Rubber composition and application thereof
By using the combination of anti-aging agents A and B in tire glue, combining diene elastomers and other components, the color changes and insufficient performance of tire glue under aging factors are solved, and heat resistance to oxygen, ozone and Improved salt spray resistance performance reduces costs and improves viscosity.
Patent Information
- Application Number
- CN202310660785.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
When existing tire glues face aging factors such as light, high temperature and chemical corrosion, color changes lead to appearance problems, and commonly used anti-aging agents have problems such as insufficient anti-thermal oxygen and ozone resistance, high cost and poor viscosity.
The combination of anti-aging agent A and anti-aging agent B is used as the anti-aging agent system, and ozone resistance is formed by adding a specific proportion of diene elastomer, sulfur, carbon black, ZnO, stearic acid, aromatic oil and accelerator to the rubber composition. , rubber composition with excellent salt spray resistance and color discoloration resistance.
It significantly improves the heat-resistant oxygen, ozone and salt spray aging resistance of rubber, reduces the amount of anti-aging agent A while maintaining excellent performance, reduces costs, and improves viscosity. It is suitable for rubber products such as tires.
Smart Images

Figure BDA0004275222790000021 
Figure BDA0004275222790000022 
Figure BDA0004275222790000041
Abstract
Description
Technical Field
[0001] The invention belongs to the field of diene elastomer compositions, and in particular relates to a rubber composition and use thereof. Background Art
[0002] Tires are an essential part of modern cars, which play the role of carrying the car and transmitting traction and braking force. Generally speaking, tires are exposed to the outside of the car and are visible parts; at the same time, tires are also affected by aging effects such as light, high temperature, and chemical corrosion, which may cause color changes. Therefore, the color of the tire has a significant impact on the overall appearance of the car.
[0003] The tread and sidewall of a tire are the outermost components of the tire, so they directly affect the appearance of the tire.
[0004] The tread rubber is the main part of the tire that contacts the ground. The part of the tire that contacts the ground will be worn continuously during driving, but the tread rubber in the groove and near the shoulder will not be worn. The color changes caused by aging such as light, high temperature, chemical corrosion, etc. will affect the appearance of the tire.
[0005] The sidewall is the most important appearance part of the tire, accounting for about 2 / 3 of the tire's surface area. The sidewall contains a lot of information such as tire specifications, brand logo, certification mark and production information, and is an important area for tires to be displayed to the outside world. The color changes caused by aging such as light, high temperature, chemical corrosion, etc. will also affect the appearance of the tire.
[0006] Since most tires are black, slight discoloration is not easy to attract attention. Therefore, the current tread and sidewall rubber materials usually use p-phenylenediamine antioxidants with good overall performance but staining properties, such as N,N'-bis-(1,4-dimethylpentyl) p-phenylenediamine (77PD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine (6PPD), etc.
[0007] Tires with high requirements for appearance will use phenolic antioxidants or saturated rubber to reduce the amount of antioxidants to reduce discoloration. Among them, the anti-aging effect of using phenolic antioxidants is not as good as that of p-phenylenediamine antioxidants. The appearance is improved, but the resistance to heat oxidation, ozone and flexural properties are greatly reduced. In addition, if saturated rubber such as EPDM is used, the antioxidant can be reduced or not used to improve the appearance, but due to the high price of such rubber, the cost increases, and the poor viscosity of such rubber is not conducive to tire bonding and molding. Summary of the invention
[0008] In view of the problems existing in the prior art, the present invention provides a rubber composition that is resistant to ozone aging, salt spray aging and discoloration. The rubber composition of the present invention uses antioxidant A and antioxidant B as an antioxidant system, has good ozone aging resistance, salt spray aging resistance and discoloration resistance, and is particularly suitable for application in all or part of the rubber matrix of a tire.
[0009] Specifically, one aspect of the present invention provides a rubber composition, wherein the raw materials of the rubber composition include 100 parts by mass of a diene elastomer, 1.5-3 parts by mass of an antioxidant A and 0.1-1.5 parts by mass of an antioxidant B;
[0010] The antioxidant A has a structure shown in Formula I:
[0011]
[0012] The antioxidant B has a structure shown in formula II:
[0013]
[0014] In one or more embodiments, in the raw materials of the rubber composition, the total amount of the antioxidant A and the antioxidant B is 2-4 parts by mass.
[0015] In one or more embodiments, in the raw materials of the rubber composition, the total amount of the antioxidant A and the antioxidant B is 2.5-3.5 parts by mass.
[0016] In one or more embodiments, in the raw materials of the rubber composition, the mass ratio of the antioxidant A to the antioxidant B is 1:1 to 30:1.
[0017] In one or more embodiments, the diene elastomer includes natural rubber and butadiene rubber.
[0018] In one or more embodiments, the mass ratio of the natural rubber to the butadiene rubber is 4:6-6:4.
[0019] In one or more embodiments, the raw materials of the rubber composition further include 0.5-3 parts by mass of sulfur.
[0020] In one or more embodiments, the raw material of the rubber composition further includes 30-70 parts by mass of a reinforcing filler.
[0021] In one or more embodiments, the reinforcing filler is carbon black.
[0022] In one or more embodiments, the raw material of the rubber composition further includes 1 to 10 parts by mass of an active agent.
[0023] In one or more embodiments, the active agent is ZnO.
[0024] In one or more embodiments, the raw material of the rubber composition further includes 1 to 10 parts by mass of a softener.
[0025] In one or more embodiments, the emollient includes stearic acid and aromatic oil.
[0026] In one or more embodiments, the raw material of the rubber composition further includes 0.2-2 parts by mass of an accelerator.
[0027] In one or more embodiments, the accelerator is N-tert-butyl-2-benzothiazole sulfenamide.
[0028] In one or more embodiments, the raw materials of the rubber composition include: 100 parts by mass of a diene elastomer, 0.5-3 parts by mass of sulfur, 1.5-3 parts by mass of an antioxidant A, 0.1-1.5 parts by mass of an antioxidant B, 30-70 parts by mass of carbon black, 3-8 parts by mass of ZnO, 1-4 parts by mass of stearic acid, 3-8 parts by mass of aromatic oil, and 0.2-2 parts by mass of N-tert-butyl-2-benzothiazolesulfonamide; wherein the diene elastomer includes natural rubber and butadiene rubber in a mass ratio of 4:6-6:4.
[0029] Another aspect of the present invention provides a rubber product, wherein the rubber product comprises the rubber composition described in any embodiment of the present invention.
[0030] In one or more embodiments, the rubber article is a tire.
[0031] Another aspect of the present invention provides a use of a combination of an antioxidant A and an antioxidant B in improving the ozone aging resistance, salt spray aging resistance and discoloration resistance of a rubber composition, the use comprising: adding 1.5-3.0 parts by mass of the antioxidant A and 0.1-1.5 parts by mass of the antioxidant B to the raw materials of the rubber composition based on 100 parts by mass of the diene elastomer contained in the raw materials of the rubber composition;
[0032] The antioxidant A has a structure shown in Formula I:
[0033]
[0034] The antioxidant B has a structure shown in formula II:
[0035]
[0036] In one or more embodiments, the total amount of the antioxidant A and the antioxidant B is 2-4 parts by mass, for example, 2.5-3.5 parts by mass.
[0037] In one or more embodiments, in the raw materials of the rubber composition, the mass ratio of the antioxidant A to the antioxidant B is 1:1 to 30:1.
[0038] In one or more embodiments, the rubber composition is as described in any of the embodiments herein. DETAILED DESCRIPTION
[0039] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0040] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0041] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0042] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0043] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0044] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0045] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0046] The present invention finds that the combination of antioxidant B and antioxidant A as an antioxidant system in a rubber composition, especially a tire rubber composition (such as a tread rubber composition, a sidewall rubber composition, etc.), can significantly improve the heat oxygen aging resistance, ozone aging resistance, salt spray aging resistance and discoloration resistance of the rubber. A certain amount of antioxidant B and antioxidant A show an unexpected synergistic effect in improving the salt spray aging resistance of the rubber composition, and can reduce the amount of antioxidant A while making the rubber composition have ozone aging resistance and discoloration resistance equivalent to the case of a high amount of antioxidant A.
[0047] In the present invention, antioxidant A refers to a compound of formula I:
[0048]
[0049] In the present invention, antioxidant B refers to a compound of formula II:
[0050]
[0051] The raw materials of the rubber composition generally include a diene elastomer, a reinforcing filler, an antioxidant and a crosslinking agent. Herein, the rubber composition includes unvulcanized rubber and vulcanized rubber. The unvulcanized rubber can be vulcanized (cured) to obtain vulcanized rubber.
[0052] The raw materials of the rubber composition of the present invention include a diene elastomer, an antioxidant A and an antioxidant B, wherein, based on 100 parts by mass of the diene elastomer, the amount of the antioxidant A is 1.5-3.0 parts by mass, and the amount of the antioxidant B is 0.1-1.5 parts by mass. Herein, unless otherwise specified, the mass parts of other components in the raw materials of the rubber composition are calculated based on 100 parts by mass of the diene elastomer in the raw materials of the rubber composition.
[0053] Herein, diene elastomer refers to an elastomer whose monomers include dienes (such as butadiene, isoprene). Suitable diene elastomers for the present invention can be various diene elastomers known in the art, including but not limited to one or more selected from natural rubber (NR), cis-1,4-butadiene rubber (BR), isoprene rubber, styrene-butadiene rubber (SBR), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), isoprene / butadiene copolymer, isoprene / styrene copolymer and isoprene / butadiene / styrene copolymer. In some preferred embodiments, diene elastomer includes natural rubber and cis-1,4-butadiene rubber, or is composed of natural rubber and cis-1,4-butadiene rubber. The mass ratio of natural rubber and cis-1,4-butadiene rubber is preferably 4:6 to 6:4, such as 4.5:5.5 to 5.5:4.5, 1:1.
[0054] The antioxidant contained in the rubber composition of the present invention includes antioxidant A and antioxidant B. In some embodiments, the rubber composition of the present invention does not contain other antioxidants except antioxidant A and antioxidant B. In the raw materials of the rubber composition of the present invention, the amount of antioxidant A can be 1.5-3.0 mass parts, such as 1.5 mass parts, 1.8 mass parts, 1.9 mass parts, 2.0 mass parts, 2.1 mass parts, 2.2 mass parts, 2.3 mass parts, 2.5 mass parts, 2.9 mass parts. In the raw materials of the rubber composition of the present invention, the amount of antioxidant B can be 0.1-1.5 mass parts, such as 0.2 mass parts, 0.3 mass parts, 0.4 mass parts, 0.5 mass parts, 0.6 mass parts, 0.7 mass parts, 1 mass parts, 1.2 mass parts. Controlling the amount of antioxidant A and antioxidant B within the aforementioned range is conducive to exerting the synergistic effect of the two in improving the salt spray aging resistance of the rubber composition, and maintaining good ozone aging resistance and anti-discoloration performance. The total amount of antioxidant A and antioxidant B can be 2-4 parts by mass, preferably 2.5-3.5 parts by mass, such as 2.8 parts by mass, 3.0 parts by mass, and 3.2 parts by mass. The mass ratio of antioxidant A and antioxidant B is preferably 1:1 to 30:1, such as 2:1, 5:1, 10:1, 15:1, and 20:1. Controlling the mass ratio of antioxidant A and antioxidant B within the aforementioned range is conducive to exerting the synergistic effect of the two in improving the salt spray aging resistance of the rubber composition, and maintaining good ozone aging resistance and anti-discoloration performance.
[0055] The raw material of the rubber composition of the present invention may include reinforcing filler. In the raw material of the rubber composition of the present invention, the amount of reinforcing filler can be 30-70 mass parts, such as 40 mass parts, 45 mass parts, 50 mass parts, 55 mass parts, 60 mass parts. Reinforcing filler suitable for the present invention can be a conventional reinforcing filler for rubber composition, including but not limited to one or more selected from carbon black, white carbon black, titanium oxide, calcium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, clay and talcum. In some preferred embodiments, reinforcing filler comprises carbon black, or reinforcing filler is carbon black.
[0056] The raw materials of the rubber composition of the present invention include a crosslinking agent, such as sulfur. In the raw materials of the rubber composition of the present invention, the amount of sulfur used can be 0.5-3 parts by mass, such as 1 part by mass, 1.5 parts by mass, 2 parts by mass, and 2.5 parts by mass.
[0057] The raw materials of the rubber composition of the present invention may further include other ingredients commonly used in rubber compositions, including but not limited to one or more selected from the group consisting of softeners, protective waxes, activators and accelerators.
[0058] Softener can be used to improve the processing properties of rubber composition. Softener can include petroleum softener, such as naphthenic oil, aromatic oil, process oil, lubricating oil, paraffin, liquid paraffin, petroleum asphalt, vaseline, etc., and can also include fatty oil softener, such as stearic acid, castor oil, linseed oil, rapeseed oil, coconut oil, wax (such as beeswax, carnauba wax and lanolin), tall oil, linoleic acid, palmitic acid, lauric acid, etc. In the raw material of rubber composition of the present invention, the amount of softener can be 1-10 mass parts, preferably 3-9 mass parts, such as 4 mass parts, 5 mass parts, 6 mass parts, 7 mass parts, 8 mass parts. In some preferred embodiments, softener includes aromatic oil and stearic acid, or is composed of aromatic oil and stearic acid. The mass ratio of aromatic oil and stearic acid can be 1:1 to 5:1, such as 2:1, 2.5:1, 3:1, 4:1. In some preferred embodiments, in the raw materials of the rubber composition of the present invention, the amount of aromatic oil used is 3-8 parts by mass, for example, 4 parts by mass, 5 parts by mass, 6 parts by mass, and 7 parts by mass; the amount of stearic acid used is 1-4 parts by mass, for example, 1.5 parts by mass, 2 parts by mass, and 3 parts by mass.
[0059] The protective wax can migrate from the inside of the rubber to the surface to form a wax film, which plays a role in isolating the rubber surface from the external environment. The protective wax is optionally added. When the raw materials of the rubber composition of the present invention include the protective wax, the amount of the protective wax can be 1-5 parts by mass, such as 1.5 parts by mass, 2 parts by mass, 3 parts by mass, and 4 parts by mass.
[0060] The activating agent can accelerate the vulcanization speed, improve the thermal conductivity, wear resistance, tear resistance and the like of rubber. In the raw material of the rubber composition of the present invention, the amount of the activating agent can be 1-10 mass parts, such as 2 mass parts, 3 mass parts, 4 mass parts, 5 mass parts, 6 mass parts, 7 mass parts, 8 mass parts, 9 mass parts. In some preferred embodiments, the activating agent includes ZnO, or the activating agent is ZnO. In some preferred embodiments, in the raw material of the rubber composition of the present invention, the amount of ZnO is 3-8 mass parts, such as 4 mass parts, 5 mass parts, 6 mass parts, 7 mass parts.
[0061] The accelerator is usually a vulcanization accelerator, which can be selected from sulfonamide vulcanization accelerators, thiazole vulcanization accelerators, thiuram vulcanization accelerators, thiourea vulcanization accelerators, guanidine vulcanization accelerators, dithiocarbamate vulcanization accelerators, aldehyde amine vulcanization accelerators, aldehyde ammonia vulcanization accelerators, imidazoline vulcanization accelerators and xanthogenic acid vulcanization accelerators. In the raw materials of the rubber composition of the present invention, the amount of the accelerator can be 0.2-2 mass parts, such as 0.5 mass parts, 0.6 mass parts, 0.8 mass parts, 1 mass parts, 1.5 mass parts. In some preferred embodiments, the accelerator is accelerator NS (N- tert-butyl -2-benzothiazole sulfonamide).
[0062] In addition, when necessary, the rubber composition may also contain plasticizers such as DMP (dimethyl phthalate), DEP (diethyl phthalate), DBP (dibutyl phthalate), DHP (diheptyl phthalate), DOP (dioctyl phthalate), DINP (diisononyl phthalate), DIDP (diisodecyl phthalate), BBP (butyl benzyl phthalate), DWP (dilauryl phthalate), and DCHP (dicyclohexyl phthalate), etc. The amount of the plasticizer may be a conventional amount in the art.
[0063] In some preferred embodiments, the raw materials of the rubber composition of the present invention include: 100 parts by mass of a diene elastomer, 0.5-3 parts by mass of sulfur, 1.5-3.0 parts by mass of an antioxidant A, 0.1-1.5 parts by mass of an antioxidant B, 30-70 parts by mass of carbon black, 3-8 parts by mass of ZnO, 1-4 parts by mass of stearic acid, 3-8 parts by mass of aromatic oil and 0.2-2 parts by mass of N-tert-butyl-2-benzothiazolesulfonamide; wherein the diene elastomer includes natural rubber and butadiene rubber in a mass ratio of 4:6-6:4.
[0064] The unvulcanized rubber of the present invention can be prepared by conventional rubber mixing methods, for example, by a two-stage mixing method: a first stage of thermomechanical (e.g., internal mixer) mixing, mixing the rubber composition raw materials except the crosslinking agent and the accelerator, kneading the entire mixture until the maximum temperature reaches between 110°C and 190°C to obtain a first stage of rubber; a second stage of thermomechanical (e.g., open mixer) mixing, after the first stage of rubber is cooled to below 100°C, mixing the first stage of rubber with the crosslinking agent and the accelerator until the maximum temperature is below 110°C to obtain a second stage of rubber, i.e., the unvulcanized rubber.
[0065] Vulcanized rubber can be obtained by vulcanizing (curing) the unvulcanized rubber. The vulcanization temperature is usually 130-200°C, such as 140-160°C, 145±5°C; the vulcanization time depends on the vulcanization temperature, the vulcanization system and the vulcanization kinetics, and is usually 15-60 minutes, such as 20-40 minutes, 30±5 minutes. Before vulcanization, the unvulcanized rubber can be rolled into a sheet with a thickness of 1-5 mm, such as 2±0.5 mm.
[0066] The rubber composition of the present invention is used in rubber products, especially tires. Compared with the rubber composition using antioxidant A or antioxidant B alone, the composition using a certain amount of antioxidant A and antioxidant B as an antioxidant system can not only significantly improve the salt spray aging resistance of the rubber product, but also enable the rubber product to have the heat oxygen aging resistance, ozone aging resistance and anti-discoloration performance equivalent to that when using a high amount of antioxidant A. Therefore, the present invention also provides a rubber product, the rubber product contains the rubber composition described herein. The rubber product can be a tire, a rubber shoe, a sealing strip, a sound insulation board, a shock pad, etc. The rubber product is preferably a tire, such as a sidewall rubber, a tread rubber, etc.
[0067] The present invention also provides the use of a combination of antioxidant A and antioxidant B in improving the ozone resistance, discoloration resistance and salt spray resistance of a rubber composition, and a method for improving the ozone resistance, discoloration resistance and salt spray resistance of a rubber composition. Preferably, the use or method of the present invention comprises: adding 1.5-3.0 parts by mass of antioxidant A and 0.1-1.5 parts by mass of antioxidant B to the raw materials of the rubber composition, based on 100 parts by mass of the diene elastomer contained in the raw materials of the rubber composition. In the use or method of the present invention, the amounts of antioxidant A and antioxidant B and the raw material composition of the rubber composition are preferably as described in any embodiment of the present invention.
[0068] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0069] The sources and specifications of the raw materials used in the examples are as follows:
[0070] Natural rubber: Xishuangbanna Sinochem Rubber Co., Ltd., SCR5;
[0071] Butadiene rubber (BR): Sinopec Qilu Petrochemical Company, BR9000;
[0072] Carbon black: Shanghai Cabot Carbon Black Co., Ltd., carbon black N550;
[0073] ZnO: Yonghua Chemical Technology (Jiangsu) Co., Ltd.;
[0074] Stearic acid (SA): Yonghua Chemical Technology (Jiangsu) Co., Ltd.;
[0075] Aromatic oil: PetroChina Karamay Petrochemical Co., Ltd.;
[0076] Antioxidant 6PPD: Shengao Chemical Technology Co., Ltd.;
[0077] Antioxidant A: Shengao Chemical Technology Co., Ltd.
[0078] Antioxidant B: Shengao Chemical Technology Co., Ltd.;
[0079] Accelerator NS: Shengao Chemical Technology Co., Ltd.;
[0080] Sulfur (S): Yonghua Chemical Technology (Jiangsu) Co., Ltd.
[0081] Example 1
[0082] According to the formulation shown in Table 1, rubber compositions 1-8 were prepared using the following process:
[0083] (1) Add natural rubber and butadiene rubber into an internal mixer, then add carbon black, ZnO, stearic acid, aromatic oil, and antioxidant, and knead until the temperature of the rubber compound rises to 130° C. to obtain a rubber section;
[0084] (2) After the first-stage rubber is cooled to 70°C, the first-stage rubber is mixed on an open mixing mill, and accelerator NS and sulfur are added. The rubber is kneaded until the temperature of the rubber material rises to 90°C and the rubber is discharged to obtain the second-stage rubber;
[0085] (3) The second-stage rubber was rolled into a sheet with a thickness of 2 mm and vulcanized at 145°C for 30 minutes to obtain a vulcanized rubber.
[0086] Table 1: Formulation of rubber composition 1-8 (unit: mass parts)
[0087] Rubber composition number 1 2 3 4 5 6 7 8 SCR5 50.0 50.0 50.0 50.0 50.0 50.0 50.0 50.0 BR 50.0 50.0 50.0 50.0 50.0 50.0 50.0 50.0 Carbon Black N550 50.0 50.0 50.0 50.0 50.0 50.0 50.0 50.0 ZnO 5.0 5.0 5.0 5.0 5.0 5.0 5.0 5.0 SA 2.0 2.0 2.0 2.0 2.0 2.0 2.0 2.0 Aromatic oil 5.0 5.0 5.0 5.0 5.0 5.0 5.0 5.0 Antioxidant 6PPD 3.0 0 0 0 0 0 0 0 Antioxidant A 0 3.0 0 2.9 2.0 1.5 1.3 1.0 Antioxidant B 0 0 3.0 0.1 1.0 1.5 1.7 2.0 Accelerator NS 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 S 1.5 1.5 1.5 1.5 1.5 1.5 1.5 1.5
[0088] Test Example 1
[0089] The vulcanization characteristics t10 and t90, mechanical properties before aging, mechanical properties after thermal oxidation aging, and mechanical properties after salt spray aging of the rubber compositions 1-6 were measured according to the following standards. The results are shown in Table 2:
[0090] Vulcanization characteristics: GB / T 16584-1996 Rubber vulcanizer without rotor for vulcanization characteristics;
[0091] Elongation at break and tensile strength: GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber;
[0092] 100℃×48H thermal oxidative aging test: GB / T 3512-2014 vulcanized rubber or thermoplastic rubber hot air accelerated aging and heat resistance test;
[0093] 5% NaCl 48H salt spray aging test: GB / T 35858-2018 Vulcanized rubber salt spray aging test method.
[0094] Table 2: Physical properties of rubber compositions
[0095]
[0096] It can be seen from Table 2 that the rubber compositions 4-8 containing antioxidant A and antioxidant B have better resistance to thermal oxidative aging.
[0097] It can be seen from Table 2 that the salt spray aging resistance of rubber compositions 4, 5, and 6 containing a certain amount of antioxidant A and antioxidant B is significantly better than that of rubber composition 2 containing only antioxidant A and rubber composition 3 containing only antioxidant B, indicating that a certain amount of antioxidant A and antioxidant B have a synergistic effect in improving the salt spray aging resistance of the rubber composition.
[0098] Test Example 2
[0099] The ozone aging resistance of rubber was tested in an ozone aging test chamber using ISO 1431-1:2004 "Ozone cracking resistance of vulcanized or thermoplastic rubber". The ozone volume concentration was 50pphm, the temperature was (40±2)℃, and the humidity was (50±5)%. During the test, the sample was stretched by 20% and continuously operated for 96 hours to observe the cracking of the sample. The results are shown in Table 3. The ozone cracking grade description is shown in Table 4.
[0100] Table 3: Cracking of rubber compositions
[0101] Rubber composition number 1 2 3 4 5 6 7 8 Crack level 4 2 4 2 2 2 3 3
[0102] Table 4: Ozone cracking grade description
[0103] grade describe 0 No cracks 1 Crack width <0.1mm 2 0.1mm≤crack width<0.2mm 3 0.2mm≤crack width<0.4mm 4 Crack width ≥ 0.4mm
[0104] It can be seen from Table 3 that the ozone aging resistance of rubber compositions 4, 5, and 6 containing a certain amount of antioxidant A and antioxidant B is equivalent to that of rubber composition 2 containing only antioxidant A, and is significantly better than that of rubber composition 3 containing only antioxidant B, indicating that the combined use of a certain amount of antioxidant A and a certain amount of antioxidant B can achieve excellent ozone aging resistance while reducing the amount of antioxidant A.
[0105] Test Example 3
[0106] The UV aging test was conducted according to GB / T 16585-1996 Test Method for Artificial Weathering of Vulcanized Rubber (Fluorescent UV Method). The UV lamp model is UVA, with a wavelength of 340nm and an irradiance of 0.89W / m 2 The experimental temperature was 60°C; a 4-hour UV exposure and 4-hour condensation cycle was used, and observation was made every 48 hours; a total of 240 hours of exposure was performed to observe the color change on the sample surface. The results are shown in Table 5.
[0107] The weather aging test is to place the sample in the open air and observe it every 7 days for a total of 49 days to observe the color change of the sample surface. The results are shown in Table 6.
[0108] The color change level description is shown in Table 7.
[0109] Table 5: UV aging test results
[0110] Rubber composition number 1 2 3 4 5 6 7 8 Color change level 4 1 3 1 1 1 2 2
[0111] Table 6 Weathering test results
[0112] Rubber composition number 1 2 3 4 5 6 7 8 Color change level 4 1 3 1 1 1 2 2
[0113] Table 7: Description of color change levels
[0114] grade describe 0 No discoloration 1 Minor discoloration in a small area, which requires careful comparison to be discovered 2 Slight discoloration over a larger area or all of the body, easy to spot after comparison 3 Severe discoloration in a small area can be detected directly 4 Larger areas or all severely discolored, can be directly detected
[0115] It can be seen from Table 3 that the anti-discoloration performance of rubber compositions 4, 5, and 6 containing a certain amount of antioxidant A and antioxidant B is equivalent to that of rubber composition 2 containing only antioxidant A, and is significantly better than that of rubber composition 3 containing only antioxidant B, indicating that the combined use of a certain amount of antioxidant A and a certain amount of antioxidant B can achieve excellent anti-discoloration performance while reducing the amount of antioxidant A.
Claims
1. A rubber composition, It is characterized in that The raw materials of the rubber composition include 100 parts by mass of a diene elastomer, 1.5-3 parts by mass of an antioxidant A and 0.1-1.5 parts by mass of an antioxidant B; The antioxidant A has a structure shown in Formula I: The antioxidant B has a structure shown in formula II:
2. The rubber composition according to claim 1, It is characterized in that In the raw materials of the rubber composition, the total amount of the antioxidant A and the antioxidant B is 2-4 parts by mass, for example, 2.5-3.5 parts by mass.
3. The rubber composition according to claim 1, It is characterized in that In the raw materials of the rubber composition, the mass ratio of the antioxidant A to the antioxidant B is 1:1 to 30:
1.
4. The rubber composition according to claim 1, It is characterized in that The rubber composition has one or more of the following characteristics: The diene elastomer comprises natural rubber and butadiene rubber; the mass ratio of the natural rubber to butadiene rubber is preferably 4:6-6:4; The raw materials of the rubber composition also include 0.5-3 parts by mass of sulfur; The raw materials of the rubber composition further include 30-70 parts by mass of a reinforcing filler; preferably, the reinforcing filler is carbon black; The raw materials of the rubber composition further include 1-10 parts by mass of an active agent; preferably, the active agent is ZnO; The raw materials of the rubber composition further include 1-10 parts by mass of a softener; preferably, the softener includes stearic acid and aromatic oil; The raw materials of the rubber composition further include 0.2-2 parts by mass of an accelerator; preferably, the accelerator is N-tert-butyl-2-benzothiazolesulfenamide.
5. The rubber composition according to claim 1, It is characterized in that The raw materials of the rubber composition include: 100 parts by mass of diene elastomer, 0.5-3 parts by mass of sulfur, 1.5-3 parts by mass of antioxidant A, 0.1-1.5 parts by mass of antioxidant B, 30-70 parts by mass of carbon black, 3-8 parts by mass of ZnO, 1-4 parts by mass of stearic acid, 3-8 parts by mass of aromatic oil and 0.2-2 parts by mass of N-tert-butyl-2-benzothiazolesulfonamide; wherein the diene elastomer includes natural rubber and butadiene rubber in a mass ratio of 4:6-6:
4.
6. A rubber product, It is characterized in that The rubber product contains the rubber composition according to any one of claims 1 to 5.
7. The rubber product according to claim 6, It is characterized in that The rubber product is a tire.
8. Use of a combination of antioxidant A and antioxidant B in improving the ozone aging resistance, salt spray aging resistance and anti-discoloration performance of a rubber composition, It is characterized in that The use comprises: based on 100 parts by mass of the diene elastomer contained in the raw materials of the rubber composition, adding 1.5-3.0 parts by mass of antioxidant A and 0.1-1.5 parts by mass of antioxidant B to the raw materials of the rubber composition; The antioxidant A has a structure shown in Formula I: The antioxidant B has a structure shown in formula II:
9. The use according to claim 8, It is characterized in that The total amount of the antioxidant A and the antioxidant B is 2-4 parts by mass, such as 2.5-3.5 parts by mass; and / or the mass ratio of the antioxidant A to the antioxidant B is 1:1 to 30:
1.
10. The use according to claim 8, It is characterized in that The rubber composition is as described in claim 4 or 5.