Rotational molding polyethylene composite powder as well as preparation method and application thereof

By using an organic phosphate nucleating agent in the rotomolded polyethylene composite powder, the sheet thickness of polyethylene is increased and molecular chain entanglement is reduced, and the problem of large amounts of bubble nucleating agents and bubble discharge agents in the prior art is solved. Excellent bubble discharge performance under small doses is achieved, avoiding changes in product performance and appearance.

CN119081273APending Publication Date: 2024-12-06ZHEJIANG ROTOUN PLASTIC TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411220464.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The amount of bubble nucleating agent and bubble discharge agent used in rotomolding processing in the prior art is too large, resulting in significant changes in product performance and appearance, and the excellent bubble discharge performance is difficult to achieve in small doses.

Method used

The organic phosphate nucleating agent is used to combine with a polyethylene blend to significantly increase the sheet thickness of polyethylene, reduce molecular chain entanglement, improve bubble spillover performance, and achieve excellent bubble discharge effect.

Benefits of technology

In the case of very small amounts, it has excellent bubble discharge performance, which significantly reduces the amount of bubble nucleating agent and bubble discharge agent, and avoids adverse effects on the performance and appearance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005022862260000081
    Figure BDA0005022862260000081
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, and discloses rotational molding polyethylene composite powder as well as a preparation method and application thereof.The rotational molding polyethylene composite powder comprises a polyethylene blend, an organic phosphate nucleating agent and other auxiliaries, and the mass ratio fraction of the organic phosphate nucleating agent is 0.05-0.2%; the rotational molding polyethylene composite powder comprises a polyethylene blend, an organic phosphate nucleating agent and other auxiliaries, after the organic phosphate nucleating agent is added into the polyethylene blend, the lamellar crystal thickness of polyethylene can be remarkably increased, entanglement among polyethylene molecular chains during rotational molding processing is remarkably reduced, and the rotational molding performance of polyethylene is improved. The effect that polyethylene molecular chain entanglement hinders bubble overflow is remarkably reduced, so that the phosphate nucleating agent still has excellent bubble discharging performance under the condition of extremely small dosage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a roto-molded polyethylene composite powder, a preparation method and application thereof. Background Art

[0002] Rotomolding, also known as rotational molding or rotational molding, is a thermoplastic plastic hollow molding method. This method is to first add plastic powder into the mold, then the mold is continuously rotated along the vertical axis and heated to gradually melt and adhere and evenly coat the entire surface of the mold cavity, and finally cooled and shaped into a product of the desired shape. Rotomolding is suitable for the processing of large and complex hollow plastic products, and is widely used in engineering machinery, automobiles, medical treatment, military industry, home appliances and other fields.

[0003] The bubble problem of roto-molded products is one of the core difficulties of roto-molded products. During the melting, sintering and densification of plastic powder, part of the gas will still be retained inside or on the surface of the plastic melt, resulting in bubbles on the inner surface and pinholes on the outer surface of the product. The surface pinholes will reduce the appearance of the product. At the same time, the bubbles inside the roto-molded product have formed stress concentration, which makes the plastic easy to crack around the bubbles when subjected to force. At present, the difficulty of roto-molding bubble removal is mainly related to surface tension and melt viscosity. The greater the surface tension and the smaller the melt viscosity, the higher the bubble removal performance. For example, a roto-molding defoaming masterbatch and its preparation method disclosed in Publication No. CN102952322B A preparation method is disclosed, in which a bubble nucleating agent and a bubble expelling agent are respectively used to solve the bubble problem of roto-molded products, wherein the bubble nucleating agent is calcium carbonate, clay or calcium sulfate, and the bubble expelling agent is erucamide or oleamide; in actual use, the present application has found that the bubble nucleating agent and the bubble expelling agent in the prior art require a very large amount during use to obtain excellent defoaming performance, but excessive amounts of the bubble nucleating agent and the bubble expelling agent will, on the one hand, significantly change the performance of the roto-molded product, and on the other hand, significantly change the appearance and color of the roto-molded product, so it is necessary to further improve the above-mentioned bubble nucleating agent and the bubble expelling agent. Summary of the invention

[0004] In order to overcome the problem in the prior art that the performance and appearance of roto-molded products are significantly changed due to the large dosage of bubble nucleating agents and bubble expelling agents used in polyethylene roto-molding processing, the present invention provides a roto-molded polyethylene composite powder, a preparation method and its application. The roto-molded polyethylene composite powder includes a polyethylene blend, an organic phosphate nucleating agent and other additives. After the organic phosphate nucleating agent of the present application is added to the polyethylene blend, it can significantly increase the thickness of the polyethylene lamellae, significantly reduce the entanglement between polyethylene molecular chains during roto-molding processing, and significantly reduce the effect of the entanglement of polyethylene molecular chains that hinders the overflow of bubbles, so that the phosphate nucleating agent still has excellent bubble removal performance when used in very small dosage.

[0005] The specific technical scheme of the present invention is: A rotomolded polyethylene composite powder comprises a polyethylene blend, an organic phosphate nucleating agent and other additives, wherein the mass ratio of the organic phosphate nucleating agent is 0.05-0.2%.

[0006] The present invention provides a roto-molded polyethylene composite powder, which consists of a polyethylene blend, a phosphate nucleating agent and other additives. The organic phosphate nucleating agent in the present invention has an advantage over a bubble nucleating agent and a bubble expelling agent used in combination in that the dosage is extremely small. The reason for the above difference is that when polyethylene melts and crystallizes, the increase in crystal thickness can reduce the entanglement points of polyethylene molecular chains. After the organic phosphate nucleating agent of the present application is added to the polyethylene blend, the crystallization starting temperature of the polyethylene blend increases, so that the polyethylene can have sufficient time to crystallize, thereby significantly increasing the thickness of the polyethylene lamellae. Therefore, during roto-molding processing, the polyethylene with increased lamellae thickness will have significantly reduced entanglement between its molecular chains, and the entanglement between the polyethylene molecular chains will be significantly reduced, and the hindering effect of the polyethylene molecular chains on the overflow of bubbles will also be significantly reduced, so that the phosphate nucleating agent still has excellent bubble expelling performance when used in a very small amount.

[0007] Preferably, the polyethylene blend includes one or more of high-density polyethylene, linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, and polyethylene elastomer.

[0008] Preferably, the organophosphate nucleating agent is an organophosphate metal salt and a composite thereof.

[0009] Preferably, the other additives include by mass percentage: Antioxidant 0.1-0.5%; Light stabilizer 0.05~0.3%; Processing aid 0.1~0.4%.

[0010] Preferably, the antioxidant is one or more of a hindered phenol antioxidant and a phosphite antioxidant; Preferably, the light stabilizer is one or more of a benzotriazole ultraviolet light absorber, a benzophenone ultraviolet light absorber and a triazine ultraviolet light absorber.

[0011] Preferably, the processing aid is one or more of low molecular weight polyethylene wax, fatty acid esters, stearamide and organosilicon compounds.

[0012] Preferably, the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the proportion of particles less than 100 mesh is less than 20%.

[0013] A method for preparing the above-mentioned roto-molded polyethylene composite powder comprises the following steps: mixing polyethylene blend, antioxidant, light stabilizer, processing aid and organic phosphate nucleating agent and then melt extruding to prepare roto-molded polyethylene composite powder.

[0014] Preferably, the extrusion temperature of the melt extrusion process is 150-220°C.

[0015] Preferably, the melt extrusion process uses a screw extruder, the aspect ratio of the screw extruder is 30 to 40:1, and the screw speed is 300 to 500 r / min.

[0016] The invention discloses an application of roto-molding polyethylene composite powder in roto-molding processing, wherein the roto-molding polyethylene composite powder is placed in a roto-molding mold for roto-molding to form a roto-molded product.

[0017] Compared with the prior art, this application has the following technical effects: The present invention provides a roto-molded polyethylene composite powder, a preparation method and an application thereof. The roto-molded polyethylene composite powder comprises a polyethylene blend, an organic phosphate nucleating agent and other additives. After the organic phosphate nucleating agent of the present application is added to the polyethylene blend, the thickness of the polyethylene lamellae can be significantly increased, the entanglement between polyethylene molecular chains during roto-molding processing can be significantly reduced, and the effect of the entanglement of polyethylene molecular chains hindering the overflow of bubbles can be significantly reduced, so that the phosphate nucleating agent still has excellent defoaming performance when used in a very small amount. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the embodiments.

[0019] Embodiment 1: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.2% organic phosphate nucleating agent, 0.3% antioxidant, 0.2% light stabilizer, and 0.3% processing aid; The polyethylene blend is polyethylene R546 (density 0.935g / cm 3 , melting fat is 5g / 10min, Sinopec Zhenhai Refining and Chemical); the organic phosphate nucleating agent is 2,2-methylenebis(4,6-di-tert-butylphenyl)aluminum phosphate (NAP-50, Chenghe Technology); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is the ultraviolet absorber UV-326; the processing aids are low molecular weight polyethylene wax, ethyl stearate and silicone oil; the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0020] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 40:1, screw speed of 300-500r / min) for melt extrusion, material making and powder grinding at 150-220°C to obtain rotational molding polyethylene composite powder.

[0021] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0022] Embodiment 2: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.05% organic phosphate nucleating agent, 0.35% antioxidant, 0.3% light stabilizer, and 0.3% processing aid; The polyethylene blend is polyethylene R546 (density 0.935g / cm 3 , melting fat is 5g / 10min, Sinopec Zhenhai Refining and Chemical); the organic phosphate nucleating agent is 2,2-methylenebis(4,6-di-tert-butylphenyl)aluminum phosphate (NAP-50, Chenghe Technology); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is the ultraviolet absorber UV-326; the processing aids are low molecular weight polyethylene wax, ethyl stearate and silicone oil; the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0023] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 30-40:1, screw speed of 300-500r / min) for melt extrusion, material making and powder grinding at 150-220°C to obtain rotomolded polyethylene composite powder.

[0024] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0025] Embodiment 3: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.1% organic phosphate nucleating agent, 0.2% antioxidant, 0.3% light stabilizer, and 0.4% processing aid; The polyethylene blend is polyethylene R546 (density 0.935g / cm 3, melting fat is 5g / 10min, Sinopec Zhenhai Refining and Chemical); the organic phosphate nucleating agent is 2,2-methylenebis(4,6-di-tert-butylphenyl)aluminum phosphate (NAP-50, Chenghe Technology); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is the ultraviolet absorber UV-326; the processing aids are low molecular weight polyethylene wax, ethyl stearate and silicone oil; the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0026] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 40:1, screw speed of 300-500r / min) for melt extrusion, material making and powder grinding at 150-220°C to obtain rotational molding polyethylene composite powder.

[0027] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0028] Embodiment 4: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.15% organic phosphate nucleating agent, 0.45% antioxidant, 0.2% light stabilizer, and 0.2% processing aid; The polyethylene blend is polyethylene LLD9630 (density 0.939 g / cm 3 , melting fat is 3g / 10min, Thailand PPT); the organic phosphate nucleating agent is 2,2-methylenebis(4,6-di-tert-butylphenyl)aluminum phosphate (NAP-50, Chenghe Technology); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is the ultraviolet absorber UV-326; the processing aids are low molecular weight polyethylene wax, ethyl stearate and silicone oil; the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0029] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 30:1, screw speed of 300-500r / min) for melt extrusion, material making and powder grinding at 150-220°C to obtain rotational molding polyethylene composite powder.

[0030] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0031] Embodiment 5: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.15% organic phosphate nucleating agent, 0.45% antioxidant, 0.2% light stabilizer, and 0.2% processing aid; Polyethylene blend (density 0.937g / cm 3 , melt index is 4g / 10min) is 60% polyethylene R546 (density is 0.935g / cm 3 , melt fat is 5g / 10min, Sinopec Zhenhai Refining) and 40% polyethylene LLD9630 (density is 0.939g / cm 3 , melting fat is 3g / 10min, Thailand PPT); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is ultraviolet absorber UV-326; the processing aids are low molecular polyethylene wax, ethyl stearate and silicone oil; the particle size of the roto-molded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0032] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 35:1, screw speed of 300-500r / min) at 150-220°C for melt extrusion, material making and powder grinding to obtain rotational molding polyethylene composite powder.

[0033] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0034] Embodiment 6: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.15% organic phosphate nucleating agent, 0.45% antioxidant, 0.2% light stabilizer, and 0.2% processing aid; Polyethylene blend (density 0.938g / cm 3 , melt index is 3.5g / 10min) is 30% polyethylene R546 (density is 0.935g / cm 3, melt fat is 5g / 10min, Sinopec Zhenhai Refining) and 70% polyethylene LLD9630 (density is 0.939g / cm 3 , melting fat is 3g / 10min, Thailand PPT); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is ultraviolet absorber UV-326; the processing aids are low molecular polyethylene wax, ethyl stearate and silicone oil; the particle size of the roto-molded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0035] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 35:1, screw speed of 300-500r / min) at 150-220°C for melt extrusion, material making and powder grinding to obtain rotational molding polyethylene composite powder.

[0036] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0037] Embodiment 7: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.15% organic phosphate nucleating agent, 0.45% antioxidant, 0.2% light stabilizer, and 0.2% processing aid; Polyethylene blend (density 0.937g / cm 3 , melt index is 4g / 10min) is 60% polyethylene R546 (density is 0.935g / cm 3 , melt fat is 5g / 10min, Sinopec Zhenhai Refining) and 40% polyethylene LLD9630 (density is 0.939g / cm 3 , melting fat is 3g / 10min, Thailand PPT); the organic phosphate nucleating agent is 2,2-methylenebis(4,6-di-tert-butylphenyl) zinc phosphate (composite of 2,2-methylenebis(4,6-di-tert-butylphenyl) phosphoric acid and zinc stearate); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is ultraviolet absorber UV-326; the processing aids are low molecular weight polyethylene wax, ethyl stearate and silicone oil; the particle size of the roto-molded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0038] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 35:1, screw speed of 300-500r / min) at 150-220°C for melt extrusion, material making and powder grinding to obtain rotational molding polyethylene composite powder.

[0039] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0040] Embodiment 8: A rotomolding polyethylene composite powder, comprising, by mass percentage: 99% polyethylene blend, 0.15% organic phosphate nucleating agent, 0.45% antioxidant, 0.2% light stabilizer, and 0.2% processing aid; Polyethylene blend (density 0.938g / cm 3 , melt index is 3.5g / 10min) is 30% polyethylene R546 (density is 0.935g / cm 3 , melt fat is 5g / 10min, Sinopec Zhenhai Refining) and 70% polyethylene LLD9630 (density is 0.939g / cm 3 , melting fat is 3g / 10min, Thailand PPT); the organic phosphate nucleating agent is 2,2-methylenebis(4,6-di-tert-butylphenyl) calcium phosphate (2,2-methylenebis(4,6-di-tert-butylphenyl) phosphoric acid and calcium stearate composite); the antioxidant is 2,6-di-tert-butyl-4-methylphenol; the light stabilizer is ultraviolet absorber UV-326; the processing aids are low molecular weight polyethylene wax, ethyl stearate and silicone oil; the particle size of the roto-molded polyethylene composite powder is less than 30 mesh and the composition less than 100 mesh is less than 20%.

[0041] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 35:1, screw speed of 300-500r / min) at 150-220°C for melt extrusion, material making and powder grinding to obtain rotational molding polyethylene composite powder.

[0042] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0043] Comparative Example 1: Compared with Examples 1, 2, 3, 7 and 8, no organic phosphate nucleating agent was used in Comparative Example 1; the other conditions were the same as those in Example 1.

[0044] Comparative Example 2: Compared with Example 4, no organic phosphate nucleating agent was used in Comparative Example 2; the other conditions were the same as those in Example 4.

[0045] Comparative Example 3: Compared with Example 5, no organic phosphate nucleating agent was used in Comparative Example 3; the other conditions were the same as those in Example 5.

[0046] Comparative Example 4: Compared with Example 6, no organic phosphate nucleating agent was used in Comparative Example 4; the other conditions were the same as those in Example 5.

[0047] Comparative Example 5: Comparative Example 5 adopts the method in the prior art CN102952322B, adding a bubble nucleating agent and a bubble defoaming agent, wherein the bubble nucleating agent is calcium carbonate and the bubble defoaming agent is erucamide; A rotomolding polyethylene composite powder comprises, by mass percentage, 77% polyethylene blend, 16% calcium carbonate (1000-2500 mesh) as a bubble nucleating agent, 6% erucic acid amide as a bubble degassing agent, 0.5% antioxidant, 0.2% light stabilizer, and 0.3% processing aid; The polyethylene blend is polyethylene R546 (density 0.935g / cm 3 , melting fat is 5g / 10min, Sinopec Zhenhai Refining and Chemical); antioxidant is; light stabilizer is; processing aid is; the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the composition is less than 100 mesh and is less than 20%.

[0048] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 35:1, screw speed of 300-500r / min) at 150-220°C for melt extrusion, material making and powder grinding to obtain rotational molding polyethylene composite powder.

[0049] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0050] Comparative Example 6: Comparative Example 6 adopts the method in CN102952322B in the prior art, adding a bubble nucleating agent and a bubble defoaming agent, wherein the bubble nucleating agent is calcium carbonate and the bubble defoaming agent is erucamide; A rotomolding polyethylene composite powder comprises, by mass percentage, 99% polyethylene blend, 0.1% calcium carbonate (1000-2500 mesh) as a bubble nucleating agent, 0.1% erucic acid amide as a bubble degassing agent, 0.3% antioxidant, 0.2% light stabilizer, and 0.3% processing aid; The polyethylene blend is polyethylene R546 (density 0.935g / cm 3 , melting fat is 5g / 10min, Sinopec Zhenhai Refining and Chemical); antioxidant is; light stabilizer is; processing aid is; the particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the composition is less than 100 mesh and is less than 20%.

[0051] A method for preparing the above-mentioned rotomolded polyethylene composite powder comprises the following steps: The polyethylene blend, organic phosphate nucleating agent, antioxidant, light stabilizer and processing aid are uniformly mixed to obtain a mixture, and then the mixture is injected into a twin-screw extruder (length-to-diameter ratio of 35:1, screw speed of 300-500r / min) at 150-220°C for melt extrusion, material making and powder grinding to obtain rotational molding polyethylene composite powder.

[0052] An application of the above roto-molded polyethylene composite powder in roto-molding processing comprises the following steps: roto-molding the roto-molded polyethylene composite powder in a roto-molding model (a cube with a side length of 30 cm and a thickness of 4 mm) to form a roto-molded product.

[0053] Test example 1: The bubble removal performance of the rotomolded products obtained in the above Examples 1 to 8 and Comparative Examples 1 to 6 was tested. The bubble removal performance test items included: surface visual inspection and cross-section visual inspection; the test results are shown in Table 1; Table 1 Test results of bubble removal performance of rotomolded products As shown in Table 1, Examples 1 to 8 are roto-molded products made of roto-molded polyethylene composite powder using an organic phosphate nucleating agent. The results of Examples 1 to 8 show that the roto-molded products of the present invention using an organic phosphate nucleating agent have no foam on the surface and inside, and have excellent defoaming properties.

[0054] No organophosphate nucleating agent was used in Comparative Examples 1 to 4. Generally, in the prior art, the defoaming performance of the polyethylene melt can be promoted by increasing the processing temperature. Therefore, when the maximum temperature in the mold (PIAT) reaches a certain temperature, the residual bubble amount of the roto-molded polyethylene product is 0%. The results of Comparative Examples 1 to 4 and Examples 1 to 8 show that when no organophosphate nucleating agent is added, the temperature of PIAT can reach 220-230°C. After the organophosphate nucleating agent is added in the present application, the temperature of PIAT can be reduced to 190-200°C, which can significantly reduce the energy consumption of the roto-molding process and significantly improve the production efficiency of the roto-molding process.

[0055] The results of Comparative Examples 5 to 6 show that when bubble nucleating agents and bubble expelling agents are used, the amount of bubble nucleating agent is extremely large, and the amount of bubble nucleating agent must reach more than 15% to have excellent defoaming performance. When the amount of bubble nucleating agent and bubble expelling agent is reduced to the amount of organic phosphate nucleating agent in the present application, obvious bubbles appear in the rotationally molded products obtained, indicating that when the amount of bubble nucleating agent and bubble expelling agent is small, the defoaming performance is poor; in addition, the use of a large amount of bubble nucleating agent and bubble expelling agent will also cause significant changes in the performance of polyethylene resin, affecting the quality of the rotationally molded product.

[0056] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A rotomolded polyethylene composite powder, characterized in that: The invention comprises a polyethylene blend, an organic phosphate nucleating agent and other additives, wherein the mass ratio of the organic phosphate nucleating agent is 0.05-0.2%.

2. The rotomolded polyethylene composite powder according to claim 1, characterized in that: The polyethylene blend includes one or more of high-density polyethylene, linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, and polyethylene elastomer.

3. The rotomolded polyethylene composite powder according to claim 1, characterized in that: The organic phosphate nucleating agent is an organic phosphate metal salt and a compound thereof.

4. The rotomolded polyethylene composite powder according to claim 1, characterized in that: The other additives include by mass percentage: Antioxidant 0.1~0.5%; Light stabilizer 0.05~0.3%; Processing aids 0.1~0.4%.

5. The rotomolded polyethylene composite powder according to claim 4, characterized in that: The antioxidant is one or more of a hindered phenol antioxidant and a phosphite antioxidant; The light stabilizer is one or more of a benzotriazole ultraviolet light absorber, a benzophenone ultraviolet light absorber and a triazine ultraviolet light absorber; The processing aid is one or more of low molecular weight polyethylene wax, fatty acid esters, fatty acid amides and organosilicon compounds.

6. The rotomolded polyethylene composite powder according to claim 1, characterized in that: The particle size of the rotomolded polyethylene composite powder is less than 30 mesh and the proportion of particles less than 100 mesh is less than 20%.

7. A method for preparing a rotomolded polyethylene composite powder according to any one of claims 1 to 6, characterized in that: The following steps are involved: The polyethylene blend, antioxidant, light stabilizer, processing aid and organic phosphate nucleating agent are mixed and then melt-extruded to prepare rotomolding polyethylene composite powder.

8. The method for preparing rotomolded polyethylene composite powder according to claim 6, characterized in that: The extrusion temperature of the melt extrusion process is 150-220°C.

9. The rotomolded polyethylene composite powder according to claim 6 or 7, characterized in that: The melt extrusion process adopts a screw extrusion device, the aspect ratio of the screw extrusion device is 30-40:1, and the screw speed is 300-500 r / min.

10. An application of a roto-molding polyethylene composite powder in roto-molding processing, characterized in that: The roto-molded polyethylene composite powder according to any one of claims 1 to 6 is placed in a roto-molding mold for roto-molding to form a roto-molded product.

Citation Information

Patent Citations

  • Defoaming master batch for rotational molding and preparation method thereof

    CN102952322B