Nonlinear optical crystal materials TFEOC and TFPOC as well as preparation method and application thereof
By introducing polyhalogenic substituents and extending π conjugated chains into nonlinear chalkone crystals, TFEOC and TFPOC crystals were designed, and photochemical synthesis was combined with a bifunctional catalyst, which solved the problem of low terahertz output intensity in the prior art. , realizes broadband terahertz output and efficient second harmonic generation, expanding its application potential in the fields of optoelectronics and communications.
Patent Information
- Application Number
- CN202411198333.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The output intensity of existing nonlinear chalkone crystals in the terahertz band is low, their performance needs to be improved, and they lack the potential for wide application in the fields of optoelectronics and communications.
By introducing multihalogenous substituents and extending π conjugated chains, two nonlinear optical crystal materials, TFEOC and TFPOC, were designed, using D-π-A-π-A molecular configuration and a dual-function catalyst combined with a metal organic framework catalyst. Photochemical synthesis, extending the alkyl chain length to optimize nonlinear optical properties and terahertz output.
It realizes broadband terahertz output, improves the second harmonic generation efficiency, broadens the application potential of crystals in the terahertz band, and reduces thermal energy demand through photochemical synthesis and reduces environmental burden.
Smart Images

Figure CN119080599A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional crystal materials, and relates to nonlinear optical crystal materials TFEOC and TFPOC, and a preparation method and application thereof. Background Art
[0002] Organic nonlinear optical (NLO) compounds are of great value in the field of new material research and development, and their unique optical properties make them the focus of attention. These compounds have many advantages, such as easy crystal processing, low manufacturing cost and high laser damage threshold. In particular, organic nonlinear crystals with non-centrosymmetric structures have shown great potential in generating terahertz waves.
[0003] The chalcone structure, consisting of an enone group bridging two aromatic rings, is considered as a potential nonlinear optical (NLO) material due to its substituent substitution and extended π-electron conjugation system. By adjusting the electron donor and acceptor groups, the internal arrangement of the molecule can be optimized and crystallization in non-centrosymmetric space groups can be promoted. Trifluoromethyl, as a polyhalogen group, has been shown to have a unique contribution to the NLO properties of aniline and chalcone structures. The introduction of polyhalogen groups helps to form more internal hydrogen bonds, making the internal arrangement more consistent and enhancing nonlinearity. However, according to the literature, the only nonlinear chalcone crystal with terahertz (THz) output is TMOAT (C 16 H 16 O4S, Pna21), but its output intensity is low and its performance needs to be improved. Therefore, it is of great significance to explore more chalcone-based high-performance nonlinear terahertz optical crystals. Summary of the invention
[0004] The present invention aims to overcome the shortcomings of the prior art, study the crystal design strategy for optimizing nonlinear and terahertz performance, and provide a nonlinear optical crystal material and its preparation method and application by extending the alkyl chain length. By introducing polyhalogenated substituents and extending the π conjugated chain, not only the nonlinear optical performance of the crystal is enhanced, but also its application potential in the terahertz band is further broadened. In particular, TFEOC and TFPOC crystals have achieved broadband terahertz output through optical rectification for the first time. These characteristics make these crystals have broader application prospects in the future optoelectronics and communications fields.
[0005] The present invention provides a nonlinear optical crystal material, wherein the crystal material is two chalcone crystals: TFEOC and TFPOC, and the chemical formulas are C 18 H 15 F3O2 and C 19 H 17F3O2 is mainly composed of the condensation reaction of trifluoromethylacetophenone and ethoxybenzaldehyde or propoxybenzaldehyde. Both crystals are molecular crystal structures with a molecular configuration of D-π-A-π-A. The structural formulas are shown in (Ⅰ) and (Ⅱ) below:
[0006]
[0007] The TFEOC crystal belongs to the orthorhombic system, the space group is Pca21, the crystal shape is hexagonal, and its unit cell parameters are: Z = 4; further, Z=4; preferably, Z=4; more preferably, a / b=1.1718, b / c=0.1752, c / a=4.8702, Z = 4;
[0008] The TFPOC crystal belongs to the monoclinic system, the space group is Pc, the crystal shape is an irregular trapezoid, and its unit cell parameters are: β=94.0-94.2, Z = 2; further, β=94.01-94.14, Z=2; preferably, β=94.011-94.098, Z=2; more preferably, β=94.009-94.019°, Z = 2;
[0009] Crystalline polarity axis and first-order hyperpolarizability β of TFEOC max The angle between the directions is 29-31 degrees, preferably 30.0 degrees; the crystal polarity axis of TFPOC and the first-order hyperpolarizability β max The angle between the directions is 33-34 degrees, preferably 33.5 degrees;
[0010] The static first hyperpolarizabilities (β) of TFEOC and TFPOC molecules were calculated by Gaussian 16w using the 6-311G(d) basis set and B3LYP functional, and were 50.014×10 -30 esu and 41.616×10 -30 esu;
[0011] The maximum symmetric nonlinear optical susceptibilities of TFEOC and TFPOC molecules calculated by GGA-PBE functional are -13.819960 pm / V and 11.762210 pm / V, respectively;
[0012] The HOMO-LUMO energy gaps of TFEOC and TFPOC molecules were calculated using the 6-311G(d) basis set and B3LYP functional, and were 3.74 eV and 3.95 eV, respectively;
[0013] The theoretical band gap sizes of TFEOC crystal and TFPOC crystal were determined by GGA-PBE functional, which were 1.949 eV and 2.247 eV, respectively;
[0014] Using DSTMS as the electro-optical detection crystal, the THz spectrum widths of TFEOC crystal and TFPOC crystal were 0.3-13THz and 0.3-18THz respectively.
[0015] The melting points of TFEOC crystal and TFPOC crystal measured under nitrogen range were 121.6℃ and 103.3℃ respectively;
[0016] The dielectric constants of TFEOC crystals and TFPOC crystals at 1KHz, 10KHz, 100KHz and 1MHz are stable between 9.4-9.7 and 4.1-4.3 respectively as the temperature changes;
[0017] The cutoff wavelength of the TFEOC crystal and the TFPOC crystal is between 420-430 nm. More preferably, the cutoff wavelength of the two crystals is 425 nm, and they exhibit a high transmittance in the range of 600-1350 nm.
[0018] The experimental band gap sizes of TFEOC crystal and TFPOC crystal were determined by Tauc formula method, and the ranges were 2.80-2.83 eV and 2.75-2.77 eV, respectively; more preferably, they were 2.81 eV and 2.76 eV, respectively;
[0019] The second harmonic generation (SHG) efficiency of TFEOC and TFPOC crystals is 4.32 times and 8.72 times that of KDP crystals, respectively.
[0020] In the present invention, one end of the nonlinear optical crystal molecule is an electron accepting group of 4-(trifluoromethyl)acetophenone, and the other end of the electron donor is extended by introducing p-ethoxybenzaldehyde or p-propoxybenzaldehyde to extend the length of the alkyl chain. The two are connected by a π conjugated system, and this structural design improves the second-order nonlinear polarizability of the molecule, and the method of extending the length of the alkyl chain and optimizing the spatial arrangement optimizes the spectrum width range of the crystal THz output and makes the crystal have a higher SHG efficiency.
[0021] In the present invention, the application of trifluoromethylphenyl ketone (-CF3) helps to construct a new chalcone structure. The strong electron-withdrawing group (-CF3) can promote charge transfer within the molecule, thereby inducing greater polarization and excellent high-order nonlinear optical (NLO) response. By introducing a highly electronegative trifluoromethyl group into the molecular structure, the introduction of a stronger hydrogen bond acceptor site is achieved compared to the non-polar methyl group used previously. The characteristics of the polyhalogen group change the spatial arrangement within the molecule, which is conducive to the formation of a non-centrosymmetric crystal structure.
[0022] In terms of electron donors, the alkyl chain length was extended by introducing p-ethoxybenzaldehyde and p-propoxybenzaldehyde, and its effect on the intramolecular nonlinear optical (NLO) performance was analyzed. When the electronic interaction between the donor and the acceptor is significant enough, the strength of the transition matrix elements related to the charge transfer transition can be maximized, thereby enhancing the NLO response.
[0023] The present invention provides a method for preparing the above-mentioned nonlinear optical crystal material, which specifically comprises the following steps:
[0024] (1) dissolving p-ethoxybenzaldehyde or p-propoxybenzaldehyde in a solvent at a ratio of 0.1 mol:100 ml;
[0025] (2) dissolving p-trifluoromethylacetophenone in a solvent at a ratio of 0.1 mol:100 ml;
[0026] The solvent in step (1) and step (2) is selected from acetonitrile, ethanol or water, and the solvent should be compatible with the MOFs catalyst and help dissolve the reactants;
[0027] (3) mixing the solutions obtained in step (1) and step (2), adding a suitable MOFs catalyst to the solution and ensuring uniform distribution; the amount of the catalyst should be optimized according to the molar amount of the reactants and the catalytic activity, preferably 0.5-10% of the total molar amount of the reactants p-ethoxybenzaldehyde or p-propoxybenzaldehyde and p-trifluoromethylacetophenone; the MOFs catalyst is specifically selected from PCN-222 (porphyrin-based zirconium metal organic framework);
[0028] (4) Place the solution under a light source to carry out a photochemical reaction; the wavelength and intensity of the light source should match the light absorption characteristics of the MOFs catalyst. In order to maximize the light absorption efficiency of PCN-222, select blue light with a wavelength in the range of 420-450nm or green light in the range of 500-600nm. The photon energy in this wavelength range is sufficient to excite the electrons in the porphyrin ligand and promote the photocatalytic reaction; the light source is preferably a visible light LED lamp, and the temperature of the photochemical reaction is room temperature or slightly above room temperature, preferably 25-50°C, to prevent overheating and side reactions; the reaction rate is controlled by adjusting the light intensity, the amount of catalyst used, and sampling and analyzing the reaction progress to ensure that the experiment achieves the expected product yield and selectivity; for the PCN-222 catalyst, maintain a medium reaction rate to obtain the best chalcone synthesis effect; the selected illumination reaction time is controlled between 2 and 8 hours;
[0029] (5) After the reaction is completed, the reaction mixture is extracted and repeatedly purified to separate a chalcone raw material with a purity of more than 99%; finally, the obtained high-purity chalcone is dissolved in methanol as a crystal growth raw material, filtered, and the filtrate is placed in a crystal growth bottle for natural evaporation; after 14 days, high-quality light yellow transparent crystals can be obtained, which are nonlinear optical crystal materials;
[0030] The organic solvent for the extraction is ether, and the volume ratio of the solvent to the aqueous phase, i.e., the solvent-to-oil ratio, is 1:1 or 2:1;
[0031] The solvent for purification is hot ethanol;
[0032] (6) Single crystal X-ray diffraction (SXRD) test is performed on the grown optical nonlinear crystal to determine its structure, and theoretical calculations and performance characterization are performed.
[0033] In the present invention, the bifunctional catalyst and photochemical synthesis technology combined with metal organic framework (MOFs) catalyst for chalcone synthesis is an innovative method. Under light conditions, the metal center in the MOFs catalyst is excited to generate high-energy electrons and holes. These excited substances will participate in the reaction path of the reactant molecules and promote the aldol condensation reaction. It utilizes the bifunctional characteristics of MOFs to provide catalytic active sites and enhance the reaction efficiency through photocatalysis. Using light energy to drive the reaction reduces the demand for thermal energy, and the MOFs catalyst can be recycled, reducing the environmental burden of the reaction. Photocatalysis can accelerate the reaction rate and may increase the yield, especially under specific light conditions, the reaction can be carried out with higher efficiency.
[0034] The present invention also provides application of the nonlinear optical crystal material in the field of broadband THz output.
[0035] Compared with the prior art, the present invention has the following advantages and progress:
[0036] (1) This invention provides a new nonlinear optical crystal material TFEOC and TFPOC for the first time by extending the alkyl chain length. Both crystal materials have molecular crystal structures and possess a molecular configuration of D-π-A-π-A. This improves the second-order nonlinear polarizability of the molecule, and by extending the alkyl chain length to optimize the spatial arrangement, the spectrum width range of the crystal THz output is optimized and the crystal has a higher SHG efficiency. The powder second harmonic generation efficiency of TFEOC and TFPOC is 4.32 times and 8.72 times that of KDP, respectively. These two crystals have a large band gap and a wide transparent range. For the first time, the terahertz output of the two crystals was obtained by optical rectification. By extending the alkyl chain length, the THz spectrum width of the TFPOC crystal is slightly higher than that of DAST.
[0037] (2) This invention proposes for the first time the use of bifunctional catalysts and photochemical synthesis technology combined with metal organic framework (MOFs) catalysts for chalcone synthesis, which is an innovative method. It utilizes the bifunctional properties of MOFs to provide catalytic active sites and enhance the reaction efficiency through photocatalysis. Using light energy to drive the reaction reduces the demand for thermal energy, and the MOFs catalyst can be recycled, reducing the environmental burden of the reaction. Photocatalysis can accelerate the reaction rate and increase the yield, especially under specific lighting conditions, the reaction can be carried out with higher efficiency.
[0038] (3) Expanding application fields and potential: By introducing polyhalogenated substituents and extending the π-conjugated chain, not only the nonlinear optical properties of the crystals are enhanced, but also their application potential in the terahertz band is further broadened. In particular, TFEOC and TFPOC crystals have achieved terahertz output for the first time through optical rectification. These characteristics make these crystals have broader application prospects in the future optoelectronics and communications fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Synthesis routes of TFEOC and TFPOC.
[0040] Figure 2 Photo of crystals grown by the present invention.
[0041] Figure 3 ORTEP3 ellipsoid structure diagram of the crystal grown by the present invention.
[0042] Figure 4 Molecular arrangement and hydrogen bond interaction between TFEOC (c) and TFPOC (d). The arrow indicates the direction of maximum first-order polarization, and the right side shows the angle between the maximum direction of first-order hyperpolarizability and the polar axis.
[0043] Figure 5 The energy gaps of HOMO and LUMO orbitals of TFEOC and TFPOC crystallized in non-centrosymmetric space groups are consistent with the theoretically calculated first-order hyperpolarizabilities.
[0044] Figure 6 Theoretical calculation results of the band structure and density of states (DOS) of TFEOC and TFPOC crystallized in non-centrosymmetric space groups.
[0045] Figure 7 Comparison of the second harmonic signal strength of TFEOC, TFPOC and KDP.
[0046] Figure 8 (a) TFEOC and (d) TFPOC THz detection crystals. Comparison of THz electric field intensity output between the designed crystal and DAST crystal, as well as comparison of the spectrum after Fourier transformation.
[0047] Fig. 9 TG-DTG and DSC of TFEOC and TFPOC Thermogravimetric analysis (TGA) and differential scanning calorimetry (DSC) experiments were performed on approximately 10 mg of TFEOC and TFPOC powder samples.
[0048] Fig.10 The change of dielectric constant of TFEOC and TFPOC with increasing temperature at different frequencies.
[0049] Fig.11 (a) UV-vis-NIR transmission spectra of TFEOC and TFPOC. (b) Two crystals (αhν) 2 The relationship between photon energy hν. DETAILED DESCRIPTION
[0050] The invention is described in detail below with reference to embodiments.
[0051] Example 1
[0052] This embodiment provides a nonlinear optical crystal material TFEOC and a preparation method thereof, and the specific preparation steps include:
[0053] (1) Dissolve 0.5 mol of p-ethoxybenzaldehyde in 100 ml of acetonitrile solution;
[0054] (2) Dissolve 0.5 mol of p-trifluoromethylacetophenone in 100 ml of acetonitrile solution;
[0055] (3) mixing the solutions obtained in step (1) and step (2), and adding an appropriate amount of MOFs catalyst PCN-222 to the solution, and ensuring uniform distribution;
[0056] (4) Selecting a visible light LED lamp with a wavelength in the range of 420-450nm, a reaction temperature of 25-50°C, and a reaction time of 2 to 8 hours;
[0057] (5) After the reaction is completed, the reaction mixture is extracted and repeatedly purified to separate a chalcone raw material with a purity of more than 99%; finally, the obtained high-purity chalcone is dissolved in methanol as a crystal growth raw material, filtered, and the filtrate is placed in a crystal growth bottle for natural evaporation; after 14 days, high-quality light yellow transparent crystals can be obtained, which are the nonlinear optical crystal material TFEOC;
[0058] The specific operation of the extraction is: adding an appropriate amount of organic solvent ether to a separatory funnel, wherein the typical volume ratio of the solvent to the aqueous phase (solvent-to-oil ratio) is 1:1 or 2:1, and is appropriately adjusted according to the volume of the solution; gently shaking the separatory funnel and venting it regularly to prevent excessive pressure; standing after shaking until the aqueous phase and the organic phase are completely separated; separating the lower organic phase (ether), and retaining it for subsequent treatment; repeating the above extraction process 2-3 times with fresh organic solvent ether for the aqueous phase to ensure that the chalcone is fully extracted into the organic phase; after combining all the organic phases, washing with a small amount of saturated brine to further remove water-soluble impurities to obtain a crude product;
[0059] The specific operation of the purification is as follows: dissolving the crude product in a small amount of hot ethanol (using the minimum amount of solvent to ensure complete dissolution); slowly cooling the solution to room temperature, and then further cooling it in an ice bath to promote the crystallization of chalcone; vacuum filtering using filter paper with a pore size of 0.2 μm to separate the crystals from the mother liquor, and washing the crystals with cold ethanol to remove impurities. The purified crystals are vacuum dried or dried in an oven at 60-80° C., and their purity is confirmed by high performance liquid chromatography (HPLC) or gas chromatography (GC) analysis, and the purity can usually reach more than 99%;
[0060] (6) Single crystal X-ray diffraction (SXRD) test is performed on the grown optical nonlinear crystal TFEOC to determine its structure, and theoretical calculations and performance characterization are performed.
[0061] Example 2
[0062] This embodiment provides a nonlinear optical crystal material TFPOC and a preparation method thereof. The specific preparation steps are the same as those in Example 1, except that p-ethoxybenzaldehyde is replaced with p-propoxybenzaldehyde to obtain an optical nonlinear crystal TFPOC.
[0063] Test Example 1
[0064] The specific reaction pathway diagram of Example 1 is as follows Figure 1 described.
[0065] The TFEOC crystal and TFPOC crystal obtained in Example 1 and Example 2 are as follows: Figure 2 As described above, parameter performance is characterized.
[0066] Its structure and space group are confirmed by SXRD test. TFEOC crystal belongs to the orthorhombic system, the space group is Pca21, and the unit cell parameters are as follows: a / b=1.1718, b / c=0.1752, c / a=4.8702, Z = 4. TFPOC crystal also belongs to the monoclinic system, the space group is Pc, and the unit cell parameters are as follows: β=94.014(5)°, Z = 2. More detailed crystal data are shown in Table 1.
[0067] Figure 3 The Ortep3 structure diagrams of the two crystals with a 65% ellipsoid probability are shown, providing an intuitive representation of the structures of the two crystals in three-dimensional space.
[0068] Figure 4 The hydrogen bonding interaction between TFEOC and TFPOC molecules in non-centrosymmetric space group crystallization was revealed. The presence of trifluoromethyl groups promoted the formation of more hydrogen bonds, significantly enhanced the stability of the molecule and optimized the spatial arrangement configuration. The red arrow represents the direction from the electron donor to the electron acceptor, which is the maximum effective direction of the first-order hyperpolarizability. The crystal polarity axis of TFEOC and TFPOC and the first-order hyperpolarizability β max The angles between the directions are 30.0 degrees and 33.5 degrees, respectively. From a theoretical point of view, TFEOC has a higher nonlinear efficiency. However, TFPOC presents a more consistent molecular arrangement compared to TFEOC. TFEOC molecules are arranged in a V-shape, resulting in a partial cancellation of the effective first-order hyperpolarizability, making the second harmonic generation (SHG) efficiency lower than that of TFPOC. In addition, because the alkyl chain length of the propoxy group is longer than that of the ethoxy group, more hydrogen bond interactions are formed between the halogen atoms and hydrogen atoms on the trifluoromethyl group in TFPOC.
[0069] Table 1 Crystallographic data of TFEOC and TFPOC
[0070]
[0071] For the characterization of nonlinear properties of crystals, the first-order hyperpolarizability directly reflects the nonlinear optical response intensity of the material. When the material is exposed to a strong electric field or light field (such as a laser), high-order harmonics (such as second harmonics) will be generated during its polarization process. The larger the β value, the stronger the nonlinear optical effect of the material. This study used the Gaussian 16w method to calculate the static first-order hyperpolarizability. The experimental results are shown in Table 2. It can be seen that the static first hyperpolarizability (β) of TFEOC molecules and TFPOC molecules are 50.014×10 -30 esu and 41.616×10 -30 This indicates that the static first hyperpolarizability (β) of TFEOC crystal is higher than that of TFPOC crystal. However, the macroscopic second-order optical nonlinearity of the crystal depends on the arrangement of molecules inside the crystal, that is, the effective hyperpolarizability, which corresponds to β along the polar axis. max Quantity. Figure 3 It is shown that the effective first-order hyperpolarizability of TFEOC is partially offset by the V-shaped arrangement of TFEOC molecules. In contrast, TFPOC molecules present a more uniform spatial arrangement, which makes its second harmonic generation (SHG) efficiency higher than that of TFEOC.
[0072] Table 2. Dipole moment (μ) and static polarizability (α) and static first-order values of hyperpolarizability of TFEOC and TFPOC molecules
[0073]
[0074] The molecular orbital energy levels of TFEOC and TFPOC were investigated by using Gaussian 16W program and density functional theory (DFT), combined with B3LYP functional and 6-31G basis set. Figure 5 ) were calculated. The analysis results show that the HOMO-LUMO energy gaps of TFEOC and TFPOC molecules are 3.74eV and 3.95eV, respectively. The contribution of halogen elements and extended alkyl chains (ethoxy and propoxy) in the electron transfer process is relatively low. The lower electron transfer competition between carbon groups and halogen elements is conducive to the molecules with D-π-A-π-A structure to exhibit greater nonlinear characteristics. The study also shows that the contribution of halogen elements and extended alkyl chains to crystal nonlinearity is achieved through the synergistic effect of optimizing and adjusting the spatial arrangement. The smaller energy gap of TFEOC compared to TFPOC corresponds to its larger first-order hyperpolarizability.
[0075] Figure 6The calculated band structures and density of states (DOS) of TFEOC and TFPOC are shown. Analysis shows that both crystals are semiconductors, that is, there is a certain energy gap between the conduction band and the valence band. TFEOC is a direct band gap crystal, while TFPOC is an indirect band gap crystal, with band gaps of 1.949 eV and 2.247 eV, respectively. The discontinuity of the exchange-correlation energy explains the reasonable differences between the calculated results and the experimental data. To ensure accuracy, the resonance phenomenon needs to occur at the appropriate energy to more accurately determine the linear and nonlinear optical properties. Figure 6 (b) and (d) show the partial density of states (PDOS) of the two crystals and the contribution of individual atoms. It is observed that near the Fermi level, the p orbitals of C and O atoms in the valence band (VB) and conduction band (CB) are the main contributors. The F atoms in the 3F group contribute less, indirectly proving that their contribution to the nonlinearity comes from the direct arrangement of the regulating molecules.
[0076] The second harmonic generation (SHG) coefficient determines the efficiency of nonlinear optical (NLO) materials used in optoelectronics. Depending on the space group of the crystal, the matrix has up to 10 elements with different symmetries. TFEOC and TFPOC belong to different space groups, Pca21 (point group: mm2) and Pc (point group: m), respectively, which determines their symmetry characteristics. The theoretical calculation results are shown in Table 3. Both TFEOC and TFPOC materials exhibit strong SHG coefficients, with maximum values of -13.82pm / V and 11.76pm / V, respectively. The response of TFPOC is more uniformly distributed in multiple directions, while the response of TFEOC is stronger in specific directions. The nonlinear response of TFEOC in a certain direction is significantly enhanced, which is consistent with its theoretically calculated larger first-order hyperpolarizability.
[0077] In order to intuitively demonstrate the nonlinear performance of the crystal, the second harmonic generation (SHG) efficiency of the material was tested using the Kurtz-Perry powder method. Figure 7 As shown, the SHG efficiency of TFEOC crystal and TFPOC crystal are 4.32 times and 8.72 times that of KDP crystal, respectively.
[0078] The crystal selected for THz output test is as follows: Figure 8 a and 8d. Figure 8 The temporal spectral intensity of TFEOC and TFPOC with DAST in b and 8e shows that the efficiency of these two crystals is comparable to that of DAST. Comparison of the terahertz domain spectra obtained by Fourier transform is shown in Figure 8c and 8f. It can be observed that the Fourier absolute amplitude of TFEOC is weaker than that of DAST, and the spectrum is limited to around 13 THz, which is weaker than 14 THz of DAST. The designed TFPOC with extended alkyl chains shows an improved THz spectrum width, although its absolute amplitude is still lower than that of DAST. However, its spectrum extends to 18 THz, and there is no obvious absorption in the frequency range of 2-18 THz.
[0079] like Fig. 9 As shown in the figure, this experiment conducted a detailed study on about 10 mg of TFEOC and TFPOC powder samples by thermogravimetric analysis (TGA) and differential scanning calorimetry (DSC). The experimental results show that the thermal stability of these two crystals exceeds 100°C, and the melting points are 121.6°C and 103.3°C, respectively. This high thermal stability feature is crucial to ensure the accuracy, stable operation and reliability of THz testing. At the same time, this feature also helps to further broaden the application boundaries of THz technology in various fields, providing a solid foundation for its wider development and application.
[0080] like Fig.10 As shown in the figure, the dielectric constants of the two crystals at different frequencies show a significant change trend. The dielectric constants at 1KHz, 10KHz, 100KHz and 1MHz are stable between 9.4-9.7 and 4.1-4.3 respectively with temperature changes. As the frequency increases, the dielectric constant of the crystal gradually decreases. This phenomenon is mainly attributed to space charge polarization, electron displacement polarization and other forms of polarization. Under high frequency conditions, the dielectric constant of the crystal is relatively low, which reflects the excellent quality of the crystal. At the same time, the experimental results show that under the same temperature increase, the dielectric constants of both crystals show a decreasing trend. This feature makes these crystals have potential application value in high-speed electro-optical modulation devices. In addition, the low dielectric constant characteristics of the crystal at higher frequencies help to improve the efficiency of terahertz generation and further broaden its application prospects in related fields.
[0081] The UV-Vis-NIR spectra of the two crystals were recorded in the wavelength range of 200 to 1800 nm using a U-4100 spectrophotometer. Fig.11As shown in a. TFEOC crystals have high transparency in the wavelength range of 600-1350nm, with a maximum transmittance of up to 94%. Similarly, TFPOC crystals have high transmittance in the range of 600-1350nm, with a maximum transmittance of 57%. The strong absorption of organic chromophores at 425nm (maximum cutoff wavelength) is mainly due to the double transition of organic chromophores. Both crystals have absorption peaks at 1138nm, 1490nm and 1670nm due to the vibration of the benzene ring. Based on the transmittance value, the light absorption coefficient and band gap (E g ).according to Fig.11 As shown in b, after analysis and calculation, it was found that the band gap values of TFEOC and TFPOC were similar, with specific values of 2.76eV and 2.81eV respectively.
[0082] Table 3 Symmetrical nonlinear optical susceptibility of TFEOC and TFPOC (pm / V)
[0083]
Claims
1. A nonlinear optical crystal material, It is characterized in that The crystal materials are two types of chalcone crystals: TFEOC and TFPOC, with chemical formulas of C 18 H 15 F 3 O 2 and C 19 H 17 F 3 O 2 , mainly obtained by the condensation reaction of p-trifluoromethylacetophenone and p-ethoxybenzaldehyde or p-propoxybenzaldehyde. Both crystals are molecular crystal structures with a molecular configuration of D-π-A-π-A. The structural formulas are shown in (Ⅰ) and (Ⅱ) below:
2. A nonlinear optical crystal material according to claim 1, It is characterized in that The TFEOC crystal belongs to the orthorhombic system and the space group is Pca2 1 , the crystal shape is hexagonal, and its unit cell parameters are: Z=4; the TFPOC crystal belongs to the monoclinic system, the space group is Pc, the crystal shape is an irregular trapezoid, and its unit cell parameters are: β=94.0-94.2, Z=2.
3. A nonlinear optical crystal material according to claim 2, It is characterized in that The unit cell parameters of the TFEOC crystal are: Z=4; the unit cell parameters of the TFPOC crystal are: β=94.01-94.14, Z=2, further, the unit cell parameters of the TFEOC crystal are: Z=4; the unit cell parameters of the TFPOC crystal are: β=94.011-94.098, Z=2.
4. A nonlinear optical crystal material according to claim 3, It is characterized in that The unit cell parameters of the TFEOC crystal are: a / b=1.1718, b / c=0.1752, c / a=4.8702, Z=4; the unit cell parameters of the TFPOC crystal are: β=94.009-94.019°, Z=2.
5. The nonlinear optical crystal material according to claim 1, It is characterized in that Crystalline polarity axis and first-order hyperpolarizability β of TFEOC max The angle between the directions is 29-31 degrees, preferably 30.0 degrees; the crystal polarity axis of TFPOC and the first-order hyperpolarizability β max The angle between the directions is 33-34 degrees, preferably 33.5 degrees; The static first hyperpolarizabilities (β) of TFEOC and TFPOC molecules were calculated by Gaussian 16w using the 6-311G(d) basis set and B3LYP functional, and were 50.014×10 -30 esu and 41.616×10 -30 esu; The maximum symmetric nonlinear optical susceptibilities of TFEOC and TFPOC molecules calculated by GGA-PBE functional are -13.819960 pm / V and 11.762210 pm / V, respectively.
6. The nonlinear optical crystal material according to claim 1, It is characterized in that The HOMO-LUMO energy gaps of TFEOC and TFPOC molecules were calculated using the 6-311G(d) basis set and B3LYP functional, and were 3.74 eV and 3.95 eV, respectively; The theoretical band gap sizes of TFEOC crystal and TFPOC crystal were determined by GGA-PBE functional, which were 1.949 eV and 2.247 eV, respectively; Using DSTMS as the electro-optical detection crystal, the THz spectrum widths of TFEOC crystal and TFPOC crystal were 0.3-13THz and 0.3-18THz respectively. The melting points of TFEOC crystal and TFPOC crystal measured under nitrogen range were 121.6℃ and 103.3℃ respectively; The dielectric constants of TFEOC crystals and TFPOC crystals at 1KHz, 10KHz, 100KHz and 1MHz are stable between 9.4-9.7 and 4.1-4.3 respectively as the temperature changes; The cutoff wavelength of the TFEOC crystal and the TFPOC crystal is between 420-430 nm. More preferably, the cutoff wavelength of the two crystals is 425 nm, and they exhibit a high transmittance in the range of 600-1350 nm. The experimental band gap sizes of TFEOC crystal and TFPOC crystal are determined by Tauc formula method, and the ranges are 2.80-2.83 eV and 2.75-2.77 eV, respectively; preferably, they are 2.81 eV and 2.76 eV, respectively.
7. The nonlinear optical crystal material according to claim 1, It is characterized in that The second harmonic generation efficiency of TFEOC crystal and TFPOC crystal is 4.32 times and 8.72 times that of KDP crystal respectively.
8. The method for preparing the nonlinear optical crystal material according to any one of claims 1 to 7, It is characterized in that The specific steps include: (1) dissolving p-ethoxybenzaldehyde or p-propoxybenzaldehyde in a solvent at a ratio of 0.1 mol:100 ml; (2) dissolving p-trifluoromethylacetophenone in a solvent at a ratio of 0.1 mol:100 ml; (3) mixing the solutions obtained in step (1) and step (2), adding a suitable MOFs catalyst to the solution and ensuring uniform distribution; the amount of the catalyst is 0.5-10% of the total molar amount of the reactants p-ethoxybenzaldehyde or p-propoxybenzaldehyde and p-trifluoromethylacetophenone; the MOFs catalyst is specifically selected from porphyrin-based zirconium metal organic framework; (4) placing the solution under a light source to carry out a photochemical reaction; the light source is blue light with a wavelength in the range of 420-450 nm or green light with a wavelength in the range of 500-600 nm, the temperature of the photochemical reaction is room temperature or slightly higher than room temperature, and the light irradiation reaction time is controlled between 2 and 8 hours; (5) After the reaction is completed, the reaction mixture is extracted and repeatedly purified to separate a chalcone raw material with a purity of more than 99%; finally, the obtained high-purity chalcone is dissolved in methanol as a crystal growth raw material, filtered, and the filtrate is placed in a crystal growth bottle for natural evaporation; after 14 days, high-quality light yellow transparent crystals can be obtained, which are nonlinear optical crystal materials; (6) Single crystal X-ray diffraction (SXRD) test is performed on the grown optical nonlinear crystal to determine its structure, and theoretical calculations and performance characterization are performed.
9. The method for preparing the nonlinear optical crystal material according to claim 8, It is characterized in that The solvent in step (1) and step (2) is selected from acetonitrile, ethanol or water; the light source in step (4) is a visible light LED lamp, and the temperature of the photochemical reaction is 25-50° C.; the organic solvent for extraction in step (5) is ether, and the volume ratio of the solvent to the aqueous phase, i.e., the solvent-to-oil ratio, is 1:1 or 2:1; and the solvent for purification is hot ethanol.
10. Application of the nonlinear optical crystal material according to any one of claims 1 to 7 in the field of broadband THz output.