Method for recovering high-valence elements from mine slag charge
By using acid-soluble stirring and amine extraction technology in mining slag materials, rare earths and aluminum are separated and purified, the problems of low rare earth content and high impurity aluminum in the existing technology are solved, and efficient resource recycling and environmental protection processes are achieved, reducing the Production costs and wastewater discharge.
Patent Information
- Application Number
- CN202411249679.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing mining slag treatment process, the rare earth content is low and the impurity aluminum content is high, resulting in high production costs, large oxalic acid consumption and large amount of high-salt wastewater, and the process is long, resulting in waste of resources and environmental pollution.
Under normal temperature, stir the water and the mine slag in a liquid-solid ratio of 1:1 to 5:1 in an acid solvent tank, slowly add 50% sulfuric acid solution, and obtain acid slag and sulfuric acid rare earth material through plate and frame filtration through plate and frame filtration to obtain acid slag and sulfuric acid rare earth material The rare earth is extracted into the organic phase using an amine extraction agent, and the rare earth and aluminum are separated by acid. The neutralization and removal process and the extraction transformation process are further purified and resourced.
It realizes efficient separation and purification of rare earths and aluminum, reduces production costs, reduces the generation of oxalic acid wastewater, improves resource recovery, and reduces wastewater discharge through the recycling and utilization of magnesium sulfate, which meets environmental protection requirements.
Smart Images

Figure QLYQS_2 
Figure QLYQS_3 
Figure QLYQS_4
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of element recovery, and in particular to a method for recovering high-value elements from mine slag. Background Art
[0002] Mine slag is produced by leaching rare earth sulfate mother liquor from southern ionic rare earth ore with magnesium sulfate in situ, and then removing impurities with sodium bicarbonate. At present, about 1 ton to 1.5 tons of mine slag are produced for every ton of rare earth carbonate produced.
[0003] In view of the low rare earth content and high impurity aluminum content of mine slag, the current industrial production processes are mainly acid method and alkali method:
[0004] The acid method uses hydrochloric acid to dissolve the mine slag, oxalic acid precipitation-burning process, and finally obtains mixed rare earth oxide products. This process consumes a lot of oxalic acid, has high production costs and produces a large amount of oxalic acid wastewater;
[0005] The alkaline method uses liquid alkali to convert aluminum hydroxide in mine slag into water-soluble sodium aluminate, removes aluminum through water washing, and the rare earths retained in the slag are then acid-dissolved to obtain rare earth chloride liquid, which is then processed through extraction separation, precipitation and calcination to obtain single rare earth oxide or mixed rare earth oxide products. This process is mature and has a high yield, but it has problems such as a long process and large amounts of high-salt wastewater produced.
[0006] Therefore, those skilled in the art provide a method for recovering high-price elements from mine slag to solve the problems raised in the above background technology. Summary of the invention
[0007] In view of the deficiencies of the prior art, the present invention provides a method for recovering high-price elements from mine slag to solve the problems raised in the above background technology.
[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions: A method for recovering high-priced elements from mine slag, comprising the following steps:
[0009] S1. Under normal temperature conditions, water and mine slag are stirred in an acid dissolving tank at a liquid-to-solid ratio of 1:1 to 5:1, and 50% sulfuric acid solution is slowly added during the stirring process;
[0010] S2. The pH value of the acid solution endpoint should be between 0.5 and 2.5;
[0011] S3, obtaining acid slag and rare earth sulfate liquid by plate and frame filter pressing;
[0012] S4, extracting the rare earth in the rare earth sulfate solution into an organic phase using an amine extractant;
[0013] S5, using acid for stripping to separate rare earth and aluminum, the raffinate is evaporated and crystallized to produce rare earth composite defluorinating agent, and the stripping solution enters the neutralization and impurity removal process;
[0014] S6, placing the stripping solution obtained in the amine extraction step into a stirring tank, and slowly adding magnesium oxide slurry to neutralize the residual acid until the pH value is about 4.5;
[0015] S7, the treated impurity removal liquid enters the extraction transformation process, using 10% to 30% magnesium oxide slurry tank saponification P507 extractant, controlling the volume ratio of the saponification extractant to the impurity removal liquid;
[0016] S8, stripping with hydrochloric acid;
[0017] S9. The magnesium sulfate in the raffinate is deoiled and returned to the mine for leaching, and the stripping solution is the chloride rare earth product.
[0018] Preferably, in the step S1, the stirring speed of the stirrer for stirring and mixing the mine slag and water in the acid dissolving tank is 50 r / min to 80 r / min, and the stirring time is 30 min;
[0019] After adding the 50% sulfuric acid solution, the stirring speed of the stirrer is 50 r / min to 80 r / min, and the stirring time is 2 hours.
[0020] Preferably, in the step S4, the amine extractant is one of N1923, N263, N235, etc., the extraction ratio is 1:1 to 3:1, and the operating temperature is 30°C to 50°C.
[0021] Preferably, in the steps S4 and S5, the amine extraction is a cascade countercurrent process, which includes four-stage extraction, six-stage stripping and two-stage water washing;
[0022]
[0023] Extraction section: It consists of 1 to 4 stages. At a temperature of 30℃ to 50℃, amine extractants and acid solutions are added to the 1st and 4th mixing chambers in a ratio of 1:1 to 3:1. The stirring time in the mixing chamber is 3min to 5min. The raffinate is separated in the 1st clarification chamber.
[0024] Stripping section: It consists of 5 to 10 stages. Hydrochloric acid or sulfuric acid is added in the 10th stage to contact the organic phase, so that the rare earth extracted into the organic phase returns to the water phase and the stripping liquid is separated from the 5-stage clarification chamber.
[0025] Water washing section: It consists of 11 to 12 stages. Water is added in the 12th stage to contact the organic phase. High-acid water washing liquid is released from the 11th stage clarification chamber. The organic phase after water washing can be returned to the 1st stage for extraction and recycling.
[0026] Preferably, in the step S1, the chemical equation for the acid dissolution treatment is:
[0027] 2RE(OH)3+3H2SO4→RE2(SO4)3+6H2O,
[0028] 2Al(OH)3+3H2SO4→Al2(SO4)3+3H2O
[0029] 2Fe(OH)3+3H2SO4→Fe2(SO4)3+3H2O
[0030] Among them, RE(OH)3 rare earth hydroxide, H2SO4 sulfuric acid, RE2(SO4)3 rare earth sulfate, H2O water, Al(OH)3 aluminum hydroxide, Al2(SO4)3 aluminum sulfate, Fe(OH)3 ferric hydroxide, Fe2(SO4)3 ferric sulfate.
[0031] Preferably, in the steps S4 and S5, the chemical equations for amine extraction and stripping are:
[0032] RE2(SO4)3+R3N→[R3N-RE2(SO4)3],
[0033] [R3N-RE2(SO4)3]+6H + →3R3N+2RE 3+ +3H2SO4,
[0034] Among them, RE2(SO4)3 rare earth sulfate, R3N amine extractant, rare earth complex in the organic phase after R3N-RE2(SO4)3 extraction, H + Sulfuric acid or hydrochloric acid, R3N amine extractant, RE 3+ Rare earth chloride or rare earth sulfate, H2SO4 sulfuric acid.
[0035] Preferably, in the step S6, the chemical equation for neutralization and impurity removal is:
[0036] H2SO4+MgO→MgSO4+H2O,
[0037] 3H2O+3MgO+Fe2(SO4)3→2Fe(OH)3+3MgSO4
[0038] Among them, H2SO4 sulfuric acid, MgO magnesium oxide, MgSO4 magnesium sulfate, H2O water, Fe(OH)3 ferric hydroxide, Fe2(SO4)3 ferric sulfate.
[0039] Preferably, in the steps S7 to S9, the chemical equation for the extraction transformation and magnesium sulfate treatment is:
[0040] H2O+MgO→Mg(OH)2,
[0041] 2(HA) 2(O) +Mg(OH)2→Mg(HA2) 2(O) +2H2O,
[0042] 3Mg(HA2) 2(O) +RE2(SO4)3→2RE(HA2) 3(O) +3MgSO4,
[0043] 2RE(HA2) 3(O) +6HCl→6(HA) 2(O) +2RECl3,
[0044] Among them, H2O water, MgO magnesium oxide, Mg(OH)2 magnesium hydroxide, (HA) 2(O) P507, Mg(HA2) 2(O) Magnesium complex in the organic phase after extraction, RE2(SO4)3 rare earth sulfate, MgSO4 magnesium sulfate, RE(HA2) 3(O) Rare earth complexes in the organic phase after extraction, HCl hydrochloric acid, RECl3 rare earth chloride.
[0045] Preferably, in the step S1, the algorithm formula for acid dissolution treatment is:
[0046] Assume the mass of mine slag is W m , the mass of water is W w The mass of sulfuric acid is
[0047] Liquid-to-solid ratio R liquid-solid :
[0048]
[0049] 1≤R liquid-solid ≤5,
[0050] Sulfuric acid addition amount:
[0051]
[0052] in, is the sulfuric acid concentration;
[0053] Assumption: W m is the mass of mine slag, in tons; W w is the mass of water, in tons; is the mass of sulfuric acid, in tons; is the concentration of sulfuric acid:
[0054] W m= 1 ton, the volume of water is 1 cubic meter to 5 cubic meters (assuming that the density of water is close to 1kg / L, the mass of water is about 1 ton to 5 tons);
[0055] The volume of the sulfuric acid solution is 0.5 cubic meters to 2 cubic meters, and the concentration is 50% (the density of a solution with a sulfuric acid concentration of 50% is about 1.4 kg / L, so the mass of the sulfuric acid solution is about 0.7 tons to 2.8 tons).
[0056] Preferably, in the step S3, the acid slag and rare earth sulfate solution are obtained by plate and frame filtration, and the calculation formula is:
[0057]
[0058] Wherein, M acid slag is the mass of acid slag, M rare earth sulfate liquid is the mass of rare earth sulfate liquid;
[0059] If the M mine slag is 1 ton, after plate and frame filtration, the following is obtained:
[0060] The volume of the rare earth sulfate liquid is 1.5 cubic meters to 7 cubic meters;
[0061] The mass of the acid slag is 0.05 ton to 0.25 ton;
[0062] Assuming the density ρ 硫酸稀土料液 ≈1 ton / cubic meter;
[0063] Mass calculation of rare earth sulfate solution:
[0064] M 硫酸稀土料液 The calculation formula can be based on its volume V 硫酸稀土料液 and ρ 硫酸稀土料液 To calculate:
[0065] M 硫酸稀土料液 =V 硫酸稀土料液 ×ρ 硫酸稀土料液 ,
[0066] Assuming that the density of rare earth sulfate liquid is 1 ton / cubic meter, then:
[0067] When the volume of rare earth sulfate liquid is 1.5 cubic meters, the mass is:
[0068] M 硫酸稀土料液 =1.5×1=1.5 tons,
[0069] When the volume of rare earth sulfate liquid is 7 cubic meters, the mass is:
[0070] M 硫酸稀土料液 =7×1=7 tons,
[0071] Therefore, the mass of the rare earth sulfate solution is in the range of 1.5 tons to 7 tons;
[0072] The mass of acid slag: According to the information, the mass of acid slag obtained after plate and frame filter pressing is 0.05 tons to 0.25 tons;
[0073] Assuming that the formula is to describe the mass relationship between the acid slag and the rare earth sulfate solution, it is expressed as follows:
[0074] M50% sulfuric acid + M mining slag = M acid slag + M rare earth sulfate liquid + M other lost or residual substances,
[0075] The formula shows that the total mass of mine slag is equal to the sum of acid slag, rare earth sulfate liquid and other losses minus the mass of added sulfuric acid.
[0076] The present invention provides a method for recovering high-value elements from mine slag, which has the following beneficial effects:
[0077] 1. The present invention uses an amine extractant to extract all rare earths in the rare earth sulfate solution obtained by acid dissolution into an organic phase, while the difficult-to-extract aluminum element remains in the solution. The raffinate is evaporated and crystallized to produce a rare earth composite defluorinating agent, thereby achieving separation of rare earth and aluminum and high-value preparation of aluminum products.
[0078] 2. The neutralization and impurity removal process of the present invention adds magnesium oxide to adjust the amine stripping solution, completes the extraction transformation process to achieve the transformation of rare earth sulfate into rare earth chloride feed solution and the resource recovery and reuse of magnesium sulfate. BRIEF DESCRIPTION OF THE DRAWINGS
[0079] Figure 1 is a flow chart of the present invention;
[0080] Figure 2 It is a process diagram of the present invention. DETAILED DESCRIPTION
[0081] In order to make the technical personnel in the technical field understand the scheme of the present invention, the technical scheme in the embodiment of the present invention will be clearly and completely described below in combination with the drawings in the embodiment of the present invention. Obviously, the described embodiment is a partial embodiment of the present invention, not a complete embodiment. Based on the embodiment of the present invention, other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present invention.
[0082] The present invention is described in detail below in conjunction with the accompanying drawings:
[0083] Example:
[0084] Please refer to the attached Figure 1 and attached Figure 2 The embodiment of the present invention provides a method for recovering high-price elements from mine slag, comprising the following steps:
[0085] S1. Under normal temperature conditions, water and mine slag are stirred in an acid dissolving tank at a liquid-to-solid ratio of 1:1 to 5:1, and 50% sulfuric acid solution is slowly added during the stirring process;
[0086] S2. The pH value of the acid solution endpoint should be between 0.5 and 2.5;
[0087] S3, obtaining acid slag and rare earth sulfate liquid by plate and frame filter pressing;
[0088] S4, extracting the rare earth in the rare earth sulfate solution into an organic phase using an amine extractant;
[0089] S5, using acid for stripping to separate rare earth and aluminum, the raffinate is evaporated and crystallized to produce rare earth composite defluorinating agent, and the stripping solution enters the neutralization and impurity removal process;
[0090] S6, placing the stripping solution obtained in the amine extraction step into a stirring tank, and slowly adding magnesium oxide slurry to neutralize the residual acid until the pH value is about 4.5;
[0091] S7, the treated impurity removal liquid enters the extraction transformation process, using 10% to 30% magnesium oxide slurry tank saponification P507 extractant, controlling the volume ratio of the saponification extractant to the impurity removal liquid;
[0092] S8, stripping with hydrochloric acid;
[0093] S9. The magnesium sulfate in the raffinate is deoiled and returned to the mine for leaching, and the stripping solution is the chloride rare earth product.
[0094] Normal temperature operation in step S1 simplifies the process flow and reduces energy consumption. Controlling the solid-liquid ratio ensures that the slag reacts fully with sulfuric acid and improves the reaction efficiency. Slow addition of sulfuric acid helps control the reaction rate and avoids overheating and overreaction. Controlling the pH value in step S2 optimizes the solubility of rare earth and aluminum, ensures complete reaction, obtains the best leaching effect, and dissolves the valuable elements in the mine slag to the maximum extent. Step S3 effectively separates the solid slag and the liquid acid solution, improves the efficiency of subsequent treatment, and the plate and frame filter press technology is mature, easy to operate, and highly efficient. In step S4, the amine extractant has high selectivity and can effectively separate rare earth and other impurities, and the extraction process is simple and easy. In step S5, the acid stripping can be effective. The process can effectively separate rare earth and aluminum and improve the purity of rare earth, and the treatment of the raffinate can produce rare earth composite defluorinating agent through evaporation and crystallization to achieve resource recovery; the neutralization reaction in step S6 can remove residual acid in the stripping solution to prevent corrosion to the equipment, and the use of magnesium oxide for neutralization is simple, efficient and safe to operate; the P507 extractant in step S7 can further purify the rare earth, and the performance and stability of the extractant can be improved through saponification treatment; the hydrochloric acid stripping in step S8 can efficiently recover the rare earth from the organic phase to the aqueous phase, and the operation is simple and easy to control; the recycling of magnesium sulfate in step S9 reduces wastewater discharge and meets environmental protection requirements, and the oil removal treatment ensures the quality of magnesium sulfate and prevents pollution of the mine leaching process.
[0095] In step S1, the stirring speed of the stirrer for stirring and mixing the mine slag and water in the acid dissolving tank is 50 r / min to 80 r / min, and the stirring time is 30 min;
[0096] After adding 50% sulfuric acid solution, the stirring speed of the stirrer is 50 r / min to 80 r / min, and the stirring time is 2 hours.
[0097] Ensure that the slag and water are evenly mixed in the acid dissolving tank to avoid local concentrations that are too high or too low. By evenly mixing, the contact area between the slag and sulfuric acid is increased to prepare for the subsequent acid dissolving reaction, and the solid particles are pre-dispersed in the water to reduce agglomeration when sulfuric acid is added later;
[0098] After the addition of sulfuric acid, the chemical reaction between the slag and sulfuric acid is promoted by continuous stirring to ensure that the reaction proceeds fully, keep the slag suspended in the acid solution, prevent the solid particles from settling, and ensure the uniformity of the reaction, which helps to control the reaction rate and avoid overheating and side reactions caused by too fast a reaction.
[0099] In step S4, the amine extractant is one of N1923, N263, N235, etc., the extraction ratio is 1:1 to 3:1, and the operating temperature is 30°C to 50°C.
[0100] The effect of extraction phase ratio: By adjusting the extraction phase ratio, the transfer efficiency of rare earth from rare earth sulfate solution to organic phase can be controlled. A higher phase ratio can increase the amount of extractant and improve the extraction rate of rare earth, while a lower phase ratio can help reduce the amount of extractant and reduce costs.
[0101] Effect of operating temperature: A higher operating temperature can increase the energy of molecular motion, improve the extraction rate, and quickly transfer rare earth ions to the organic phase. The appropriate temperature can reduce the viscosity of the solution, increase the separation rate of the organic and aqueous phases, reduce interphase mixing, and improve the efficiency of the extraction process.
[0102] In step S5, the acid stripping process is four-stage extraction, six-stage stripping and two-stage water washing;
[0103] In step S1, the chemical formula for acid dissolution treatment is:
[0104] 2RE(OH)3+3H2SO4→RE2(SO4)3+6H2O,
[0105] 2Al(OH)3+3H2SO4→Al2(SO4)3+3H2O
[0106] 2Fe(OH)3+3H2SO4→Fe2(SO4)3+3H2O
[0107] Among them, RE(OH)3 rare earth hydroxide, H2SO4 sulfuric acid, RE2(SO4)3 rare earth sulfate, H2O water, Al(OH)3 aluminum hydroxide, Al2(SO4)3 aluminum sulfate, Fe(OH)3 ferric hydroxide, Fe2(SO4)3 ferric sulfate.
[0108] The rare earth oxides and alumina in the mine slag can be effectively dissolved and converted into soluble rare earth sulfate and aluminum sulfate, providing high-concentration, low-impurity rare earth liquid for subsequent extraction and purification steps, thereby improving the efficiency of the overall recovery process and product quality.
[0109] In steps S4 and S5, the chemical equations for amine extraction and stripping are:
[0110] RE2(SO4)3+R3N→[R3N-RE2(SO4)3],
[0111] [R3N-RE2(SO4)3]+6H + →3R3N+2RE 3+ +3H2SO4,
[0112] Among them, RE2(SO4)3 rare earth sulfate, R3N amine extractant, rare earth complex in the organic phase after R3N-RE2(SO4)3 extraction, H + Sulfuric acid or hydrochloric acid, R3N amine extractant, RE3+ Rare earth chloride or rare earth sulfate, H2SO4 sulfuric acid.
[0113] In step S4, the amine extractant transfers the rare earth ions in the rare earth sulfate solution to the organic phase to form a rare earth complex, which enriches the rare earth and provides a basis for subsequent purification;
[0114] In step S5, rare earth is released from the organic phase through hydrochloric acid back extraction and transferred to the aqueous phase to form rare earth chloride. At the same time, the amine extractant is regenerated to ensure the recycling of the extractant. The process improves the recovery rate and purity of rare earth, effectively utilizes resources, reduces production costs, and improves the economy and sustainability of the process.
[0115] In step S6, the chemical equation for neutralization and impurity removal is:
[0116] H2SO4+MgO→MgSO4+H2O,
[0117] 3H2O+3MgO+Fe2(SO4)3→2Fe(OH)3+3MgSO4
[0118] Among them, H2SO4 sulfuric acid, MgO magnesium oxide, MgSO4 magnesium sulfate, H2O water, Fe(OH)3 ferric hydroxide, Fe2(SO4)3 ferric sulfate.
[0119] In step S6, by adding magnesium oxide slurry to neutralize the residual acid in the stripping solution, the acidity of the solution can be effectively reduced, impurities can be removed, and soluble magnesium sulfate and magnesium chloride can be generated. The process helps to protect equipment, reduce acid corrosion, and provide a purer and more stable solution environment for subsequent rare earth extraction and processing steps, thereby improving the overall process efficiency and product quality.
[0120] In steps S7 to S9, the chemical equations for extraction transformation and magnesium sulfate treatment are:
[0121] H2O+MgO→Mg(OH)2,
[0122] 2(HA) 2(O) +Mg(OH)2→Mg(HA2) 2(O) +2H2O,
[0123] 3Mg(HA2) 2(O) +RE2(SO4)3→2RE(HA2) 3(O) +3MgSO4,
[0124] 2RE(HA2) 3(O) +6HCl→6(HA) 2(O) +2RECl3,
[0125] Among them, H2O water, MgO magnesium oxide, Mg(OH)2 magnesium hydroxide, (HA) 2(O) P507, Mg(HA2) 2(O) Magnesium complex in the organic phase after extraction, RE2(SO4)3 rare earth sulfate, MgSO4 magnesium sulfate, RE(HA2) 3(O) Rare earth complexes in the organic phase after extraction, HCl hydrochloric acid, RECl3 rare earth chloride.
[0126] Through the extraction transformation and magnesium sulfate treatment in steps S7 to S9, rare earth elements can be efficiently recovered and purified, and by-products can be recycled, reducing environmental pollution, lowering production costs, and improving the economic and environmental benefits of the overall process. The chemical reactions and treatment processes in the steps ensure efficient recovery and purification of rare earth elements, while achieving sustainable utilization of resources.
[0127] In step S1, the algorithm formula for acid dissolution treatment is:
[0128] Assume the mass of mine slag is W m , the mass of water is W w The mass of sulfuric acid is
[0129] Liquid-to-solid ratio R liquid-solid :
[0130]
[0131] 1≤R liquid-solid ≤5,
[0132] Sulfuric acid addition amount:
[0133]
[0134] in, is the sulfuric acid concentration;
[0135] Assumption: W m is the mass of mine slag, in tons; W w is the mass of water, in tons; is the mass of sulfuric acid, in tons; is the concentration of sulfuric acid:
[0136] W m = 1 ton, the volume of water is 1 cubic meter to 5 cubic meters (assuming that the density of water is close to 1kg / L, the mass of water is about 1 ton to 5 tons);
[0137] The volume of the sulfuric acid solution is 0.5 cubic meters to 2 cubic meters, and the concentration is 50% (the density of a solution with a sulfuric acid concentration of 50% is about 1.4 kg / L, so the mass of the sulfuric acid solution is about 0.7 tons to 2.8 tons).
[0138] By setting the solid-liquid ratio, the slag and water can be fully mixed, the reaction can be uniform, and the dissolution efficiency can be improved. The setting of the solid-liquid ratio range can adjust the concentration conditions of the reaction to avoid over-dilution or over-concentration, thereby improving the reaction efficiency and effect.
[0139] By setting the amount of sulfuric acid added, it can be ensured that the rare earth oxides and aluminum oxide in the mine slag can be fully dissolved. The addition of sulfuric acid can improve the dissolution efficiency of rare earth oxides and aluminum oxide, ensure the full progress of the reaction, and generate soluble rare earth sulfate and aluminum sulfate;
[0140] By controlling the solid-liquid ratio, the slag and water can be fully mixed to avoid local concentrations that are too high or too low. A reasonable solid-liquid ratio can optimize the reaction conditions, improve the reaction efficiency, and ensure that the effective ingredients in the slag are fully dissolved.
[0141] In step S3, the acid slag and rare earth sulfate solution are obtained by plate and frame filtration, and the calculation formula is:
[0142]
[0143] Wherein, M acid slag is the mass of acid slag, M rare earth sulfate liquid is the mass of rare earth sulfate liquid;
[0144] If the M mine slag is 1 ton, after plate and frame filtration, the following is obtained:
[0145] The volume of the rare earth sulfate liquid is 1.5 cubic meters to 7 cubic meters;
[0146] The mass of the acid slag is 0.05 ton to 0.25 ton;
[0147] Assume that the density ρ of rare earth sulfate liquid is ≈ 1 ton / cubic meter;
[0148] Mass calculation of rare earth sulfate solution:
[0149] The calculation formula of M rare earth sulfate solution can be calculated based on its volume V rare earth sulfate solution and ρ rare earth sulfate solution:
[0150] M rare earth sulfate liquid = V rare earth sulfate liquid × ρ rare earth sulfate liquid,
[0151] Assuming that the density of rare earth sulfate liquid is 1 ton / cubic meter, then:
[0152] When the volume of rare earth sulfate liquid is 1.5 cubic meters, the mass is:
[0153] M rare earth sulfate liquid = 1.5 × 1 = 1.5 tons,
[0154] When the volume of rare earth sulfate liquid is 7 cubic meters, the mass is:
[0155] M rare earth sulfate liquid = 7 × 1 = 7 tons,
[0156] Therefore, the mass of the rare earth sulfate solution is in the range of 1.5 tons to 7 tons;
[0157] The mass of acid slag: According to the information, the mass of acid slag obtained after plate and frame filter pressing is 0.05 tons to 0.25 tons;
[0158] Assuming that the formula is to describe the mass relationship between the acid slag and the rare earth sulfate solution, it is expressed as follows:
[0159] M50% sulfuric acid + M mining slag = M acid slag + M rare earth sulfate liquid + M other lost or residual substances,
[0160] The formula shows that the total mass of mine slag is equal to the sum of acid slag, rare earth sulfate liquid and other losses minus the mass of added sulfuric acid.
[0161] Acid slag is the solid residue separated from the mixture by plate and frame filter press after acid dissolution treatment. It mainly contains unreacted minerals and other impurities. By separating the acid slag, the impurity content in the subsequent treatment process can be reduced and the purity of the rare earth sulfate liquid can be improved.
[0162] Rare earth sulfate liquid is the liquid part separated from the mixture by plate and frame filter press after acid dissolution treatment. It mainly contains dissolved rare earth sulfate and other dissolved substances. The rare earth sulfate liquid contains the target rare earth elements to be recovered. The subsequent extraction and stripping steps will extract and purify the rare earths based on this liquid.
[0163] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for recovering high-priced elements from mine slag, wherein the mine slag is produced in the process of magnesium sulfate in-situ leaching and sodium bicarbonate impurity removal and precipitation: characterized in that: The steps include: S1. Under normal temperature conditions, water and mine slag are stirred in an acid dissolving tank at a liquid-to-solid ratio of 1:1 to 5:1, and 50% sulfuric acid solution is slowly added during the stirring process; S2. The pH value of the acid solution endpoint should be between 0.5 and 2.5; S3, obtaining acid slag and rare earth sulfate liquid by plate and frame filter pressing; S4, extracting the rare earth in the rare earth sulfate solution into an organic phase using an amine extractant; S5, using acid for stripping to separate rare earth and aluminum, the raffinate is evaporated and crystallized to produce rare earth composite defluorinating agent, and the stripping solution enters the neutralization and impurity removal process; S6, placing the stripping solution obtained in the amine extraction step into a stirring tank, and slowly adding magnesium oxide slurry to neutralize the residual acid until the pH value is about 4.5; S7, the treated impurity removal liquid enters the extraction transformation process, using 10% to 30% magnesium oxide slurry tank saponification P507 extractant, controlling the volume ratio of the saponification extractant to the impurity removal liquid; S8, stripping with hydrochloric acid; S9. The magnesium sulfate in the raffinate is deoiled and returned to the mine for leaching, and the stripping solution is the chloride rare earth product.
2. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the step S1, the stirring speed of the stirrer for stirring and mixing the mine slag and water in the acid dissolving tank is 50 r / min to 80 r / min, and the stirring time is 30 min; After adding the 50% sulfuric acid solution, the stirring speed of the stirrer is 50 r / min to 80 r / min, and the stirring time is 2 hours.
3. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the step S4, the amine extractant is one of N1923, N263, N235, etc., the extraction ratio is 1:1 to 3:1, and the operating temperature is 30°C to 50°C.
4. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the steps S4 and S5, the amine extraction is a cascade countercurrent process, which includes four-stage extraction, six-stage stripping and two-stage water washing; Extraction section: It consists of 1 to 4 stages. At a temperature of 30℃ to 50℃, amine extractants and acid solutions are added to the 1st and 4th stage mixing chambers in a ratio of 1:1 to 3:
1. The stirring time in the mixing chamber is 3min to 5min. The raffinate is separated in the 1st stage clarification chamber. Stripping section: It consists of 5 to 10 stages. Hydrochloric acid or sulfuric acid is added in the 10th stage to contact the organic phase, so that the rare earth extracted into the organic phase returns to the water phase and the stripping liquid is separated from the 5-stage clarification chamber. Water washing section: It consists of 11 to 12 stages. Water is added in the 12th stage to contact the organic phase. High-acid water washing liquid is released from the 11th stage clarification chamber. The organic phase after water washing can be returned to the 1st stage for extraction and recycling.
5. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the step S1, the chemical equation for the acid dissolution treatment is: 2RE(OH)3+3H2SO4→RE2(SO4)3+6H2O, 2Al(OH)3+3H2SO4→Al2(SO4)3+3H2O 2Fe(OH)3+3H2SO4→Fe2(SO4)3+3H2O Among them, RE(OH)3 rare earth hydroxide, H2SO4 sulfuric acid, RE2(SO4)3 rare earth sulfate, H2O water, Al(OH)3 aluminum hydroxide, Al2(SO4)3 aluminum sulfate, Fe(OH)3 ferric hydroxide, Fe2(SO4)3 ferric sulfate.
6. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the steps S4 and S5, the chemical equations for amine extraction and stripping are: RE2(SO4)3+R3N→[R3N-RE2(SO4)3], [R3N-RE2(SO4)3]+6H + →R3N+2RE 3+ +3H2SO4, Among them, RE2(SO4)3 rare earth sulfate, R3N amine extractant, rare earth complex in the organic phase after R3N-RE2(SO4)3 extraction, H + Sulfuric acid or hydrochloric acid, RE 3+ Rare earth chloride or rare earth sulfate, H2SO4 sulfuric acid.
7. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the step S6, the chemical equation for neutralization and impurity removal is: H2SO4+MgO→MgSO4+H2O, 3H2O+3MgO+Fe2(SO4)3→2Fe(OH)3+3MgSO4 Among them, H2SO4 sulfuric acid, MgO magnesium oxide, MgSO4 magnesium sulfate, H2O water, Fe(OH)3 ferric hydroxide, Fe2(SO4)3 ferric sulfate.
8. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the steps S7 to S9, the main chemical equation is: H2O+MgO→Mg(OH)2, <h2 style=";text-align:left;direction:ltr">2(HA)<h2 style=";text-align:left;direction:ltr"> 2(O) <h2 style=";text-align:left;direction:ltr"> +Mg(OH)2→Mg(HA2)<h2 style=";text-align:left;direction:ltr"> 2(O) <h2 style=";text-align:left;direction:ltr"> +2H2O, <h2 style=";text-align:left;direction:ltr">3Mg(HA2)<h2 style=";text-align:left;direction:ltr"> 2(O) <h2 style=";text-align:left;direction:ltr"> +RE2(SO4)3→2RE(HA2)<h2 style=";text-align:left;direction:ltr"> 3(O) <h2 style=";text-align:left;direction:ltr"> +3MgSO4, <h2 style=";text-align:left;direction:ltr">2RE(HA2)<h2 style=";text-align:left;direction:ltr"> 3(O) <h2 style=";text-align:left;direction:ltr"> +6HCl→6(HA)<h2 style=";text-align:left;direction:ltr"> 2(O) <h2 style=";text-align:left;direction:ltr"> +2RECl3, Among them, H2O water, MgO magnesium oxide, Mg(OH)2 magnesium hydroxide, (HA) 2(O) P507, Mg(HA2) 2(O) Magnesium complex in the organic phase after extraction, RE2(SO4)3 rare earth sulfate, MgSO4 magnesium sulfate, RE(HA2) 3(O) Rare earth complexes in the organic phase after extraction, HCl hydrochloric acid, RECl3 rare earth chloride.
9. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the step S1, the algorithm formula for acid dissolution treatment is: Assume the mass of mine slag is W m , the mass of water is W w The mass of sulfuric acid is Liquid-to-solid ratio R liquid-solid : 1≤R liquid-solid ≤5, Sulfuric acid addition amount: in, is the sulfuric acid concentration; Assumption: W m is the mass of mine slag, in tons; W w is the mass of water, in tons; is the mass of sulfuric acid, in tons; is the concentration of sulfuric acid: W m = 1 ton, the volume of water is 1 cubic meter to 5 cubic meters (assuming that the density of water is close to 1kg / L, the mass of water is about 1 ton to 5 tons); The volume of the sulfuric acid solution is 0.5 cubic meters to 2 cubic meters, and the concentration is 50% (the density of a solution with a sulfuric acid concentration of 50% is about 1.4 kg / L, so the mass of the sulfuric acid solution is about 0.7 tons to 2.8 tons).
10. The method for recovering high-price elements from mine slag according to claim 1, characterized in that: In the step S3, the acid slag and rare earth sulfate solution are obtained by plate and frame filtration, and the calculation formula is: Wherein, M acid slag is the mass of acid slag, M rare earth sulfate liquid is the mass of rare earth sulfate liquid; If the M mine slag is 1 ton, after plate and frame filtration, the following is obtained: The volume of the rare earth sulfate liquid is 1.5 cubic meters to 7 cubic meters; The mass of the acid slag is 0.05 ton to 0.25 ton; Assuming the density ρ 硫酸稀土料液 ≈1 ton / cubic meter; Mass calculation of rare earth sulfate solution: M 硫酸稀土料液 The calculation formula can be based on its volume V 硫酸稀土料液 and ρ 硫酸稀土料液 To calculate: M 硫酸稀土料液 =V 硫酸稀土料液 ×ρ 硫酸稀土料液 , Assuming that the density of rare earth sulfate liquid is 1 ton / cubic meter, then: When the volume of rare earth sulfate liquid is 1.5 cubic meters, the mass is: M 硫酸稀土料液 =1.5×1=1.5 tons, When the volume of rare earth sulfate liquid is 7 cubic meters, the mass is: M 硫酸稀土料液 =7×1=7 tons, Therefore, the mass of the rare earth sulfate solution is in the range of 1.5 tons to 7 tons; The mass of acid slag: According to the information, the mass of acid slag obtained after plate and frame filter pressing is 0.05 tons to 0.25 tons; Assuming that the formula is to describe the mass relationship between the acid slag and the rare earth sulfate solution, it is expressed as follows: M50% sulfuric acid + M mining slag = M acid slag + M rare earth sulfate liquid + M other lost or residual substances, The formula shows that the total mass of mine slag is equal to the sum of acid slag, rare earth sulfate liquid and other losses minus the mass of added sulfuric acid.
Citation Information
Patent Citations
Method for recovering thorium, uranium and rare earth from monazite smelting acid-insoluble slag
CN104278165A
Method for recovering and recycling valuable elements from low-content rare earth solution and precipitation sludge
CN106367621A
Method for recovering rare earth by fractional extraction
WO2016106732A1
Cited By
A method for separating light, medium and heavy rare earths and aluminum by synergic-coupling extraction
CN122979672A