Solvent-free polyester-based adhesive capable of being coated at room temperature and preparation method thereof

By designing the polyester molecular chain structure and process steps, solvent-free polyester-based adhesive was developed, which solved the problem of high melt viscosity of polyester hot melt adhesive, achieved room temperature fluidity and structural strength, and met the bonding under different conditions Performance requirements have improved the molding process of polyester glue.

CN119081625APending Publication Date: 2024-12-06无锡海特新材料研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411240563.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Polyester hot melt adhesive has a high melt viscosity, resulting in unfavorable coating or molding processing.

Method used

Using solvent-free polyester-based adhesive, consisting of diacid monomer, alcohol monomer, triol monomer, ester synthesis catalyst, thermal stabilizer, antioxidant, polyurethane synthesis catalyst and polyisocyanate, through specific process steps such as Nitrogen-vacuo operation, esterification and polycondensation, adjusting the polyester molecular chain structure to achieve room temperature fluidity and structural strength.

Benefits of technology

The solvent-free and room temperature flow coating characteristics of polyester are realized, which meets the adhesive performance requirements under different conditions and improves the molding process of hot melt polyester glue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081625A_ABST
    Figure CN119081625A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, in particular to a solvent-free polyester-based adhesive capable of being coated at room temperature and a preparation method of the solvent-free polyester-based adhesive. The problems that a polyester hot melt adhesive formed by a common technology is high in melting viscosity and is not beneficial to coating or forming are solved. Comprising a diacid monomer, a diol monomer, a triol monomer, an ester synthesis catalyst, a heat stabilizer, an antioxidant, a polyurethane synthesis catalyst and polyisocyanate. The structural strength of the polyester adhesive is adjusted by changing the variety and dosage of the polyisocyanate, so that the adhesive meets the performance requirements of materials on adhesion under different conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a polyester-based adhesive which is solvent-free and can be coated at room temperature and a preparation method thereof. Background Art

[0002] Polyester is a general term for polymers obtained by polycondensation of polyols and polyacids. It mainly refers to polyethylene terephthalate, and also includes linear thermoplastic resins such as polybutylene terephthalate and polyarylate. Polyester is a type of engineering plastic with excellent performance and wide application.

[0003] Polyester is widely used in clothing, automobiles, footwear, electronic appliances, packaging, wood processing, and the bonding of reflective materials due to its excellent rigidity, toughness, insulation, water resistance, heat resistance, cold resistance, medium resistance, and high bonding strength. However, polyester usually has a high melting point and is difficult to be dissolved by solvents, so it is mainly used in hot melt processes. However, the polyester hot melt adhesive formed by common processes has a high melt viscosity, which is not conducive to coating or molding processing.

[0004] Therefore, there is an urgent need to provide a solvent-free polyester-based adhesive that can be coated at room temperature and a preparation method thereof to solve the above technical problems. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that the polyester hot melt adhesive formed by the common technology has a large melt viscosity, which is not conducive to coating or molding. A brief overview of the present invention is given below to provide a basic understanding of certain aspects of the present invention. It should be understood that this overview is not an exhaustive overview of the present invention. It is not intended to determine the key or important parts of the present invention, nor is it intended to limit the scope of the present invention.

[0006] The technical solution of the present invention:

[0007] A solvent-free polyester-based adhesive that can be coated at room temperature, the solvent-free polyester-based adhesive that can be coated at room temperature comprising a diacid monomer, a diol monomer, a triol monomer, an ester synthesis catalyst, a heat stabilizer, an antioxidant, a polyurethane synthesis catalyst, and a polyisocyanate;

[0008] Among them, the mass component of the diacid monomer is 340-450 parts, the mass component of the diol monomer is 260-370 parts, the mass component of the triol monomer is 10-110 parts, the mass component of the ester synthesis catalyst is 0.01-0.06 parts, the mass component of the heat stabilizer is 0.02-0.06 parts, the mass component of the antioxidant is 0.02-0.06 parts, the mass component of the polyurethane synthesis catalyst is 1-3 parts, and the mass component of the polyisocyanate is 35-86 parts.

[0009] Preferably, the diacid monomer is one or more of terephthalic acid, isophthalic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid.

[0010] Preferably, the diol monomer is one or more of ethylene glycol, diethylene glycol, triethylene glycol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol and 1,12-dodecanediol.

[0011] Preferably, the triol monomer is one or more of propylene glycol and trimethylolpropane, and the polyester synthesis catalyst is one or more of ethylene glycol antimony, germanium oxide, tetrabutyl titanate, and tetraisopropyl titanate.

[0012] Preferably, the heat stabilizer is one or more of trimethyl phosphate, triphenyl phosphate, phosphorous acid, and triphenyl phosphite.

[0013] Preferably, the antioxidant is one or more of 2,6-di-tert-butylphenol and 3,3-thiodipropionate.

[0014] Preferably, the polyurethane synthesis catalyst is one or more of dibutyltin dilaurate and didodecylsulfide dibutyltin.

[0015] Preferably, the polyisocyanate is one or more of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane, and HDI trimer.

[0016] A method for preparing a solvent-free polyester-based adhesive that can be coated at room temperature comprises the following steps:

[0017] Step 1: Mix and slurry the diacid monomer, diol monomer and triol monomer, add the slurried mixture into a Polytex-1L polyester synthesis reactor, pass nitrogen and evacuate, then stir and heat, keep the reactor and esterification tower valves open, and adjust the esterification pressure valve to maintain its pressure at 400 kPa;

[0018] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage, and the esterification pressure valve is adjusted to reduce the pressure to normal pressure. When the amount of water discharged from the esterification tower to be collected reaches 54g-65g, the pressure is released again to obtain a liquid polyester prepolymer;

[0019] Step 3: Mix and slurry the diacid monomer and the diol monomer, add the slurried mixture into a Polytex-1L polyester synthesis reactor, conduct nitrogen-vacuuming operation, then stir and heat, keep the reactor and esterification tower valves open, and adjust the esterification pressure valve to maintain its pressure at 400 kPa;

[0020] Step 4: When water starts to be discharged from the esterification tower, the reactor enters the esterification stage, and the esterification pressure valve is adjusted to reduce the pressure to normal pressure. After the collected esterification tower water volume reaches 95% of the theoretical total volume, the pressure is released again;

[0021] Step 5: After unloading the pressure, the catalyst, heat stabilizer and antioxidant are pressed into the reactor, the esterification valve is closed, the polycondensation valve is opened to enter the pre-polycondensation stage, the system is heated up, after heating up, the vacuum pump is opened and the polycondensation pressure valve is adjusted to slowly reduce the system pressure from normal pressure to 20Pa, the pre-polycondensation time is 0.5-1h, and then the final polycondensation stage is entered;

[0022] Step 6: When the motor power of the reactor is increased to 55w-65w due to the polycondensation of polyester, turn off the vacuum pump and stop stirring, enter the pre-polycondensation stage, fill the reactor with nitrogen until the pressure inside the reactor is higher than normal pressure, press out the synthesized polyester, cut the polyester into pellets and dry it;

[0023] Step 7: Add the liquid polyester prepolymer and polyester into a container, stir and heat to dissolve, the dissolution time is 2-3 hours, and cool down after dissolution to obtain a polyester solution;

[0024] Step 8: The polyurethane synthesis catalyst, polyisocyanate and polyester solution are stirred evenly and then ripened for 6-12 hours to obtain a polyester adhesive.

[0025] Preferably: the stirring rate in steps 7 to 8 is 100-200r / min, the pressure in step 6 is 120-140kPa, the heating temperature in steps 1 and 3 is 150-180°C, the heating temperature in step 5 is 240-260°C, the heating temperature in step 7 is 60-80°C, and the heating temperature in step 8 is 70-80°C.

[0026] The present invention has the following beneficial effects:

[0027] The present invention designs the polyester molecular chain structure so that the polyester has the characteristics of being solvent-free and flowable at room temperature and can be coated;

[0028] The invention adjusts the structural strength of the polyester adhesive by changing the type and dosage of the polyisocyanate, so that the adhesive can meet the bonding performance requirements of the material under different conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the preparation of the solvent-free coatable polyester adhesive in Example 1. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described below by the specific embodiments shown in the accompanying drawings. However, it should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0031] Specific implementation method 1: Combination Figure 1 The present embodiment is described. The present embodiment is a solvent-free polyester-based adhesive that can be coated at room temperature. The solvent-free polyester-based adhesive that can be coated at room temperature is composed of a diacid monomer, a diol monomer, a triol monomer, an ester synthesis catalyst, a heat stabilizer, an antioxidant, a polyurethane synthesis catalyst, and a polyisocyanate.

[0032] Among them, the mass component of the diacid monomer is 340-450 parts, the mass component of the diol monomer is 260-370 parts, the mass component of the triol monomer is 10-110 parts, the mass component of the ester synthesis catalyst is 0.01-0.06 parts, the mass component of the heat stabilizer is 0.02-0.06 parts, the mass component of the antioxidant is 0.02-0.06 parts, the mass component of the polyurethane synthesis catalyst is 1-3 parts, and the mass component of the polyisocyanate is 35-86 parts.

[0033] Specific implementation method 2: Combination Figure 1 To illustrate this embodiment, a solvent-free polyester-based adhesive that can be coated at room temperature is provided in this embodiment, wherein the diacid monomer is composed of one or more of terephthalic acid, isophthalic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid.

[0034] Specific implementation method three: Combination Figure 1 To illustrate this embodiment, a solvent-free polyester-based adhesive that can be coated at room temperature is provided in this embodiment, wherein the diol monomer is composed of one or more of ethylene glycol, diethylene glycol, triethylene glycol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol.

[0035] Specific implementation method four: Combination Figure 1 To illustrate this embodiment, a solvent-free polyester-based adhesive that can be coated at room temperature is used in this embodiment, wherein the triol monomer is composed of one or more of propylene glycol and trimethylolpropane, and the polyester synthesis catalyst is composed of one or more of ethylene glycol antimony, germanium oxide, tetrabutyl titanate, and tetraisopropyl titanate.

[0036] Specific implementation method five: Combination Figure 1The present embodiment is described as a solvent-free polyester-based adhesive that can be coated at room temperature, wherein the heat stabilizer is composed of one or more of trimethyl phosphate, triphenyl phosphate, phosphorous acid, and triphenyl phosphite.

[0037] Specific implementation method six: Combination Figure 1 The present embodiment is described as a solvent-free polyester-based adhesive that can be coated at room temperature, wherein the antioxidant is composed of one or more of 2,6-di-tert-butylphenol and 3,3-thiodipropionate.

[0038] Specific implementation method seven: Combination Figure 1 The present embodiment is described as a solvent-free polyester-based adhesive that can be coated at room temperature, wherein the polyurethane synthesis catalyst is composed of one or more of dibutyltin dilaurate and didodecyl dibutyltin.

[0039] Specific implementation method eight: Combination Figure 1 The present embodiment is described as a solvent-free polyester-based adhesive that can be coated at room temperature, wherein the polyisocyanate is composed of one or more of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane, and HDI trimer.

[0040] Specific implementation method nine: Combination Figure 1 The present embodiment is described. A method for preparing a solvent-free polyester-based adhesive that can be coated at room temperature in the present embodiment comprises the following steps:

[0041] Step 1: Weigh the diacid monomer, diol monomer, and triol monomer and mix them for slurrying. Add the slurrying mixture into the Polytex-1L polyester synthesis reactor. After strictly deoxygenating the synthesis system by "nitrogen-vacuuming", nitrogen is introduced to make the system have a certain initial pressure of 200-300 kPa. Then stir and heat the system to the set temperature. During this period, the pressure in the reactor continues to rise. The esterification pressure valve is adjusted to maintain the system pressure at 400 kPa.

[0042] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage, and the esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. After the collected water output from the esterification tower reaches the expected value, the system is unloaded to normal pressure, and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0043] Step 3: Weigh the diacid monomer and diol monomer, mix and beat, and add the beaten mixture into the Polytex-1L polyester synthesis reactor; at the same time, weigh the polyester synthesis catalyst, heat stabilizer, and antioxidant and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to give the system a certain initial pressure of 200-300kPa, and then the system is stirred and heated to the set temperature. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0044] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0045] Step 5: Use nitrogen to pressurize the catalyst, heat stabilizer and antioxidant in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to the set temperature, turn on the vacuum pump and adjust the polycondensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 0.5-1h, and then enter the final polycondensation stage;

[0046] Step 6: When the motor power of the reactor reaches 55w-65w, turn off the vacuum pump and stop stirring, enter the pre-condensation stage, fill the reactor with nitrogen until the pressure inside the reactor is higher than normal pressure, press out the synthesized polyester, cut the polyester into pellets and dry it;

[0047] Step 7: Add the liquid polyester prepolymer and polyester into a container, stir and heat to dissolve, the dissolution time is 2-3 hours, and cool down after dissolution to obtain a polyester solution;

[0048] Step 8: The polyurethane synthesis catalyst, polyisocyanate and polyester solution are stirred evenly and then ripened for 6-12 hours to obtain a polyester adhesive.

[0049] Specific implementation method ten: Combination Figure 1 The present embodiment is described. The present embodiment provides a method for preparing a solvent-free polyester-based adhesive that can be coated at room temperature. The stirring rate in steps seven to eight is 100-200 r / min, the pressure in step six is ​​120-140 kPa, the heating temperature in steps one and three is 150-180°C, the heating temperature in step five is 240-260°C, the heating temperature in step seven is 60-80°C, and the heating temperature in step eight is 70-80°C.

[0050] The present invention is described in detail below in conjunction with various embodiments, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.

[0051] Example 1

[0052] Step 1: Weigh 300g of adipic acid, 220g of diethylene glycol, and 35g of trimethylolpropane, mix and beat, add the beaten mixture into a Polytex-1L polyester synthesis reactor, perform a "nitrogen-vacuum" operation on the synthesis system to strictly deoxygenate, introduce nitrogen to make the system have an initial pressure of 300kPa, then stir at a motor power of 50Hz, and heat the system to 150°C. During this period, the pressure in the reactor continues to increase, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0053] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. The esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. When the collected water output from the esterification tower reaches 65 g, the system is unloaded to normal pressure and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0054] Step 3: Weigh 20g of terephthalic acid, 40g of glutaric acid, 40g of azelaic acid, 20g of ethylene glycol, and 45g of 1,6-hexanediol, mix and beat, and add the beaten mixture to the Polytex-1L polyester synthesis reactor; at the same time, weigh 0.02g of tetrabutyl titanate, 0.04g of trimethyl phosphate, and 0.04g of 3,3-thiodipropionate and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to give the system an initial pressure of 200kPa, and then the system is stirred at a motor power of 50Hz and the temperature of the system is raised to 180°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0055] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0056] Step 5: Use nitrogen to pressurize tetrabutyl titanate, trimethyl phosphate, and 3,3-thiodipropionate in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to 260°C, turn on the vacuum pump and adjust the condensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 1h, and then enter the final condensation stage;

[0057] Step 6: When the motor power of the reactor reaches 55W, the final polycondensation stage of the polyester is ended, the vacuum pump is turned off and the stirring is stopped, nitrogen is passed until the pressure in the reactor reaches 120 kPa, the synthesized polyester is pressed out, the material is discharged, pelletized and dried;

[0058] Step 7: Add the liquid polyester prepolymer and polyester into a container, stir at a rate of 100 r / min and heat to 80° C. for dissolution, the dissolution time is 2 h, and then cool down to obtain a polyester solution;

[0059] Step 8: Weigh 2g of dibutyltin dilaurate, 30g of HDI, and 13g of HDI trimer and polyester solution, stir evenly, and then ripen at 80°C for 6h. After complete ripening, a polyester adhesive is obtained.

[0060] Example 2

[0061] Step 1: Weigh 250g of adipic acid, 230g of triethylene glycol and 10g of propylene glycol and mix them for pulping. Add the pulped mixture into a Polytex-1L polyester synthesis reactor. Perform a "nitrogen-vacuum" operation on the synthesis system to strictly deoxygenate it, then introduce nitrogen to give the system an initial pressure of 200kPa. Then stir at a motor power of 50Hz and heat the system to 180°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa.

[0062] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. The esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. When the collected water output from the esterification tower reaches 54 g, the system is unloaded to normal pressure and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0063] Step 3: Weigh 20g of isophthalic acid, 70g of sebacic acid, 16g of ethylene glycol, and 90g of 1,10-decanediol, mix and beat, and add the beaten mixture to the Polytex-1L polyester synthesis reactor; at the same time, weigh 0.04g of tetraisopropyl titanate, 0.02g of phosphorous acid, and 0.06g of 2,6-di-tert-butylphenol and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to give the system an initial pressure of 300kPa, and then the system is stirred at a motor power of 50Hz and the temperature of the system is raised to 170°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0064] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0065] Step 5: Use nitrogen to pressurize tetraisopropyl titanate, phosphorous acid, and 2,6-di-tert-butylphenol in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to 260°C, turn on the vacuum pump and adjust the condensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 0.5h, and then enter the final condensation stage;

[0066] Step 6: When the motor power of the reactor reaches 55W, the final polycondensation stage of the polyester is ended, the vacuum pump is turned off and the stirring is stopped, nitrogen is passed until the pressure in the reactor reaches 120 kPa, the synthesized polyester is pressed out, the material is discharged, pelletized and dried;

[0067] Step 7: adding the liquid polyester prepolymer and the solid polyester product into a container, stirring at a rate of 100 r / min and heating to 80° C. for dissolution, the dissolution time is 2 h, and then cooling to obtain a polyester solution;

[0068] Step 8: Weigh 1.5 g of dibutyltin didodecylsulfide, 26 g of TDI, 9 g of HDI trimer and polyester solution, stir evenly and ripen at 70° C. for 12 h. After complete ripening, a polyester adhesive is obtained.

[0069] Example 3

[0070] Step 1: Weigh 300g of adipic acid, 160g of diethylene glycol, 36g of 1,4-butanediol, and 40g of trimethylolpropane, mix and beat, add the beaten mixture into a Polytex-1L polyester synthesis reactor, perform a "nitrogen-vacuum" operation on the synthesis system to strictly deoxygenate, introduce nitrogen to make the system have an initial pressure of 300kPa, then stir at a motor power of 50Hz, and heat the system to 160°C. During this period, the pressure in the reactor continues to increase, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0071] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. The esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. When the collected water output from the esterification tower reaches 65 g, the system is unloaded to normal pressure and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0072] Step 3: Weigh 40g of terephthalic acid, 80g of suberic acid, 18g of ethylene glycol, and 60g of 1,8-octanediol, mix and beat, and add the beaten mixture to the Polytex-1L polyester synthesis reactor; at the same time, weigh 0.01g of germanium oxide, 0.06g of triphenyl phosphite, and 0.02g of 3,3-thiodipropionate and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to make the system have an initial pressure of 200kPa, and then the system is stirred at a motor power of 50Hz and the temperature of the system is raised to 150°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0073] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0074] Step 5: Use nitrogen to pressurize germanium oxide, triphenyl phosphite, and 3,3-thiodipropionate in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to 240°C, turn on the vacuum pump and adjust the condensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 1h, and then enter the final condensation stage;

[0075] Step 6: When the motor power of the reactor reaches 55W, the final polycondensation stage of the polyester is ended, the vacuum pump is turned off and the stirring is stopped, nitrogen is passed until the pressure in the reactor reaches 140 kPa, the synthesized polyester is pressed out, the material is discharged, pelletized and dried;

[0076] Step 7: adding the liquid polyester prepolymer and the solid polyester product into a container, stirring at a rate of 100 r / min and heating to 60° C. for dissolution, the dissolution time is 3 h, and then cooling to obtain a polyester solution;

[0077] Step 8: Weigh 1.2 g of dibutyltin dilaurate, 22 g of IPDI, 25 g of HDI trimer and polyester solution, stir evenly and ripen at 80° C. for 12 h. After complete ripening, a polyester adhesive is obtained.

[0078] Example 4

[0079] Step 1: Weigh 300g of adipic acid, 110g of diethylene glycol and 110g of trimethylolpropane and mix and beat, add the beaten mixture into a Polytex-1L polyester synthesis reactor, perform a "nitrogen-vacuum" operation on the synthesis system to strictly deoxygenate, introduce nitrogen to make the system have an initial pressure of 200kPa, then stir at a motor power of 50Hz, and heat the system to 160°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0080] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. The esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. When the collected water output from the esterification tower reaches 60 g, the system is unloaded to normal pressure and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0081] Step 3: Weigh 40g of terephthalic acid, 60g of dodecanedioic acid, 15g of ethylene glycol, and 60g of 1,4-dihydroxycyclohexane, mix and beat, and add the beaten mixture to the Polytex-1L polyester synthesis reactor; at the same time, weigh 0.06g of ethylene glycol antimony, 0.06g of triphenyl phosphate, and 0.06g of 3,3-thiodipropionate and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to give the system an initial pressure of 200kPa, and then the system is stirred at a motor power of 50Hz and the temperature of the system is raised to 180°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0082] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0083] Step 5: Use nitrogen to pressurize the ethylene glycol antimony, triphenyl phosphate, and 3,3-thiodipropionate in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to 250°C, turn on the vacuum pump and adjust the polycondensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 1h, and then enter the final polycondensation stage;

[0084] Step 6: When the motor power of the reactor reaches 60W, the final polycondensation stage of the polyester is ended, the vacuum pump is turned off and the stirring is stopped, nitrogen is passed until the pressure in the reactor reaches 140 kPa, the synthesized polyester is pressed out, the material is discharged, pelletized and dried;

[0085] Step 7: adding the liquid polyester prepolymer and the solid polyester product into a container, stirring at a rate of 200 r / min and heating to 80° C. for dissolution, the dissolution time is 2 h, and then cooling to obtain a polyester solution;

[0086] Step 8: Weigh 3g of dibutyltin dilaurate, 25g of HDI, 42g of HDI trimer and polyester solution, stir evenly and ripen at 70°C for 12h. After complete ripening, a polyester adhesive is obtained.

[0087] Example 5

[0088] Step 1: Weigh 280g of adipic acid, 260g of triethylene glycol, and 12g of propylene glycol and mix them for pulping. Add the pulped mixture into a Polytex-1L polyester synthesis reactor. Perform a "nitrogen-vacuum" operation on the synthesis system to strictly deoxygenate it, then introduce nitrogen to give the system an initial pressure of 300kPa. Then stir at a motor power of 50Hz, and heat the system to 180°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa.

[0089] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. The esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. When the collected water output from the esterification tower reaches 55 g, the system is unloaded to normal pressure and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0090] Step 3: Weigh 10g of terephthalic acid, 20g of isophthalic acid, 70g of adipic acid, 30g of ethylene glycol, and 80g of 1,12-dodecanediol, mix and beat, and add the beaten mixture to the Polytex-1L polyester synthesis reactor; at the same time, weigh 0.02g of tetrabutyl titanate, 0.02g of trimethyl phosphate, and 0.02g of 3,3-thiodipropionate and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to give the system an initial pressure of 300kPa, and then the system is stirred at a motor power of 50Hz and the temperature of the system is raised to 160°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0091] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0092] Step 5: Use nitrogen to pressurize tetrabutyl titanate, trimethyl phosphate, and 3,3-dithiodipropionate in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to 240°C, turn on the vacuum pump and adjust the condensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 1h, and then enter the final condensation stage;

[0093] Step 6: When the motor power of the reactor reaches 65W, the final polycondensation stage of the polyester is ended, the vacuum pump is turned off and the stirring is stopped, nitrogen is passed until the pressure in the reactor reaches 140 kPa, the synthesized polyester is pressed out, the material is discharged, pelletized and dried;

[0094] Step 7: adding the liquid polyester prepolymer and the solid polyester product into a container, stirring at a rate of 100 r / min and heating to 70° C. for dissolution, the dissolution time is 3 h, and then cooling to obtain a polyester solution;

[0095] Step 8: Weigh 1g of dibutyltin didodecylsulfide, 26g of HMDI, 60g of HDI trimer and polyester solution, stir evenly and ripen at 80°C for 12h. After complete ripening, a polyester adhesive is obtained.

[0096] Example 6

[0097] Step 1: Weigh 300g of adipic acid, 80g of diethylene glycol, 90g of triethylene glycol, and 50g of propylene glycol, mix and beat, add the beaten mixture into a Polytex-1L polyester synthesis reactor, perform a "nitrogen-vacuum" operation on the synthesis system to strictly deoxygenate, introduce nitrogen to make the system have an initial pressure of 300kPa, then stir at a motor power of 50Hz, and heat the system to 180°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0098] Step 2: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. The esterification pressure valve is adjusted to slowly reduce the system pressure from 400 kPa to normal pressure. When the collected water output from the esterification tower reaches 60 g, the system is unloaded to normal pressure and the material is discharged to obtain a polyester prepolymer that is liquid at room temperature;

[0099] Step 3: Weigh 100g of adipic acid, 50g of azelaic acid, 50g of ethylene glycol, and 40g of neopentyl glycol, mix and beat, and add the beaten mixture to the Polytex-1L polyester synthesis reactor; at the same time, weigh 0.04g of tetraisopropyl titanate, 0.06g of trimethyl phosphate, and 0.06g of 2,6-di-tert-butylphenol and place them in the storage tank of the synthesis device for standby use. After the synthesis system is strictly deoxygenated by the "nitrogen-vacuum" operation, nitrogen is introduced to give the system an initial pressure of 300kPa, and then the system is stirred at a motor power of 50Hz and the temperature of the system is raised to 180°C. During this period, the pressure in the reactor continues to rise, and the esterification pressure valve is adjusted to maintain the system pressure at 400kPa;

[0100] Step 4: When water begins to be discharged from the esterification tower, the reactor enters the esterification stage. Adjust the esterification pressure valve to slowly reduce the system pressure from 400kPa to normal pressure. When the collected esterification tower water volume reaches 95% of the theoretical total volume, the esterification stage is ended and the system is unloaded to normal pressure;

[0101] Step 5: Use nitrogen to pressurize tetraisopropyl titanate, trimethyl phosphate, and 2,6-di-tert-butylphenol in the storage tank into the reactor to enter the pre-condensation stage. Heat the system to 240°C, turn on the vacuum pump and adjust the condensation pressure valve to slowly reduce the system pressure from normal pressure to 20Pa. The pre-condensation time is 1h, and then enter the final condensation stage;

[0102] Step 6: When the motor power of the reactor reaches 60W, the final polycondensation stage of the polyester is ended, the vacuum pump is turned off and the stirring is stopped, nitrogen is passed until the pressure in the reactor reaches 130 kPa, the synthesized polyester is pressed out, the material is discharged, pelletized and dried;

[0103] Step 7: adding the liquid polyester prepolymer and the solid polyester product into a container, stirring at a rate of 100 r / min and heating to 70° C. for dissolution, the dissolution time is 2 h, and then cooling to obtain a polyester solution;

[0104] Step 8: Weigh 1.5 g of dibutyltin dilaurate, 8 g of HDI, 50 g of HDI trimer and polyester solution, stir evenly and ripen at 80° C. for 12 h. After complete ripening, a polyester adhesive is obtained.

[0105] The performance test results of the liquid polyester prepolymers obtained in Examples 1 to 6 are shown in the following table:

[0106]

[0107] The performance test results of the solid polyester obtained in Examples 1 to 6 are shown in the following table:

[0108]

[0109] The performance test results of the polyester adhesives obtained in Examples 1 to 6 are shown in the following table:

[0110]

[0111] Molecular weight test: Weigh 3-5 mg of sample and dissolve it in tetrahydrofuran as solvent, and use gel permeation chromatography to test the molecular weight. The test temperature is 25°C, the solution concentration is 3 mg / L, and the flow rate is 1 mL / min.

[0112] Hydroxyl value test: The hydroxyl value of the sample was determined by the acetylation method according to the national standard GB / T7383-2020. The arithmetic mean of the data of five parallel experiments was taken as the test result. The deviation of the test result was no more than 1% of the arithmetic mean. The test temperature was 25°C.

[0113] Glass transition temperature, melting temperature, and crystallinity test: In a N2 atmosphere, a differential scanning calorimeter (DSC) was used to test the samples. The test temperature ranged from room temperature to 200°C, and the heating rate was 5°C / min.

[0114] Viscosity test: The sample viscosity is tested using a rotational viscometer, with the rotor volume and speed being based on the test sample's percentage scale torque at 50-70% and the test temperature being 25°C.

[0115] Intrinsic viscosity test: The polyester was dissolved in a phenol / tetrachloroethane solution (m / m=50:50), and the intrinsic viscosity was measured using an Ubbelohde viscometer in a glass thermostatic water bath at 25°C. The intrinsic viscosity was calculated using the following formula, where η sp — specific viscosity; t1—solution flow time s; t0—solvent flow time s; [η]—intrinsic viscosity dL / g; c—copolyester solution concentration g / dL.

[0116]

[0117] Tensile strength and elongation at break test: Based on GB / T 1040-2006 as the test standard, the molded samples were cut into 1BA-type specimens. Each group of test specimens has 5 specimens, with a thickness of 2-3mm, a test gauge length of 25mm, a fixture spacing of 58mm, a displacement rate of 100mm / min, and a test temperature of 25°C.

[0118] Adhesion strength test: GB / T 2790-1995 is used as the test standard. The bonded PET film is cut into 25mm wide strips. The unbonded end of the PET film is bent 180° and clamped on a fixed chuck. The other end of the bonded PET film is clamped on another chuck. Each group of test strips has 5 samples. The separation rate of the chuck is 100mm / min. The test temperature is 25℃.

[0119] From the test results in the above table, it can be seen that the prepared liquid polyester prepolymer has a low melting point and low viscosity, the solid polyester has a low crystallinity, and the polyester adhesive has excellent flexibility and bonding strength to PET. The present invention provides a new idea for the preparation of solvent-free coatable polyester adhesives. The prepared adhesives meet the development trend of green chemistry, meet the bonding requirements of polar materials, and effectively improve the molding process of general hot-melt polyester adhesives.

[0120] It should be noted that in the above embodiments, as long as the technical solutions are not contradictory, they can be arranged and combined, and those skilled in the art can exhaust all possibilities based on the mathematical knowledge of arrangement and combination. Therefore, the present invention will no longer describe the technical solutions after arrangement and combination one by one, but it should be understood that the technical solutions after arrangement and combination have been disclosed by the present invention.

[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A solvent-free polyester-based adhesive that can be coated at room temperature, characterized in that: The solvent-free polyester-based adhesive that can be coated at room temperature is composed of a diacid monomer, a diol monomer, a triol monomer, an ester synthesis catalyst, a heat stabilizer, an antioxidant, a polyurethane synthesis catalyst, and a polyisocyanate; Among them, the mass component of the diacid monomer is 340-450 parts, the mass component of the diol monomer is 260-370 parts, the mass component of the triol monomer is 10-110 parts, the mass component of the ester synthesis catalyst is 0.01-0.06 parts, the mass component of the heat stabilizer is 0.02-0.06 parts, the mass component of the antioxidant is 0.02-0.06 parts, the mass component of the polyurethane synthesis catalyst is 1-3 parts, and the mass component of the polyisocyanate is 35-86 parts.

2. A solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The diacid monomer is composed of one or more of terephthalic acid, isophthalic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid.

3. A solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The diol monomer is composed of one or more of ethylene glycol, diethylene glycol, triethylene glycol, neopentyl glycol, 1,4-dihydroxycyclohexane, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol.

4. A solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The triol monomer is one or more of propylene glycol and trimethylolpropane, and the polyester synthesis catalyst is one or more of ethylene glycol antimony, germanium oxide, tetrabutyl titanate, and tetraisopropyl titanate.

5. A solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The heat stabilizer is composed of one or more of trimethyl phosphate, triphenyl phosphate, phosphorous acid, and triphenyl phosphite.

6. A solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The antioxidant is composed of one or more of 2,6-di-tert-butylphenol and 3,3-thiodipropionate.

7. A solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The polyurethane synthesis catalyst is composed of one or more of dibutyltin dilaurate and didodecylsulfide dibutyltin.

8. The solvent-free room temperature coatable polyester-based adhesive according to claim 1, characterized in that: The polyisocyanate is composed of one or more of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4-diisocyanate dicyclohexylmethane, and HDI trimer.

9. A method for preparing a solvent-free polyester-based adhesive that can be coated at room temperature, characterized in that: The steps include: Step 1: diacid monomer, diol monomer and triol monomer are mixed and slurried, and the slurried mixture is added into a reaction kettle, and nitrogen is passed through and vacuumized, followed by stirring and heating, while adjusting the esterification pressure valve to maintain the pressure at 400 kPa; Step 2, when water begins to be discharged from the esterification tower, the reactor enters the esterification stage, the esterification pressure valve is adjusted to reduce the pressure to normal pressure, and when the water output of the esterification tower to be collected reaches 54g-65g, the pressure is released again to obtain a liquid polyester prepolymer after the pressure is released; Step 3: Mix and slurry the diacid monomer and the diol monomer, add the slurried mixture into a reaction kettle, pass nitrogen and evacuate, then stir and heat, and adjust the esterification pressure valve to maintain the pressure at 400 kPa; Step 4: When water starts to be discharged from the esterification tower, the reactor enters the esterification stage, and the esterification pressure valve is adjusted to reduce the pressure to normal pressure. After the collected esterification tower water volume reaches 95% of the theoretical total volume, the pressure is released again; Step 5: After the pressure is released, the catalyst, heat stabilizer and antioxidant are pressed into the reactor to enter the pre-polycondensation stage. The system is heated. After the temperature is raised, the vacuum pump is turned on and the polycondensation pressure valve is adjusted to slowly reduce the system pressure from normal pressure to 20Pa. The pre-polycondensation time is 0.5-1h, and then the final polycondensation stage is entered; Step 6: When the motor power of the reactor reaches 55w-65w, turn off the vacuum pump and stop stirring, enter the pre-condensation stage, fill the reactor with nitrogen until the pressure inside the reactor is higher than normal pressure, press out the synthesized polyester, cut the polyester into pellets and dry it; Step 7, adding the liquid polyester prepolymer and polyester into a container, stirring and heating to dissolve, the dissolution time is 2-3 hours, and cooling after dissolution to obtain a polyester solution; Step 8: The polyurethane synthesis catalyst, polyisocyanate and polyester solution are stirred evenly and then ripened for 6-12 hours to obtain a polyester adhesive.

10. The method for preparing a solvent-free polyester-based adhesive that can be coated at room temperature according to claim 9, characterized in that: The stirring rate in steps 7 to 8 is 100-200 r / min, the pressure in step 6 is 120-140 kPa, the heating temperature in steps 1 and 3 is 150-180°C, the heating temperature in step 5 is 240-260°C, the heating temperature in step 7 is 60-80°C, and the heating temperature in step 8 is 70-80°C.