Nickel-saving environment-friendly austenitic stainless steel flux-cored wire for LNG ultralow-temperature valve additive manufacturing and preparation method thereof

The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire addresses the challenges of high strength and low-temperature toughness in LNG valves by using a specialized composition, enhancing weld performance and reducing pollution and costs.

CN119077216APending Publication Date: 2024-12-06SHANGHAI UNIV OF ENG SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411421372.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing welding materials for ultra-low temperature applications, such as LNG valves, face challenges in achieving high strength, low-temperature toughness, and corrosion resistance, while also generating environmental pollution and being costly due to the use of nickel and toxic chromium.

Method used

A nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire with a specific chemical composition, including elements like nitrogen, molybdenum, manganese, and rare earth praseodymium, is designed to enhance strength, toughness, and reduce pollution, featuring a low-carbon stainless steel strip and a flux core with controlled component ratios.

Benefits of technology

The welding wire achieves high yield strength of over 544MPa and low-temperature impact toughness greater than 40J at -196°C, with reduced environmental pollution and cost through the use of zinc instead of chromium and nitrogen instead of nickel, ensuring excellent weld performance and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005080890320000071
    Figure BDA0005080890320000071
Patent Text Reader

Abstract

The invention discloses a nickel-saving environment-friendly austenitic stainless steel flux-cored wire for LNG ultralow-temperature valve additive manufacturing and a preparation method of the nickel-saving environment-friendly austenitic stainless steel flux-cored wire. A flux core of the flux-cored wire comprises the following chemical components in percentage by weight: less than or equal to 0.03% of C, 10.35%-11.25% of Cr, 11.50%-12.50% of Ni, 0.10%-0.20% of N, 0.30%-0.90% of Mo, 5.00%-8.00% of Mn, 0.30%-0.90% of Si, 0.01%-0.02% of Pr, 0.3%-1.1% of Zn, 0.2%-0.6% of V and the balance of Fe and inevitable impurities. Chemical components of the welding wire are reasonably designed, regulated and controlled, low-temperature-resistant and corrosion-resistant rare earth elements are introduced, the welding wire is used for LNG ultralow-temperature valve additive manufacturing, the precision of a deposition layer and the mechanical property of a printed piece are remarkably improved, and the special requirement for LNG ultralow-temperature application is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of welding materials, and in particular relates to a nickel-saving and environment-friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves and a preparation method thereof. Background Art

[0002] Steels used in storage equipment and transportation pipelines for liquefied natural gas, liquid nitrogen, and liquid oxygen require high ultra-low temperature toughness to ensure the safety and reliability of components. As traditional ultra-low temperature steels, austenitic stainless steels such as AISI 304 have been widely used. Although austenitic stainless steels have high corrosion resistance and ultra-low temperature toughness, their low strength, especially low yield strength, is their fatal weakness. The yield strength of high nitrogen austenitic stainless steel is only about 400MPa. 5Ni and 9Ni steels have high ultra-low temperature toughness through grain refinement and the formation of stable residual / reverse transformation austenite, which can meet the safety and reliability requirements of some ultra-low temperature components. However, this type of steel has weak corrosion resistance and cannot be used in harsh environments, especially environments such as liquefied natural gas containing CO, HS, etc.

[0003] Semi-austenitic stainless steels such as 07Cr16Ni6 and 08Cr14NiTMo are significantly stronger than austenitic stainless steels. As long as the austenite is properly controlled, sufficient ultra-low temperature toughness can be guaranteed. However, the window of alloying elements such as Cr and Ni to control the amount of austenite is very narrow, and industrial production is difficult. In addition, semi-austenitic stainless steels have the problem of sensitization, and the performance of welds and heat-affected zones cannot be guaranteed. After the size of 07Cr16Ni6 steel is increased, a network of carbides is formed during quenching, which not only seriously damages toughness, but also reduces intergranular corrosion resistance. Russian scholars developed 0Cr12Ni10MoTi high-strength martensitic stainless steel by reducing Mo and Ti on the basis of 0OCr11Ni10Mo2Ti martensitic aging stainless steel, and finally adjusted it to 0Cr12NilOMo. According to the needs of ultra-low temperature engineering, it is currently used after tempering at 250℃ and 500℃ respectively. The ultra-low carbon content makes it have good weldability and corrosion resistance, but the strength is still relatively low. The maximum strength (aged at 500°C) is only about 1000MPa, which still cannot meet the increasingly high strength requirements for steel used in ultra-low temperature equipment.

[0004] Since C-Mn steel and low alloy steel will become brittle at low temperatures, and the brittleness is very obvious when the temperature reaches below -100℃, austenitic stainless steel has good low-temperature impact resistance, and still has good impact energy even at -196℃. Therefore, austenitic stainless steel is widely used as an ideal material in low-temperature environments. However, the organization and state of austenitic stainless steel welds are somewhat different from those of the parent material, and it is still difficult to achieve the impact energy required by the standard at -196℃. According to GB150-2011, the low-temperature impact energy of the weld metal at -196℃ shall not be less than 31J. At this temperature, it is difficult to ensure the impact energy using ordinary stainless steel welding materials and welding processes. Therefore, special requirements must be made on the chemical composition of the welding materials, and specific welding processes must be used to ensure their low-temperature impact resistance.

[0005] Low-nickel nitrogen-containing austenitic stainless steel mainly uses nitrogen to partially or even completely replace the alloying element nickel to obtain a single-phase austenite structure. Using nitrogen for alloying has many advantages. For example, compared with carbon, nitrogen is a more effective solid solution strengthening element and can promote grain refinement. Nitrogen is also a strong austenite-forming element, which can save nickel content and reduce the chance of ferrite and deformation martensite formation, greatly improving the material's resistance to pitting corrosion. In addition, harmful gases and smoke are inevitably produced during stainless steel welding, which directly affects environmental protection and the health of welders. At present, a flux-cored welding wire that is nickel-saving and environmentally friendly and used in additive manufacturing of LNG ultra-low temperature valves has not yet been developed. Summary of the invention

[0006] In view of the above-mentioned problems in the prior art, the main purpose of the present invention is to provide a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for the additive manufacturing of LNG ultra-low temperature valves. The chemical composition of the welding wire is rationally designed and regulated, and rare earth elements with low temperature resistance and corrosion resistance are introduced. The wire has good welding process performance and mechanical properties. It is applied to the additive manufacturing of LNG ultra-low temperature valves to significantly improve the accuracy of the deposition layer and the sealing and low-temperature toughness of the LNG valves.

[0007] Another object of the present invention is to provide a method for preparing the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of the above-mentioned LNG ultra-low temperature valve, which has a simple process.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] The invention provides a nickel-saving and environment-friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, comprising an outer skin and a flux core, wherein the outer skin adopts a low-carbon stainless steel strip; the flux core is composed of the following components in percentage by mass: C≤0.03%, Cr: 10.35%-11.25%, Ni: 11.50%-12.50%, N: 0.10%-0.20%, Mo: 0.30%-0.90%, Mn: 5.00%-8.00%, Si: 0.30%-0.90%, Pr: 0.01%-0.02%, Zn: 0.3%-1.1%, V: 0.2%-0.6%, and the balance is Fe and inevitable impurities.

[0010] Preferably, the low-carbon stainless steel strip used for the outer skin has a width of 8 to 14 mm and a thickness of 0.9 to 1.8 mm.

[0011] Preferably, the composition and mass percentage of the low-carbon stainless steel strip used in the outer skin are: C≤0.08%, Cr: 18%-20%, Ni: 8%-10.5%, N: 0.1%-0.2%, Mo: 0.3%-0.9%, Mn: 1.0%-2.0%, Si: 0.3%-0.75%, and the remainder is Fe and unavoidable impurities.

[0012] Preferably, the filling rate of the drug core is controlled at 15% to 20%.

[0013] Preferably, the particle size of the component of the drug core is 70-100 meshes.

[0014] Preferably, in the core, Mn is added in the form of electrolytic manganese, and C is added in the form of graphite.

[0015] Preferably, the component contents of the drug core satisfy the following requirements: the contents of the impurity elements S and P are both less than 0.003%.

[0016] Preferably, the component contents of the core satisfy the following requirement: the ratio of Cr / Ni is not greater than 0.9.

[0017] Preferably, the core consists of the following components in percentage by mass: C: 0.03%, Cr: 10.50%, Ni: 12.00%, N: 0.15%, Mo: 0.50%, Mn: 6.00%, Si: 0.50%, Pr: 0.015%, Zn: 1.00%, V: 0.3%, and the remainder is Fe and unavoidable impurities.

[0018] After the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves of the present invention is additively manufactured, the sealing performance of the obtained LNG ultra-low temperature valve is improved by nearly 20%, a small amount of Zn is used to replace toxic Cr, and the toxic smoke pollution generated during the welding process is greatly reduced compared with the traditional welding wire, and part of N is used to replace the precious Ni, which greatly reduces the cost of the welding wire. Its cladding metal has excellent low-temperature toughness, and excellent welding processability and mechanical properties. Its design idea is: in the flux core, the addition of a certain amount of C element can improve the strength of the weld, the addition of Si and Mn can deoxidize the weld and greatly improve the strength of the weld, the addition of Ni and N can improve the toughness of the weld, the addition of Mo improves the strength and hardness of the weld, and improves its wear resistance, the addition of Ti greatly promotes the refinement of the needle-shaped body, Cr and Zn improve the strength and hardness of the weld metal, the addition of V promotes grain refinement, improves density, and enhances strength, the addition of Pr promotes inclusion refinement and spheroidization, dehydrogenation and deoxidation, refines grains, and improves its low-temperature toughness. Further, the functions of each component are as follows:

[0019] C: The carbide formed by the reaction with other alloy elements in the weld overlay is a high-hardness hard phase, which plays a role in solid solution strengthening of the weld metal.

[0020] Cr: Solid solution strengthens the weld, promotes the formation of martensite, and improves strength and hardness.

[0021] Ni: expands the austenite phase region, the proportion of proeutectoid ferrite in the weld gradually decreases, while the acicular ferrite gradually increases, and the low-temperature toughness, weld hardness, yield strength and tensile strength are all improved.

[0022] N: Expands the austenite phase region and has a strengthening effect when dissolved in steel, improving tensile strength, yield strength and low-temperature toughness.

[0023] Mo: It has the effect of solid solution strengthening, improving the strength and rigidity of the weld metal, making the proportion of proeutectoid ferrite in the weld metal gradually decrease, while the proportion of acicular ferrite gradually increase. 0.6% Mo can make the weld obtain the best mechanical properties and reduce temper brittleness.

[0024] Mn: Deoxidation, improves the strength and hardness of the weld, increases the amount of acicular ferrite, and refines the acicular ferrite and coarse-grained areas of the weld.

[0025] Si: It can stabilize the arc. An appropriate amount of silicon can eliminate the influence of oxygen in the weld and improve the strength and hardness of the steel.

[0026] Zn: Improves the strength and hardness of the weld metal, while replacing Cr with a small amount of Zn to reduce welding pollution.

[0027] V: Increase the density of steel, promote grain refinement, improve its mechanical strength, increase tempering stability, and make carbides evenly distributed in the steel.

[0028] Pr: It has the functions of deoxidation, desulfurization, reducing inclusions, purifying weld structure and refining grains, promoting the refinement and spheroidization of inclusions, refining austenite grains, dividing austenite grains with needles, inhibiting the growth of upper bainite and martensite, and improving the low-temperature toughness of the weld.

[0029] The present invention also provides a method for preparing the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, comprising the following steps:

[0030] Step 1: Decontaminate and rust the low-carbon stainless steel strip and dry it;

[0031] Step 2: Weigh the raw materials of the drug core powder components according to the ratio, mix them evenly, and dry them at 220° C. for 3 hours to obtain the drug core powder;

[0032] Step 3: placing the low-carbon stainless steel strip on a tape unwinder of a welding wire forming machine, rolling the low-carbon stainless steel strip into a U-shaped groove through the pressing groove of the forming machine, filling the flux core powder obtained in step 2 into the U-shaped groove, and controlling the filling rate at 15% to 20%. After the U-shaped groove is rolled and closed, drawing is performed until the diameter meets the specification requirements, and the oil and moisture on the surface of the welding wire are removed by a degreasing machine and a drying machine respectively.

[0033] The present invention also provides the use of the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves in the welding, manufacturing or repair of liquefied natural gas low-temperature pipelines manufactured by electric arc, high-energy beam or composite heat source additive manufacturing.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves of the present invention has good arc stability, beautiful weld formation, and good strength of the weld metal, which can reach more than 544MPa. At the same time, it has good low-temperature impact toughness, and the low-temperature impact toughness at -196°C is greater than 40J.

[0036] 2. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves of the present invention adds an appropriate amount of rare earth element Pr, which is helpful for the refinement and spheroidization of inclusions, the refinement of austenite grains, the nucleation and growth of acicular ferrite preferentially within the austenite grain boundaries, the division of austenite grains, the inhibition of the growth of upper bainite and martensite, the formation of a complex phase division structure, and the improvement of the low-temperature toughness of the weld.

[0037] 3. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves of the present invention maximizes the low-temperature toughness of the weld by controlling Cr / Ni to be no greater than 0.9.

[0038] 4. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves of the present invention reduces the smoke pollution generated during welding to the greatest extent by using a small amount of Zn instead of Cr, which can be reduced by 15% to 20% compared with the same type of flux-cored welding wire. At the same time, N is used instead of expensive Ni, which reduces costs, saves Ni resources, and has excellent comprehensive performance. DETAILED DESCRIPTION

[0039] In order to more fully understand and demonstrate the technical solutions, purposes and advantages of the present invention, the technical effects produced by the present invention are further described in detail and completely in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all. It should be pointed out that for those of ordinary skill in the art, other embodiments obtained without departing from the concept of the present invention all belong to the protection scope of the present invention, and the present invention is specifically described in conjunction with the embodiments below.

[0040] Unless otherwise specified in the following examples, all reagents and materials used were commercially available.

[0041] In the following embodiments, the outer skin of the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves uses a low-carbon stainless steel strip with a width of 10 to 12 mm and a thickness of 0.6 to 2.0 mm. The composition and mass percentage of the low-carbon stainless steel strip are: C≤0.03%, Cr: 10.35 to 11.25%, Ni: 11.50 to 12.50%, N: 0.10% to 0.20%, Mo: 0.30% to 0.90%, Mn: 5.00% to 8.00%, Si: 0.30% to 0.90%, Pr: 0.01% to 0.02%, and the balance is Fe and unavoidable impurities.

[0042] Example 1

[0043] The present embodiment provides a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, wherein the flux core components and their mass percentages are: C: 0.03%, Cr: 10.35%, Ni: 11.50%, N: 0.10%, Mo: 0.40%, Mn: 5.00%, Si: 0.40%, Zn: 0.30%, V: 0.30%, Pr: 0.01%, and the balance is iron powder.

[0044] The flux-cored welding wire is prepared by the following method: weigh all the above raw materials and mix them evenly, dry them in a drying furnace at 220°C for 3 hours to obtain flux-cored powder. Place a low-carbon steel strip on the unwinding machine of a welding wire forming machine, roll the low-carbon stainless steel strip into a U-shaped groove through the groove pressing of the forming machine, and fill the dried flux-cored powder into the U-shaped groove with a filling rate of 17%. Then use a forming machine to roll the U-shaped groove closed, wipe it clean with anhydrous alcohol, and then draw it to a diameter of 1.4 mm. Finally, use a cotton cloth dipped in anhydrous alcohol to wipe off the oil stains on the welding wire to obtain the product.

[0045] Example 2

[0046] The present embodiment provides a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, wherein the flux core components and their mass percentages are: C: 0.02%, Cr: 10.48%, Ni: 12%, N: 0.10%, Mo: 0.50%, Mn: 6.00%, Si: 0.30%, Zn: 0.40%, V: 0.20%, Pr: 0.01%, and the remainder is iron powder.

[0047] The flux-cored welding wire is prepared by the following method: weigh all the above raw materials and mix them evenly, dry them in a drying furnace at 220°C for 3 hours to obtain flux-cored powder. Place a low-carbon steel strip on the unwinding machine of a welding wire forming machine, roll the low-carbon stainless steel strip into a U-shaped groove through the groove pressing of the forming machine, and fill the dried flux-cored powder into the U-shaped groove with a filling rate of 17%. Then use a forming machine to roll the U-shaped groove closed, wipe it clean with anhydrous alcohol, and then draw it to a diameter of 1.4 mm. Finally, use a cotton cloth dipped in anhydrous alcohol to wipe off the oil stains on the welding wire to obtain the product.

[0048] Example 3

[0049] The present embodiment provides a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, wherein the flux core components and their mass percentages are: C: 0.03%, Cr: 10.50%, Ni: 12.00%, N: 0.15%, Mo: 0.50%, Mn: 6.00%, Si: 0.50%, Zn: 1.00%, V: 0.30%, Pr: 0.015%, and the balance is iron powder.

[0050] The flux-cored welding wire is prepared by the following method: weigh all the above raw materials and mix them evenly, dry them in a drying furnace at 220°C for 3 hours to obtain flux-cored powder. Place a low-carbon steel strip on the unwinding machine of a welding wire forming machine, roll the low-carbon stainless steel strip into a U-shaped groove through the groove pressing of the forming machine, and fill the dried flux-cored powder into the U-shaped groove with a filling rate of 17%. Then use a forming machine to roll the U-shaped groove closed, wipe it clean with anhydrous alcohol, and then draw it to a diameter of 1.4 mm. Finally, use a cotton cloth dipped in anhydrous alcohol to wipe off the oil stains on the welding wire to obtain the product.

[0051] Example 4

[0052] The present embodiment provides a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, wherein the flux core components and their mass percentages are: C: 0.02%, Cr: 10.48%, Ni: 11.80%, N: 0.20%, Mo: 0.60%, Mn: 7.00%, Si: 0.30%, Zn: 0.40%, V: 0.20%, Pr: 0.01%, and the balance is iron powder.

[0053] The flux-cored welding wire is prepared by the following method: weigh all the above raw materials and mix them evenly, dry them in a drying furnace at 220°C for 3 hours to obtain flux-cored powder. Place a low-carbon steel strip on the unwinding machine of a welding wire forming machine, roll the low-carbon stainless steel strip into a U-shaped groove through the groove pressing of the forming machine, and fill the dried flux-cored powder into the U-shaped groove with a filling rate of 17%. Then use a forming machine to roll the U-shaped groove closed, wipe it clean with anhydrous alcohol, and then draw it to a diameter of 1.4 mm. Finally, use a cotton cloth dipped in anhydrous alcohol to wipe off the oil stains on the welding wire to obtain the product.

[0054] Example 5

[0055] The present embodiment provides a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, wherein the flux core components and their mass percentages are: C: 0.01%, Cr: 11.15%, Ni: 12.30%, N: 0.20%, Mo: 0.90%, Mn: 6.00%, Si: 0.40%, Zn: 0.70%, V: 0.40%, Pr: 0.02%, and the remainder is iron powder.

[0056] The flux-cored welding wire is prepared by the following method: weigh all the above raw materials and mix them evenly, dry them in a drying furnace at 220°C for 3 hours to obtain flux-cored powder. Place a low-carbon steel strip on the unwinding machine of a welding wire forming machine, roll the low-carbon stainless steel strip into a U-shaped groove through the groove pressing of the forming machine, and fill the dried flux-cored powder into the U-shaped groove with a filling rate of 17%. Then use a forming machine to roll the U-shaped groove closed, wipe it clean with anhydrous alcohol, and then draw it to a diameter of 1.4 mm. Finally, use a cotton cloth dipped in anhydrous alcohol to wipe off the oil stains on the welding wire to obtain the product.

[0057] Example 6

[0058] The present embodiment provides a nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, wherein the flux core components and their mass percentages are: C: 0.01%, Cr: 10.42%, Ni: 11.70%, N: 0.20%, Mo: 0.90%, Mn: 8.00%, Si: 0.90%, Zn: 1.10%, V: 0.60%, Pr: 0.02%, and the remainder is iron powder.

[0059] The flux-cored welding wire is prepared by the following method: weigh all the above raw materials and mix them evenly, dry them in a drying furnace at 220°C for 3 hours to obtain flux-cored powder. Place a low-carbon steel strip on the unwinding machine of a welding wire forming machine, roll the low-carbon stainless steel strip into a U-shaped groove through the groove pressing of the forming machine, and fill the dried flux-cored powder into the U-shaped groove with a filling rate of 17%. Then use a forming machine to roll the U-shaped groove closed, wipe it clean with anhydrous alcohol, and then draw it to a diameter of 1.4 mm. Finally, use a cotton cloth dipped in anhydrous alcohol to wipe off the oil stains on the welding wire to obtain the product.

[0060] The flux-cored welding wires prepared in Examples 1 to 6 were selected, and welding experiments were carried out with conventional nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wires (Comparative Example 1 and Comparative Example 2) on the market for additive manufacturing of LNG ultra-low temperature valves: metal-metallic gas shielded welding was adopted, the shielding welding gas was 80% Ar + 20% CO2, the base material was 304 / 304L austenitic stainless steel, and the welding process parameters were as shown in Table 1.

[0061] Table 1: Welding process parameters

[0062] Welding current / A Arc voltage / V Gas flow / (L / min) Welding speed / (cm / min) Preheating temperature / ℃ 240~280 24~26 24 18 150

[0063] After welding, the surfacing surface was polished and smoothed. The low-temperature toughness test was carried out according to the GB / T 2650-2008 weld joint impact test method. The impact specimen was taken at a distance of 2 mm from the upper surface of the weld joint. The impact notch was a Charpy V-notch with the center of the notch at the center of the weld. The test temperature was -190 °C and the blade of the pendulum impact was 2 mm. The comprehensive evaluation of the weld metal is shown in Table 2.

[0064] Table 2: Comprehensive evaluation of weld metal

[0065]

[0066] It can be seen from Table 2 that the comprehensive evaluations of Examples 1 to 6 are all greater than those of Comparative Examples 1 and 2. It can be concluded that the performance of the flux-cored welding wire of the present invention after additive manufacturing is better than that of the comparative examples, and meets the welding requirements of LNG ultra-low temperature valves. Adding an appropriate amount of rare earth elements can greatly improve the low-temperature toughness. By controlling the element ratio of the flux-cored welding wire, the welding fume and the chromium content in the welding fume can be greatly reduced.

[0067] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the protection scope of the present invention.

Claims

1. A nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves, characterized in that: including a sheath and a core; The outer skin is made of low-carbon stainless steel strip; The core consists of the following components in percentage by mass: C≤0.03%, Cr: 10.35%-11.25%, Ni: 11.50%-12.50%, N: 0.10%-0.20%, Mo: 0.30%-0.90%, Mn: 5.00%-8.00%, Si: 0.30%-0.90%, Pr: 0.01%-0.02%, Zn: 0.3%-1.1%, V: 0.2%-0.6%, and the balance is Fe and unavoidable impurities.

2. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to claim 1 is characterized in that: The low-carbon stainless steel strip used for the outer skin has a width of 8 to 14 mm and a thickness of 0.9 to 1.8 mm.

3. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to claim 1 is characterized in that: The composition and mass percentage of the low-carbon stainless steel strip used in the outer skin are: C≤0.08%, Cr: 18%-20%, Ni: 8%-10.5%, N: 0.1%-0.2%, Mo: 0.3%-0.9%, Mn: 1.0%-2.0%, Si: 0.3%-0.75%, and the remainder is Fe and unavoidable impurities.

4. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to claim 1 is characterized in that: The filling rate of the drug core is controlled at 15% to 20%.

5. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to claim 1 is characterized in that: The particle size of the component of the drug core is 70 to 100 mesh; And / or in the core, Mn is added in the form of electrolytic manganese, and C is added in the form of graphite; And / or the component contents of the core satisfy that the contents of the impurity elements S and P are both less than 0.003%.

6. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to claim 1 is characterized in that: The component contents of the core satisfy that the ratio of Cr / Ni is not greater than 0.

9.

7. The nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to claim 1 is characterized in that: The core consists of the following components in percentage by mass: C: 0.03%, Cr: 10.50%, Ni: 12.00%, N: 0.15%, Mo: 0.50%, Mn: 6.00%, Si: 0.50%, Pr: 0.015%, Zn: 1.00%, V: 0.3%, and the remainder is Fe and unavoidable impurities.

8. The method for preparing the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: Decontaminate and rust the low-carbon stainless steel strip and dry it; Step 2: Weigh the raw materials of the drug core powder components according to the ratio, mix them evenly, and dry them at 220° C. for 3 hours to obtain the drug core powder; Step 3: placing the low-carbon stainless steel strip on a tape unwinder of a welding wire forming machine, rolling the low-carbon stainless steel strip into a U-shaped groove through the pressing groove of the forming machine, filling the flux core powder obtained in step 2 into the U-shaped groove, and controlling the filling rate at 15% to 20%. After the U-shaped groove is rolled and closed, drawing is performed until the diameter meets the specification requirements, and the oil and moisture on the surface of the welding wire are removed by a degreasing machine and a drying machine respectively.

9. Application of the nickel-saving and environmentally friendly austenitic stainless steel flux-cored welding wire for additive manufacturing of LNG ultra-low temperature valves as described in any one of claims 1 to 7 in the welding, manufacturing or repair of liquefied natural gas cryogenic pipelines manufactured by arc, high-energy beam or composite heat source additive manufacturing.

Citation Information

Cited By

  • Austenitic stainless steel metal powder cored wire for additive manufacturing and preparation method thereof

    CN121798223A