Boron-doped niobium carbide nanosheet as well as preparation method and application thereof
Through the preparation of boron-doped niobium carbide nanosheets, the problem of insufficient resistance performance of niobium carbide materials was solved, and efficient preparation of memristors and simulation of biological synaptic behavior were achieved.
Patent Information
- Application Number
- CN202411193567.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Niobium carbide materials lack resistance properties and cannot be used to prepare memristors.
The preparation method of boron-doped niobium carbide nanosheets is adopted, and the aluminum niobium carbide is used as the precursor, and the intercalation is treated with tetramethylammonium hydroxide, and reacted with boric acid in the autoclave to form boron-doped niobium carbide nanosheets. Increase its conductivity and resistance.
Boron-doped niobium carbide nanosheets significantly improve the conductivity and memristor performance, and can exhibit simulated resistance characteristics under voltage changes, which are suitable for preparing memristors and simulating biological synaptic behavior.
Smart Images

Figure CN119079998A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano materials and components, and specifically relates to a boron-doped niobium carbide nanosheet and a preparation method and application thereof. Background Art
[0002] Memristor is a new type of component that can reflect the relationship between charge and magnetic flux. Unlike ordinary resistors, memristors are nonlinear resistors with memory functions. Even when the external voltage or current is removed, the device can still keep the stored information from being lost.
[0003] The resistive switching characteristic of a memristor refers to the characteristic that the resistance state of a memristor changes under the action of an external voltage. This characteristic usually allows the memristor to have multiple resistance states. The current-voltage (IV) characteristic curve measured by a memristor under the action of a DC voltage has a hysteresis phenomenon. According to the IV curve, memristors can be divided into two types: digital resistive switching memristors and analog resistive switching memristors. A digital resistive switching memristor refers to a device whose resistance changes suddenly, and the resistance values of high and low resistance generally differ by several orders of magnitude. An analog resistive switching memristor refers to a device whose resistance changes slowly, and the device has a series of adjustable continuous states. This resistive switching characteristic is highly similar to the working mechanism of neural synapses in biological bodies, so memristors with analog resistive switching behavior can be used to simulate biological synaptic behavior.
[0004] There is no report on the application of niobium carbide two-dimensional layered materials in memristors. 2 C) is a metal carbide with unique physical and chemical properties. Niobium carbide has a stable sodium chloride cubic crystal structure, which makes its internal electronic configuration and energy band structure relatively stable and not easy to change significantly under external conditions, thus limiting the variable range of its resistance value; at the same time, the electrons in niobium carbide are easy to flow and it is not easy to form barriers or traps that hinder electron transmission. Therefore, when external conditions change, the change in its resistance value is relatively small; in addition, under normal conditions, niobium carbide is not easy to undergo phase change, and its phase state remains relatively stable, so it does not have significant resistive switching performance. How to achieve the resistive switching performance of niobium carbide and apply it to the preparation of memristors is one of the technical problems that have not yet been solved. Summary of the invention
[0005] The problem to be solved by the present invention is to provide a boron-doped niobium carbide nanosheet and a preparation method and application thereof, so as to solve the problem that niobium carbide has no resistive switching performance and cannot be used to prepare a memristor.
[0006] The technical solution adopted to solve the technical problem is to provide a method for preparing boron-doped niobium carbide nanosheets, comprising the following steps:
[0007] (1) Preparing niobium carbide solid using niobium aluminum carbide as a precursor;
[0008] (2) dissolving niobium carbide solid in tetramethylammonium hydroxide solution, stirring and reacting, and then centrifuging to obtain niobium carbide precipitation;
[0009] (3) dissolving the niobium carbide precipitate in water and performing ultrasonic peeling, centrifuging to obtain the supernatant, and freeze-drying to obtain niobium carbide powder;
[0010] (4) dissolving niobium carbide powder in water to obtain solution A;
[0011] (5) dissolving boric acid in solution A and stirring to obtain suspension B;
[0012] (6) transferring the suspension B to an autoclave for reaction, taking it out, washing it and drying it to obtain boron-doped niobium carbide powder;
[0013] (7) Mechanically exfoliating the boron-doped niobium carbide powder and transferring it to a silicon dioxide substrate to obtain boron-doped niobium carbide nanosheets.
[0014] The beneficial effects of the above technical solution of the present invention are as follows: In the present invention, tetramethylammonium hydroxide (TMAOH) is used as an intercalation agent to 2 C) Intercalation treatment: Tetramethylammonium hydroxide can be inserted into the layered structure of niobium carbide, increasing the interlayer spacing and weakening the interlayer interaction. This intercalation treatment not only helps the stripping of niobium carbide in the subsequent steps, but also changes the physical and chemical properties of niobium carbide to a certain extent. Then it is dissolved in water for ultrasonic stripping, which can effectively strip the intercalated niobium carbide layered structure into thinner nanosheets or nanoparticles. Boron is used for doping, which is an acceptor doping. After boron doping, it replaces the C atoms in niobium carbide. Boron atoms have three valence electrons. When they form covalent bonds with the four surrounding carbon atoms, they still lack an electron and must take an electron from other carbon atoms to form a hole in niobium carbide. After the boron atoms accept the electrons, they form negatively charged boron ions, which generate electrostatic attraction with the positively charged holes. When boron-doped niobium carbide is used to prepare a memristor, when a voltage is applied to the memristor, the holes will break free from this binding force and jump to the valence band to form conductive holes. Therefore, the conductivity of boron-doped niobium carbide is enhanced and the memristive performance is improved.
[0015] Preferably, step (1) comprises the following steps: dissolving niobium aluminum carbide in a hydrofluoric acid solution and stirring for reaction, then centrifuging to obtain a precipitate, and vacuum drying to obtain a niobium carbide solid.
[0016] More preferably, the material-liquid ratio of niobium aluminum carbide to hydrofluoric acid solution is 1 g:15-25 mL; the stirring reaction temperature is 55-65° C., and the time is 46-50 h.
[0017] More preferably, the material-liquid ratio of niobium aluminum carbide to hydrofluoric acid solution is 1 g:20 mL; the stirring reaction temperature is 60° C. and the time is 48 h.
[0018] Preferably, in step (2), the solid-liquid ratio of niobium carbide solid to tetramethylammonium hydroxide solution is 1 g:15-25 mL; the stirring reaction temperature in step (2) is 25-30° C., and the time is 23-25 h.
[0019] More preferably, in step (2), the solid-liquid ratio of niobium carbide solid to tetramethylammonium hydroxide solution is 1 g:20 mL; and the stirring reaction temperature in step (2) is 25° C. and the reaction time is 24 h.
[0020] Preferably, the centrifugal speed in step (1), step (2) and step (3) is 3000-4000 r / min, and the time is 25-35 min.
[0021] More preferably, in step (3), the ultrasonic stripping power is 90-100W, the time is 25-35min, and the temperature is 25-30°C.
[0022] Preferably, the mass ratio of niobium carbide powder to boric acid in suspension B is 1:150-160.
[0023] More preferably, the mass ratio of niobium carbide powder to boric acid in suspension B is 1:154.58.
[0024] More preferably, the stirring in step (5) is magnetic stirring, the temperature is room temperature, and the time is 25 to 35 minutes.
[0025] Preferably, step (6) comprises the following steps: transferring the suspension B to a stainless steel high-pressure reactor lined with Teflon and reacting at 180-220° C. for 4.5-5.5 hours, taking it out and cooling it to room temperature, washing it with deionized water and anhydrous ethanol for 2-3 times respectively, and drying it at 65-75° C. for 11-13 hours to obtain boron-doped niobium carbide powder.
[0026] More preferably, step (6) comprises the following steps: transferring the suspension B to a stainless steel high-pressure reactor lined with Teflon and reacting at 200°C for 5 hours, cooling to room temperature after taking out, washing with deionized water and anhydrous ethanol for 3 times respectively, and drying at 70°C for 12 hours to obtain boron-doped niobium carbide powder.
[0027] The present invention also provides boron-doped niobium carbide nanosheets prepared by the above preparation method.
[0028] The present invention also provides the use of the boron-doped niobium carbide nanosheets in preparing a memristor device.
[0029] Preferably, the use of boron-doped niobium carbide nanosheets in the preparation of a memristor device comprises the following steps:
[0030] The boron-doped niobium carbide nanosheets are placed on a coating machine, and 1 to 2 drops of photoresist are added to the surface of the substrate, and the coating is performed twice, and the substrate is dried for standby use; a photolithography machine is used to perform photolithography, exposure and development on both ends of the boron-doped niobium carbide nanosheets, and the nanosheets are taken out and dried; the dried boron-doped niobium carbide nanosheets are placed on the stage of a sputtering instrument and the height of the stage is adjusted, and a high-purity Au target is used for sputtering 2 to 3 times, each time for 15 to 20 seconds; the nanosheets are then soaked in acetone for 10 to 15 minutes, washed with deionized water, ultrasonicated, and dried to obtain Au / B-Nb 2 C / Au memristor device.
[0031] The beneficial effect of the above technical solution of the present invention is: using inert metal Au as the electrode of the memristor device, compared with the commonly used Pt, Au has a lower work function, and its Schottky barrier in contact with the boron-doped niobium carbide nanosheets is small, so that the contact resistance is small.
[0032] More preferably, the two coating steps include the following steps: coating at 400-600 r / min for 15-25 s, and then coating at 900-1100 r / min for 25-35 s; exposure time is 10-20 s; and development time is 0.5-1.5 min.
[0033] The present invention has the following beneficial effects:
[0034] (1) The present invention enables niobium carbide, which originally does not have resistive switching properties, to exhibit good simulated resistive switching properties through boron doping. The prepared boron-doped niobium carbide can be well used to prepare memristor devices.
[0035] (2) The boron-doped niobium carbide nanosheets of the present invention are used in the preparation of memristor devices, exhibiting simulated resistive switching performance, can simulate biological synaptic behavior, and are further used in the fields of simulating artificial neural synapses and neuromorphic computing. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The Au / B-Nb prepared in Example 1 2 Optical microscope image of C / Au memristor device;
[0037] Figure 2 This is a SEM characterization image of the boron-doped niobium carbide nanosheets prepared in Example 1;
[0038] Figure 3 This is an EDS characterization image of the boron-doped niobium carbide nanosheets prepared in Example 1;
[0039] Figure 4 The Au / Nb prepared in Comparative Example 1 2IV test diagram of C / Au memristor device;
[0040] Figure 5 The Au / B-Nb prepared in Example 1 2 Simulated resistance switching performance of C / Au memristor device under positive voltage scan;
[0041] Figure 6 The Au / B-Nb prepared in Example 1 2 Simulated resistive switching performance of C / Au memristor device under negative voltage scan. DETAILED DESCRIPTION
[0042] The features and performance of the present invention are further described in detail below in conjunction with embodiments.
[0043] Example 1
[0044] A method for preparing boron-doped niobium carbide nanosheets comprises the following steps:
[0045] (1) Weighing 2 g of niobium aluminum carbide, adding it into a polytetrafluoroethylene beaker containing 40 mL of hydrofluoric acid solution, stirring and reacting at 60° C. for 48 h, then centrifuging at 3500 r / min for 30 min to obtain a precipitate, vacuum filtering the precipitate and vacuum drying at 70° C. to obtain niobium carbide solid;
[0046] (2) dissolving 1 g of niobium carbide solid in 20 mL of tetramethylammonium hydroxide solution at 25° C. for 24 h of stirring, and then centrifuging at 3500 r / min for 30 min to obtain niobium carbide precipitate;
[0047] (3) dissolving the niobium carbide precipitate in water and subjecting it to ultrasonic stripping at 100W and 25°C for 30 minutes, centrifuging it at 3500r / min for 30 minutes, taking the supernatant, and freeze-drying it to obtain niobium carbide powder;
[0048] (4) Weigh 0.01 g of niobium carbide powder and dissolve it in 25 mL of deionized water to obtain solution A;
[0049] (5) Weigh 1.5458 g of boric acid and dissolve it in solution A. Stir magnetically at room temperature for 30 min to obtain suspension B.
[0050] (6) Transfer the suspension B to a 100 mL stainless steel autoclave lined with Teflon, and then place the stainless steel autoclave in a 200° C. oven for reaction for 5 h. After being taken out, the suspension is naturally cooled to room temperature and transferred to a 100 mL beaker. The suspension is washed with deionized water and anhydrous ethanol for 3 times respectively, and dried in an oven at 70° C. for 12 h to obtain boron-doped niobium carbide powder.
[0051] (7) Mechanically exfoliating the boron-doped niobium carbide powder, and transferring the exfoliated boron-doped niobium carbide to the Si / SiO 2 On the substrate, boron-doped niobium carbide nanosheets are obtained.
[0052] This embodiment also includes boron-doped niobium carbide nanosheets prepared by the above method.
[0053] The boron-doped niobium carbide nanosheets prepared in this example are useful in the preparation of Au / B-Nb 2 The application of C / Au memristor device includes the following steps:
[0054] The substrate is Si / SiO 2 The boron-doped niobium carbide nanosheets are placed on a coating machine, and 1 to 2 drops of photoresist are added to the surface of the substrate, and the coating is spread at 500 r / min for 20 seconds, and then at 1000 r / min for 30 seconds, and dried at 45°C for 2 minutes for use; a photolithography machine is used to photolithography on both ends of the boron-doped niobium carbide nanosheets, and the exposure is 15 seconds; the exposed boron-doped niobium carbide nanosheets are immersed in a developer for 1 minute and then taken out, and dried at 45°C for 2 minutes; the dried boron-doped niobium carbide nanosheets are placed on the stage of the sputtering instrument and the height of the stage is adjusted, and a high-purity Au target is used for sputtering 3 times, each time for 20 seconds; then it is soaked in acetone for 10 minutes, washed with deionized water, ultrasonicated, and dried to obtain Au / B-Nb 2 C / Au memristor device.
[0055] Example 2
[0056] A method for preparing boron-doped niobium carbide nanosheets comprises the following steps:
[0057] (1) Weighing 2 g of niobium aluminum carbide, adding it into a polytetrafluoroethylene beaker containing 30 mL of hydrofluoric acid solution, stirring and reacting at 55° C. for 50 h, then centrifuging at 3000 r / min for 25 min to obtain a precipitate, vacuum filtering the precipitate and vacuum drying at 65° C. to obtain niobium carbide solid;
[0058] (2) dissolving 1 g of niobium carbide solid in 15 mL of tetramethylammonium hydroxide solution at 30° C. for 23 h under stirring, and then centrifuging at 3000 r / min for 25 min to obtain niobium carbide precipitate;
[0059] (3) dissolving the niobium carbide precipitate in water and subjecting it to ultrasonic stripping at 100W and 25°C for 30 minutes, centrifuging it at 3000r / min for 25 minutes, taking the supernatant, and freeze-drying it to obtain niobium carbide powder;
[0060] (4) Weigh 0.01 g of niobium carbide powder and dissolve it in 25 mL of deionized water to obtain solution A;
[0061] (5) Weigh 1.5 g of boric acid and dissolve it in solution A. Stir magnetically at room temperature for 25 min to obtain suspension B.
[0062] (6) Transfer the suspension B to a 100 mL stainless steel autoclave lined with Teflon, and then place the stainless steel autoclave in an oven at 180° C. for reaction for 5.5 h. After being taken out, the suspension is naturally cooled to room temperature and transferred to a 100 mL beaker. The suspension is washed with deionized water and anhydrous ethanol for three times, respectively, and dried in an oven at 65° C. for 13 h to obtain boron-doped niobium carbide powder.
[0063] (7) Mechanically exfoliating the boron-doped niobium carbide powder, and transferring the exfoliated boron-doped niobium carbide to the Si / SiO 2 On the substrate, boron-doped niobium carbide nanosheets are obtained.
[0064] This embodiment also includes boron-doped niobium carbide nanosheets prepared by the above method.
[0065] The boron-doped niobium carbide nanosheets prepared in this example are useful in the preparation of Au / B-Nb 2 The application of C / Au memristor device includes the following steps:
[0066] The substrate is SiO 2 The boron-doped niobium carbide nanosheets of / Si are placed on a coating machine, and 1-2 drops of photoresist are dropped on the surface of the substrate, and the coating is spread at 400r / min for 25s, and then at 1100r / min for 25s, and dried at 45°C for 2min for use; a photolithography machine is used to photolithograph the two ends of the boron-doped niobium carbide nanosheets, and the exposure is 15s; the exposed boron-doped niobium carbide nanosheets are immersed in a developer for 0.5min, then taken out, and dried at 45°C for 2min; the dried boron-doped niobium carbide nanosheets are placed on the stage of a sputtering instrument and the height of the stage is adjusted, and a high-purity Au target is used for sputtering 3 times, each time for 15s; then the Au / B-Nb nanosheets are soaked in acetone for 10min, washed with deionized water, ultrasonicated, and dried to obtain Au / B-Nb nanosheets. 2 C / Au memristor device.
[0067] Example 3
[0068] A method for preparing boron-doped niobium carbide nanosheets comprises the following steps:
[0069] (1) Weighing 2 g of niobium aluminum carbide, adding it into a polytetrafluoroethylene beaker containing 50 mL of hydrofluoric acid solution, stirring and reacting at 65° C. for 46 h, then centrifuging at 4000 r / min for 25 min to obtain a precipitate, vacuum filtering the precipitate and vacuum drying it at 70° C. to obtain niobium carbide solid;
[0070] (2) dissolving 1 g of niobium carbide solid in 25 mL of tetramethylammonium hydroxide solution at 30° C. for 25 h of stirring, and then centrifuging at 4000 r / min for 25 min to obtain niobium carbide precipitate;
[0071] (3) dissolving the niobium carbide precipitate in water and subjecting it to ultrasonic stripping at 100W and 25°C for 30 minutes, centrifuging it at 4000r / min for 25 minutes, taking the supernatant, and freeze-drying it to obtain niobium carbide powder;
[0072] (4) Weigh 0.01 g of niobium carbide powder and dissolve it in 25 mL of deionized water to obtain solution A;
[0073] (5) Weigh 1.6 g of boric acid and dissolve it in solution A. Stir magnetically at room temperature for 35 min to obtain suspension B.
[0074] (6) Transfer the suspension B to a 100 mL stainless steel autoclave lined with Teflon, and then place the stainless steel autoclave in an oven at 220° C. for reaction for 4.5 h. After being taken out, the suspension is naturally cooled to room temperature and transferred to a 100 mL beaker. The suspension is washed with deionized water and anhydrous ethanol for three times, respectively, and dried in an oven at 75° C. for 11 h to obtain boron-doped niobium carbide powder.
[0075] (7) Mechanically exfoliating the boron-doped niobium carbide powder, and transferring the exfoliated boron-doped niobium carbide to the Si / SiO 2 On the substrate, boron-doped niobium carbide nanosheets are obtained.
[0076] This embodiment also includes boron-doped niobium carbide nanosheets prepared by the above method.
[0077] The boron-doped niobium carbide nanosheets prepared in this example are useful in the preparation of Au / B-Nb 2 The application of C / Au memristor device includes the following steps:
[0078] The substrate is Si / SiO 2 The boron-doped niobium carbide nanosheets are placed on a coating machine, and 1 to 2 drops of photoresist are added to the surface of the substrate. The coating is spread at 600 r / min for 15 seconds, and then at 900 r / min for 35 seconds, and then dried at 45°C for 2 minutes for use; a photolithography machine is used to photolithography at both ends of the boron-doped niobium carbide nanosheets, and the exposure is 20 seconds; the exposed boron-doped niobium carbide nanosheets are immersed in a developer for 1.5 minutes, then taken out, and dried at 45°C for 2 minutes; the dried boron-doped niobium carbide nanosheets are placed on the stage of the sputtering instrument and the height of the stage is adjusted, and a high-purity Au target is used for sputtering 3 times, each time for 20 seconds; then it is soaked in acetone for 15 minutes, washed with deionized water, ultrasonicated, and dried to obtain Au / B-Nb 2 C / Au memristor device.
[0079] Comparative Example 1
[0080] A method for preparing niobium carbide nanosheets comprises the following steps:
[0081] (1) Weighing 2 g of niobium aluminum carbide, adding it into a polytetrafluoroethylene beaker containing 40 mL of hydrofluoric acid solution, stirring and reacting at 60° C. for 48 h, then centrifuging at 3500 r / min for 30 min to obtain a precipitate, vacuum filtering the precipitate and vacuum drying at 70° C. to obtain niobium carbide solid;
[0082] (2) dissolving 1 g of niobium carbide solid in 20 mL of tetramethylammonium hydroxide solution at 25° C. for 24 h of stirring, and then centrifuging at 3500 r / min for 30 min to obtain niobium carbide precipitate;
[0083] (3) dissolving the niobium carbide precipitate in water and subjecting it to ultrasonic stripping at 100W and 25°C for 30 minutes, centrifuging it at 3500r / min for 30 minutes, taking the supernatant, and freeze-drying it to obtain niobium carbide powder;
[0084] (4) Mechanically exfoliating the niobium carbide powder and transferring the exfoliated niobium carbide powder to a Si / SiO 2 On the substrate, niobium carbide nanosheets are obtained.
[0085] This comparative example also includes niobium carbide nanosheets prepared by the above method.
[0086] The niobium carbide nanosheets prepared in this example are used in the preparation of Au / Nb 2 The application in the C / Au memristor device has the same steps as those in Example 1.
[0087] Experimental example
[0088] 1. Boron-doped niobium carbide nanosheets Au / B-Nb 2 C / Au memristor device for structural analysis, the structure is as follows Figures 1 to 3 shown.
[0089] from Figure 1 It can be seen that the Au / B-Nb 2 The C / Au memristor device presents a two-dimensional layered structure; Figure 2 It can be seen from the SEM characterization diagram that the present application successfully prepared boron-doped niobium carbide nanosheets, and the boron-doped niobium carbide nanosheets are specifically a two-dimensional layered structure; Figure 3 Niobium (Nb), carbon (C) and boron (B) elements can be observed in the EDS image, indicating that the boron element has been successfully doped into the boron-doped niobium carbide nanosheets prepared in Example 1.
[0090] 2. The performance of the memristor device obtained in Example 1 and Comparative Example 1 was measured. The results are as follows: Figures 4 to 6 shown.
[0091] from Figures 4 to 6 It can be seen that the Au / Nb 2 The C / Au memristor device has almost no resistance switching performance; while the Au / B-Nb 2 The C / Au memristor device exhibits good analog resistive switching performance under both positive and negative voltages, and can be subsequently applied to the simulation of biological synapses.
[0092] The present invention has been described according to the above embodiments. It should be understood that the above embodiments do not limit the present invention in any form. Any technical solutions obtained by equivalent replacement or equivalent transformation shall fall within the scope of the present invention.
Claims
1. A method for preparing boron-doped niobium carbide nanosheets, characterized in that: The following steps are involved: (1) Preparing niobium carbide solid using niobium aluminum carbide as a precursor; (2) dissolving niobium carbide solid in tetramethylammonium hydroxide solution, stirring and reacting, and then centrifuging to obtain niobium carbide precipitation; (3) dissolving the niobium carbide precipitate in water and performing ultrasonic peeling, centrifuging to obtain the supernatant, and freeze-drying to obtain niobium carbide powder; (4) dissolving niobium carbide powder in water to obtain solution A; (5) dissolving boric acid in solution A and stirring to obtain suspension B; (6) transferring the suspension B to an autoclave for reaction, taking it out, washing it and drying it to obtain boron-doped niobium carbide powder; (7) Mechanically exfoliating the boron-doped niobium carbide powder and transferring it to a silicon dioxide substrate to obtain boron-doped niobium carbide nanosheets.
2. The method for preparing boron-doped niobium carbide nanosheets according to claim 1, characterized in that: The step (1) comprises the following steps: dissolving niobium aluminum carbide in a hydrofluoric acid solution for stirring reaction, then centrifuging to obtain a precipitate, and vacuum drying to obtain a niobium carbide solid.
3. The method for preparing boron-doped niobium carbide nanosheets according to claim 2, characterized in that: The material-liquid ratio of the niobium aluminum carbide to the hydrofluoric acid solution is 1 g:15-25 mL; the temperature of the stirring reaction is 55-65° C., and the time is 46-50 hours.
4. The method for preparing boron-doped niobium carbide nanosheets according to claim 1, characterized in that: In the step (2), the solid-liquid ratio of niobium carbide solid to tetramethylammonium hydroxide solution is 1 g:15-25 mL; the stirring reaction temperature in the step (2) is 25-30° C. and the time is 23-25 h.
5. The method for preparing boron-doped niobium carbide nanosheets according to claim 1, characterized in that: The mass ratio of niobium carbide powder to boric acid in the suspension B is 1:150-160.
6. The method for preparing boron-doped niobium carbide nanosheets according to claim 1, characterized in that: The step (6) comprises the following steps: transferring the suspension B to a stainless steel high-pressure reactor lined with Teflon, reacting at 180-220° C. for 4.5-5.5 hours, cooling to room temperature after taking out, washing with deionized water and anhydrous ethanol for 2-3 times respectively, and drying at 65-75° C. for 11-13 hours to obtain boron-doped niobium carbide powder.
7. Boron-doped niobium carbide nanosheets prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the boron-doped niobium carbide nanosheets according to claim 7 in the preparation of a memristor device.
9. The use according to claim 8, characterized in that The following steps are involved: The boron-doped niobium carbide nanosheets are placed on a coating machine, and 1 to 2 drops of photoresist are added to the surface of the substrate, and the coating is performed twice, and the substrate is dried for use; a photolithography machine is used to perform photolithography, exposure and development on both ends of the boron-doped niobium carbide nanosheets, and the nanosheets are taken out and dried; the dried boron-doped niobium carbide nanosheets are placed on the stage of a sputtering instrument and the height of the stage is adjusted, and the nanosheets are sputtered 2 to 3 times with a high-purity Au target material, each time for 15 to 20 seconds; the nanosheets are then soaked in acetone for 10 to 15 minutes, washed with deionized water, ultrasonicated, and dried to obtain an Au / B-Nb2C / Au memristor device.
10. The use according to claim 9, characterized in that The two times of coating include the following steps: coating at 400-600 r / min for 15-25 s, and then coating at 900-1100 r / min for 25-35 s; the exposure time is 10-20 s; and the development time is 0.5-1.5 min.