Acid activated hard carbon negative electrode material and preparation method thereof, electrode plate and sodium ion battery
Through the preparation method of acid-activated hard carbon anode material, the problems of high cost of negative electrode materials and shortage of lithium resources of sodium ion batteries are solved, efficient sodium ion storage and battery performance improvement are achieved, and low-cost and easy to produce large-scale solutions plan.
Patent Information
- Application Number
- CN202410901445.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-12-06
AI Technical Summary
Existing sodium ion batteries face the challenge of large-scale preparation of low-cost negative electrode materials, and the shortage of lithium resources limits the development of electrochemical energy storage.
The preparation method of acid-activated hard carbon negative electrode material is adopted. By pickling and purification of biomass pre-carbonized raw materials and high concentration acid activation, ultramicropore structure is formed, and calcined at high temperature to close the pore structure, thereby improving the sodium storage space and Material properties.
It realizes a low-cost, easy to mass-produce hard carbon negative electrode material, improves the first-time Coulomb efficiency and reversible capacity, reduces the degree of graphitization and chaos of the material, and enhances the application prospects of the battery.
Smart Images

Figure CN119079971A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemical energy storage batteries, and in particular relates to an acid-activated hard carbon negative electrode material and a preparation method thereof, an electrode sheet and a sodium ion battery. Background Art
[0002] In recent years, with the continuous growth of population and the development of industrial activities in countries around the world, a series of environmental problems have been triggered. Today, the main energy resources are fossil fuels that produce greenhouse gases, which are the culprits for global warming and climate change. Although renewable energy sources (e.g., light, wind, and tides) have the advantages of being green and environmentally friendly, their current scale is still very limited compared to fossil fuels. Therefore, society's demand for renewable and clean energy is imminent, and this demand has promoted the widespread application of electrochemical energy storage devices in power conversion, storage, and use, covering electric vehicles, electronic products, smart grids, and large-scale energy storage. For this reason, lithium-ion batteries have become the most widely used electrochemical energy storage devices due to their low cost and high energy density.
[0003] However, with the increasing demand for batteries and the rapid development of the energy storage market, lithium resource shortage is becoming a serious limiting problem. In fact, the available lithium resources are limited; in addition, their distribution around the world is uneven. For these reasons, great efforts have been made in recent years to find alternatives to lithium-ion batteries. Sodium is a metallic element belonging to the same main group as lithium and has similar chemical properties, but sodium is more abundant in the earth's crust than lithium and is easier to obtain. These characteristics make sodium-ion batteries one of the most likely alternatives to lithium-ion batteries. At present, the main challenge facing the practical application of sodium-ion batteries is the large-scale preparation of low-cost negative electrode materials.
[0004] Carbon-based materials are considered to be the most promising negative electrode materials for sodium-ion batteries due to their structural diversity, good electrochemical properties and low cost. Among them, using waste biomass as a precursor to prepare negative electrode materials for sodium-ion batteries is a very good choice. A large amount of waste biomass materials, such as coconut shells, walnut shells, wood, etc., are used as precursors for preparing carbonaceous materials. Therefore, using waste biomass as a precursor for hard carbon negative electrode materials can not only reduce environmental pollution and alleviate the energy crisis, but also has good economic benefits and market prospects. Summary of the invention
[0005] The purpose of the present invention is to provide an acid-activated hard carbon negative electrode material and a preparation method thereof, an electrode sheet and a sodium ion battery in view of the deficiencies in the prior art.
[0006] The technical solution of the present invention is as follows: A first aspect of the present invention provides a method for preparing an acid-activated hard carbon negative electrode material, comprising the following steps: S1, acid-washing and purifying the biomass pre-carbonized raw material, crushing and sieving to obtain a hard carbon precursor material; S2, adding the hard carbon precursor material to an acid solution for acid activation, heating and stirring, filtering, washing and vacuum drying to obtain an acid-activated hard carbon precursor material; S3, placing the acid-activated hard carbon precursor material in a tubular furnace with an inert protective atmosphere, cooling it to room temperature after heat treatment, and preparing a hard carbon negative electrode material.
[0007] Preferably, in step S1, the biomass pre-carbonized raw material is at least one of coconut shell, walnut shell, wood, and bamboo pre-carbonized at 400-600° C. More preferably, it is at least one of coconut shell, walnut shell, wood, and bamboo pre-carbonized at 450-550° C.
[0008] Preferably, hydrochloric acid or sulfuric acid is used to carry out acid washing and purification on the biomass pre-carbonized raw material, and the concentration of the hydrochloric acid or sulfuric acid is 1 mol / L.
[0009] Preferably, in step S1, the ash content of the biomass pre-carbonized raw material after acid washing and purification is 0.1%-0.5%, and more preferably, 0.2%-0.4%.
[0010] Preferably, in step S2, the acid solution is concentrated nitric acid or concentrated sulfuric acid, and the concentration of concentrated nitric acid or concentrated sulfuric acid is 7.2-14.4 mol / L, more preferably 7.2-11 mol / L; the solid-liquid ratio of the hard carbon precursor material to the acid solution is 5%~35%, more preferably 10%~30%.
[0011] Preferably, in step S2, the heating temperature of the acid activation process is 40-80°C, more preferably 50-70°C; the stirring time of the acid activation process is 18-24 h, more preferably 20-22 h.
[0012] Preferably, in step S3, the heat treatment temperature is 1300~1500°C, more preferably 1350~1450°C; the heat treatment time is 2~4 h, more preferably 2.5~3.5 h; the heating rate is 1~5°C / min, more preferably 3~5°C / min; the inert protective atmosphere is high-purity argon or nitrogen.
[0013] The second aspect of the present invention provides an acid-activated hard carbon negative electrode material obtained by the above-mentioned preparation method.
[0014] The third aspect of the present invention provides a hard carbon negative electrode material electrode sheet, comprising the acid-activated hard carbon negative electrode material obtained by the above-mentioned preparation method or the acid-activated hard carbon negative electrode material as described above.
[0015] Preferably, the acid-activated hard carbon negative electrode material is mixed with a conductive agent, a binder and a solvent, coated on a metal substrate, and vacuum dried to obtain a hard carbon negative electrode material electrode sheet.
[0016] A fourth aspect of the present invention provides a sodium ion battery, comprising the above-mentioned hard carbon negative electrode material electrode sheet.
[0017] The present invention has at least one of the following beneficial effects: The present invention first uses low-concentration acid for acid washing and purification to react with metal oxide impurities in the biomass carbon precursor to remove metal oxide impurities; then uses high-concentration acid for acid activation, and the high-concentration acid reacts with carbon to produce an ultra-microporous structure. Therefore, compared with the prior art, the present invention forms more ultra-microporous structures through the chemical reaction of the hard carbon precursor with a higher concentration of acid; in the subsequent high-temperature calcination process, these ultra-micropores are thermally closed, thereby producing more closed-cell structures, which increases the sodium storage space of the hard carbon negative electrode material. In addition, the degree of graphitization of the hard carbon negative electrode material treated with acid activation is reduced, and the disorder of the microcrystalline structure is increased, which ultimately improves the first coulomb efficiency and reversible capacity of the hard carbon negative electrode material. The method provided by the present invention uses low-cost, widely available biomass such as coconut shells, walnut shells, wood and bamboo as raw materials, and has a simple preparation process, good product consistency, and is easy to achieve large-scale preparation, with huge future application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 The figure shows a scanning electron microscope image of the hard carbon precursor material after acid activation in Example 1 and high temperature treatment; Figure 2 Shown are nitrogen adsorption / desorption isotherms of the acid-activated hard carbon precursor material of Example 1 before and after high temperature treatment; Figure 3 The hard carbon material after acid activation and high temperature calcination in Example 1 is shown in 30 mAg -1 The charge and discharge curve of the first cycle at the current density of; Figure 4 Shown is an XRD comparison diagram of the hard carbon material after acid activation and high temperature calcination in Example 1 and Comparative Example 1; Figure 5 Shown is a Raman comparison chart of the hard carbon material after acid activation and high-temperature calcination in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0019] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0020] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples.
[0021] Example 1 An acid-activated hard carbon negative electrode material, the preparation method of which comprises the following steps: Weigh 20g of large-particle coconut shell carbon material respectively, pickle it with 1mol / L hydrochloric acid solution, and then dry it to obtain large-particle coconut shell carbon material after pickling. The large-particle coconut shell carbon material after pickling obtained in step (1) is crushed in a wall breaker for 20s, and passed through a 200-mesh sieve to obtain a hard carbon precursor material. Use a measuring cylinder to weigh 20ml of concentrated nitric acid solution with a concentration of 7.2mol / L and pour it into a beaker. Weigh 4g of the powder obtained in step (2) and add it to the beaker with a solid-liquid ratio of 20%. Then heat it in a water bath at 40°C and stir it for 24h. Then filter it and wash it with deionized water, and vacuum dry it at 60°C for 10h to obtain a hard carbon precursor after acid activation. (4) The hard carbon precursor obtained in step (3) is evenly ground in a mortar and placed in a corundum crucible, which is then placed in a tubular furnace filled with argon atmosphere. The temperature is raised to 1500°C at a rate of 3°C / min, kept at this temperature for 2 h, then cooled to 500°C at a rate of 4°C / min, and then naturally cooled to room temperature to obtain a hard carbon negative electrode material after acid activation.
[0022] A button battery, the preparation method of which comprises the following steps: The prepared acid-activated hard carbon negative electrode material, super-p conductive agent and polyvinylidene fluoride binder were mixed into a uniform slurry in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone was added. The mixture was evenly coated on the copper foil by coating, and then punched into a circular electrode sheet after drying, and vacuum dried at 120℃ for 12h. The prepared acid-activated hard carbon was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1M NaClO4 and EC / DMC (volume ratio of 1:1) were used as the electrolyte, and the glass fiber separator was used to assemble a button cell in a glove box.
[0023] Example 2 An acid-activated hard carbon negative electrode material, the preparation method of which comprises the following steps: (1) Weigh 15 g of large-particle walnut shell carbon material, wash it with 1 mol / L sulfuric acid solution, and then dry it to obtain large-particle walnut shell carbon material after acid washing.
[0024] (2) The large-particle walnut shell carbon material obtained after acid washing in step (1) is crushed in a wall breaking machine for 15 seconds and passed through a 200-mesh sieve to obtain a hard carbon precursor material.
[0025] (3) Use a measuring cylinder to weigh 20 ml of a concentrated nitric acid solution with a concentration of 10.08 mol / L and pour it into a beaker. Weigh 2 g of the powder obtained in step (2) and add it to the beaker. The solid-liquid ratio is 10%. Then heat it in a water bath at 40°C and stir it for 22 hours. Then filter it and wash it with deionized water. Then vacuum dry it at 60°C for 10 hours to obtain an acid-activated hard carbon precursor.
[0026] (4) The hard carbon precursor obtained in step (3) is evenly ground in a mortar and placed in a corundum crucible, which is then placed in a tubular furnace filled with argon atmosphere. The temperature is raised to 1300°C at a rate of 3°C / min, kept at this temperature for 2 h, then cooled to 500°C at a rate of 4°C / min, and then naturally cooled to room temperature to obtain an acid-activated hard carbon negative electrode material.
[0027] A button battery, the preparation method of which comprises the following steps: The prepared acid-activated hard carbon negative electrode material, super-p conductive agent and polyvinylidene fluoride binder were mixed into a uniform slurry in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone was added. The mixture was evenly coated on the copper foil by coating, and then punched into a circular electrode sheet after drying, and vacuum dried at 120℃ for 12h. The prepared acid-activated hard carbon was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1M NaClO4 and EC / DMC (volume ratio of 1:1) were used as the electrolyte, and the glass fiber separator was used to assemble a button cell in a glove box.
[0028] Example 3 An acid-activated hard carbon negative electrode material, the preparation method of which comprises the following steps: (1) Weigh 15 g of large-particle bamboo carbon material, wash it with 1 mol / L hydrochloric acid solution, and then dry it to obtain large-particle walnut shell carbon material after acid washing.
[0029] (2) The large-particle walnut shell carbon material obtained after acid washing in step (1) is crushed in a wall breaking machine for 15 seconds and passed through a 200-mesh sieve to obtain a hard carbon precursor material.
[0030] (3) Use a measuring cylinder to weigh 20 ml of a concentrated sulfuric acid solution with a concentration of 7.2 mol / L and pour it into a beaker. Weigh 6 g of the powder obtained in step (2) and add it to the beaker. The solid-liquid ratio is 30%. Then heat it in a water bath at 60°C and stir it for 20 hours. Then filter it and wash it with deionized water. Then vacuum dry it at 60°C for 10 hours to obtain an acid-activated hard carbon precursor.
[0031] (4) The hard carbon precursor obtained in step (3) is evenly ground in a mortar and placed in a corundum crucible, which is then placed in a tubular furnace filled with argon atmosphere. The temperature is raised to 1400°C at a rate of 5°C / min, kept at this temperature for 2 h, then cooled to 500°C at a rate of 4°C / min, and then naturally cooled to room temperature to obtain an acid-activated hard carbon negative electrode material.
[0032] A button battery, the preparation method of which comprises the following steps: The prepared acid-treated hard carbon negative electrode material, super-p conductive agent and polyvinylidene fluoride binder were mixed into a uniform slurry in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone was added. The mixture was evenly coated on the copper foil by coating, and then punched into a circular electrode sheet after drying, and vacuum dried at 120℃ for 12h. The prepared acid-activated hard carbon was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1M NaClO4 and EC / DMC (volume ratio of 1:1) were used as the electrolyte, and the glass fiber separator was used to assemble a button cell in a glove box.
[0033] Comparative Example 1 A method for preparing a hard carbon material comprises the following steps: The coconut shell hard carbon precursor was evenly ground in a mortar and placed in a corundum crucible, which was then placed in a tubular furnace filled with argon atmosphere. The temperature was raised to 1500 °C at a rate of 3 °C / min, kept for 2 h, then cooled to 500 °C at a rate of 4 °C / min, and then naturally cooled to room temperature to obtain a hard carbon negative electrode material.
[0034] A button battery, the preparation method of which comprises the following steps: The prepared hard carbon negative electrode material, super-p conductive agent and polyvinylidene fluoride binder were mixed into a uniform slurry in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone was added. The mixture was evenly coated on the copper foil by coating, and then punched into a circular electrode sheet after drying, and vacuum dried at 120℃ for 12h. The prepared acid-fired hard carbon was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1M NaClO4 and EC / DMC (volume ratio of 1:1) were used as the electrolyte, and the glass fiber separator was used to assemble the button battery in the glove box.
[0035] Comparative Example 2 A method for preparing a hard carbon material comprises the following steps: The walnut shell hard carbon precursor was evenly ground in a mortar and placed in a corundum crucible, which was then placed in a tubular furnace filled with argon atmosphere. The temperature was raised to 1300°C at a rate of 3°C / min, kept for 2 hours, then cooled to 500°C at a rate of 4°C / min, and then naturally cooled to room temperature to obtain a hard carbon negative electrode material.
[0036] A button battery, the preparation method of which comprises the following steps: The prepared hard carbon negative electrode material, super-p conductive agent and polyvinylidene fluoride binder were mixed into a uniform slurry in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone was added. The mixture was evenly coated on the copper foil by coating, and then punched into a circular electrode sheet after drying, and vacuum dried at 120℃ for 12h. The prepared acid-fired hard carbon was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1M NaClO4 and EC / DMC (volume ratio of 1:1) were used as the electrolyte, and the glass fiber separator was used to assemble the button battery in the glove box.
[0037] Comparative Example 3 A method for preparing a hard carbon material comprises the following steps: The bamboo hard carbon precursor was evenly ground in a mortar and placed in a corundum crucible, which was then placed in a tubular furnace filled with argon atmosphere. The temperature was raised to 1400°C at a rate of 5°C / min, kept for 2 hours, then cooled to 500°C at a rate of 4°C / min, and then naturally cooled to room temperature to obtain a hard carbon negative electrode material.
[0038] A button battery, the preparation method of which comprises the following steps: The prepared hard carbon negative electrode material, super-p conductive agent and polyvinylidene fluoride binder were mixed into a uniform slurry in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone was added. The mixture was evenly coated on the copper foil by coating, and then punched into a circular electrode sheet after drying, and vacuum dried at 120℃ for 12h. The prepared acid-fired hard carbon was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1M NaClO4 and EC / DMC (volume ratio of 1:1) were used as the electrolyte, and the glass fiber separator was used to assemble the button battery in the glove box.
[0039] Comparative Example 4 An acid-activated hard carbon negative electrode material, the processing steps are the same as those of Example 1, except that: the "concentrated nitric acid with a concentration of 7.2 mol / L" in step (3) is changed to "concentrated nitric acid with a concentration of 4 mol / L"; A button battery, the preparation method is the same as that of Example 1.
[0040] Comparative Example 5 An acid-activated hard carbon negative electrode material, the processing steps are the same as those of Example 1, except that: the "concentrated nitric acid with a concentration of 7.2 mol / L" in step (3) is changed to "concentrated nitric acid with a concentration of 20 mol / L"; A button battery, the preparation method is the same as that of Example 1.
[0041] test 1. The hard carbon precursor material treated in Example 1 was measured, and the results were as follows: Figures 1 to 5 shown.
[0042] Figure 1The figure shows the SEM image of the acid-activated hard carbon precursor material after high temperature treatment in Example 1. Figure 1 It can be seen that the material shape is mainly blocky and the particle sizes vary.
[0043] Figure 2 The nitrogen adsorption / desorption isotherms of the acid-activated hard carbon precursor material in Example 1 before and after high temperature treatment are shown. Figure 2 It can be seen that the specific surface area of the material after acid activation is significantly increased, which can explain the existence of ultrafine pores on the surface of the material after acid activation. After high-temperature calcination, these ultrafine pores on the surface are closed to form closed pores, resulting in a decrease in the specific surface area.
[0044] Figure 3 The hard carbon material after acid activation and high temperature calcination in Example 1 is shown in 30 mAg -1 The charge and discharge curve of the first cycle at a current density of Figure 3 It can be seen that the material charge and discharge curve is clearly divided into a slope section and a platform section, which is an obvious feature of the charge and discharge curve of hard carbon materials. From the curve, it can be seen that the material has considerable reversible capacity and high first-cycle coulombic efficiency.
[0045] Figure 4 The XRD comparison diagram of the hard carbon material after acid activation and high temperature calcination in Example 1 and Comparative Example 1 is shown. Figure 4 It can be seen that the (002) peak after acid activation shifts significantly toward the low angle direction, which indicates that the interlayer spacing and surface disorder of the material increase after acid activation.
[0046] Figure 5 The Raman comparison diagram of the hard carbon material after acid activation and high temperature calcination in Example 1 and Comparative Example 1 is shown. Figure 5 It can be seen that after acid activation, the area ratio of the D peak to the G peak of the material is D / I G Obviously greater than that of Comparative Example 1 D / I G , which indicates that the degree of graphitization on the material surface after acid activation is significantly reduced and the degree of disorder is significantly increased.
[0047] 2. The button batteries prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were subjected to the first coulombic efficiency and charge specific capacity tests, and the test methods were as follows: 0.1C discharge to 0.001V, 0.1C charge to 2V, and cycle 3 times; 0.5C discharge to 0.001V, 0.5C charge to 2V, and cycle 200 times.
[0048] The results are shown in Table 1: Table 1 It can be seen from Table 1 that the first coulombic efficiency of the button cells prepared in Examples 1-3 is improved compared with that in Comparative Examples 1-5.
[0049] Comparing Examples 1 to 3 with Comparative Example 1, it can be seen that the first coulombic efficiency and charging specific capacity of the button batteries prepared in Examples 1 to 3 are improved, which indicates that whether acid activation is performed and the acid concentration during the acid activation treatment will affect the first coulombic efficiency and reversible capacity of the button batteries. This is because, compared with Comparative Examples 1 to 5, the hard carbon materials in Examples 1 to 3 form an ultra-microporous structure on the surface after acid activation treatment, and these ultra-micropores are closed to form closed pores after high-temperature calcination, providing more active sites for sodium ions; at the same time, after acid activation, the degree of graphitization of the material surface is reduced and the disorder of the microcrystalline structure is increased, thereby improving the reversible capacity and first coulombic efficiency of the hard carbon negative electrode material.
[0050] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing an acid-activated hard carbon negative electrode material, characterized in that: The following steps are involved: S1, acid-washing and purifying the biomass pre-carbonized raw material, crushing and sieving to obtain a hard carbon precursor material; S2, adding the hard carbon precursor material to an acid solution for acid activation, heating and stirring, filtering, washing and vacuum drying to obtain an acid-activated hard carbon precursor material; S3, placing the acid-activated hard carbon precursor material in a tubular furnace with an inert protective atmosphere, cooling it to room temperature after heat treatment, and preparing a hard carbon negative electrode material.
2. The method for preparing an acid-activated hard carbon negative electrode material according to claim 1, characterized in that: In step S1, the biomass pre-carbonization raw material is at least one of coconut shells, walnut shells, wood, and bamboo that have been pre-carbonized at 400-600°C.
3. The method for preparing an acid-activated hard carbon negative electrode material according to claim 1, characterized in that: In step S1, hydrochloric acid or sulfuric acid is used to acid-wash and purify the biomass pre-carbonized raw material, and the ash content of the biomass pre-carbonized raw material after acid-washing and purification is 0.1%-0.5%.
4. The method for preparing an acid-activated hard carbon negative electrode material according to claim 1, characterized in that: In step S2, the acid solution is concentrated nitric acid or concentrated sulfuric acid, and the concentration of the concentrated nitric acid or concentrated sulfuric acid is 7.2-14.4 mol / L; the solid-liquid ratio of the hard carbon precursor material to the acid solution is 5%-35%.
5. The method for preparing an acid-activated hard carbon negative electrode material according to claim 1, characterized in that: In step S2, the heating temperature of the acid activation process is 40-80° C.; the stirring time of the acid activation process is 18-24 h.
6. The method for preparing an acid-activated hard carbon negative electrode material according to claim 1, characterized in that: In step S3, the heat treatment temperature is 1300-1500° C., the heat treatment time is 2-4 h, the heating rate is 1-5° C. / min, and the inert protective atmosphere is high-purity argon or nitrogen.
7. An acid-activated hard carbon negative electrode material obtained by the preparation method according to any one of claims 1 to 6.
8. A hard carbon negative electrode material electrode sheet, characterized in that it comprises the acid-activated hard carbon negative electrode material obtained by the preparation method according to any one of claims 1 to 6 or the acid-activated hard carbon negative electrode material according to claim 7.
9. A hard carbon negative electrode material electrode sheet according to claim 8, characterized in that the acid-activated hard carbon negative electrode material is mixed with a conductive agent, a binder and a solvent, coated on a metal substrate, and vacuum dried to obtain a hard carbon negative electrode material electrode sheet.
10. A sodium ion battery, characterized in that it comprises the hard carbon negative electrode material electrode sheet according to claim 9.
Citation Information
Patent Citations
Biomass hard carbon negative electrode material for sodium ion battery, preparing method and sodium ion battery
CN106299365A
Sodium-ion battery carbon negative electrode material prepared based on waste wood chips and preparation method thereof
CN113651307A
Hard carbon material, preparation method and application thereof, and sodium ion battery
CN114835104A
Biomass-based hard carbon material, preparation method and application thereof, and sodium / potassium ion battery
CN118231656A
Composite hard carbon material, preparation method therefor, and use thereof
WO2024109849A1
Cited By
Hard carbon material based on water-soluble organic acid as well as preparation method and application of hard carbon material
CN120518059A
Preparation method and application of cellulose-based hard carbon negative electrode material
CN120681745A