Macromolecular nano heat-insulating color water-based finishing paint and preparation method thereof
By applying polymer nano-insulated color water-based topcoat on the vehicle, using nanomaterials and other components to block the outside heat, the problem of temperature increase in the vehicle is solved, and the effect of energy saving and emission reduction and vehicle life is achieved.
Patent Information
- Application Number
- CN202411366132.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
AI Technical Summary
Existing vehicle paint cannot effectively block the transmission of heat outside the vehicle into the vehicle, causing the temperature inside the vehicle to rise, increasing electricity consumption and vehicle energy consumption, shortening the service life of the vehicle, and posing a threat to the safety of passengers.
Using polymer nano-insulated color water-based topcoat, the combination of polymer aqueous single-component acrylic resin, nanomaterials, deionized water, alcohol cosolvents, pigments, leveling agents and adhesion promoters is applied to the vehicle. , a topcoat with high heat insulation rate, good leveling properties and bright colors were prepared to prevent heat transfer from outside the vehicle.
Effectively reduce the temperature inside the car, save electricity consumption, extend the vehicle's range, protect the environment, extend the vehicle's service life, and indirectly improve the safety of passengers.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of polymer coatings for vehicles, in particular to a polymer nano heat-insulating colored water-based topcoat and a preparation method thereof. Background Art
[0002] On December 3, 2015, our company was authorized to obtain the invention patent for "A kind of vehicle paint", with the patent number "ZL201310218567.1", and on November 17, 2020, it was authorized to obtain the invention patent for "A kind of environmentally friendly water-based automotive metallic glitter paint and its preparation method", with the patent number "ZL201811169790.0", and on October 26, 2021, it was authorized to obtain the invention patent for "A self-healing water-based polyurethane coating composition and coating", with the patent number "ZL202010748471.6". Through these three patented technologies, a series of vehicle topcoats of various colors can be produced with water-based hydroxyl acrylic resin, water-based alkyd resin, and water-based polyester resin as the main film-forming substances, with the addition of leveling agent, drying agent, and alcohol organic solvents such as n-butanol. By mixing these topcoats in different proportions, topcoats of various colors for different vehicles can be obtained, and by spraying with a spray gun, a bright-colored coating can be obtained on the vehicle body.
[0003] Before the invention of this technology, vehicle paint only has the function of anti-corrosion for vehicle sheet metal and beautification of the vehicle. With the rise and popularization of new energy vehicles, energy is an important source of power for various vehicles, and energy consumption is crucial. Whether it is a pure electric vehicle (BEV), a hybrid electric vehicle (HEV) or a fuel cell vehicle (FCEV), energy consumption determines the range of new energy vehicles, and even more determines human protection of the atmosphere and the environment.
[0004] Tests have shown that when a car is exposed to the sun for a long time at a high temperature of 40°C outdoors, the temperature inside the car is above 70 degrees and can reach up to 90 degrees. At this time, after starting the vehicle, it is necessary to use air conditioning to cool the temperature inside the car. In this cooling process, a lot of energy is needed for cooling. In summer, when the vehicle is driving under the scorching sun, a lot of energy is also needed to cool the car so that passengers can ride in a comfortable temperature. When the vehicle is exposed outdoors, it is not only the problem of high temperature inside the car, but also many plastic parts and circuits inside and outside the car will accelerate aging. If it continues for a long time, it will cause serious damage to the vehicle, reduce the service life of the vehicle, and also threaten the personal safety of the passengers.
[0005] At present, all vehicles require a lot of electricity for air conditioning and cooling. The outdoor temperature and the temperature setting inside the car directly determine the amount of electricity consumed. Now many electric vehicles consume 1%-5% of the battery power per hour (different manufacturers have different consumption). Turning on the air conditioner in a gasoline vehicle will also increase the consumption of gasoline or diesel, which means that turning on the air conditioner will reduce the vehicle's range and increase the vehicle's energy consumption. How to effectively block the heat outside the car from being transferred to the inside of the car through the body coating is a technology that is worth studying.
[0006] In order to solve the above problems, the car body can be coated with a heat-insulating topcoat when it leaves the factory or is repaired, which can block the heat outside the car from being transferred into the car, reduce the impact of the outside temperature on the temperature inside the car, and make the temperature inside the car rise slightly or not rise at all, which will inevitably save the consumption of electricity, extend the vehicle's cruising range, achieve energy conservation and emission reduction, and protect the atmosphere and environment. At the same time, it can also extend the service life of the vehicle and indirectly protect the lives of passengers. After years of research and development, our company has developed a polymer nano-insulating color water-based topcoat and its preparation method, and at the same time transformed the preparation method into a series of nano-insulating topcoat products for vehicles, which effectively solves and reduces the problem of energy consumption of vehicle air conditioning. Summary of the invention
[0007] The purpose of the present invention is to provide a polymer nano thermal insulation color water-based topcoat for vehicles and a preparation method thereof, so as to solve the problems raised in the above background technology. To achieve the above purpose, the present invention provides the following technical solutions:
[0008] A polymer nano thermal insulation colored water-based topcoat comprises the following materials in parts by weight: 50-70 parts of polymer water-based single-component acrylic resin, 2-15 parts of nano materials, 5-20 parts of deionized water, 2-10 parts of alcohol cosolvent, 1-30 parts of pigment, 0.1-5 parts of leveling agent, 1-10 parts of dispersant and 0.5-1 parts of adhesion promoter.
[0009] As a further solution of the present invention: the following materials are included in parts by weight: 40-60 parts of polymer water-based single-component acrylic resin, 1-12 parts of nanomaterials, 5-15 parts of deionized water, 1-8 parts of alcohol cosolvent, 2-25 parts of pigment, 0.1-3 parts of leveling agent, 1-5 parts of dispersant, and 0.2-3 parts of adhesion promoter.
[0010] As a further solution of the present invention: the following materials are included in parts by weight: 40-65 parts of polymer water-based single-component acrylic resin, 2-10 parts of nanomaterials, 3-10 parts of deionized water, 2-5 parts of alcohol cosolvent, 3-35 parts of pigment, 0.2-3 parts of leveling agent, 2-5 parts of dispersant, and 0.1-3 parts of adhesion promoter.
[0011] As a further solution of the present invention: the following materials are included in parts by weight: 45-70 parts of polymer water-based single-component acrylic resin, 1-15 parts of nanomaterials, 4-10 parts of deionized water, 2-8 parts of alcohol cosolvent, 2-10 parts of pigment, 0.1-2 parts of leveling agent, 1-4 parts of dispersant, and 0.2-3 parts of adhesion promoter.
[0012] As a further solution of the present invention: the high molecular weight water-based single-component acrylic resin is a water-based single-component acrylic resin with a solid content of 40-70%, the drying temperature of the resin is 5-180°C, the room temperature drying time is less than 12 hours, and the baking drying time is less than 10 minutes. It can be any model product of any manufacturer.
[0013] As a further solution of the present invention: the nanomaterial is modified ATO nano-slurry, nano-ITO dispersion, nano-ATO dispersion, nano-ITO, nano-GTO insulation powder, nano-zirconium oxide, nano-AZO, silica aerogel powder or silica aerogel paste. According to the thermal insulation performance and cost control, at least one or more combinations are used. The nanomaterial has a low thermal conductivity (after drying, 25°C) of 0.001 to 3W / (m·K) and a particle size of 0.1 to 20μm.
[0014] As a further solution of the present invention: the deionized water is obtained by an industrial pure water machine.
[0015] As a further embodiment of the present invention: the pigment is an organic pigment and an inorganic pigment, and the pigment can be titanium dioxide or light-fast yellow or isoindoline yellow or cadmium yellow or medium chrome yellow or iron oxide yellow or toluidine red or iron oxide red or phthalocyanine blue or indanthrene blue or phthalocyanine green or carbon black or silver powder or mica pearl powder or purple, etc.
[0016] As a further solution of the present invention: the leveling agent is an organic silicon leveling agent, an acrylate leveling agent, or a fluorine-modified leveling agent, which can be any one of them, or a combination of any two or any three of them in any proportion.
[0017] As a further solution of the present invention: the dispersant is selected from anionic wetting and dispersing agents, nonionic wetting and dispersing agents, electrically neutral wetting and dispersing agents, or polymeric super dispersants according to the type of pigment selected.
[0018] As a further solution of the present invention: the adhesion promoter is a silane coupling agent, which has good compatibility with the selected water-based single-component acrylic resin, and the product can be of any model from any manufacturer.
[0019] A preparation method of a polymer nano thermal insulation color water-based topcoat comprises the following steps:
[0020] S1. Prepare raw materials and test each material according to the standards;
[0021] S2. Weigh a high molecular weight water-based single-component acrylic resin by weight and slowly add it into a container, and slowly add the above-mentioned deionized water, alcohol cosolvent, dispersant, leveling agent, and adhesion promoter under stirring, and disperse it at a speed of 500-800r / min in an explosion-proof disperser for 10-20min, and slowly add pigment under stirring, and disperse it at a speed of 500-800r / min in an explosion-proof disperser for 10min; obtain a mixed color paste;
[0022] S3, grinding the mixed color paste obtained in S2 with a sand mill, and testing the fineness with a fineness meter after each grinding. When the fineness of the mixed color paste is ≤20 μm, stop grinding, weigh the mixed color paste, and make up the weight lost by volatilization during the grinding process with deionized water;
[0023] At the same time, in this step, 20% by weight of the high molecular water-based single-component acrylic resin and 20% by weight of deionized water are reserved, 15% by weight of the high molecular water-based single-component acrylic resin and 15% by weight of deionized water are used to clean the sand mill, and the remaining 5% by weight of the high molecular water-based single-component acrylic resin and 5% by weight of deionized water are used to adjust the viscosity of the nano-color paste mixture;
[0024] S4. Use an explosion-proof disperser to disperse the color paste with qualified fineness at a speed of 200-300r / min. Under stirring, slowly add the nanomaterial, gradually increase the dispersion speed to 800r / min, and disperse for 30 minutes to obtain a nano color paste mixture;
[0025] The various indicators of the nano-color paste mixture prepared by S5 and S4 are tested. During the test, if the fineness is unqualified, it is quickly ground again with a sand mill until the fineness is qualified. When the viscosity is higher than 202s, add an appropriate amount of deionized water reserved in S2 to lower it. When the viscosity is less than 198s, add the high molecular water-based single-component acrylic resin reserved in S2 to increase it. Pay special attention to the fact that when measuring the viscosity, the coating 4 cups itself is also required to be 25℃±1. When the indoor temperature is higher than 26℃, the coating 4 cups needs to be cooled with a refrigerator or ice cubes. When the indoor temperature is less than 24℃, the coating 4 cups needs to be heated with an oven. The specific indicators are shown in the table below:
[0026]
[0027] S6. Filter the qualified nano-color paste mixture with a 200-mesh filter cloth.
[0028] The above-mentioned vehicle polymer nano thermal insulation water-based topcoat of various colors is used in the field of coating preparation.
[0029] Compared with the prior art, the beneficial effects of the present invention are: a kind of polymer nano thermal insulation water-based topcoat of various colors for vehicles is realized, and the polymer water-based single-component acrylic resin is used as the main material, and by adding nano materials, alcohol cosolvents, deionized water, different pigments, dispersants, leveling agents, adhesion promoters, and certain detection indicators, a series of topcoats with high thermal insulation rate, good leveling, bright colors, no floating color, easy color adjustment, good weather resistance, and low VOC content can be prepared. After being applied to the vehicle spraying, the heat outside the vehicle is blocked from being transferred to the inside of the vehicle, and the influence of the outside temperature on the temperature inside the vehicle is reduced, so that the temperature inside the vehicle is slightly increased or not increased, the temperature inside the vehicle is reduced, the power is saved, the vehicle's cruising range is increased, energy saving and emission reduction are achieved, and the protection of the atmosphere and the environment is improved. At the same time, it can extend the service life of the vehicle and indirectly protect the life safety of passengers. This product has high thermal insulation, is easy to adjust color, does not float, is easy to construct, has high construction efficiency, good surface effect, good weather resistance, low VOC content and low emissions. It can be widely used in original vehicle body spraying. It can be dried at room temperature for 10-15 minutes, or it can be baked at 120-180℃ for 2-5 minutes to dry. The construction efficiency is very high. DETAILED DESCRIPTION
[0030] In order to make the public better understand the present invention, the technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.
[0031] Implementation Example 1
[0032] A preparation method for a polymer nano thermal insulation colored water-based topcoat for vehicles comprises the following materials in parts by weight: 50-70 parts of a polymer water-based single-component acrylic resin, 2-15 parts of a nano material, 5-20 parts of deionized water, 2-10 parts of an alcohol cosolvent, 1-30 parts of a pigment, 0.1-5 parts of a leveling agent, 1-10 parts of a dispersant, and 0.5-1 parts of an adhesion promoter.
[0033] Specifically, in this embodiment, the polymer water-based one-component acrylic resin is a water-based one-component acrylic resin with a solid content of 40-70%, the drying temperature of the resin is 5-180°C, the room temperature drying time is less than 12 hours, and the baking drying time is less than 10 minutes; it can be imported or domestic;
[0034] Specifically, in this embodiment, the nanomaterial is a modified ATO nano-slurry, a nano-ITO dispersion, a nano-ATO dispersion, a nano-ITO, a nano-GTO thermal insulation powder, a nano-zirconium oxide, a nano-AZO, a silica aerogel powder or a silica aerogel paste. According to the thermal insulation performance and cost control, at least one or more combinations are used. The nanomaterial has a low thermal conductivity (after drying, 25° C.) of 0.001 to 3 W / (m·K) and a particle size of 0.1 to 20 μm.
[0035] Specifically, in this embodiment, the alcohol co-solvent used is n-butanol, isobutanol or isopropanol.
[0036] Specifically, in this embodiment, the deionized water used is obtained from an industrial pure water machine;
[0037] Specifically, in this embodiment, the pigment is an organic pigment and an inorganic pigment, and the pigment can be titanium dioxide or light-fast yellow or isoindoline yellow or cadmium yellow or medium chrome yellow or iron oxide yellow or toluidine red or iron oxide red or phthalocyanine blue or indanthrene blue or phthalocyanine green or carbon black or silver powder or mica pearl powder or purple, etc.
[0038] Specifically, in this embodiment, the leveling agent is a silicone leveling agent, an acrylate leveling agent, a fluorine-modified leveling agent, and products of manufacturers such as BYK, BASF, and Axal can be used;
[0039] Specifically, in this embodiment, the dispersant is an anionic wetting dispersant, a nonionic wetting dispersant, an electrically neutral wetting dispersant, or a polymeric super dispersant, and the manufacturer is not limited;
[0040] Specifically, in this embodiment, the adhesion promoter is a silane coupling agent, which has good compatibility with the selected water-based one-component acrylic resin, and the product can be any model from any manufacturer;
[0041] Implementation Example 2
[0042] A preparation method for a polymer nano thermal insulation colored water-based topcoat for vehicles comprises the following materials in parts by weight: 40-60 parts of a polymer water-based single-component acrylic resin, 1-12 parts of a nano material, 5-15 parts of deionized water, 1-8 parts of an alcohol cosolvent, 2-25 parts of a pigment, 0.1-3 parts of a leveling agent, 1-5 parts of a dispersant, and 0.2-3 parts of an adhesion promoter.
[0043] Specifically, in this embodiment, the polymer water-based one-component acrylic resin is a water-based one-component acrylic resin with a solid content of 40-70%, the drying temperature of the resin is 5-180°C, the room temperature drying time is less than 12 hours, and the baking drying time is less than 10 minutes; it can be imported or domestic;
[0044] Specifically, in this embodiment, the nanomaterial is a modified ATO nano-slurry, a nano-ITO dispersion, a nano-ATO dispersion, a nano-ITO, a nano-GTO thermal insulation powder, a nano-zirconium oxide, a nano-AZO, a silica aerogel powder or a silica aerogel paste. According to the thermal insulation performance and cost control, at least one or more combinations are used. The nanomaterial has a low thermal conductivity (after drying, 25° C.) of 0.001 to 3 W / (m·K) and a particle size of 0.1 to 20 μm.
[0045] Specifically, in this embodiment, the alcohol co-solvent used is n-butanol, isobutanol or isopropanol.
[0046] Specifically, in this embodiment, the deionized water used is obtained from an industrial pure water machine;
[0047] Specifically, in the present embodiment, the pigment is yellow pigment such as 81# yellow, 83# yellow, lemon yellow, 2900 medium chrome yellow, iron oxide yellow, etc., or rutile titanium dioxide pigment, or green pigment such as phthalocyanine green, or high-pigment or low-pigment carbon black pigment, or red pigment such as Lithol Red, Pigment Red 179, Pigment Red 122, or iron oxide red, or phthalocyanine blue pigment such as 15:3, 15:1, or 15:4, or aluminum silver paste pigment such as non-leafing silver or silver flash, or colored aluminum silver paste pigment, or colored mica pigment such as white, red, blue, green, or purple;
[0048] Specifically, in this embodiment, the leveling agent is a silicone leveling agent, an acrylate leveling agent, a fluorine-modified leveling agent, and can be products of manufacturers such as BYK, BASF, and Axalta, or can be products of domestic manufacturers;
[0049] Specifically, in this embodiment, the dispersant is an anionic wetting dispersant or a nonionic wetting dispersant or an electrically neutral wetting dispersant or a polymeric super dispersant, and can be a product of an imported manufacturer such as Efka, BYK, BASF, or a product of a domestic manufacturer;
[0050] Specifically, in this embodiment, the adhesion promoter is a silane coupling agent, which has good compatibility with the selected water-based one-component acrylic resin, and the product can be any model from any manufacturer;
[0051] Implementation Example 3
[0052] A preparation method for a polymer nano thermal insulation colored water-based topcoat for vehicles comprises the following materials in parts by weight: 40-65 parts of a polymer water-based single-component acrylic resin, 2-10 parts of a nano material, 3-10 parts of deionized water, 2-5 parts of an alcohol cosolvent, 3-35 parts of a pigment, 0.2-3 parts of a leveling agent, 2-5 parts of a dispersant, and 0.1-3 parts of an adhesion promoter.
[0053] Specifically, in this embodiment, the polymer water-based one-component acrylic resin is a water-based one-component acrylic resin with a solid content of 40-70%, the drying temperature of the resin is 5-180°C, the room temperature drying time is less than 12 hours, and the baking drying time is less than 10 minutes; it can be imported or domestic;
[0054] Specifically, in this embodiment, the nanomaterial is a modified ATO nano-slurry, a nano-ITO dispersion, a nano-ATO dispersion, a nano-ITO, a nano-GTO thermal insulation powder, a nano-zirconium oxide, a nano-AZO, a silica aerogel powder or a silica aerogel paste. According to the thermal insulation performance and cost control, at least one or more combinations are used. The nanomaterial has a low thermal conductivity (after drying, 25° C.) of 0.001 to 3 W / (m·K) and a particle size of 0.1 to 20 μm.
[0055] Specifically, in this embodiment, the alcohol co-solvent used is n-butanol, isobutanol or isopropanol.
[0056] Specifically, in this embodiment, the deionized water used is obtained from an industrial pure water machine;
[0057] Specifically, in the present embodiment, the pigment is yellow pigment such as 81# yellow, 83# yellow, lemon yellow, 2900 medium chrome yellow, iron oxide yellow, etc., or rutile titanium dioxide pigment, or green pigment such as phthalocyanine green, or high-pigment or low-pigment carbon black pigment, or red pigment such as Lithol Red, Pigment Red 179, Pigment Red 122, or iron oxide red, or phthalocyanine blue pigment such as 15:3, 15:1, or 15:4, or aluminum silver paste pigment such as non-leafing silver or silver flash, or colored aluminum silver paste pigment, or colored mica pigment such as white, red, blue, green, or purple;
[0058] Specifically, in this embodiment, the leveling agent is a silicone leveling agent, an acrylate leveling agent, a fluorine-modified leveling agent, and can be products of manufacturers such as BYK, BASF, and Axalta, or can be products of domestic manufacturers;
[0059] Specifically, in this embodiment, the dispersant is an anionic wetting dispersant or a nonionic wetting dispersant or an electrically neutral wetting dispersant or a polymeric super dispersant, and can be a product of an imported manufacturer such as Efka, BYK, BASF, or a product of a domestic manufacturer;
[0060] Specifically, in this embodiment, the adhesion promoter is a silane coupling agent, which has good compatibility with the selected water-based one-component acrylic resin, and the product can be any model from any manufacturer;
[0061] Implementation Example 4
[0062] A preparation method for a polymer nano thermal insulation colored water-based topcoat for vehicles comprises the following materials in parts by weight: 45-70 parts of a polymer water-based single-component acrylic resin, 1-15 parts of a nano material, 4-10 parts of deionized water, 2-8 parts of an alcohol cosolvent, 2-10 parts of a pigment, 0.1-2 parts of a leveling agent, 1-4 parts of a dispersant, and 0.2-3 parts of an adhesion promoter.
[0063] Specifically, in this embodiment, the polymer water-based one-component acrylic resin is a water-based one-component acrylic resin with a solid content of 40-70%, the drying temperature of the resin is 5-180°C, the room temperature drying time is less than 12 hours, and the baking drying time is less than 10 minutes; it can be imported or domestic;
[0064] Specifically, in this embodiment, the nanomaterial is a modified ATO nano-slurry, a nano-ITO dispersion, a nano-ATO dispersion, a nano-ITO, a nano-GTO thermal insulation powder, a nano-zirconium oxide, a nano-AZO, a silica aerogel powder or a silica aerogel paste. According to the thermal insulation performance and cost control, at least one or more combinations are used. The nanomaterial has a low thermal conductivity (after drying, 25° C.) of 0.001 to 3 W / (m·K) and a particle size of 0.1 to 20 μm.
[0065] Specifically, in this embodiment, the alcohol co-solvent used is n-butanol, isobutanol or isopropanol.
[0066] Specifically, in this embodiment, the deionized water used is obtained from an industrial pure water machine;
[0067] Specifically, in the present embodiment, the pigment is yellow pigment such as 81# yellow, 83# yellow, lemon yellow, 2900 medium chrome yellow, iron oxide yellow, etc., or rutile titanium dioxide pigment, or green pigment such as phthalocyanine green, or high-pigment or low-pigment carbon black pigment, or red pigment such as Lithol Red, Pigment Red 179, Pigment Red 122, or iron oxide red, or phthalocyanine blue pigment such as 15:3, 15:1, or 15:4, or aluminum silver paste pigment such as non-leafing silver or silver flash, or colored aluminum silver paste pigment, or colored mica pigment such as white, red, blue, green, or purple;
[0068] Specifically, in this embodiment, the leveling agent is a silicone leveling agent, an acrylate leveling agent, a fluorine-modified leveling agent, and can be products of manufacturers such as BYK, BASF, and Axalta, or can be products of domestic manufacturers;
[0069] Specifically, in this embodiment, the dispersant is an anionic wetting dispersant or a nonionic wetting dispersant or an electrically neutral wetting dispersant or a polymeric super dispersant, and can be a product of an imported manufacturer such as Efka, BYK, BASF, or a product of a domestic manufacturer;
[0070] Specifically, in this embodiment, the adhesion promoter is a silane coupling agent, which has good compatibility with the selected water-based one-component acrylic resin, and the product can be any model from any manufacturer;
[0071] A preparation method of a polymer nano thermal insulation color water-based topcoat for a vehicle comprises the following steps:
[0072] S1. Prepare raw materials and test each material according to the standards;
[0073] S2. Weigh a high molecular weight water-based single-component acrylic resin by weight and slowly add it into a container, and slowly add the above-mentioned deionized water, alcohol cosolvent, dispersant, leveling agent, and adhesion promoter under stirring, and disperse it at a speed of 500-800r / min in an explosion-proof disperser for 10-20min, and slowly add pigment under stirring, and disperse it at a speed of 500-800r / min in an explosion-proof disperser for 10min; obtain a mixed color paste;
[0074] S3, grinding the mixed color paste obtained in S2 with a sand mill, and testing the fineness with a fineness meter after each grinding. When the fineness of the mixed color paste is ≤20 μm, stop grinding, weigh the mixed color paste, and make up the weight lost by volatilization during the grinding process with deionized water;
[0075] At the same time, in this step, 20% by weight of the high molecular water-based single-component acrylic resin and 20% by weight of deionized water are reserved, 15% by weight of the high molecular water-based single-component acrylic resin and 15% by weight of deionized water are used to clean the sand mill, and the remaining 5% by weight of the high molecular water-based single-component acrylic resin and 5% by weight of deionized water are used to adjust the viscosity of the nano-color paste mixture;
[0076] S4. Use an explosion-proof disperser to disperse the color paste with qualified fineness at a speed of 200-300r / min. Under stirring, slowly add the nanomaterial, gradually increase the dispersion speed to 800r / min, and disperse for 30 minutes to obtain a nano color paste mixture;
[0077] The various indicators of the nano-color paste mixture prepared by S5 and S4 are tested. During the test, if the fineness is unqualified, it is quickly ground again with a sand mill until the fineness is qualified. When the viscosity is higher than 202s, add an appropriate amount of deionized water reserved in S2 to lower it. When the viscosity is less than 198s, add the high molecular water-based single-component acrylic resin reserved in S2 to increase it. Pay special attention to the fact that when measuring the viscosity, the coating 4 cups itself is also required to be 25℃±1. When the indoor temperature is higher than 26℃, the coating 4 cups needs to be cooled with a refrigerator or ice cubes. When the indoor temperature is less than 24℃, the coating 4 cups needs to be heated with an oven. The specific indicators are shown in the table below:
[0078]
[0079] S6. Filter the qualified nano-color paste mixture with a 200-mesh filter cloth.
[0080] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
[0081] The above-mentioned polymer nano thermal insulation color water-based topcoat for vehicles is used in the field of coating preparation.
[0082] In addition, compared with the various color topcoats used for vehicles in the prior art, the key is to use nanomaterials with low thermal conductivity, which can effectively block the increase in the temperature inside the vehicle caused by the external heat of the vehicle, reduce the temperature inside the vehicle, and reduce the energy consumption of air conditioning, which can greatly increase the vehicle's mileage, save energy and reduce emissions, and improve the protection of the atmosphere and the environment. At the same time, it can extend the service life of the vehicle and indirectly protect the lives of passengers. The product has high thermal insulation rate, easy color adjustment, no floating color, easy construction, high construction efficiency, good surface effect, good weather resistance, low VOC content and emission, and can be widely used in original vehicle body spraying and vehicle after-sales body repair.
[0083] The comparison of the external and internal temperatures of vehicles after various colored topcoat products prepared by a method for preparing a polymer nano thermal insulation colored water-based topcoat are sprayed on the vehicle body surface and after various colored topcoat products are sprayed on the vehicle body surface for ordinary vehicles is as follows:
[0084]
[0085] It can be seen from the above table that the use of the polymer nano thermal insulation color water-based topcoat for vehicles of the present invention can obtain a significant thermal insulation effect.
Claims
1. A polymer nano thermal insulation color water-based topcoat for vehicles, characterized in that The invention comprises the following materials in parts by weight: 50-70 parts of high molecular water-based single-component acrylic resin, 2-15 parts of nanomaterials, 5-20 parts of deionized water, 2-10 parts of alcohol auxiliary solvents, 1-30 parts of pigments, 0.1-5 parts of leveling agents, 1-10 parts of dispersants and 0.5-1 parts of adhesion promoters.
2. The vehicle-use polymer nano thermal insulation color water-based topcoat according to claim 1, characterized in that The invention comprises the following materials in parts by weight: 40-60 parts of high molecular water-based single-component acrylic resin, 1-12 parts of nanomaterials, 5-15 parts of deionized water, 1-8 parts of alcohol auxiliary solvents, 2-25 parts of pigments, 0.1-3 parts of leveling agents, 1-5 parts of dispersants and 0.2-3 parts of adhesion promoters.
3. The vehicle-use polymer nano thermal insulation color water-based topcoat according to claim 1, characterized in that The invention comprises the following materials in parts by weight: 40-65 parts of high molecular water-based single-component acrylic resin, 2-10 parts of nanomaterials, 3-10 parts of deionized water, 2-5 parts of alcohol auxiliary solvents, 3-35 parts of pigments, 0.2-3 parts of leveling agents, 2-5 parts of dispersants and 0.1-3 parts of adhesion promoters.
4. The vehicle-use polymer nano thermal insulation color water-based topcoat according to claim 1, characterized in that The invention comprises the following materials in parts by weight: 45-70 parts of high molecular water-based single-component acrylic resin, 1-15 parts of nanomaterials, 4-10 parts of deionized water, 2-8 parts of alcohol auxiliary solvents, 2-10 parts of pigments, 0.1-2 parts of leveling agents, 1-4 parts of dispersants and 0.2-3 parts of adhesion promoters.
5. The polymer nano thermal insulation color water-based topcoat for vehicles according to any one of claims 1 to 4, characterized in that The polymer water-based single-component acrylic resin used in the various color water-based topcoat for vehicles is a water-based single-component acrylic resin with a solid content of 40-70%. The drying temperature of the resin is 5-180°C, the room temperature drying time is less than 12 hours, and the baking drying time is less than 10 minutes.
6. The polymer nano thermal insulation color water-based topcoat for vehicles according to any one of claims 1 to 4, characterized in that The nanomaterials used in the vehicle polymer nano thermal insulation water-based topcoat of various colors are modified ATO nano slurry, nano ITO dispersion, nano ATO dispersion, nano ITO, nano GTO thermal insulation powder, nano zirconium oxide, nano AZO, silica aerogel powder or silica aerogel paste. According to the thermal insulation performance and cost control, at least one or more combinations are used. The nanomaterial has a low thermal conductivity (after drying, 25° C.) of 0.001 to 3 W / (m·K) and a particle size of 0.1 to 20 μm.
7. The polymer nano thermal insulation color water-based topcoat for vehicles according to any one of claims 1 to 4, characterized in that: The alcohol cosolvent used in the various colors of the vehicle polymer nano thermal insulation water-based topcoat is n-butanol, isobutanol or isopropanol; The deionized water used in the polymer nano thermal insulation color water-based topcoat for vehicles is prepared by an industrial pure water machine.
8. The polymer nano thermal insulation color water-based topcoat for vehicles according to any one of claims 1 to 4, characterized in that: The pigments used in the various colors of the polymer nano thermal insulation water-based topcoat for vehicles are organic pigments and inorganic pigments, and the pigments can be titanium dioxide or light-fast yellow or isoindoline yellow or cadmium yellow or medium chrome yellow or iron oxide yellow or toluidine red or iron oxide red or phthalocyanine blue or indanthrene blue or phthalocyanine green or carbon black or silver powder or mica pearl powder or purple; the leveling agent used in the various colors of the polymer nano thermal insulation water-based topcoat for vehicles is an organic silicon leveling agent, an acrylate leveling agent, a fluorine-modified leveling agent, any one of them, or any two or any three of them in any proportion; The dispersant used in the various colors of polymer nano thermal insulation water-based topcoat for vehicles is an anionic wetting dispersant, a nonionic wetting dispersant, an electrically neutral wetting dispersant, or a polymer super dispersant; The adhesion promoter used in the various colors of the vehicle polymer nano thermal insulation water-based topcoat is a silane coupling agent, and the coupling agent should have good compatibility with the selected water-based single-component acrylic resin.
9. An application of a polymer nano thermal insulation color water-based topcoat for vehicles as claimed in any one of claims 1 to 4, characterized in that: The polymer nano heat-insulating color water-based topcoat is used in the field of coating preparation.
10. A method for preparing the polymer nano thermal insulation color water-based topcoat for vehicles as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Prepare raw materials and test each material according to the standards; S2. Weigh a high molecular weight water-based single-component acrylic resin by weight and slowly add it into a container, and slowly add the above-mentioned deionized water, alcohol cosolvent, dispersant, leveling agent, and adhesion promoter under stirring, and disperse it at a speed of 500-800r / min in an explosion-proof disperser for 10-20min, and slowly add pigment under stirring, and disperse it at a speed of 500-800r / min in an explosion-proof disperser for 10min; obtain a mixed color paste; At the same time, this step requires reserving 20% by weight of a high molecular weight aqueous single-component acrylic resin and 20% by weight of deionized water, using 15% by weight of a high molecular weight aqueous single-component acrylic resin and 15% by weight of deionized water to clean the sand mill, and the remaining 5% by weight of a high molecular weight aqueous single-component acrylic resin and 5% by weight of deionized water to adjust the viscosity of the nano-color paste mixture. S3, grinding the mixed color paste obtained in S2 with a sand mill, and testing the fineness with a fineness meter after each grinding. When the fineness of the mixed color paste is ≤20 μm, stop grinding, weigh the mixed color paste, and make up the weight lost by volatilization during the grinding process with deionized water; S4. Use an explosion-proof disperser to disperse the color paste with qualified fineness at a speed of 200-300r / min. Under stirring, slowly add the nanomaterial, gradually increase the dispersion speed to 800r / min, and disperse for 30 minutes to obtain a nano color paste mixture; The various indicators of the nano-color paste mixture prepared by S5 and S4 are tested. During the test, if the fineness is unqualified, it is quickly ground again with a sand mill until the fineness is qualified; when the viscosity is higher than 202s, add an appropriate amount of deionized water reserved in S2 to lower it. When the viscosity is less than 198s, add the high molecular water-based single-component acrylic resin reserved in S2 to increase it; when measuring the viscosity, the coating 4 cups itself is also required to be 25℃±1. When the indoor temperature is higher than 26℃, the coating 4 cups needs to be cooled with a refrigerator or ice cubes. When the indoor temperature is less than 24℃, the coating 4 cups needs to be heated with an oven. The specific indicators are shown in the table below: S6. Filter the qualified nano-color paste mixture with a 200-mesh filter cloth.
Citation Information
Patent Citations
Nanometer compound water-based heat insulation anticorrosion paint used for metal and preparation method thereof
CN101665645A
Water-based thermal insulating nano-coating and preparation method thereof
CN103709871A
Preparation method and application of water-based silicon dioxide aerogel reflective heat insulation coating
CN105820690A
Preparation method of various-color finished paint for vehicle appearance repair
CN111826039A
Water-based fluorosilicone modified acrylic emulsion, self-cleaning heat-insulating coating and preparation method and application of self-cleaning heat-insulating coating
CN117050230A