Heat treatment method of laser cladding nickel-based single crystal alloy

The heat treatment method for nickel-based single crystal alloys addresses the issues of uneven precipitation and structural degradation by using DSC and simulation to determine optimal heat treatment parameters, enhancing microstructure and mechanical properties.

CN119082635APending Publication Date: 2024-12-06NORTHWESTERN POLYTECHNICAL UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411239782.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The complex solidification conditions during laser cladding of nickel-based single crystal alloys lead to uneven precipitation of the γ′ strengthening phase, resulting in unsatisfactory microstructure and mechanical properties, while standard solution heat treatment can destroy the single crystal structure and reduce mechanical properties.

Method used

A heat treatment method involving differential scanning calorimetry (DSC) and simulation to determine specific solution temperatures and times, followed by solution and aging heat treatments, to inhibit recrystallization and maintain the single crystal structure integrity.

Benefits of technology

The method effectively inhibits recrystallization and improves the microstructure and mechanical properties of laser-clad nickel-based single crystal alloys, ensuring high-quality alloy production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082635A_ABST
    Figure CN119082635A_ABST
Patent Text Reader

Abstract

The invention provides a heat treatment method of a laser cladding nickel-based single crystal alloy, and relates to the technical field of alloys. The method comprises the following steps: performing a laser cladding process on the nickel-based single crystal alloy to obtain a laser-cladded alloy, and extracting an alloy test piece; a DSC experiment and a material thermophysical property simulation process are executed based on the laser-clad alloy, so that a DSC experiment result and a simulation result are obtained respectively; determining each solid solution temperature of solid solution heat treatment by utilizing a DSC experiment result and a simulation result, and determining corresponding solid solution time; carrying out solid solution heat treatment on the alloy test piece according to each solid solution temperature and the solid solution time corresponding to each solid solution temperature, and determining an initial solid solution temperature when a dendritic crystal dry gamma'phase is completely dissolved and a secondary solid solution temperature when an interdendritic crystal gamma 'phase is completely dissolved by combining the morphological characteristics after the solid solution heat treatment; and carrying out heat treatment by utilizing the initial solid solution temperature and the secondary solid solution temperature. According to the invention, the heat treatment effect after laser cladding can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of alloys, and in particular to a heat treatment method for laser cladding nickel-based single crystal alloys. Background Art

[0002] Nickel-based single crystal alloys have become important materials for hot-end components of advanced aero-engines and gas turbines due to their excellent high-temperature mechanical properties. The working environment of hot-end components is harsh, and they are prone to damage such as cracks, wear, deformation, and even material loss and fracture, which requires a lot of repairs on hot-end components. In order to restore the geometry and mechanical properties of damaged parts of hot-end components, a variety of repair technologies such as laser cladding have emerged. They complete the remanufacturing of damaged parts by transporting powder to the damaged area, and have been initially applied to components such as turbine disks and turbine blades. However, the complex solidification conditions during laser cladding may cause the γ′ strengthening phase to be too small and uneven, affecting the high-temperature mechanical properties. In order to achieve uniform microstructure and good mechanical properties, appropriate heat treatment can be carried out to make the γ′ strengthening phase grow, thereby realizing the recovery of the mechanical properties of the material.

[0003] However, if standard solution heat treatment is performed directly, the deformation of the high dislocation density area in the heat affected zone of the laser cladding single crystal alloy provides a driving force for recrystallization. Recrystallization occurs under high temperature heat treatment, destroying the single crystal structure and reducing the mechanical properties of the material, resulting in deterioration of the alloy quality.

[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0005] The purpose of the present disclosure is to provide a heat treatment method for laser-clad nickel-based single crystal alloy and a nickel-based single crystal alloy, thereby at least to a certain extent overcoming the problem of alloy quality deterioration after heat treatment of nickel-based single crystal alloy after laser cladding.

[0006] According to a first aspect of the present disclosure, a heat treatment method for a laser-clad nickel-based single crystal alloy is provided, comprising: performing a laser cladding process on a nickel-based single crystal alloy to obtain a laser-clad alloy, and extracting an alloy specimen from the laser-clad alloy; performing a differential scanning calorimetry (DSC) experiment and a material thermophysical property simulation process based on the laser-clad alloy to obtain a DSC experimental result and a simulation result, respectively; determining each solution temperature of the solution heat treatment using the DSC experimental result and the simulation result, and determining the solution time corresponding to each solution temperature; performing a solution heat treatment on the alloy specimen according to each solution temperature and the solution time corresponding to each solution temperature, and determining an initial solution temperature when the dendrite main γ′ phase is completely dissolved and a secondary solution temperature when the interdendritic γ′ phase is completely dissolved in combination with the morphological characteristics after the solution heat treatment; and performing a heat treatment on the laser-clad alloy using the initial solution temperature and the secondary solution temperature.

[0007] Optionally, a laser cladding process is performed on the nickel-based single crystal alloy to obtain a laser-clad alloy, including: performing surface grinding and polishing, cleaning and drying treatments on the nickel-based single crystal alloy in sequence; obtaining spherical single crystal alloy powder as a raw material for laser cladding forming; and conveying the spherical single crystal alloy powder to each layer of the laser forming molten pool under a protective gas atmosphere to obtain a laser-clad alloy.

[0008] Optionally, performing a differential scanning calorimetry (DSC) experiment based on the laser-clad alloy includes: obtaining the size of the DSC crucible; cutting a DSC experimental piece from the nickel-based single crystal alloy and / or the laser-clad alloy according to the size of the DSC crucible; placing the DSC experimental piece in the DSC crucible and performing the DSC experiment.

[0009] Optionally, using DSC experimental results and simulation results to determine the various solution temperatures of the solution heat treatment includes: determining the first γ′ phase dissolution temperature from the DSC experimental results, determining the second γ′ phase dissolution temperature from the simulation results, and determining the smaller temperature of the first γ′ phase dissolution temperature and the second γ′ phase dissolution temperature as the minimum solution temperature; determining the first solid phase line from the DSC experimental results, determining the second solid phase line from the simulation results, and determining the corresponding larger temperature of the first solid phase line and the second solid phase line as the maximum solution temperature; dividing the solution temperature range composed of the minimum solution temperature and the maximum solution temperature into equal parts to determine the various solution temperatures of the solution heat treatment.

[0010] Optionally, determining the solution time corresponding to each solution temperature includes: determining the diffusion time of an element with the smallest diffusion coefficient in the nickel-based single crystal alloy at the solution temperature as the solution time corresponding to the solution temperature.

[0011] Optionally, the number of alloy specimens is consistent with the number of solution temperatures, the alloy specimens include target alloy specimens, and the solution temperature includes a target solution temperature; wherein, performing solution heat treatment on the alloy specimens according to each solution temperature and the solution time corresponding to each solution temperature includes: performing solution heat treatment on the target alloy specimen at the target solution temperature for a solution time corresponding to the target solution temperature.

[0012] Optionally, the heat treatment method of laser cladding nickel-based single crystal alloy also includes: after the alloy specimen is subjected to solution heat treatment, using an embedding machine to embed the alloy specimen into a hot embedding material to obtain a metallographic specimen; grinding and polishing the surface of the metallographic specimen; corroding the surface of the metallographic specimen after the grinding and polishing operations using a corrosive liquid; obtaining the corroded metallographic specimen, and obtaining the morphological characteristics after the solution heat treatment through a scanning electron microscope.

[0013] Optionally, heat treating the laser clad alloy using the initial solution temperature and the secondary solution temperature includes: performing solution heat treatment on the laser clad alloy at the initial solution temperature for a solution time corresponding to the initial solution temperature to obtain a first intermediate alloy; increasing the temperature from the initial solution temperature to the secondary solution temperature, performing solution heat treatment on the first intermediate alloy to obtain a second intermediate alloy; and performing aging heat treatment on the second intermediate alloy.

[0014] Optionally, performing aging heat treatment on the second master alloy includes: air cooling the second master alloy; performing a first aging heat treatment on the air-cooled second master alloy, and air cooling after the first aging heat treatment to obtain a third master alloy; performing a second aging heat treatment on the third master alloy to obtain a target alloy; wherein the temperature of the first aging heat treatment is higher than the temperature of the second aging heat treatment.

[0015] According to a second aspect of the present disclosure, there is provided a nickel-based single crystal alloy, which is obtained by processing according to any one of the above-mentioned heat treatment methods for laser cladding nickel-based single crystal alloys.

[0016] Through the nickel-based single crystal alloy processing scheme of the embodiment of the present disclosure, for the heat treatment process after laser cladding, multiple solid solution temperatures and corresponding solid solution times are determined by combining DSC experiments and simulations, and then the initial solid solution temperature when the dendrite stem γ′ phase is completely dissolved and the secondary solid solution temperature when the interdendritic γ′ phase is completely dissolved are determined in combination with the morphological characteristics of each sample after solid solution treatment. The heat treatment of the alloy after laser cladding is achieved based on these two solid solution temperatures. By determining the above initial solid solution temperature and secondary solid solution temperature, it is applied to the actual heat treatment process, which improves the effect of heat treatment after laser cladding, can effectively inhibit the growth of impurity crystals, ensure the integrity of the single crystal structure and the mechanical properties of the alloy, and help to obtain high-quality nickel-based single crystal alloys.

[0017] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0019] Figure 1 The figure shows the scanning electron microscope (SEM) microscopic morphology of the alloy obtained by heat treatment after laser cladding using some technologies.

[0020] Figure 2 The flowchart of the heat treatment method of the laser cladding nickel-based single crystal alloy according to the embodiment of the present disclosure is schematically shown.

[0021] Figure 3 A schematic diagram of an alloy and an alloy specimen after laser cladding treatment according to an embodiment of the present disclosure is shown.

[0022] Figure 4 A schematic diagram of the microscopic morphology corresponding to the complete dissolution of the dendrite trunk γ′ phase and the partial dissolution of the interdendritic γ′ phase at the initial solution temperature of the embodiment of the present disclosure is shown.

[0023] Figure 5 A schematic diagram of the microscopic morphology corresponding to the complete dissolution of the dendrite trunk γ′ phase and the interdendritic γ′ phase at the secondary solution temperature of an embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0024] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, processes, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0025] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated descriptions will be omitted. The flowcharts shown in the accompanying drawings are only exemplary illustrations and do not necessarily include all the steps. For example, some steps can also be decomposed, while some steps can be combined or partially combined, so the actual execution order may change according to actual conditions. In addition, all the terms "first", "second", etc. below are only for the purpose of distinction and should not be used as limitations of the present disclosure.

[0026] At present, a pain point of laser cladding of nickel-based single crystal alloys is that the solidification conditions during the laser cladding process are complex, which affects the precipitation of the strengthening phase and the brittle phase, resulting in unsatisfactory microstructure and mechanical properties after deposition. Therefore, it is necessary to regulate the precipitation of the strengthening phase through heat treatment, thereby realizing the recovery of the mechanical properties of the material.

[0027] However, the laser cladding process will introduce high residual stress and a large number of dislocations. If the standard solution heat treatment process is directly carried out, the γ′ phase will be completely dissolved, allowing high-density dislocations to move almost unimpeded, which can easily lead to recrystallization nucleation or growth of stray grains, resulting in a polycrystalline structure with large-angle grain boundaries, destroying the integrity of the single crystal. Figure 1 The schematic diagram of the scanning electron microscope microstructure of the alloy obtained by these techniques after laser cladding and heat treatment is shown. Figure 1 , these techniques induce a large amount of recrystallization, which will destroy the integrity of the single crystal.

[0028] Therefore, a heat treatment process is needed that can inhibit recrystallization, reduce the dislocation density of the deposited layer, and adjust the microstructure to improve the performance of the repaired alloy material while avoiding recrystallization.

[0029] In view of this, the embodiments of the present disclosure provide a new heat treatment method for laser cladding nickel-based single crystal alloys, which first determines the initial solution temperature and the secondary solution temperature by testing, and then uses these two solution temperatures for solution heat treatment. The treatment process takes into account the size, content and distribution uniformity of the strengthening phase in the alloy during the heat treatment and the inhibitory effect of recrystallization, which can effectively avoid recrystallization while inhibiting the growth of impurity crystals, and effectively restore the performance of the laser cladding nickel-based single crystal alloy.

[0030] Figure 2 The flowchart of the heat treatment method of the laser cladding nickel-based single crystal alloy according to the embodiment of the present disclosure is schematically shown. Figure 2 The heat treatment method of the laser cladding nickel-based single crystal alloy according to the embodiment of the present disclosure may include the following steps:

[0031] S20. Performing a laser cladding process on the nickel-based single crystal alloy to obtain a laser-clad alloy, and extracting an alloy specimen from the laser-clad alloy.

[0032] In an exemplary embodiment of the present disclosure, the nickel-based single crystal alloy may also be referred to as a nickel-based single crystal alloy substrate, a nickel-based single crystal alloy matrix, etc., which is the alloy to be laser clad. The present disclosure does not limit the specific type of the nickel-based single crystal alloy.

[0033] First, the nickel-based single crystal alloy can be subjected to surface grinding and polishing, cleaning and drying in sequence. Specifically, the grinding and polishing can use 600# to 800# sandpaper to make the surface of the nickel-based single crystal alloy flat and the scratch direction consistent and uniform. After grinding and polishing, the alloy surface can be wiped with acetone and alcohol in sequence and air-dried.

[0034] In addition, spherical single crystal alloy powder is obtained as a raw material for laser cladding forming. Specifically, the distribution of the particle size of the alloy powder can be 53 μm to 150 μm. The alloy powder can be prepared, for example, by a vacuum gas atomization (VIGA) method or a plasma rotating electrode (PREP) method, and the powder is placed in a vacuum environment at 120° C. and dried for 150 minutes to eliminate moisture that may be contained in the powder.

[0035] Next, under a protective gas atmosphere, the spherical single crystal alloy powder can be transported to each layer of the laser forming molten pool to obtain a laser clad alloy. Specifically, under an argon protective gas, the above alloy powder can be transported to each layer of the laser forming molten pool of the metal material through a powder feeding head coaxial with the laser source to obtain a laser clad alloy.

[0036] After obtaining the laser-clad alloy, alloy specimens can be extracted therefrom for use in subsequent steps. On the one hand, in order to determine the initial solid solution temperature and the secondary solid solution temperature described below, multiple alloy specimens are required, that is, in this step, multiple alloy specimens can be extracted from the laser-clad alloy. On the other hand, the embodiment of the present disclosure does not limit the size of the alloy specimen, for example, the size of the alloy specimen is 5mm×5mm×2.5mm. In addition, it can be understood that the sizes of the multiple alloy specimens used in the embodiment of the present disclosure may be the same or different, and the present disclosure does not limit this.

[0037] Figure 3 Schematic diagram of the alloy and alloy specimen after laser cladding treatment according to the embodiment of the present disclosure is shown. Figure 3 , a laser-clad alloy 32 can be generated based on the nickel-based single crystal alloy 31 and the above alloy powder, and an alloy specimen 321 can be cut from the laser-clad alloy 32 .

[0038] S22. Perform differential scanning calorimetry (DSC) experiments and material thermophysical properties simulation processes based on the laser cladding alloy to obtain DSC experimental results and simulation results, respectively.

[0039] According to some embodiments of the present disclosure, a DSC experiment may be directly performed on the nickel-based single crystal alloy and / or the laser-clad alloy obtained in step S20 to obtain a DSC experiment result.

[0040] According to some other embodiments of the present disclosure, due to reasons such as the limited size of the DSC crucible, it may be necessary to cut out a DSC experimental piece and use the DSC experimental piece to perform the DSC experiment.

[0041] First, the size of the DSC crucible can be obtained, which is, for example, 5 mm in inner diameter and 3 mm in height. The size of the DSC test piece needs to be smaller than the crucible size.

[0042] Next, a DSC test piece is cut from the nickel-based single crystal alloy and / or the laser-clad alloy according to the size of the DSC crucible. For example, a DSC test piece with a size of 3 mm×3 mm×1.5 mm can be cut from the nickel-based single crystal alloy and / or the laser-clad alloy using an electric spark wire, and the surface is polished and ultrasonically cleaned for 5 minutes.

[0043] Subsequently, the DSC experimental block can be placed in a DSC crucible and heated from room temperature to 1400° C. at a heating rate of 5° C. / min to obtain DSC experimental results.

[0044] It is to be understood that the DSC experimental results mentioned in the embodiments of the present disclosure include a DSC curve, from which the γ′ phase dissolution temperature and the solidus can be determined.

[0045] In addition, the material thermophysical properties simulation process can be performed on the nickel-based single crystal alloy and / or the laser-clad alloy to obtain simulation results. Specifically, the thermophysical properties of the material can be simulated using material properties simulation software to obtain the γ′ phase dissolution temperature and solidus. The present disclosure does not limit the type of simulation software used. In addition, the simulation results can also include the liquidus of the material, etc., which is not limited by the present disclosure.

[0046] It should be noted that when DSC experiments are performed on both nickel-based single crystal alloys and laser-clad alloys, the DSC experimental results obtained from the two can be used as references to avoid large deviations in the analysis data that affect the subsequent heat treatment process. As for the simulation of the thermophysical properties of the material, since the elemental composition of the material is the same, the nickel-based alloy material can be directly used in the metal material phase diagram calculation and performance analysis software to simulate the thermophysical properties of the material.

[0047] S24. Use the DSC experimental results and simulation results to determine the various solution temperatures of the solution heat treatment, and determine the solution time corresponding to each solution temperature.

[0048] On the one hand, the first γ′ phase dissolution temperature can be determined from the DSC experimental results, the second γ′ phase dissolution temperature can be determined from the simulation results, and the smaller temperature of the first γ′ phase dissolution temperature and the second γ′ phase dissolution temperature can be determined as the minimum solid solution temperature. On the other hand, the first solid phase line can be determined from the DSC experimental results, the second solid phase line can be determined from the simulation results, and the corresponding larger temperature of the first solid phase line and the second solid phase line can be determined as the maximum solid solution temperature.

[0049] The solution temperature range consisting of the minimum solution temperature and the maximum solution temperature can then be divided equally to determine the individual solution temperatures for the solution heat treatment.

[0050] For example, let the minimum solution temperature be T 11 The maximum solution temperature is denoted as T 1n , then you can 11 With T 1n The specific operation of dividing the solution into equal parts is not limited in the present disclosure.

[0051] According to some embodiments of the present disclosure, a solution temperature may be set every 10°C. It can be understood that the second solution temperature T 12 =T 11 +10, and so on, we can get n solid solution temperatures T 11 , T 12 ,…,T 1n It should be noted that the above-mentioned interval of 10°C is only an exemplary description, and it can also be every 5°C, 15°C, 20°C, etc.

[0052] In the process of determining the solution time corresponding to each solution temperature, the diffusion time of the element with the smallest diffusion coefficient in the nickel-based single crystal alloy at the solution temperature can be determined as the solution time corresponding to the solution temperature.

[0053] Specifically, assuming that the diffusion length d diff When the distance between the dendrite arms is equal to half of the distance between the maximum and minimum values ​​of the element concentration, homogenization is achieved. The solution temperature t can be determined using Formula 1:

[0054]

[0055] Among them, the diffusion coefficient of the element changes with temperature, D (A) is the diffusion coefficient of the least soluble element (i.e. the element with the smallest diffusion coefficient). In addition, the solution time at different solution temperatures can be recorded as t11 ,t 12 ,…,t 1n .

[0056] According to other embodiments of the present disclosure, several experiments can be used to fit the law of the solution time, and each solution time can be matched with the solution temperature one by one. The present disclosure does not limit this.

[0057] S26. Perform solution heat treatment on the alloy specimens according to each solution temperature and the solution time corresponding to each solution temperature, and determine the initial solution temperature when the dendrite trunk γ′ phase is completely dissolved and the secondary solution temperature when the interdendritic γ′ phase is completely dissolved based on the morphological characteristics after solution heat treatment.

[0058] In an exemplary embodiment of the present disclosure, the number of alloy specimens determined in step S20 is consistent with the number of solution temperatures and corresponds one to one. For example, the alloy specimens include target alloy specimens, the solution temperatures include target solution temperatures, and the target alloy specimens may be subjected to solution heat treatment at the target solution temperature for a solution time corresponding to the target solution temperature.

[0059] If the alloy specimens are numbered 1, 2, ..., n, they can be placed in a heat treatment furnace in sequence, and the heating rate is configured to be 15°C / min, for example. The solution heat treatment method is shown in Table 1, and air cooling can be performed after the heat treatment.

[0060] Table 1

[0061]

[0062] For each alloy specimen, after the solution heat treatment, an electron microscope scan can be performed to obtain the microscopic morphology of each alloy specimen after the solution heat treatment.

[0063] Specifically, the solution temperature when the γ′ phase in the dendrite is completely dissolved can be recorded as the initial solution temperature. At the initial solution temperature, dislocations move freely and are completely annihilated in the dendrite, which can eliminate the stored energy that drives the nucleation of new recrystallized grains, while the remaining precipitates between dendrites can hinder the movement and interaction of dislocations, the nucleation of recrystallization, and the growth of impurity grains. Figure 4 A schematic diagram of the microscopic morphology corresponding to the complete dissolution of the dendrite trunk γ′ phase and the partial dissolution of the interdendritic γ′ phase at the initial solution temperature of the embodiment of the present disclosure is shown.

[0064] In addition, the solution temperature at which the interdendritic γ′ phase completely dissolves can be recorded as the secondary solution temperature. At the secondary solution temperature, the remaining γ′ phase in the interdendritic space is completely dissolved, and a uniformly sized reinforcement phase can be obtained. Figure 5A schematic diagram of the microscopic morphology corresponding to the complete dissolution of the dendrite trunk γ′ phase and the interdendritic γ′ phase at the secondary solution temperature of an embodiment of the present disclosure is shown.

[0065] After solution heat treatment and air cooling and before electron microscope scanning, the alloy specimens may be further processed to ensure that the alloy surface microstructure can be observed through an electron microscope.

[0066] First, after the alloy specimen is subjected to solution heat treatment, a mounting machine can be used to mount the alloy specimen into a hot mounting material to obtain a metallographic specimen.

[0067] Next, the surface of the metallographic sample can be ground and polished. Specifically, 600#, 800#, 1000#, 1500#, and 2000# sandpaper can be used for grinding and the grinding surface can be observed until the scratches on the surface of the sample are small and uniform. Then, the sample is polished with a flannel cloth on an automatic grinder, and polished with abrasive pastes with a particle size of 1μm and 0.5μm step by step until the surface of the sample is smooth.

[0068] Subsequently, the surface of the metallographic sample after grinding and polishing can be corroded by using a corrosive solution. Specifically, the corrosive solution can contain, for example, 20 g of CuSO 4 5ml of H 2 SO 4 , 50 ml of HCl and 100 ml of H 2 In addition, the corrosion time can be configured to be 3 seconds, for example, and after the corrosion is completed, the test piece is pried out of the embedding material with a hot melt gun.

[0069] Through the above treatment, a corroded metallographic sample can be obtained, and the morphological characteristics after solution heat treatment can be obtained by scanning electron microscopy.

[0070] S28. Heat treat the laser clad alloy using the initial solution temperature and the secondary solution temperature.

[0071] First, the laser clad alloy may be subjected to a solution heat treatment at an initial solution temperature for a solution time corresponding to the initial solution temperature to obtain a first master alloy.

[0072] Next, the first intermediate alloy is subjected to solution heat treatment by increasing the temperature from the initial solution temperature to the secondary solution temperature, thereby obtaining the second intermediate alloy. It should be noted that when the temperature reaches the secondary solution temperature, no heat preservation is performed. This method of increasing the temperature from the initial solution temperature to the secondary solution temperature can avoid the occurrence of recrystallization.

[0073] Then, the second master alloy is subjected to aging heat treatment.

[0074] Specifically, the second master alloy may be air-cooled, and after air-cooling, the second master alloy is subjected to a first aging heat treatment, and after the first aging heat treatment, air-cooled to obtain a third master alloy. The third master alloy is then subjected to a second aging heat treatment to obtain a target alloy. It is understood that the target alloy is an alloy corresponding to the nickel-based single crystal alloy in step S20 after laser cladding and heat treatment.

[0075] The temperature of the first aging heat treatment is higher than that of the second aging heat treatment. For example, the first aging heat treatment is 1100°C for 6 hours, and the second aging heat treatment is 870°C for 20 hours.

[0076] Furthermore, the present disclosure also provides a nickel-based single crystal alloy, which is obtained by processing based on the above-mentioned heat treatment method of laser cladding nickel-based single crystal alloy.

[0077] It should be noted that although the steps of the method in the present disclosure are described in a specific order in the drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.

[0078] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0079] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing what is disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and embodiments are to be considered merely as exemplary, and the true scope and spirit of the present disclosure are indicated by the claims.

[0080] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A heat treatment method for laser cladding nickel-based single crystal alloy, characterized in that: include: performing a laser cladding process on a nickel-based single crystal alloy to obtain a laser-clad alloy, and extracting an alloy specimen from the laser-clad alloy; Performing a differential scanning calorimetry (DSC) experiment and a material thermophysical properties simulation process based on the laser cladding alloy to obtain a DSC experimental result and a simulation result, respectively; Determine each solution temperature of the solution heat treatment using the DSC experimental results and the simulation results, and determine the solution time corresponding to each solution temperature; Performing a solution heat treatment on the alloy specimen according to each of the solution temperatures and the solution time corresponding to each of the solution temperatures, and determining an initial solution temperature when the dendrite trunk γ′ phase is completely dissolved and a secondary solution temperature when the interdendritic γ′ phase is completely dissolved in combination with the morphological characteristics after the solution heat treatment; The laser clad alloy is heat treated using the initial solution temperature and the secondary solution temperature.

2. The heat treatment method of laser cladding nickel-based single crystal alloy according to claim 1, characterized in that: The laser cladding process is performed on the nickel-based single crystal alloy to obtain a laser clad alloy, including: The nickel-based single crystal alloy is subjected to surface grinding and polishing, cleaning and drying in sequence; Obtaining spherical single crystal alloy powder as raw material for laser cladding forming; Under a protective gas atmosphere, the spherical single crystal alloy powder is transported to each layer of laser forming molten pool to obtain a laser cladding alloy.

3. The heat treatment method of laser cladding nickel-based single crystal alloy according to claim 1, characterized in that: The differential scanning calorimetry (DSC) experiments performed on the laser clad alloys include: Get the size of the DSC crucible; Cutting a DSC test piece from the nickel-based single crystal alloy and / or the laser-clad alloy according to the size of the DSC crucible; The DSC test piece is placed in the DSC crucible, and a DSC experiment is performed.

4. The heat treatment method of laser cladding nickel-based single crystal alloy according to claim 1, characterized in that: Determining various solution temperatures of solution heat treatment using the DSC experimental results and the simulation results includes: Determining a first γ′ phase dissolution temperature from the DSC experimental results, determining a second γ′ phase dissolution temperature from the simulation results, and determining a smaller temperature between the first γ′ phase dissolution temperature and the second γ′ phase dissolution temperature as a minimum solution temperature; Determine a first solidus from the DSC experimental results, determine a second solidus from the simulation results, and determine a larger temperature corresponding to the first solidus and the second solidus as a maximum solution temperature; The solution temperature range consisting of the minimum solution temperature and the maximum solution temperature is equally divided to determine each solution temperature of the solution heat treatment.

5. The heat treatment method of laser cladding nickel-based single crystal alloy according to claim 1, characterized in that: Determining the solution time corresponding to each of the solution temperatures comprises: The diffusion time of the element with the smallest diffusion coefficient in the nickel-based single crystal alloy at the solid solution temperature is determined as the solid solution time corresponding to the solid solution temperature.

6. The heat treatment method of laser cladding nickel-based single crystal alloy according to claim 1, characterized in that: The number of the alloy specimens is consistent with the number of the solution temperatures, the alloy specimens include target alloy specimens, and the solution temperatures include target solution temperatures; wherein performing solution heat treatment on the alloy specimens according to the solution temperatures and the solution times corresponding to the solution temperatures includes: The target alloy specimen is subjected to a solution heat treatment at the target solution temperature for a solution time corresponding to the target solution temperature.

7. The heat treatment method of laser cladding nickel-based single crystal alloy according to claim 1 or 6, characterized in that: The heat treatment method of the laser cladding nickel-based single crystal alloy also includes: After the alloy specimen is subjected to solution heat treatment, the alloy specimen is embedded into a hot embedding material using an embedding machine to obtain a metallographic specimen; Grinding and polishing the surface of the metallographic sample; Using a corrosive liquid to corrode the surface of the metallographic sample after grinding and polishing operations; The corroded metallographic sample is obtained, and the morphological characteristics after the solution heat treatment are obtained by scanning electron microscopy.

8. The heat treatment method for laser cladding nickel-based single crystal alloy according to claim 1, characterized in that: Using the initial solution temperature and the secondary solution temperature to heat treat the laser clad alloy comprises: performing a solution heat treatment on the laser clad alloy at the initial solution temperature for a solution time corresponding to the initial solution temperature to obtain a first master alloy; The first master alloy is subjected to a solution heat treatment by increasing the temperature from the initial solution temperature to the secondary solution temperature to obtain a second master alloy; The second master alloy is subjected to aging heat treatment.

9. The heat treatment method for laser cladding nickel-based single crystal alloy according to claim 8, characterized in that: Performing aging heat treatment on the second master alloy comprises: air cooling the second master alloy; performing a first aging heat treatment on the air-cooled second master alloy, and performing air cooling after the first aging heat treatment, so as to obtain a third master alloy; Performing a second aging heat treatment on the third master alloy to obtain a target alloy; Wherein, the temperature of the first aging heat treatment is higher than the temperature of the second aging heat treatment.

10. A nickel-based single crystal alloy, characterized in that: The nickel-based single crystal alloy is obtained by processing according to any one of the heat treatment methods for laser cladding nickel-based single crystal alloys in claims 1 to 9.

Citation Information

Patent Citations

  • Ni-base single crystal superalloy solution treatment method

    CN104928604A

  • Nickel-based single crystal superalloy solid solution heat treatment method

    CN111640472A

  • Method of determining homogenization / solid solution heat treatment institution of nickel-base monocrystal high temperature alloy

    CN111763897A

  • Heat treatment method of nickel-based single-crystal superalloy

    CN113528993A

  • Solid solution heat treatment method for reducing solid solution hole content of high-rhenium nickel-based single crystal superalloy

    CN114250519A