Deep titanium extraction method for pre-activating full-size ilmenite
Through multi-step enrichment and efficient pre-activation technology, the problem of low grade and recovery of whole-grain ilmenite concentrate is solved, and the depth of titanium improvement of high-efficiency ilmenite is achieved, which improves the utilization rate of titanium resources and stable production. sex.
Patent Information
- Application Number
- CN202411423053.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
The existing ore dressing technology is difficult to effectively treat whole-grain ilmenite, resulting in insufficient concentrate grade and recovery rate of ilmenite, increasing production costs and environmental pollution.
Multi-step enrichment method is used to combine efficient pre-activation and sulfur component enrichment, including tail pre-enrichment, strong magnetic pre-enrichment, fine grinding and quality improvement, iron removal and impurity reduction, strong magnetic re-enrichment, efficient pre-activation, Sulfur component enrichment and titanium component deep enrichment optimize mineral surfactant sites through multiple flotation and selection steps to improve the floatability and recovery of ilmenite.
It has achieved efficient recycling of TiO2 grade of titanium concentrate at a stable level of more than 47.2%, reducing agent consumption, improving production stability and comprehensive utilization rate of titanium resources.
Smart Images

Figure CN119076203A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ore dressing, in particular to a method for deep titanium extraction by pre-activating full-grained ilmenite. Background Art
[0002] Titanium is an important strategic metal material, which is widely used in aerospace, transportation, petrochemical and other fields. At present, the main recycled titanium resource is ilmenite, but with years of development and utilization, the properties of the ore have gradually shown the characteristics of poor fineness and hybridity. In recent years, many concentrators have often processed the ore by fine grinding to further improve the grade of vanadium-titanium magnetite concentrate. This has directly led to an increase in the proportion of difficult-to-select fine-grained materials in the original ore. Fine-grained minerals will consume a lot of reagents during the flotation process, and concentration and filtration will also be more difficult, which will increase production costs in all aspects.
[0003] In addition, production enterprises often use the magnetic-flotation combined process to obtain ilmenite products, but the floatability of ilmenite is not excellent. In actual production, enterprises often sacrifice the recovery rate of ilmenite in order to further improve the quality of concentrate, which also leads to the comprehensive recovery rate of TiO2 in many concentrators being less than 30%. Therefore, strengthening the deep extraction of titanium from full-grained ilmenite is of great significance to the comprehensive utilization rate of titanium resources in the concentrator.
[0004] In summary, providing a flotation method that can process full-size ilmenite and improve the grade and recovery rate of ilmenite concentrate is a technical problem that needs to be solved urgently. Summary of the invention
[0005] The object of the present invention is to provide a method for deep titanium extraction by preactivating full-grained ilmenite to solve the problems raised by the above-mentioned background technology.
[0006] The present invention solves the above problems through the following technical solutions:
[0007] A method for deep titanium extraction by preactivation of full-grained ilmenite, comprising the following steps:
[0008] S1. Pre-enrichment of tailings: Use a linear screen to pre-screen the iron ore tailings. The fine-grained materials under the screen are used as the raw materials for a strong magnetic pre-enrichment, and the coarse-grained materials on the screen are directly treated as tailings.
[0009] S2, one-stage strong magnetic pre-enrichment: directly carry out one-stage strong magnetic separation pre-enrichment on the fine-grained materials under the S1 linear screen to obtain a stage of strong magnetic concentrate; and carry out concentration, classification, and grinding treatment on the stage of strong magnetic concentrate to obtain overflow products and sedimentation products;
[0010] S3, fine grinding and quality improvement: Grinding and classifying the sedimentation products in S2 to increase the dissociation degree of mineral monomers, release the ilmenite in the coarse-grained intergrowth, and return to S2 for hydraulic classification after fine grinding, forming a closed-loop grinding and classification system;
[0011] S4, iron removal and impurity reduction: weak magnetic iron removal treatment is performed on the overflow product in S2 to remove the magnetite mixed in the overflow product, optimize the subsequent flotation environment, and obtain iron-removed tailings as the raw material for the second stage strong magnetic re-enrichment;
[0012] S5, two-stage strong magnetic re-enrichment: the iron-removing tailings in S4 are re-enriched by strong magnetic separation to obtain the two-stage strong magnetic concentrate as the flotation ore;
[0013] S6. High-efficiency pre-activation: pre-activate the flotation ore obtained in S5 with an activator, selectively change the types of active sites on the surface of the target mineral particles, reduce the active sites on the surface of the gangue mineral particles, and increase the selectivity of the collector for the target mineral in the flotation ore;
[0014] S7, sulfur component enrichment: the flotation ore after efficient pre-activation in S6 is subjected to sulfur roughing, sulfur scavenging and sulfur concentration at least once, and finally sulfur concentrate, sulfur middlings and desulfurization tailings are obtained;
[0015] S8, deep enrichment of titanium component: the desulfurized tailings in S7 are subjected to titanium roughing, titanium scavenging and titanium concentration to obtain titanium concentrate, titanium middlings and de-titanium tailings.
[0016] As a further improvement, in S2, the magnetic field strength is set to 1.1-1.4T, and the diameter of the strong magnetic rod medium is 2-3.5mm.
[0017] As a further improvement, in S2, the first stage of strong magnetic concentrate is concentrated, classified and ground;
[0018] Specifically, the concentration of the concentrated first-stage strong magnetic concentrate is 45-55%, and then it is subjected to the first hydraulic classification by a cyclone to be divided into a first-stage fine-grained strong magnetic concentrate, i.e., an overflow product, and a first-stage coarse-grained strong magnetic concentrate, i.e., a sedimentation product, and the yield of the overflow product is 20-30%.
[0019] As a further improvement, in S4, the magnetic field strength of the weak magnetic iron removal is 220-250Mt.
[0020] As a further improvement, in S5, the magnetic field strength is set to 1.0-1.3T, and the diameter of the strong magnetic rod medium is 1.5-3mm.
[0021] As a further improvement, in S6, the activator is one or more strong oxidizing agents.
[0022] As a further improvement, the strong oxidizing agent is permanganate, ferrate, Fenton's reagent or sulfuric acid.
[0023] As a further improvement, the S7 further includes: returning the sulfur middlings to S5 and combining them with the second stage strong magnetic concentrate as part of the flotation ore; and / or
[0024] The step S8 also includes: adding the titanium middlings to the desulfurization tailings to re-perform the step of deep enrichment of the titanium component.
[0025] As a further improvement, the step S8 further includes: returning the titanium middlings to the previous titanium concentration step in sequence.
[0026] In the flotation process for enriching sulfur components, the pH value of the flotation tank for sulfur roughing is 4-6, the pH value of the flotation tank for sulfur cleaning is 2-4, and the pH value of the flotation tank for sulfur scavenging is less than 6; and / or
[0027] In S8, the titanium roughing, titanium scavenging and titanium concentrating all adopt flotation process;
[0028] In the flotation process for deep enrichment of titanium components, the pH value of the titanium flotation tank for titanium roughing is 4-5; the pH value of the titanium flotation tank for titanium fine selection is 2.5-4, and the pH value of the titanium flotation tank for titanium fine selection decreases successively with the increase of the number of titanium fine selections; the pH value of the titanium flotation tank for titanium scavenging is 3-4.
[0029] As a further improvement, the reagents used in the sulfur roughing, sulfur scavenging and sulfur cleaning include a regulator, a collector and a frother, which are sulfuric acid, xanthate and pine oil respectively; and / or
[0030] The reagents used in the titanium roughing, titanium scavenging and titanium concentrating include adjusting agents, collecting agents, depressants and foaming agents.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] (1) The present invention can ensure to the greatest extent that the titanium concentrate with a stable TiO2 grade of more than 47.2% is obtained through multiple enrichment steps in combination with efficient pre-activation and sulfur component enrichment, as well as titanium component deep enrichment and other concentrating operations. It has strong adaptability to raw ores with complex properties and can ensure production stability.
[0033] (2) The present invention performs multiple enrichment step processing through steps S1-S5, which can optimize the subsequent flotation environment, improve the monomer dissociation degree of the target mineral, and reduce the consumption of reagents.
[0034] (3) If sulfuric acid is selected as the efficient activator of the present invention, the flotation operation can be carried out in an acidic slurry from the beginning. The acidic environment can play a decisive and positive role in the flotation of sulfide ores, especially the flotation of pyrite, so it can play an additional role in the selection of sulfur component enrichment while preactivating ilmenite. And the efficient preactivation of ilmenite can be easily achieved by oxidation method. The Fe2+ on the surface of ilmenite is oxidized to Fe3+ which is easier to adsorb with the reagent, and with strong acidic conditions, the Ti4+ on the surface of ilmenite can also act as a new active site with the reagent, providing a positive effect for the capture of the target mineral, that is, enhancing the capture of the target mineral by the reagent, and prolonging the oxidation time can give full play to the preactivation effect. In addition, by using sulfuric acid for preactivation treatment, sulfuric acid can dissolve a variety of gangue minerals including carbonate minerals and silicate minerals to a certain extent, reducing the active sites such as Ca2+ and Mg2+ on their surfaces that may be adsorbed with the reagent. In short, acid activation pretreatment of the ilmenite surface can increase the floatability difference between ilmenite and gangue minerals, enhance the separation selectivity of the flotation agent for the two, and thus ensure the maximum TiO2 grade of titanium concentrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic flow diagram of a method for deep titanium extraction by preactivation of full-grained ilmenite of the present invention;
[0036] Figure 2 Schematic diagram of Gibbs free energy of ilmenite preactivation according to the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the present application clearer, the technical solutions in the embodiments of the present application will be described in more detail below in conjunction with the drawings in the preferred embodiments of the present application. In the drawings, the same or similar reference numerals throughout represent the same or similar parts or parts with the same or similar functions. The described embodiments are part of the embodiments of the present application, not all of the embodiments. The embodiments described below with reference to the drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limitations on the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0038] The embodiments of the present application are described in detail below with reference to the accompanying drawings.
[0039] In the description of the present application, it should be noted that, unless expressly provided and limited otherwise, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or display comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units that are not explicitly listed or inherent to these processes, methods, products or displays.
[0040] The following will be combined Figure 1-2 , a method for deep titanium extraction by pre-activation of full-grained ilmenite involved in the embodiments of the present application is described in detail. It is worth noting that the following embodiments are only used to explain the present application and do not constitute a limitation on the present application.
[0041] Combined with Figure 1 As shown, a method for deep titanium extraction by preactivation of full-grained ilmenite of the present invention specifically comprises the following steps:
[0042] S1. Pre-enrichment of tailings: Use a linear screen to pre-screen the iron ore tailings. The fine-grained materials under the screen are used as the raw materials for a strong magnetic pre-enrichment, and the coarse-grained materials on the screen are directly treated as tailings.
[0043] As a further optimization, the mesh size of the linear screen should be 1-2 mm.
[0044] The present invention can directly discard about 2-5% of the coarse-grained iron ore tailings through step S1. The TiO2 grade of this part of tailings is less than 4%. Directly discarding can prevent the tailings from clogging the medium box of the strong magnetic machine. At the same time, the pre-waste discarding process can reduce the amount of grinding and grading materials, increase the process processing capacity, increase the ore selection grade, reduce energy consumption, save costs, and improve the overall economic benefits.
[0045] S2, one-stage strong magnetic pre-enrichment: the fine-grained material under the above-mentioned linear screen is directly subjected to a stage of strong magnetic separation pre-enrichment to obtain a stage of strong magnetic concentrate;
[0046] As a further optimization, the magnetic field strength is preferably set to 1.1-1.4 T, and the diameter of the strong magnetic rod medium is 2-3.5 mm.
[0047] The first stage of strong magnetic concentrate is concentrated, classified and ground to obtain overflow products and sedimentation products;
[0048] As a further optimization, the concentration of the concentrated first-stage strong magnetic concentrate should be 45-55%, and then it is hydraulically classified through a cyclone to be divided into a fine-grained first-stage strong magnetic concentrate, i.e., overflow product, and a coarse-grained first-stage strong magnetic concentrate, i.e., sand settling product. The yield of the overflow product should be 20-30%.
[0049] S3, fine grinding and quality improvement: The sand settling products in the above S2 are subjected to grinding and classification treatment to increase the dissociation degree of mineral monomers and release the ilmenite in the coarse-grained intergrowth. The proportion of -0.074 mm materials in the ball mill discharge products should be greater than 40%. After fine grinding, they are returned to the cyclone of S2 for hydraulic classification to form a grinding and classification closed-loop circulation system.
[0050] S4, iron removal and impurity reduction: weak magnetic iron removal is performed on the overflow product in S2 to remove the magnetite mixed in the overflow product and optimize the subsequent flotation environment. The iron removal tailings are used as the raw material for the second stage of strong magnetic re-enrichment.
[0051] As a further optimization, the magnetic field strength for weak magnetic iron removal should be 220-250mT.
[0052] S5, two-stage strong magnetic re-enrichment: the iron-removing tailings in the above S3 are subjected to strong magnetic separation and re-enrichment to obtain a two-stage strong magnetic concentrate as the flotation ore.
[0053] As a further optimization, the magnetic field strength is preferably set to 1.0-1.3 T, and the diameter of the strong magnetic rod medium is 1.5-3 mm.
[0054] As a further optimization, the second-stage strong magnetic concentrate is concentrated and used as flotation ore. The concentration of the flotation ore is preferably 55-65%.
[0055] As a further optimization, the TiO2 grade of the flotation ore should be 18%-25%.
[0056] The present invention further discards about 65-70% of tailings through steps S2-S5, so that the TiO2 grade in the iron ore tailings is increased from less than 10% to more than 18%, and the TiO2 recovery rate reaches more than 60%. Through two-stage strong magnetic separation and fine grinding and quality improvement methods, the subsequent flotation environment is further optimized, the monomer dissociation degree of the target mineral is improved, and the reagent consumption is reduced.
[0057] S6. High-efficiency pre-activation: Use high-efficiency activators to pre-activate the above flotation ore, selectively change the types of active sites on the surface of the target mineral particles, reduce the active sites on the surface of the gangue mineral particles, and thus increase the selectivity of the collector for the target mineral in the flotation ore. The activator is mainly used for oxidative flotation ore, and controls the difference in oxidation degree between the target mineral and the gangue mineral by oxidation, thereby controlling the difference in surface floatability between the target mineral and the gangue mineral.
[0058] As a further optimization, the activator can be a strong oxidizing agent, such as permanganate, ferrate, Fenton's reagent, sulfuric acid, etc. In order to achieve a better pre-activation effect, a combination of agents can also be used to give full play to the synergistic effect between agents. Taking sulfuric acid as an example, the main chemical equations related to the reaction of ilmenite and sulfuric acid are as follows:
[0059] FeTiO3 + 3H2SO4 = Ti(SO4)2 + FeSO4 + 3H2O Formula (1);
[0060] FeTiO3 + 2H2SO4 = TiOSO4 + FeSO4 + 2H2O Formula (2);
[0061] 4FeSO4 + O2 + 2H2SO4 = 2Fe2(SO4)3 + 2H2O Formula (3);
[0062] Ti(SO4)2 + 3H2O = TiO2·H2O↓+ 2H2SO4 Formula (4);
[0063] TiOSO4 + 2H2O = TiO2·H2O↓+ H2SO4 Formula (5);
[0064] Equations (1), (2), and (3) are the first-stage series of reactions between the ilmenite surface and sulfuric acid, while equations (4) and (5) are further series of reactions.
[0065] The Gibbs free energy of equations (1), (2), and (3) was calculated using thermodynamic analysis. The results are shown in the attached figure. Figure 2 As shown, in the temperature range of 0-1000℃, the Gibbs free energy of chemical reaction equations (1), (2) and (3) is less than 0, and the oxidation reaction of ferrous sulfate represented by equation (3) is more likely to occur. From the results, it can be seen that the chemical reactions represented by equations (1), (2) and (3) can all proceed spontaneously under the daily production conditions of the concentrator.
[0066] As a further optimization, the effect of pre-activation can be enhanced by prolonging the action time of the reagent and the flotation ore. Therefore, the number of mixing barrels can be increased, preferably 5-7.
[0067] In step S6 of the present invention, if sulfuric acid is selected as the efficient activator, the flotation operation can be carried out in the acidic slurry from the beginning. As is well known, the acidic environment can play a decisive and positive role in the flotation of sulfide ores, especially the flotation of pyrite, so it can play an additional effect of enhancing the enrichment of sulfur components while pre-activating ilmenite.
[0068] In addition, in step S6 of the present invention, the strong oxidizing agent can easily achieve efficient pre-activation of ilmenite by oxidation, and the Fe2+ on the surface of ilmenite is oxidized to Fe3+ which is more easily adsorbed by the agent, and with strong acidic conditions, the Ti4+ on the surface of ilmenite can also act as a new active site with the agent, providing a positive effect for the capture of the target mineral, that is, enhancing the capture of the target mineral by the agent, and extending the oxidation time can give full play to the pre-activation effect. In addition, sulfuric acid is used for pre-activation treatment, and sulfuric acid can dissolve a variety of gangue minerals including carbonate minerals and silicate minerals to a certain extent, reducing the active sites such as Ca2+ and Mg2+ on its surface that may be adsorbed by the agent. In short, the acid activation pretreatment on the surface of ilmenite can increase the floatability difference between ilmenite and gangue minerals, and enhance the separation selectivity of the flotation agent to the two.
[0069] S7, sulfur component enrichment: the flotation ore after efficient pre-activation in the above S6 is subjected to one or more sulfur roughing, one or more sulfur scavenging, and one or more sulfur concentrating to obtain sulfur concentrate, sulfur middlings and desulfurized tailings;
[0070] The specific steps of obtaining sulfur concentrate, sulfur middlings and desulfurized tailings are as follows:
[0071] The flotation ore is subjected to sulfur roughing at least once to obtain sulfur roughing concentrate and sulfur roughing tailings; the sulfur roughing concentrate is subjected to sulfur concentrating at least once to obtain sulfur concentrating concentrate and sulfur concentrating tailings; the sulfur roughing tailings are subjected to sulfur scavenging at least once to obtain sulfur scavenging concentrate and sulfur scavenging tailings; then, the sulfur concentrating tailings and the sulfur scavenging concentrate are combined as sulfur middlings, the sulfur concentrating concentrate is used as sulfur concentrate, and the sulfur scavenging tailings are used as desulfurization tailings, and finally sulfur concentrate, sulfur middlings, and desulfurization tailings are obtained; the sulfur roughing, sulfur concentrating, and sulfur scavenging all adopt flotation technology. The sulfur middlings are returned and combined with the second-stage strong magnetic concentrate as part of the flotation ore.
[0072] As a further optimization, the reagents used in sulfur roughing, sulfur scavenging and sulfur cleaning in sulfur-rich resources include adjusters, collectors, foaming agents, etc., and sulfuric acid, xanthate and pine oil can be selected respectively.
[0073] As a further optimization, in the enrichment of sulfur components, in addition to controlling the amount of sulfuric acid added, it is also necessary to ensure the pH value range in the flotation tanks of each process. The pH value of sulfur roughing is preferably controlled in the range of 4-6, the pH value of sulfur cleaning is preferably controlled in the range of 2-4, and the pH value of sulfur scavenging is controlled in the range of <6.
[0074] S8, deep enrichment of titanium component: the desulfurized tailings in S7 are subjected to one or more titanium roughing, five or more titanium concentrating, and two or more titanium scavenging to obtain titanium concentrate, titanium middlings and de-titanium tailings, and the titanium middlings are returned to the previous titanium concentrating step in sequence; finally, titanium concentrate and titanium tailings are obtained. The titanium roughing, titanium concentrating and titanium scavenging all adopt flotation process.
[0075] The specific steps of deep enrichment of titanium component are:
[0076] Performing titanium roughing on the desulfurized tailings for at least one time to obtain titanium roughing concentrate and titanium roughing tailings;
[0077] The titanium rougher tailings are subjected to titanium scavenging at least twice to obtain titanium scavenging concentrate and titanium scavenging tailings;
[0078] The titanium rougher concentrate is subjected to titanium concentration for no less than five times to obtain titanium concentrate and titanium concentrate tailings, and in this process, the titanium scavenger concentrate can be added to the titanium rougher concentrate for titanium concentration together, and the titanium concentrate tailings after each titanium concentration are returned to the previous titanium concentration step in sequence;
[0079] Finally, the titanium scavenging tailings are obtained as desulfurization tailings and detitanium tailings, the titanium concentration concentrate is used as titanium concentrate, and the titanium scavenging concentrate and the titanium concentration tailings obtained in each titanium concentration are used as titanium middlings.
[0080] As a further optimization, the reagents used in the titanium roughing, titanium scavenging and titanium concentrating in the deep enrichment of the titanium component include regulators, collectors, inhibitors, foaming agents and the like.
[0081] As a further optimization, in the deep enrichment of titanium components, in addition to controlling the amount of sulfuric acid added, the pH value range in the titanium flotation tank must be guaranteed. The pH value of the titanium roughing is preferably controlled within the range of 4-5; the pH value of the titanium flotation tank of the titanium concentrating is 2.5-4, and the pH value of the titanium flotation tank of the titanium concentrating decreases with the increase of the number of titanium concentrating; specifically, the pH value of titanium concentrating I is preferably controlled within the range of 3.5-4; the pH value of titanium concentrating II is preferably controlled within the range of 3-3.5; the pH value of titanium concentrating III and titanium concentrating IV is preferably controlled within the range of 2.5-3; the pH value of titanium concentrating V is preferably controlled within the range of 2-2.5; the pH value of titanium scavenging I and titanium scavenging II is preferably controlled within the range of 3-4.
[0082] The multiple pre-enrichment steps shown in the present invention, combined with efficient pre-activation and multiple concentration operations, can ensure to the greatest extent that the titanium concentrate with a stable TiO2 grade of more than 47.2% is obtained. Therefore, the method shown in the present invention has strong adaptability to raw ores with complex properties and can ensure the stability of production.
[0083] Two specific embodiments are listed below to illustrate the method and effect of deep titanium extraction by preactivation of full-grained ilmenite involved in the present invention:
[0084] Embodiment 1:
[0085] The iron ore tailings used in this embodiment have a TFe grade of 12.20%, a TiO2 grade of 8.17%, a S grade of 0.91%, and a P2O5 grade of 2.00%. -0.074mm materials account for about 36.10%, and -0.038mm materials account for about 21.62%.
[0086] Based on the titanium extraction method provided by the present invention, the specific implementation method is as follows:
[0087] S1. Pre-enrichment of tailings: Use a linear sieve with a sieve hole of 1.5 mm to separate the coarse tailings.
[0088] S2, one-stage strong magnetic pre-enrichment: the material under the linear screen is subjected to one-stage strong magnetic separation under a magnetic field strength of 1.2T, and the medium diameter of the one-stage strong magnetic rod is 3mm. The one-stage strong magnetic concentrate is concentrated, classified, and ground. The concentration of the concentrated one-stage strong magnetic concentrate reaches about 46%, and then the cyclone is classified, and the overflow product yield is about 22%.
[0089] S3, fine grinding and quality improvement: The sand settling products in the above S2 are ground and graded, and the proportion of -0.074mm materials in the ball mill discharge products is about 41.47%.
[0090] S4, iron removal and impurity reduction: the overflow product in the above S2 is treated with a magnetic drum with a magnetic field strength of 250mT.
[0091] S5, second stage strong magnetic re-enrichment: the iron-removing tailings in S3 are treated at a magnetic field strength of 1.1 T, and the diameter of the second stage strong magnetic rod medium is 2 mm. The second stage strong magnetic concentrate is concentrated to a concentration of about 56.10%.
[0092] S6. High-efficiency pre-activation: dilute sulfuric acid is used to carry out high-efficiency pre-activation treatment on the above-mentioned second-stage strong magnetic concentrate. In order to improve the pre-activation effect, 10% sulfuric acid is used on site, and the amount used reaches 12,000 g / t, and 6 mixing drums are used.
[0093] S7, sulfur component enrichment: the flotation ore in S6 is subjected to a sulfur roughing, a sulfur scavenging and a sulfur concentrating. The amount of xanthate used in the roughing is 80g / t, and the amount of pine oil is 30g / t; the amount of xanthate used in the scavenging is 50g / t, and the amount of pine oil is 10g / t; the amount of xanthate used in the concentrating is 30g / t, the amount of pine oil used is 10g / t, and the amount of sulfuric acid used is 500g / t;
[0094] S8, deep enrichment of titanium component: the sulfur tailings in the above S7 are subjected to one titanium roughing selection, five titanium concentrating selections, and two titanium sweeping selections to finally obtain titanium concentrate and titanium tailings. The dosage of fatty acid composite collector for titanium roughing is 1100g / t, the dosage of diesel is 300g / t, the dosage of fluorosilicate is 4200g / t, the dosage of pine oil is 50g / t, and the dosage of sulfuric acid is 3000g / t; the dosage of sulfuric acid for titanium selection I is 2000g / t; the dosage of sulfuric acid for titanium selection II is 1000g / t; the dosage of sulfuric acid for titanium selection III is 800g / t; the dosage of sulfuric acid for titanium selection IV is 500g / t; the dosage of sulfuric acid for titanium selection V is 500g / t; the dosage of fatty acid composite collector for titanium scavenging I is 200g / t; the dosage of fatty acid composite collector for titanium scavenging II is 100g / t;
[0095] Finally, titanium concentrate with a TiO2 grade of 47.62% and a recovery rate of 53.65% and titanium tailings with a TiO2 grade of 4.17% and a recovery rate of 46.34% were obtained.
[0096] Embodiment 2:
[0097] The iron ore tailings used in this embodiment have a TFe grade of 10.16%, a TiO2 grade of 7.24%, a S grade of 0.69%, and a P2O5 grade of 0.09%. -0.074mm materials account for about 30.06%, and -0.038mm materials account for about 16.14%.
[0098] Based on the titanium extraction method provided by the present invention, the specific implementation method is as follows:
[0099] S1. Separate the coarse and discard the tailings: Use a linear sieve with a mesh size of 1.5mm to separate the coarse and discard the tailings.
[0100] S2, one-stage strong magnetic pre-enrichment: the material under the linear screen is subjected to one-stage strong magnetic separation under a magnetic field strength of 1.3T, and the medium diameter of the one-stage strong magnetic rod is 2mm. The one-stage strong magnetic concentrate is concentrated, classified, and ground. The concentration of the concentrated one-stage strong magnetic concentrate reaches about 41%, and then the cyclone is classified, and the overflow product yield is about 18%.
[0101] S3, iron removal and impurity reduction: The overflow product in the above S2 is treated with a magnetic drum with a magnetic field strength of 220mT.
[0102] S4, fine grinding and quality improvement: The sand settling products in the above S2 are ground and graded, and the proportion of -0.074mm materials in the ball mill discharge products is about 35.10%.
[0103] S5, second stage strong magnetic re-enrichment: the iron removal tailings in S3 are treated at a magnetic field strength of 1.2 T, and the diameter of the second stage strong magnetic rod medium is 1.5 mm. The second stage strong magnetic concentrate is concentrated to a concentration of about 56.10%.
[0104] S6. High-efficiency pre-activation: dilute sulfuric acid is used to carry out high-efficiency pre-activation treatment on the above-mentioned second-stage strong magnetic concentrate. In order to improve the pre-activation effect, 10% sulfuric acid is used on site, and the amount used reaches 15,000g / t, and 5 mixing drums are used.
[0105] S7, sulfur component enrichment: the flotation ore in S6 is subjected to a sulfur roughing, a sulfur scavenging and a sulfur concentrating. The amount of xanthate used in the roughing is 50g / t, and the amount of pine oil used is 10g / t; the amount of xanthate used in the scavenging is 20g / t, and the amount of pine oil used is 10g / t; the amount of sulfuric acid used in the concentrating is 200g / t;
[0106] S8, deep enrichment of titanium component: the sulfur tailings in the above S7 are subjected to one titanium roughing, four titanium concentrating and two titanium scavenging, and finally titanium concentrate and titanium tailings are obtained. The dosage of fatty acid composite collector for titanium roughing is 1000g / t, the dosage of diesel is 450g / t, the dosage of pine oil is 80g / t, and the dosage of sulfuric acid is 2000g / t; the dosage of sulfuric acid for titanium concentrating I is 1500g / t; the dosage of sulfuric acid for titanium concentrating II is 1000g / t; the dosage of sulfuric acid for titanium concentrating III is 500g / t; the dosage of sulfuric acid for titanium concentrating IV is 300g / t; the dosage of fatty acid composite collector for titanium scavenging I is 300g / t; the dosage of fatty acid composite collector for titanium scavenging II is 200g / t;
[0107] Finally, titanium concentrate with a TiO2 grade of 47.52% and a recovery rate of 50.10% and titanium tailings with a TiO2 grade of 3.91% and a recovery rate of 49.80% were obtained.
[0108] Although the present invention is described herein with reference to the illustrative embodiments of the present invention, the above embodiments are only preferred embodiments of the present invention, and the embodiments of the present invention are not limited to the above embodiments. It should be understood that those skilled in the art can design many other modifications and embodiments, which will fall within the scope and spirit of the principles disclosed in this application.
Claims
1. A method for deep titanium extraction by preactivation of full-grained ilmenite, characterized in that: The following steps are involved: S1, tailing pre-enrichment: The iron ore tailings are pre-screened using a linear screen. The fine-grained materials under the screen are used as raw materials for a strong magnetic pre-enrichment, and the coarse-grained materials on the screen are directly discarded. S2, a strong magnetic pre-enrichment: The fine-grained material under the S1 linear screen is directly subjected to a stage of high-intensity magnetic separation pre-enrichment to obtain a stage of high-intensity magnetic concentrate; and the stage of high-intensity magnetic concentrate is concentrated, graded, and ground to obtain overflow products and sedimentation products; S3, fine grinding and quality improvement: The sand settling products in S2 are subjected to grinding and classification treatment to increase the dissociation degree of mineral monomers and release the ilmenite in the coarse-grained intergrowth. After fine grinding, they are returned to S2 for hydraulic classification to form a grinding and classification closed-loop circulation system; S4, iron removal and impurity reduction: The overflow product in S2 is subjected to weak magnetic iron removal treatment to remove the magnetite mixed in the overflow product, optimize the subsequent flotation environment, and obtain iron-removed tailings as the raw material for the second stage of strong magnetic re-enrichment; S5, Second stage strong magnetic re-enrichment: The iron-removing tailings in S4 are re-enriched by strong magnetic separation to obtain the second-stage strong magnetic concentrate as the flotation ore; S6, efficient pre-activation: The flotation ore obtained by S5 is pre-activated by using an activator to selectively change the types of active sites on the surface of the target mineral particles and reduce the active sites on the surface of the gangue mineral particles, so as to increase the selectivity of the collector for the target mineral in the flotation ore; S7, Sulfur component enrichment: The flotation ore in S6 that has been efficiently pre-activated is subjected to sulfur roughing, sulfur cleaning and sulfur scavenging to obtain sulfur concentrate, sulfur middlings and desulfurized tailings; S8, Deep enrichment of titanium components: The desulfurized tailings in S7 are subjected to titanium roughing, titanium scavenging and titanium concentrating to obtain titanium concentrate, titanium middlings and desulfurized tailings.
2. A method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: In S2, the magnetic field strength is set to 1.1-1.4T, and the diameter of the strong magnetic rod medium is 2-3.5mm.
3. The method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: In S2, a section of strong magnetic concentrate is concentrated, classified and ground; Specifically, the concentration of the concentrated first-stage strong magnetic concentrate is 45-55%, and then Cyclone The first hydraulic classification is carried out to separate the fine-grained first-stage strong magnetic concentrate, i.e., overflow product, and the coarse-grained first-stage strong magnetic concentrate, i.e., sedimentation product, and the yield of the overflow product is 20-30%.
4. The method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: In S4, the magnetic field strength of weak magnetic iron removal is 220-250Mt.
5. The method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: In the S5, the magnetic field strength is set to 1.0-1.3T, and the diameter of the strong magnetic rod medium is 1.5-3mm.
6. The method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: In S6, the activator is one or more strong oxidizing agents.
7. A method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 6, characterized in that: The strong oxidizing agent is permanganate, ferrate, Fenton's reagent or sulfuric acid.
8. The method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: The step S7 further includes: returning the sulfur middlings to step S5 and combining them with the second stage strong magnetic concentrate as part of the flotation ore; and / or The step S8 also includes: returning the titanium middlings to the previous titanium concentration step in sequence.
9. The method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 1, characterized in that: In S7, the sulfur roughing, sulfur cleaning and sulfur scavenging all adopt flotation process; In the flotation process for enriching the sulfur component, the pH value of the flotation tank for sulfur roughing is 4-6, the pH value of the flotation tank for sulfur cleaning is 2-4, and the pH value of the flotation tank for sulfur scavenging is less than 6; and / or In S8, the titanium roughing, titanium scavenging and titanium concentrating all adopt flotation process; In the flotation process for deep enrichment of titanium components, the pH value of the titanium flotation tank for titanium roughing is 4-5; the pH value of the titanium flotation tank for titanium fine selection is 2.5-4, and the pH value of the titanium flotation tank for titanium fine selection decreases successively with the increase of the number of titanium fine selections; the pH value of the titanium flotation tank for titanium scavenging is 3-4.
10. A method for deep titanium extraction by preactivation of full-grained ilmenite according to claim 9, characterized in that: The reagents used in the sulfur roughing, sulfur scavenging and sulfur cleaning include a regulator, a collector and a frother, which are sulfuric acid, xanthate and pine oil respectively; and / or The reagents used in the titanium roughing, titanium scavenging and titanium concentrating include adjusting agents, collecting agents, depressants and foaming agents.
Citation Information
Cited By
Titanium middling physical and chemical coupling enhanced upgrading method
CN119702257A