amount of collector added is 400g / t;
[0036] S3, one-time scavenging: the roughing flotation pulp in S2 is used as roughing tailings, the collector YM8-1 is added, stirred, and then sent to the flotation machine for scavenging and scraping foam. Specifically, the stirring time is 5 minutes, the scraped foam is sent to the roughing flotation machine in step S2, and the tailings are sent to the belt filter, wherein the amount of collector added is 300g / t;
[0037] S4, secondary flotation machine selection: the primary roughing flotation foam obtained in S2 is fed into the 2# stirring barrel as the primary selection feed, sodium hexametaphosphate is added and stirred, and then fed into the flotation machine for primary selection to obtain primary selection flotation foam and ore pulp, the primary selected foam is used as the secondary selection feed, the ore pulp is pumped into the 1# stirring barrel of the roughing in step S2, and the amount of sodium hexametaphosphate added is 50g / t; the secondary selected foam is lepidolite concentrate, and the secondary selected ore pulp is pumped into the 1# stirring barrel of the roughing in step S2.
[0038] The process flow diagram of the flotation method of Example 1 is as follows Figure 1 shown.
[0039] The above flotation results are shown in Table 1:
[0040] Table 1
[0041] name Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Concentrate 15.89 1.810 75.29 Tailings 84.11 0.112 24.71 Magnetic Concentrate 100.00 0.382 100.00
[0042] Example 2
[0043] A method for secondary lithium extraction from iron slag after magnetic separation of lithium-containing mica, comprising the following steps:
[0044] S1. Cyclone concentration: The lithium mica iron slag (grade 0.38%, particle size -200 mesh accounting for 50%, mass concentration 7%) provided by a lithium mica concentrator in Yifeng County, Jiangxi Province is sent to the cyclone for concentration to obtain the overflow of the concentrator classifier and the underflow of the concentrator classifier with a mass concentration of 60%;
[0045] S2, slurry adjustment, roughing: the thickening and classifying machine bottom flow obtained in S1 is sent to the 1# stirring barrel, soda ash is added to the 1# stirring barrel to adjust the pH to 7.0, and then sodium hexametaphosphate is added, stirred for 8 minutes, and collector YM8-1 is added, stirred for 8 minutes. After the slurry adjustment is completed, it is sent to the self-priming roughing flotation machine, and the foam is scraped under the conditions of mechanical stirring and air introduction to obtain roughing flotation foam and roughing flotation pulp, wherein, based on the mass of the material in the 1# stirring barrel, the amount of sodium hexametaphosphate added is 200g / t, and the amount of collector added is 400g / t;
[0046] S3, one-time scavenging: the roughing flotation pulp in S2 is used as roughing tailings, the collector YM8-1 is added, stirred, and then sent to the flotation machine for scavenging and scraping foam. Specifically, the stirring time is 10 minutes, the scraped foam is sent to the roughing flotation machine in step S2, and the tailings are sent to the belt filter, wherein the amount of collector added is 300g / t;
[0047] S4, secondary flotation machine selection: the primary roughing flotation foam obtained in S2 is fed into the 2# stirring barrel as the primary selection feed, sodium hexametaphosphate is added and stirred, and then fed into the flotation machine for primary selection to obtain primary selection flotation foam and ore pulp, the primary selected foam is used as the secondary selection feed, the ore pulp is pumped into the 1# stirring barrel of the roughing in step S2, and the amount of sodium hexametaphosphate added is 100g / t; the secondary selected foam is lepidolite concentrate, and the secondary selected ore pulp is pumped into the 1# stirring barrel of the roughing in step S2.
[0048] The process flow diagram of the flotation method of Example 2 is as follows Figure 1 shown.
[0049] The above flotation results are shown in Table 2:
[0050] Table 2
[0051] name Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Concentrate 12.35 1.860 60.13 Tailings 87.65 0.174 39.87 Magnetic Concentrate 100.00 0.382 100.00
[0052] Example 3
[0053] A method for secondary lithium extraction from iron slag after magnetic separation of lithium-containing mica, comprising the following steps:
[0054] S1. Cyclone concentration: The lithium mica iron slag (grade 0.38%, particle size -200 mesh accounting for 60%, mass concentration 6%) provided by a lithium mica concentrator in Yifeng County, Jiangxi Province is sent to a cyclone for concentration to obtain a thickening and classifying machine overflow and a thickening and classifying machine underflow with a mass concentration of 40%;
[0055] S2, slurry adjustment, roughing: the thickening and classifying machine bottom flow obtained in S1 is sent to the 1# stirring barrel, soda ash is added to the 1# stirring barrel to adjust the pH to 7.0, and then sodium hexametaphosphate is added, stirred for 10 minutes, and collector YM8-1 is added, stirred for 10 minutes. After the slurry adjustment is completed, it is sent to the self-priming roughing flotation machine, and the foam is scraped under the conditions of mechanical stirring and air introduction to obtain roughing flotation foam and roughing flotation pulp, wherein, based on the mass of the material in the 1# stirring barrel, the amount of sodium hexametaphosphate added is 200g / t, and the amount of collector added is 600g / t;
[0056] S3, primary scavenging: the roughing flotation pulp is fed into the primary scavenging flotation machine, and the collector YM8-1 is added and stirred to perform a scavenging and scraping foam. Specifically, the stirring time is 7.5 min, and the scraped foam is fed into the roughing flotation machine of step S2, and the tailings are fed into the belt filter, wherein the amount of the collector added is 400 g / t;
[0057] S4, secondary flotation machine selection: the primary roughing flotation foam obtained in S2 is fed into the 2# stirring barrel as the primary selection feed, sodium hexametaphosphate is added and stirred, and then fed into the flotation machine for primary selection to obtain primary selection flotation foam and ore pulp, the primary selected foam is used as the secondary selection feed, the ore pulp is pumped into the roughing stirring barrel, and the amount of sodium hexametaphosphate added is 75g / t; the secondary selected foam is lepidolite concentrate, and the secondary selected ore pulp is pumped into the roughing stirring barrel.
[0058] The process flow diagram of the flotation method of Example 3 is as follows Figure 1 shown.
[0059] The above flotation results are shown in Table 3:
[0060] Table 3
[0061] name Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Concentrate 16.70 1.750 76.51 Tailings 83.30 0.108 23.49 Magnetic Concentrate 100.00 0.382 100.00
[0062] Example 4
[0063] A method for secondary lithium extraction from iron slag after magnetic separation of lithium-containing mica, comprising the following steps:
[0064] S1, cyclone concentration: The lithium mica iron slag (grade 0.35%, particle size -200 mesh accounted for 40%, mass concentration 5.5%) provided by a lithium mica concentrator in Yifeng County, Jiangxi Province was sent to the cyclone for concentration to obtain the overflow of the concentrator and the underflow of the concentrator with a mass concentration of 30%;
[0065] S2, slurry adjustment, roughing: the thickening and classifying machine bottom flow obtained in S1 is sent to the 1# stirring barrel, soda ash is added to the 1# stirring barrel to adjust the pH to 7.5, and then sodium hexametaphosphate is added, stirred for 5 minutes, and collector YM8-1 is added, stirred for 5 minutes. After the slurry adjustment is completed, it is sent to the self-priming roughing flotation machine, and the foam is scraped under the conditions of mechanical stirring and air introduction to obtain roughing flotation foam and roughing flotation pulp, wherein, based on the mass of the material in the 1# stirring barrel, the addition amount of sodium hexametaphosphate is 300g / t, and the addition amount of collector is 400g / t;
[0066] S3, primary scavenging: send the roughing flotation pulp into the primary scavenging flotation machine, add the collector YM8-1 and stir it for a scavenging and scraping foam, the stirring time is 5min, send the scraped foam into the roughing flotation machine in step S2, and send the tailings into the belt filter, wherein the amount of collector added is 500g / t;
[0067] S4, secondary flotation machine selection: the primary roughing flotation foam obtained in S2 is fed into the 2# stirring barrel as the primary selection feed, sodium hexametaphosphate is added and stirred, and then fed into the flotation machine for primary selection to obtain primary selection flotation foam and ore pulp, the primary selected foam is used as the secondary selection feed, the ore pulp is pumped into the roughing stirring barrel, and the amount of sodium hexametaphosphate added is 50g / t; the secondary selected foam is lepidolite concentrate, and the secondary selected ore pulp is pumped into the roughing stirring barrel.
[0068] The process flow diagram of the flotation method of Example 4 is as follows Figure 1 shown.
[0069] The above flotation results are shown in Table 4:
[0070] Table 4
[0071] name Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Concentrate 16.12 1.791 82.25 Tailings 83.88 0.074 17.75 Magnetic Concentrate 100.00 0.351 100.00
[0072] The experimental results show that the lithium extraction method of iron slag containing lithium mica concentrate of the present invention can greatly improve the concentrate grade and recovery rate of lithium mica.
[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for secondary lithium extraction from iron slag after magnetic separation of lepidolite, characterized in that: The steps include: S1, cyclone concentration: after magnetic separation, the iron slag is re-selected and the tailings of the chute are sent to the cyclone thickener and classifier to obtain the thickener and classifier overflow and thickener and classifier underflow; S2, slurry adjustment, roughing: the underflow of the thickening and classifying machine obtained in S1 is sent to the 1# stirring barrel, soda ash is added to the 1# stirring barrel to adjust the pH to 7.0-8.0, and then inhibitors and collectors are added to stir and adjust the slurry. After the slurry adjustment is completed, it is sent to the roughing flotation machine, and the foam is scraped under the conditions of mechanical stirring and air introduction to obtain roughing flotation foam and roughing flotation pulp; S3, one-time scavenging: the roughing flotation pulp in S2 is used as roughing tailings, and the collector is added and stirred, and then sent to the flotation machine for scavenging to obtain flotation foam and flotation pulp after one-time scavenging; S4, secondary flotation machine selection: the primary roughing flotation foam obtained in S2 is fed into the 2# stirring barrel as the primary selection feed, after adding the inhibitor and stirring, it is fed into the flotation machine for primary selection to obtain primary selection flotation foam and flotation pulp, and the secondary selection foam obtained by the primary selection flotation foam entering the secondary selection is the lithium mica concentrate product; S5, filtration and dehydration: The overflow of S1 thickener and classifier is pumped into the belt filter to obtain return water and iron slag products after dehydration.
2. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: The lithium mica iron slag described in step S1 is the tailings of the conventional lithium mica beneficiation plant, and its technical parameters are as follows: Li2O grade ≥0.3%, -200 mesh particle size ratio ≥30%, and slurry concentration of 5-7%.
3. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S1, a cyclone classifier is used to remove moisture from the slurry, and the material is concentrated to a mass concentration of 20-60%.
4. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S2, based on the mass of the material in the 1# stirring barrel, the amount of the inhibitor added is 100-300 g / t, and the amount of the collector added is 300-600 g / t.
5. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S2, the slurry adjustment step includes: adding an inhibitor, stirring for 5-10 minutes, and then adding a collector, stirring for 5-10 minutes.
6. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: The foam obtained in step S3 is fed to the roughing flotation machine in step S2, and the tailings are fed to the belt filter.
7. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S3, the amount of collector added is 300-500 g / t based on the mass of the material in the flotation machine after one sweep.
8. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S3, the collector is added and stirred for 5-10 minutes.
9. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S4, the amount of inhibitor added is 50-100 g / t.
10. The method for secondary lithium extraction from iron slag after lepidolite magnetic separation according to claim 1, characterized in that: In step S4, the underflow obtained from the primary and secondary selection is sent to the 1# mixing barrel of the rough selection in step S2.
Citation Information
Patent Citations
Flotation method for fine-fraction lepidolite with high silt content
CN115780065A
Beneficiation method of lepidolite ore
CN116832957A