Preparation method of low-ash columnar coal-based activated carbon
By modifying activated carbon with micro-powdered ultrapure carbon and lignin, the pore structure of activated carbon is optimized, solving the problems of high activation difficulty, high ignition loss rate and high energy consumption in the preparation of columnar activated carbon from Taixi coal, and realizing efficient and low-consumption activated carbon production.
Patent Information
- Application Number
- CN202411276565.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-09-12
AI Technical Summary
When preparing columnar activated carbon using Taixi coal, due to its inherent characteristics, there are problems such as high activation difficulty, high loss on ignition rate, low yield, and high energy consumption.
By doping with ultrapure carbon and lignin, the pore structure of activated carbon is optimized. A network structure is formed by the polycondensation reaction of caprolactone and oxalic acid, which improves the adhesion of the powder and forms a polymer protective film after molding. The activation process is optimized to reduce the burn-off rate and energy consumption.
It effectively changed the pore distribution of Taixi coal-based activated carbon, improved the activation yield and efficiency, reduced production energy consumption, and the product had an ash content of ≤8%, strength of ≥96%, bulk density of 480±g/L, iodine value of ≥1000mg/g, CTC of ≥60%, dimethylacetamide capacity of ≥80%, and methylene blue of ≥220mg/g.
Abstract
Description
Technical Field
[0001] This invention relates to the field of activated carbon preparation technology, and more specifically, to a method for preparing low-ash columnar coal-based activated carbon. Background Technology
[0002] With increasingly stringent environmental protection requirements in my country, the types of air pollutants being controlled are increasing, and emission standards are becoming more stringent, making the need for industrial flue gas pollution control more urgent. Activated carbon flue gas purification technology has several significant advantages, including the combined removal of multiple pollutants, high desulfurization and denitrification efficiency, and the recoverability of sulfur resources, providing a comprehensive solution for air pollution control. Activated carbon, as an effective material for purifying flue gas and particulate matter, has been extensively researched and applied both domestically and internationally. Traditional activated carbon mainly uses raw coal, coal tar, and pitch as raw materials, and the production process mainly includes coal blending, grinding, mixing, molding, drying, carbonization, activation, screening, and packaging. Currently, most activated carbon manufacturers in China use high-quality coking coal, bituminous coal, semi-coke, or anthracite as raw materials.
[0003] Taixi coal is a high-quality coal characterized by three lows (low phosphorus, low ash, and low sulfur) and six highs (high calorific value, high lump coal rate, high resistivity, high chemical activity, high clean coal recovery rate, and high mechanical strength), making it one of the preferred raw materials for low-ash activated carbon. However, when using Taixi coal as a raw material to prepare columnar activated carbon, due to the inherent characteristics of Taixi coal and the relatively small specific surface area of columnar activated carbon, it suffers from application drawbacks such as difficulty in activation, high loss on ignition rate, and high production consumption per ton. Summary of the Invention
[0004] The technical problem to be solved by this invention is to provide a method for preparing low-ash columnar coal-based activated carbon. By blending and modifying Taixi coal powder as raw materials, the pore structure of activated carbon is optimized, which facilitates the contact activation of activated carbon with activating agents, reduces the loss on ignition rate, resource consumption, and energy consumption, and solves the problems of high activation difficulty, low yield, and high energy consumption that accompany the production of columnar activated carbon using high-quality coal in the activated carbon industry.
[0005] This invention provides a method for preparing low-ash columnar coal-based activated carbon, comprising the following steps:
[0006] (1) Powdering: The raw materials Taixi coal and ultrapure carbon are crushed by a crusher, then ground by a ball mill and screened to obtain Taixi coal powder and ultrapure carbon powder with a mesh size of less than 200 for later use.
[0007] (2) Ingredients: Weigh out 50-70 parts of Taixi coal, 30-50 parts of micronized ultrapure carbon, 33-34 parts of coal tar, 3-10 parts of lignin, 1-3 parts of caprolactone, 1-3 parts of oxalic acid, and 0.5-1 parts of triethylamine according to the following weight proportions: Taixi coal and micronized ultrapure carbon are initially mixed to obtain mixed powder A; lignin is dissolved in an appropriate amount of dimethylacetamide at a temperature of 40-60℃, and then coal tar is added and mixed for 5-10 minutes to obtain mixed solution B; oxalic acid and triethylamine are added to an appropriate amount of dimethylacetamide at a temperature of 40-60℃ and mixed evenly to obtain mixed solution C;
[0008] (3) Kneading and shaping: Add the mixed powder A to a kneader at a constant temperature of 60-100℃ and mix evenly. Then add the mixed liquid B and mix for 5-10 minutes. Then add the mixed liquid C and stir and knead for 10-20 minutes to obtain coal slime. Extrude the obtained coal slime into Ф1.8mm coal strips on a shaping device and spread them out to air dry naturally.
[0009] (4) Carbonization: Heat the carbonization furnace to 280-320℃, put the sample tube containing the coal strip obtained in step (3) into the carbonization furnace, heat it to 550-650℃ at a heating rate of 10℃ / min, hold it for 40-60min to complete the carbonization, cool it to obtain carbonized material, discharge it and weigh it.
[0010] (5) Activation: Heat the activation furnace to 550-650℃, put the sample tube containing the carbonized material obtained in step (4) into the activation furnace, heat it to 850-950℃ at a heating rate of 10℃ / min, then pass dimethylacetamide vapor at a flow rate of 10mL / min and keep it at the temperature for 60-100min to complete the activation.
[0011] (6) Discharge: Cut off the power supply, turn off the dimethylacetamide vapor, allow it to cool naturally, and after discharge, screen to remove the broken material and dust to obtain the activated carbon product.
[0012] Preferably, the mixture B in step (2) further includes 1 to 3 parts of caprolactone.
[0013] Preferably, in step (2), the ingredients are 60 parts of Taixi coal, 40 parts of ultrapure carbon powder, 33 parts of coal tar, 5 parts of lignin, 2 parts of caprolactone, 2 parts of oxalic acid, and 0.7 parts of triethylamine.
[0014] Preferably, the total amount of dimethylacetamide used in mixture B and mixture C in step (2) is 12 to 15 parts.
[0015] Preferably, the ultrapure carbon powder has the following characteristics: ash content 2-3 d%, volatile matter < 8 d%, sulfur 0.7-1 d%, particle size 15 (D90) μm, calorific value > 8000 kcal / kg, fixed carbon ≥ 90 FCd%, moisture content < 25 Mt%, and tap density 0.4-0.5 t / m³. 3 Specific surface area 55m² 2 / g;
[0016] The Taixi coal has an ash content ≤12% d, volatile matter <10% d, sulfur <1.3% d, calorific value >7000 kcal / kg, and moisture content <18% t.
[0017] Preferably, the temperature of the dimethylacetamide in step (2) is 50°C, and the temperature of the kneader in step (3) is 90°C.
[0018] Preferably, the coal tar in step (2) has a pitch content > 65.9%, a light oil content ≤ 2.46%, a heavy oil content ≤ 21.22%, a dimethylacetamide content ≤ 0.28%, and an ash content ≤ 0.06%.
[0019] Preferably, the carbonization process in step (4) is as follows: the carbonization furnace is heated to 300°C, a sample tube containing the coal strip obtained in step (3) is placed in the carbonization furnace, the temperature is raised to 600°C at a heating rate of 10°C / min, and then held for 45 minutes to complete the carbonization. The carbonized material is then cooled, discharged, and weighed.
[0020] Preferably, the activation process in step (5) is as follows: the activation furnace is heated to 600°C, the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 920°C at a heating rate of 10°C / min, and dimethylacetamide vapor is passed through at a flow rate of 10 mL / min, and the temperature is maintained for 90 min to complete the activation.
[0021] Working principle of the invention:
[0022] First, the micronized ultrapure carbon has the characteristics of low ash, low sulfur and high fixed carbon content. It is mixed with Taixi coal as the main raw material and the auxiliary materials are all organic materials. No activated carbon ash is generated at high temperature, and the prepared activated carbon has the characteristics of low ash.
[0023] Secondly, micronized ultrapure carbon contains a significant amount of cellulose and fibrous carbon, which readily forms a more disordered pore structure upon heating, facilitating activation and pore formation. This invention utilizes Taixi coal doped with micronized ultrapure carbon to prepare activated carbon, altering the pore structure of activated carbon products produced from single-coal sources. It reduces the number of micropores and increases the number of mesopores and macropores, forming a disordered pore structure and optimizing the activated carbon's pore structure. By optimizing the pore structure, water vapor can uniformly and rapidly react with the interior and surface of the carbon particles, reducing carbon loss on ignition, increasing activation yield and efficiency, and improving single-furnace output. This reduces energy consumption in activated carbon production, ultimately solving the problems of difficult activation and high energy consumption per ton of Taixi coal.
[0024] In addition, lignin contains active groups such as aromatic groups, phenolic hydroxyl groups, alcoholic hydroxyl groups, and carbonyl conjugated double bonds in its molecular structure, thus enabling it to undergo chemical reactions such as condensation polymerization or graft copolymerization. In step (3) of this invention, mixed powder A is added to a kneader and mixed evenly, and then mixed liquid B is added to it. The aromatic hydrocarbons and heterocyclic organic compounds in coal tar react with lignin to increase the active groups. Then, mixed liquid C is added to it and stirred and kneaded. Oxalic acid and lignin undergo a condensation reaction under the catalysis of triethylamine to form a network structure that coats the mixed powder. In addition, caprolactone contains a five-membered lactone ring and an alkyl side chain. The presence of the alkyl side chain gives caprolactone good solubility and compatibility in solvents. Since caprolactone contains a carbonyl group, it has certain reactivity and can undergo various chemical reactions such as esterification, addition, and nucleophilic substitution, which facilitates condensation polymerization with lignin to form a more complete network structure. The lignin network structure, together with the pitch in coal tar, improves the adhesion of the powder and forms a polymer protective film on the surface of the molded activated carbon, which can reduce the loss on ignition and prevent breakage during the activated carbon processing. At the same time, the condensate and the oily components of coal tar, light oil and heavy oil, decompose during carbonization, further enriching and optimizing the pore structure of the activated carbon.
[0025] The beneficial effects of this invention are as follows: This invention provides a method for preparing low-ash columnar coal-based activated carbon. The feasibility of coal blending was analyzed from the perspectives of coal quality and coal reactivity. Activated carbon is prepared by doping Taixi coal with ultrapure carbon powder. This coal blending technique alters the pore structure of activated carbon products from single-coal sources, effectively changing the pore distribution of Taixi coal-based activated carbon, reducing the number of micropores, increasing the number of medium and large pores, and forming a randomly arranged pore structure. By forming larger and randomly arranged pores, water vapor can uniformly and rapidly react with the interior and surface of the carbon particles, reducing carbon loss on ignition, and improving activation yield, efficiency, and single-furnace output. After key processes such as kneading, molding, carbonization, and activation, the yield of activated carbon is not less than 45%. Furthermore, lignin is utilized through a condensation reaction as a binder and protective film, improving the quality of the activated carbon. This invention solves the problems of difficult activation, small pore structure, and poor decolorization effect in the preparation of activated carbon from Taixi coal. The technical specifications of the product prepared by this invention are as follows: ash content ≤8%, strength ≥96%, bulk density 480±g / L, iodine value ≥1000mg / g, CTC ≥60%, dimethylacetamide capacity ≥80%, and methylene blue ≥220mg / g. Detailed Implementation
[0026] To make the technical solution of the present invention easier to understand, specific embodiments are now used to clearly and completely describe the technical solution of the present invention.
[0027] Example 1:
[0028] The method for preparing low-ash columnar coal-based activated carbon in this embodiment includes the following steps:
[0029] (1) Powdering: The raw materials Taixi coal and ultrapure carbon are crushed by a crusher, then ground by a ball mill and screened to obtain Taixi coal powder and ultrapure carbon powder with a mesh size of less than 200 for later use.
[0030] (2) Ingredients: Weigh out 50 parts of Taixi coal, 50 parts of micronized ultrapure carbon, 33 parts of coal tar, 10 parts of lignin, 1 part of oxalic acid and 1 part of triethylamine according to the following weight parts; mix Taixi coal and micronized ultrapure carbon to obtain mixed powder A; dissolve lignin in an appropriate amount of dimethylacetamide at 40℃, then add coal tar and mix for 10 min to obtain mixed solution B; add oxalic acid and triethylamine to an appropriate amount of dimethylacetamide at 40℃ and mix evenly to obtain mixed solution C;
[0031] (3) Kneading and shaping: Add the mixed powder A to a kneader at a constant temperature of 60℃ and mix evenly. Then add the mixed liquid B and mix for 10 minutes. Then add the mixed liquid C and stir and knead for 100 minutes to obtain coal slime. Extrude the obtained coal slime into Ф1.8mm coal strips on a shaping device and spread them out to air dry naturally.
[0032] (4) Carbonization: Heat the carbonization furnace to 280℃, put the sample tube containing the coal strip obtained in step (3) into the carbonization furnace, heat it to 550℃ at a heating rate of 10℃ / min, keep it at the temperature for 60min to complete the carbonization, cool it to obtain carbonized material, discharge it and weigh it.
[0033] (5) Activation: Heat the activation furnace to 550°C, put the sample tube containing the carbonized material obtained in step (4) into the activation furnace, heat it to 850°C at a heating rate of 10°C / min, and then pass dimethylacetamide vapor through it at a flow rate of 10 mL / min and keep it at the temperature for 100 min to complete the activation.
[0034] (6) Discharge: Cut off the power supply, turn off the dimethylacetamide vapor, allow it to cool naturally, and after discharge, screen to remove the broken material and dust to obtain the activated carbon product.
[0035] Example 2:
[0036] The method for preparing low-ash columnar coal-based activated carbon in this embodiment includes the following steps:
[0037] (1) Powdering: The raw materials Taixi coal and ultrapure carbon are crushed by a crusher, then ground by a ball mill and screened to obtain Taixi coal powder and ultrapure carbon powder with a mesh size of less than 200 for later use.
[0038] (2) Ingredients: Weigh out 60 parts of Taixi coal, 40 parts of micronized ultrapure carbon, 33 parts of coal tar, 5 parts of lignin, 2 parts of caprolactone, 2 parts of oxalic acid and 0.7 parts of triethylamine according to the following weight parts: Taixi coal and micronized ultrapure carbon are initially mixed to obtain mixed powder A; lignin and caprolactone are dissolved in an appropriate amount of dimethylacetamide at 50℃, and then coal tar is added and mixed for 8 minutes to obtain mixed solution B; oxalic acid and triethylamine are added to an appropriate amount of dimethylacetamide at 50℃ and mixed evenly to obtain mixed solution C;
[0039] (3) Kneading and shaping: Add the mixed powder A to a kneader at a constant temperature of 90℃ and mix evenly. Then add the mixed liquid B and mix for 8 minutes. Then add the mixed liquid C and stir and knead for 15 minutes to obtain coal slime. Extrude the obtained coal slime into Ф1.8mm coal strips on a shaping device and spread them out to air dry naturally.
[0040] (4) Carbonization: Heat the carbonization furnace to 300℃, put the sample tube containing the coal strip obtained in step (3) into the carbonization furnace, heat it to 600℃ at a heating rate of 10℃ / min, hold it for 45min to complete the carbonization, cool it to obtain carbonized material, discharge it and weigh it.
[0041] (5) Activation: Heat the activation furnace to 600℃, put the sample tube containing the carbonized material obtained in step (4) into the activation furnace, heat it to 920℃ at a heating rate of 10℃ / min, and then pass dimethylacetamide vapor at a flow rate of 10mL / min and keep it at the temperature for 90min to complete the activation.
[0042] (6) Discharge: Cut off the power supply, turn off the dimethylacetamide vapor, allow it to cool naturally, and after discharge, screen to remove the broken material and dust to obtain the activated carbon product.
[0043] Example 3:
[0044] The method for preparing low-ash columnar coal-based activated carbon in this embodiment includes the following steps:
[0045] (1) Powdering: The raw materials Taixi coal and ultrapure carbon are crushed by a crusher, then ground by a ball mill and screened to obtain Taixi coal powder and ultrapure carbon powder with a mesh size of less than 200 for later use.
[0046] (2) Ingredients: Weigh out 70 parts of Taixi coal, 30 parts of micronized ultrapure carbon, 34 parts of coal tar, 3 parts of lignin, 3 parts of caprolactone, 3 parts of oxalic acid and 0.5 parts of triethylamine according to the following weight parts: Taixi coal and micronized ultrapure carbon are initially mixed to obtain mixed powder A; lignin and caprolactone are dissolved in an appropriate amount of dimethylacetamide at 60℃, and then coal tar is added and mixed for 5 minutes to obtain mixed solution B; oxalic acid and triethylamine are added to an appropriate amount of dimethylacetamide at 60℃ and mixed evenly to obtain mixed solution C;
[0047] (3) Kneading and shaping: Add the mixed powder A to a kneader at a constant temperature of 100℃ and mix evenly. Then add the mixed liquid B and mix for 5 minutes. Then add the mixed liquid C and stir and knead for 20 minutes to obtain coal slime. Extrude the obtained coal slime into Ф1.8mm coal strips on a shaping device and spread them out to air dry naturally.
[0048] (4) Carbonization: Heat the carbonization furnace to 320°C, put the sample tube containing the coal strip obtained in step (3) into the carbonization furnace, heat it to 650°C at a heating rate of 10°C / min, keep it at the temperature for 40 minutes to complete the carbonization, cool it to obtain carbonized material, discharge it and weigh it.
[0049] (5) Activation: Heat the activation furnace to 650°C, put the sample tube containing the carbonized material obtained in step (4) into the activation furnace, heat it to 950°C at a heating rate of 10°C / min, and then pass dimethylacetamide vapor through it at a flow rate of 10 mL / min and keep it at the temperature for 60 min to complete the activation.
[0050] (6) Discharge: Cut off the power supply, turn off the dimethylacetamide vapor, allow it to cool naturally, and after discharge, screen to remove the broken material and dust to obtain the activated carbon product.
[0051] It should be noted that the embodiments described herein are only some embodiments of the present invention, and not all implementations of the present invention. These embodiments are merely illustrative and are intended only to provide a more intuitive and clear way to understand the content of the present invention, not to limit the technical solutions described herein. All other implementation methods that can be conceived by those skilled in the art without creative effort, as well as other simple substitutions and variations of the technical solutions of the present invention, without departing from the concept of the present invention, are within the protection scope of the present invention.
Claims
1. A method for preparing low-ash columnar coal-based activated carbon, characterized in that, Includes the following steps: (1) Powdering: The raw materials Taixi coal and ultrapure carbon are crushed by a crusher, then ground by a ball mill and screened to obtain Taixi coal powder and ultrapure carbon powder with a mesh size of less than 200 for later use. (2) Ingredients: Weigh out 50-70 parts of Taixi coal, 30-50 parts of micronized ultrapure carbon, 33-34 parts of coal tar, 3-10 parts of lignin, 1-3 parts of oxalic acid and 0.5-1 parts of triethylamine according to the following weight: Mix Taixi coal and micronized ultrapure carbon to obtain mixed powder A; Dissolve lignin in an appropriate amount of dimethylacetamide at a temperature of 40-60℃, and then add coal tar and mix for 5-10 minutes to obtain mixed solution B; Add oxalic acid and triethylamine to an appropriate amount of dimethylacetamide at a temperature of 40-60℃ and mix evenly to obtain mixed solution C; (3) Kneading and molding: Add the mixed powder A to a kneader at a constant temperature of 60~100℃ and mix evenly. Then add the mixed liquid B and mix for 5~10 minutes. Then add the mixed liquid C and stir and knead for 10~20 minutes to obtain coal slime. Extrude the obtained coal slime into Ф1.8mm coal strips on a molding device and spread them out to air dry naturally. (4) Carbonization: Heat the carbonization furnace to 280~320℃, put the sample tube containing the coal strip obtained in step (3) into the carbonization furnace, heat it to 550~650℃ at a heating rate of 10℃ / min, and hold it for 40~60min to complete the carbonization. Cool it to obtain the carbonized material, discharge it and weigh it. (5) Activation: Heat the activation furnace to 550~650℃, put the sample tube containing the carbonized material obtained in step (4) into the activation furnace, heat it to 850~950℃ at a heating rate of 10℃ / min, then pass dimethylacetamide vapor at a flow rate of 10mL / min and keep it at the temperature for 60~100min to complete the activation. (6) Discharge: Cut off the power supply, turn off the dimethylacetamide vapor, allow it to cool naturally, and after discharge, screen to remove the broken material and dust to obtain the activated carbon product.
2. The method for preparing low-ash columnar coal-based activated carbon as described in claim 1, characterized in that, The mixture B mentioned in step (2) also includes 1 to 3 parts of caprolactone.
3. The method for preparing low-ash columnar coal-based activated carbon as described in claim 2, characterized in that, The ingredients in step (2) are: 60 parts of Taixi coal, 40 parts of ultrapure carbon powder, 33 parts of coal tar, 5 parts of lignin, 2 parts of caprolactone, 2 parts of oxalic acid and 0.7 parts of triethylamine.
4. The method for preparing low-ash columnar coal-based activated carbon as described in claim 1, characterized in that, The total amount of dimethylacetamide used in mixtures B and C in step (2) is 12 to 15 parts.
5. The method for preparing low-ash columnar coal-based activated carbon as described in claim 1, characterized in that, The ultrapure carbon powder has an ash content of 2-3% (ad), volatile matter <8% (vd), sulfur of 0.7-1% (St, d), particle size D90 ≤ 15 μm, calorific value > 8000 kcal / kg, fixed carbon ≥ 90% (FCd), moisture content < 25% (Mt), and tap density of 0.4-0.5 t / m³. 3 Specific surface area 55m² 2 / g; The Taixi coal has an ash content of ≤12% and a volatile matter content of <10% and a sulfur content of <1.3% and a calorific value of >7000 kcal / kg, and a moisture content of <18%.
6. The method for preparing low-ash columnar coal-based activated carbon as described in claim 1, characterized in that, The temperature of the dimethylacetamide in step (2) is 50°C, and the temperature of the kneader in step (3) is 90°C.
7. The method for preparing low-ash columnar coal-based activated carbon as described in claim 1, characterized in that, The carbonization process described in step (4) is as follows: the carbonization furnace is heated to 300°C, the sample tube containing the coal strip obtained in step (3) is placed into the carbonization furnace, the temperature is raised to 600°C at a heating rate of 10°C / min, and then held for 45 minutes to complete the carbonization. The carbonized material is cooled and discharged and weighed.
8. The method for preparing low-ash columnar coal-based activated carbon as described in claim 1, characterized in that, The activation process in step (5) is as follows: the activation furnace is heated to 600°C, the sample tube containing the carbonized material obtained in step (4) is placed in the activation furnace, the temperature is raised to 920°C at a heating rate of 10°C / min, and dimethylacetamide vapor is passed through at a flow rate of 10 mL / min. The activation is completed after holding the temperature for 90 min.
Citation Information
Patent Citations
Columnar activated carbon based on coal pitch binders and preparation method of columnar activated carbon
CN102674341A
Additive for improving activated carbon microporous structure and method for preparing activated carbon by using additive
CN112299409A