Branched polymer as well as preparation method and application thereof
By using a naphthalene-based branched polymer produced by Schiff base reaction of polyetheramine, trimethylformaldehyde and naphthalene diamine, the problem of poor dispersion in graphene composite materials is solved, and graphene and carbon nanotubes are realized The stable dispersion of carbon materials has improved the complexing capacity of lithium ions, is suitable for new energy batteries, and is simple and easy to use.
Patent Information
- Application Number
- CN202411424486.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to achieve stable dispersion in graphene composite materials, resulting in a decrease in volume energy density of lithium-ion batteries and an increase in the difficulty of the electrode sheet coating process. The existing dispersant has limited dispersion effect on graphene and carbon nanotubes.
The naphthalene branched polymer produced by Schiff base reaction is adopted by the Schiff base, and its rich aromatic ring, naphthalene ring and amide bond structure is used to achieve graphene by ultrasonic dispersion. , uniform dispersion of carbon materials such as carbon nanotubes.
It achieves good dispersion effect of carbon materials, improves the complexing capacity of lithium ions, is suitable for the dispersion of carbon materials in new energy batteries, and is simple in preparation and is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dispersants, and in particular relates to a branched polymer and a preparation method and application thereof. Background Art
[0002] At present, the main use of graphene in the field of lithium-ion batteries is to use the special two-dimensional flexible structure of graphene and its high ionic and electronic conductivity to combine with various active materials to improve its cycle characteristics and high current discharge characteristics. Graphene is a new type of carbon nanomaterial with a much larger specific surface area than traditional materials, and its carrier mobility is as high as 1.5×10 4 cm 2 / (V·s), which is twice that of the indium antimonide material with the highest mobility known so far. It can effectively reduce the migration path of lithium ions and improve the rate performance of the battery. Material nano-sizing helps to improve the high-power discharge characteristics of the material, but graphene composite materials are very easy to agglomerate with each other in application, have low stacking density and are difficult to disperse, which will reduce the volume energy density of the battery and increase the difficulty of the pole piece coating process.
[0003] Stable and good dispersion effect is the premise for graphene conductive slurry to be used as a conductive agent in electrodes and form an efficient conductive network. The dispersion methods of graphene can be roughly divided into physical dispersion method, covalent bond modification dispersion method and non-covalent bond modification dispersion method.
[0004] Physical dispersion refers to the process of destroying the van der Waals forces between graphene in a solvent by mechanical force, inhibiting the aggregation between the sheets, and obtaining a stably dispersed graphene dispersion. It includes ultrasonic dispersion, stirring dispersion, ball milling dispersion and other means. Mechanical dispersion has the advantages of low operating equipment requirements and low cost, but it will cause certain damage to the structure of graphene. The covalent bond modification dispersion method is to modify the surface of graphene by combining graphene with some organic small molecules, polymers and other materials that have good dispersion effects in the solution through certain chemical reactions, thereby improving its dispersion ability in the solution. The non-covalent bond modification dispersion method uses the effects of π-π bonds, ionic bonds, hydrogen bonds and other non-covalent bonds to combine graphene with hydrophobic functional groups to improve the dispersion stability of graphene. This method does not require chemical reaction with graphene, can effectively maintain the structural integrity of graphene while improving its dispersion stability, and has good application value.
[0005] Chinese patent application CN101773801A proposes to disperse carbon nanotubes with biomolecules, which can achieve the dispersion of CNTs without destroying the structure of carbon nanotubes. However, the production process of such bio-based dispersants is complicated, difficult to obtain, and expensive. Chinese patent application CN106587013A designs a switch-type dispersant that can disperse CNTs in an aqueous solution, but the dispersant needs to be introduced with nitrogen, air or heated and decomposed during use. The method of use is complicated, and it can only be dispersed in an aqueous solution, and the application conditions are relatively limited. Chinese patent application CN113248739A discloses an olefinic carbon material dispersion and its application, and the olefinic carbon material dispersion includes: an olefinic carbon material, a dispersant, and a solvent. The olefinic carbon material dispersion can be used for olefinic carbon composite aramid fiber, which is low-cost, green and environmentally friendly, simple in process, and has excellent dispersion effect. It is greatly beneficial to prepare olefinic carbon composite aramid fiber, improve the comprehensive performance of aramid fiber, and accelerate the upgrading and innovation of the aramid industry. However, the dispersing effect of this dispersant on graphene, carbon nanotubes, etc. is limited, and there is room for further improvement; and this dispersant is mainly used in the preparation of aramid fiber composite materials, and whether it can be applied to lithium-ion batteries remains to be discussed. Summary of the invention
[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a branched polymer and a preparation method and use thereof. The branched polymer has a good dispersing effect on carbon black, carbon nanotubes and graphene, and can be used for dispersing carbon materials in new energy batteries.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A branched polymer obtained by reacting the following components:
[0009] (a) polyetheramines;
[0010] (b) trimesaldehyde;
[0011] (c) Naphthalenediamine.
[0012] The M of the branched polymer n 3000-100000.
[0013] Preferably, the (a) is a single-terminal primary amino polyether, the structural formula of which is R-(CH 2 CH 2 O) y (CH 2 CHCH 3 O) x -NH 2 ; wherein x is an integer between 0 and 100; y is an integer between 0 and 100; x+y≥20, and R is a straight-chain alkyl group having 1 to 18 carbon atoms.
[0014] Preferably, the (a) is a single-terminal primary amino polyether, the structural formula of which is R-(CH 2 CH 2 O) y (CH 2 CHCH 3 O) x -NH 2 ; wherein x is an integer between 20 and 80; y is an integer between 0 and 70; x+y≥20, and R is a straight-chain alkyl group having 1 to 18 carbon atoms.
[0015] Preferably, the naphthalenediamine may be 1,4-naphthalenediamine, 1,8-naphthalenediamine, 1,5-naphthalenediamine, or 2,3-naphthalenediamine.
[0016] Preferably, the molar ratio of (a), (b) and (c) is 6:3:2.
[0017] The present invention also protects a method for preparing the branched polymer as described above, comprising the following raw materials:
[0018] Components (a) and (b) are added into a flask, followed by an organic solvent, and after being stirred evenly, component (c) is added, dispersed by ultrasonication, reacted, and cooled to room temperature to obtain the branched polymer.
[0019] In the present invention, through high temperature Schiff base reaction, since the reaction rate of amino groups in polyetheramine is faster than that of amino groups in naphthalene diamine, polyetheramine reacts with trimesaldehyde first to obtain a macromonomer, and then the macromonomer reacts with naphthalene diamine to obtain a branched polymer.
[0020] Preferably, the organic solution is one or more of N-methylpyrrolidone, dimethyl sulfoxide, and N,N-dimethylacetamide.
[0021] Preferably, the reaction temperature is 160-220° C. and the reaction time is 10-20 h.
[0022] In the present invention, the reaction temperature can be 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, and the reaction time can be 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h.
[0023] Preferably, the ultrasonic dispersion time is 10-20 min.
[0024] The present invention also protects the use of the branched polymer as described above in dispersing carbon black, carbon nanotubes and graphene.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The branched polymer provided by the present invention uses polyetheramine, trimesic acid or naphthalene diamine as raw materials, and utilizes the Schiff base reaction principle to generate a naphthalene-based branched polymer in a one-step process. The naphthalene-based branched polymer contains abundant aromatic rings, naphthalene rings, and amide bond structures. Since the benzene rings, naphthalene rings, amide bonds, etc. have good affinity for carbon, the carbon material can be effectively dispersed evenly. At the same time, the introduced polyether chain segments can provide dispersibility and lithium ion complexing ability, making the naphthalene-based branched polymer very suitable for the dispersion of carbon materials in new energy batteries.
[0027] (2) The branched polymer provided by the present invention has a simple preparation method, and the raw materials used are easily available, which is suitable for industrial production and has good application prospects. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The polyetheramines are Huntsman M1000, Huntsman M2070 and Huntsman M3085, all of which were purchased from Hubei Maidehao Chemical Co., Ltd.
[0030] Example 1
[0031] A method for preparing a branched polymer comprises the following steps:
[0032] 100 g of polyetheramine M2070 (molecular weight 2070) and 3.91 g of trimesic acid were added to a flask, followed by 500 mL of N-methylpyrrolidone, stirred evenly, and then 2.54 g of 1,4-naphthalenediamine was added, ultrasonically dispersed for 15 min, reacted at 210° C. for 15 h, and cooled to room temperature to obtain the naphthyl branched polymer. n is 12000.
[0033] Example 2
[0034] A method for preparing a branched polymer comprises the following steps:
[0035] 100 g of polyetheramine M1000 (molecular weight 1000) and 8.1 g of trimesic acid were added to a flask, followed by 500 mL of N-methylpyrrolidone. After stirring evenly, 5.27 g of 1,5-naphthalenediamine was added, ultrasonically dispersed for 15 min, reacted at 200 ° C for 16 h, and cooled to room temperature to obtain the naphthyl branched polymer. The branched polymer M n is 6000.
[0036] Example 3
[0037] A method for preparing a branched polymer comprises the following steps:
[0038] 90g of polyetheramine M3085 (molecular weight 3085) and 4.73g of trimesic acid were added to a flask, followed by 500mL of N-methylpyrrolidone, stirred evenly, and then 4.61g of 1,8-naphthalenediamine was added, ultrasonically dispersed for 15min, reacted at 200°C for 17h, and cooled to room temperature to obtain the naphthyl branched polymer. n is 24000.
[0039] Example 4
[0040] A method for preparing a branched polymer comprises the following steps:
[0041] 100 g of polyetheramine M2070 (molecular weight 2070) and 3.91 g of trimesic acid were added to a flask, followed by 500 mL of dimethyl sulfoxide, stirred evenly, and then 2.54 g of 2,3-naphthalenediamine was added, ultrasonically dispersed for 10 min, reacted at 190° C. for 20 h, and cooled to room temperature to obtain the naphthyl branched polymer. n is 8000.
[0042] Example 5
[0043] A method for preparing a branched polymer comprises the following steps:
[0044] 100 g of polyetheramine M2070 (molecular weight 2070) and 3.91 g of trimesic acid were added to a flask, followed by 500 mL of N,N-dimethylacetamide, stirred evenly, and then 2.54 g of 1,4-naphthalenediamine was added, ultrasonically dispersed for 20 min, reacted at 220° C. for 11 h, and cooled to room temperature to obtain the naphthyl branched polymer. The branched polymer M n is 11000.
[0045] Comparative Example 1
[0046] A method for preparing a branched polymer comprises the following steps:
[0047] 100 g of polyetheramine M2070 (molecular weight 2070) and 3.91 g of trimesaldehyde were added to a flask, followed by 500 mL of N-methylpyrrolidone. After stirring evenly, ultrasonic dispersion was performed for 15 min, the mixture was reacted at 200° C. for 15 h, and cooled to room temperature to obtain the branched polymer.
[0048] Compared with Example 1, no melamine was added in this comparative example.
[0049] Comparative Example 2
[0050] A method for preparing a branched polymer comprises the following steps:
[0051] 3.91 g of trimesaldehyde was added to a flask, followed by 500 mL of N-methylpyrrolidone. After stirring evenly, 2.54 g of 1,4-naphthalenediamine was added, ultrasonically dispersed for 15 minutes, reacted at 200° C. for 15 hours, and cooled to room temperature to obtain the naphthyl branched polymer.
[0052] Compared with Example 1, no polyetheramine was added in this comparative example.
[0053] The branched polymers prepared in Examples 1-5 and Comparative Examples 1-2 were subjected to a dispersion test on carbon nanotubes. The test conditions were: ambient humidity of 75% and ambient temperature of 25°C. The dispersion method was as follows: 50g carbon nanotubes, 5g branched polymers, and 945g N-methylpyrrolidone were first dispersed uniformly at 2000rpm and then added to a 1000mL desktop nano grinder and ground at 25°C for 3 hours. The prepared slurry was tested for particle size and viscosity using a Malvern particle size analyzer and a viscometer, respectively. The evaluation results are shown in Table 1:
[0054] Table 1 Evaluation results of carbon nanotube dispersion slurry
[0055] Group Carbon nanotube particle size / nm Slurry viscosity / mPas Apparent state after 60 days of static storage Example 1 293 368 Evenly dispersed Example 2 337 461 Evenly dispersed Example 3 325 447 Evenly dispersed Example 4 314 439 Evenly dispersed Example 5 306 413 Evenly dispersed Comparative Example 1 627 881 Layered, with sediment at the bottom Comparative Example 2 958 2573 Layered, with a lot of sediment at the bottom
[0056] As can be seen from Table 1, the branched polymer prepared in the present invention can stably and uniformly disperse carbon nanotubes into a high-concentration dispersion, and the particle size of the carbon nanotubes and the viscosity of the slurry are lower than those in the comparative example, indicating that the branched polymer in the embodiment of the present invention has a good dispersion effect on carbon nanotubes and excellent performance.
[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A branched polymer, It is characterized in that Obtained by the following reaction: (a) polyetheramines; (b) trimesaldehyde; (c) Naphthalenediamine.
2. The branched polymer according to claim 1, It is characterized in that The M of the branched polymer n 3000-100000.
3. The branched polymer according to claim 1, It is characterized in that The (a) is a single-terminal primary amino polyether, and its structural formula is R-(CH 2 CH 2 O) y (CH 2 CHCH 3 O) x -NH 2 ; wherein x is an integer between 0 and 100; y is an integer between 0 and 100; x+y≥20, and R is a straight-chain alkyl group having 1 to 18 carbon atoms.
4. The branched polymer according to claim 3, It is characterized in that The (a) is a single-terminal primary amino polyether, and its structural formula is R-(CH 2 CH 2 O) y (CH 2 CHCH 3 O) x -NH 2 ; wherein x is an integer between 20 and 80; y is an integer between 0 and 70; x+y≥20, and R is a straight-chain alkyl group having 1 to 18 carbon atoms.
5. The branched polymer according to claim 1, It is characterized in that The molar ratio of (a), (b) and (c) is 6:3:
2.
6. A method for preparing a branched polymer as claimed in any one of claims 1 to 5, characterized in that it comprises the following raw materials: Components (a) and (b) are added into a flask, followed by an organic solvent, and after being stirred evenly, component (c) is added, dispersed by ultrasonication, reacted, and cooled to room temperature to obtain the branched polymer.
7. The preparation method according to claim 6, It is characterized in that The organic solution is one or more of N-methylpyrrolidone, dimethyl sulfoxide, and N,N-dimethylacetamide.
8. The preparation method according to claim 6, It is characterized in that The reaction temperature is 160-220° C. and the reaction time is 10-20 h.
9. The preparation method according to claim 6, It is characterized in that The ultrasonic dispersion time is 10-20 min.
10. Use of the branched polymer according to any one of claims 1 to 5 in dispersing carbon black, carbon nanotubes and graphene.
Citation Information
Patent Citations
Dispersant for dispersing carbon nano-tube and preparation method of carbon nano-tube film
CN101773801A
Switch-type carbon nanotube dispersant
CN106587013A
Olefinic carbon material dispersion liquid and application thereof
CN113248739A