Regulation and control method for heat treatment recrystallization of laser cladding nickel-based single crystal alloy

Through the multi-stage solid solution heat treatment of the solid solution temperature, the problem of poor material performance after the heat treatment of laser clad nickel-based single crystal alloy is solved, and the growth of the γ′ reinforced phase and the recovery of mechanical properties are achieved, and the recrystallization phenomenon is avoided. occur.

CN119082636APending Publication Date: 2024-12-06NORTHWESTERN POLYTECHNICAL UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411239854.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The material performance of laser clad nickel-based single crystal alloy after heat treatment is poor, the reinforcement phase is small, and direct solid solution heat treatment may destroy the single crystal structure, resulting in deterioration of mechanical properties.

Method used

By determining the multi-stage solid solution temperature of the laser clad nickel-based single crystal alloy, performing a graded solid solution heat treatment, gradually releasing residual stress, suppressing recrystallization, and achieving the growth of the γ′ reinforced phase.

Benefits of technology

Effectively suppress recrystallization phenomenon, restore the mechanical properties of the alloy, improve the material quality, and maintain the stability of the single crystal structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082636A_ABST
    Figure CN119082636A_ABST
Patent Text Reader

Abstract

The invention provides a regulation and control method for heat treatment recrystallization of a laser cladding nickel-based single crystal alloy, and relates to the technical field of alloys. The regulation and control method for heat treatment recrystallization of the laser-clad nickel-based single crystal alloy comprises the steps that the critical temperature at which recrystallization does not occur and the critical temperature at which recrystallization occurs during solid solution heat treatment of the laser-clad nickel-based single crystal alloy are determined to serve as the first-stage solid solution temperature; determining the temperature at which the gamma'phase is completely dissolved when the laser-clad nickel-based single crystal alloy is subjected to solid solution heat treatment as the final-stage solid solution temperature; determining multi-stage solid solution temperatures based on the first-stage solid solution temperature and the last-stage solid solution temperature; and carrying out heat treatment on the current laser cladding nickel-based single crystal alloy by utilizing the multi-stage solid solution temperature. According to the invention, the heat treatment effect after laser cladding can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of alloy technology, and in particular to a method for regulating recrystallization of a laser-clad nickel-based single crystal alloy during heat treatment. Background Art

[0002] Laser cladding, also known as directed energy deposition, is a high-energy beam additive manufacturing and surface modification technology with the advantages of controllable heat input, small heat-affected zone, small deformation of the substrate structure, and fine cladding layer. It can achieve high-quality and rapid repair of hot-end components of nickel-based single crystal alloys, for example.

[0003] However, the repaired γ′ strengthening phase of the nickel-based single crystal alloy is small and has a large difference in size from the cast γ′ phase. This is because the temperature of the molten pool rises rapidly and then cools rapidly during the laser cladding process, resulting in insufficient dissolution of the elements that form the strengthening phase, which limits the size of the strengthening phase. In addition, the extremely high cooling rate makes the dendrites in the deposition area small, which also limits the size of the strengthening phase. In order to achieve a uniform microstructure and good mechanical properties, appropriate heat treatment is required to promote the growth of the γ′ strengthening phase and thus restore the mechanical properties of the material.

[0004] The residual stress and high strain state generated during the laser cladding process will affect the instability of the single crystal alloy microstructure. If some technical solution heat treatment is directly performed, the single crystal structure may be destroyed and the mechanical properties of the alloy material will still be deteriorated.

[0005] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0006] The purpose of the present disclosure is to provide a method for regulating recrystallization of laser-clad nickel-based single crystal alloy heat treatment and a nickel-based single crystal alloy, thereby overcoming the problem of poor performance of laser-clad nickel-based single crystal alloy heat treatment materials at least to a certain extent.

[0007] According to a first aspect of the present disclosure, a method for regulating recrystallization of a laser-clad nickel-based single crystal alloy during heat treatment is provided, comprising: determining a critical temperature between when the laser-clad nickel-based single crystal alloy undergoes solution heat treatment and when recrystallization occurs as a first-stage solution temperature; determining a temperature at which the γ′ phase is completely dissolved when the laser-clad nickel-based single crystal alloy undergoes solution heat treatment as a last-stage solution temperature; determining multiple-stage solution temperatures based on the first-stage solution temperature and the last-stage solution temperature; and heat treating the current laser-clad nickel-based single crystal alloy using the multiple-stage solution temperatures.

[0008] Optionally, determining the critical temperature between no recrystallization and recrystallization during solution heat treatment of the laser-clad nickel-based single crystal alloy as the first-level solution temperature includes: performing a differential scanning calorimetry (DSC) experiment on the laser-clad nickel-based single crystal alloy to determine the temperature at which the γ′ phase of the laser-clad nickel-based single crystal alloy begins to dissolve as the first intermediate temperature; performing solution heat treatment on the laser-clad nickel-based single crystal alloy using the first intermediate temperature to obtain a first intermediate alloy; when it is determined through the morphology of the first intermediate alloy that recrystallization has occurred in the first intermediate alloy, lowering the first intermediate temperature by a first temperature to obtain a new first intermediate temperature; when it is determined through the morphology of the first intermediate alloy that recrystallization has not occurred in the first intermediate alloy, determining the first intermediate temperature as the first-level solution temperature.

[0009] Optionally, determining the temperature at which the γ′ phase is completely dissolved when the laser-clad nickel-based single crystal alloy is subjected to solution heat treatment as the last-stage solution temperature includes: performing a differential scanning calorimetry (DSC) experiment on the laser-clad nickel-based single crystal alloy to determine the temperature at which the γ′ phase of the laser-clad nickel-based single crystal alloy is completely dissolved as the second intermediate temperature; performing solution heat treatment on the laser-clad nickel-based single crystal alloy using the second intermediate temperature to obtain a second intermediate alloy; when it is determined through the morphology of the second intermediate alloy that the γ′ phase is not completely dissolved, raising the second intermediate temperature by a second temperature to obtain a new second intermediate temperature; when it is determined through the morphology of the second intermediate alloy that the γ′ phase is completely dissolved, determining the second intermediate temperature as the last-stage solution temperature.

[0010] Optionally, determining the multi-stage solution temperature based on the first-stage solution temperature and the last-stage solution temperature includes: equally dividing the solution temperature range formed by the first-stage solution temperature and the last-stage solution temperature to determine the multi-stage solution temperature.

[0011] Optionally, using a multi-stage solution temperature to heat treat the current laser-clad nickel-based single crystal alloy includes: using the multi-stage solution temperature to determine a plurality of solution heat treatment processes to be performed step by step, wherein the heating rate and / or holding time of each solution heat treatment process are consistent; performing a plurality of solution heat treatment processes on the current laser-clad nickel-based single crystal alloy.

[0012] Optionally, the control method also includes: performing surface grinding and polishing, cleaning and drying treatments on the original nickel-based single crystal alloy in sequence; obtaining spherical single crystal alloy powder as raw material for laser cladding forming; and conveying the spherical single crystal alloy powder to each layer of laser forming molten pool under a protective gas atmosphere to obtain a laser-clad nickel-based single crystal alloy.

[0013] Optionally, the spherical single crystal alloy powder is conveyed into each layer of the laser forming molten pool to obtain a laser-clad nickel-based single crystal alloy, comprising: conveying the spherical single crystal alloy powder into each layer of the laser forming molten pool to obtain a candidate alloy; performing structural detection on the candidate alloy; and determining the candidate alloy as a laser-clad nickel-based single crystal alloy when it is determined that the structural detection result of the candidate alloy is a single crystal structure and the candidate alloy has no cracks.

[0014] Optionally, heat treating the current laser-clad nickel-based single crystal alloy using a multi-stage solid solution temperature includes: heat treating the current laser-clad nickel-based single crystal alloy using a multi-stage solid solution temperature to obtain a third master alloy; and performing aging heat treatment on the third master alloy.

[0015] Optionally, performing aging heat treatment on the third intermediate alloy includes: performing a first aging heat treatment on the third intermediate alloy, and air cooling after the first aging heat treatment to obtain a fourth intermediate alloy; performing a second aging heat treatment on the fourth intermediate alloy to obtain a target nickel-based single crystal alloy; wherein the temperature of the first aging heat treatment is higher than the temperature of the second aging heat treatment.

[0016] According to a second aspect of the present disclosure, there is provided a nickel-based single crystal alloy, which is obtained by processing based on any of the above-mentioned methods for regulating recrystallization of laser cladding nickel-based single crystal alloys during heat treatment.

[0017] Through the control scheme for recrystallization of laser-clad nickel-based single crystal alloy heat treatment in the disclosed embodiment, the highest temperature at which recrystallization does not occur and the temperature at which the γ′ phase is completely dissolved are used as temperature constraints to determine a multi-stage solid solution temperature, and then the multi-stage solid solution temperature is used to perform heat treatment on the current laser-clad nickel-based single crystal alloy. The construction and application of the multi-stage solid solution temperature can achieve the effect of gradually releasing material stress, help inhibit the occurrence of recrystallization, and then achieve the recovery of the mechanical properties of the laser-clad nickel-based single crystal alloy and improve the quality of the alloy material.

[0018] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0020] Figure 1A schematic diagram showing the morphology of the γ′ strengthening phase in the repaired area of ​​the laser clad nickel-based single crystal alloy without heat treatment is shown.

[0021] Figure 2 A schematic diagram showing the comparison between the heat treatment results of some technologies and the heat treatment results of the embodiments of the present disclosure is shown.

[0022] Figure 3 The flowchart of the method for regulating recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to an exemplary embodiment of the present disclosure is schematically shown.

[0023] Figure 4 The flowchart of determining the first-stage solid solution temperature according to an embodiment of the present disclosure is schematically shown.

[0024] Figure 5 The flowchart of determining the final stage solid solution temperature according to an embodiment of the present disclosure is schematically shown.

[0025] Figure 6 A schematic diagram showing the morphology of the γ′ strengthening phase in the repaired area of ​​the laser clad nickel-based single crystal alloy after the heat treatment process according to an embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0026] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, processes, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0027] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same figure numbers in the figures represent the same or similar parts, and thus their repeated descriptions will be omitted. The flowcharts shown in the accompanying drawings are only exemplary illustrations and do not necessarily include all the steps. For example, some steps can also be decomposed, while some steps can be combined or partially combined, so the actual execution order may change according to actual conditions. In addition, all the terms "first", "second", "third", "fourth", etc. below are only for the purpose of distinction and should not be used as limitations of the present disclosure.

[0028] The γ′ strengthening phase of the nickel-based single crystal alloy after laser cladding repair is small, and its size is about one order of magnitude different from that of the cast γ′ phase. Figure 1 The figure shows the morphology of the γ′ strengthening phase in the repaired area of ​​the nickel-based single crystal alloy after laser cladding repair. Laser cladding of nickel-based single crystal alloy cannot form a uniform microstructure and good mechanical properties. In view of this, after the laser cladding process, the alloy needs to be heat treated to promote the growth of the γ′ strengthening phase and realize the recovery of the mechanical properties of the material.

[0029] However, the residual stress and high strain state generated during laser cladding will cause instability in the microstructure of single crystal alloys. If some technical solution heat treatment is directly performed, it will promote the release of residual stress and grain growth, leading to grain boundary reorganization and grain rearrangement, thus causing recrystallization. Recrystallization will destroy the single crystal structure and reduce the mechanical properties of single crystal alloys under high temperature conditions.

[0030] In order to solve or at least alleviate the recrystallization phenomenon of laser-clad nickel-based single crystal alloy during heat treatment, the embodiments of the present disclosure provide a new control scheme for heat treatment recrystallization of laser-clad nickel-based single crystal alloy.

[0031] Specifically, the scheme of the embodiment of the present disclosure can slowly increase the temperature through graded solution heat treatment to achieve step-by-step temperature control and gradually release residual stress. Thus, the occurrence of recrystallization can be effectively suppressed, and the mechanical properties of the nickel-based single crystal alloy repaired by laser cladding can be restored.

[0032] Figure 2 A schematic diagram showing the comparison of the heat treatment results of some technologies and the heat treatment results of the embodiments of the present disclosure is shown. Figure 2 After laser cladding nickel-based single crystal alloy undergoes ungraded solution heat treatment in some technologies, recrystallization easily occurs, which affects the performance of the alloy. However, the graded solution heat treatment method of the embodiment of the present disclosure can effectively inhibit the occurrence of recrystallization, which helps to improve the microstructure consistency and performance of the alloy.

[0033] The following is an explanation of the method for regulating recrystallization of a laser cladding nickel-based single crystal alloy during heat treatment according to an embodiment of the present disclosure.

[0034] Figure 3 The flowchart of the method for regulating the recrystallization of the laser cladding nickel-based single crystal alloy during heat treatment according to an exemplary embodiment of the present disclosure is schematically shown. Figure 3 The method for regulating and controlling the recrystallization of the laser cladding nickel-based single crystal alloy heat treatment according to the embodiment of the present disclosure comprises the following steps:

[0035] S32. Determine the critical temperature between when recrystallization does not occur and when recrystallization occurs during solution heat treatment of laser cladding nickel-based single crystal alloy as the first-stage solution temperature.

[0036] In an exemplary embodiment of the present disclosure, the laser-clad nickel-based single crystal alloy is a nickel-based single crystal alloy repaired by laser cladding. The process of obtaining the laser-clad nickel-based single crystal alloy is described below.

[0037] First, the original nickel-based single crystal alloy can be subjected to surface grinding and polishing, cleaning and drying in sequence. Specifically, grinding and polishing can use 600# to 800# sandpaper to make the surface of the original nickel-based single crystal alloy flat and the scratch direction consistent and uniform. After grinding and polishing, acetone and alcohol can be used to wipe the alloy surface in sequence and air-dry. It is understandable that the original nickel-based single crystal alloy can also be referred to as a nickel-based single crystal alloy substrate, a nickel-based single crystal alloy matrix, etc.

[0038] In addition, spherical single crystal alloy powder is obtained as a raw material for laser cladding forming. Specifically, the distribution of the particle size of the alloy powder can be 53 μm to 150 μm. The alloy powder can be prepared, for example, by a vacuum gas atomization (VIGA) method or a plasma rotating electrode (PREP) method, and the powder is placed in a vacuum environment at 120° C. and dried for 150 minutes to eliminate moisture that may be contained in the powder.

[0039] Taking the original nickel-based single crystal alloy as DD6 substrate and the single crystal alloy powder as DD6 powder as an example, Table 1 exemplarily shows their chemical compositions (in wt%):

[0040] Table 1

[0041]

[0042] Next, under a protective gas atmosphere, the spherical single crystal alloy powder can be transported to each layer of the laser forming molten pool to obtain a laser-clad nickel-based single crystal alloy. Specifically, the above alloy powder can be transported to each layer of the laser forming molten pool of the metal material through a powder feeding head coaxial with the laser source under argon protective gas to obtain a laser-clad nickel-based single crystal alloy. For example, the laser scans along the (100) direction of the single crystal substrate, and the deposition direction is (001). The repair of the thin-walled specimen is achieved by layer-by-layer stacking. The thin wall thickness is 1mm to 2mm, which is consistent with the thickness of the single crystal blade.

[0043] According to some embodiments of the present disclosure, the alloy after laser cladding may also be tested, and after passing the test, it may be used as the laser cladding nickel-based single crystal alloy mentioned in the embodiments of the present disclosure.

[0044] Specifically, a spherical single crystal alloy powder is transported to each layer of the laser forming molten pool to obtain a candidate alloy. On the one hand, the candidate alloy is subjected to structural detection, for example, by using X-Ray Diffraction (XRD) to detect whether there are polycrystalline features. On the other hand, the candidate alloy can be detected by human eye observation or instrument to detect whether there are cracks. When it is determined that the structural detection result of the candidate alloy is a single crystal structure and the candidate alloy has no cracks, the candidate alloy is determined to be a laser clad nickel-based single crystal alloy.

[0045] In addition, if it is determined that the structural inspection result of the candidate alloy is not a single crystal structure or the candidate alloy has cracks, the laser cladding process can be adjusted until the alloy repaired by laser cladding has a single crystal structure and no cracks.

[0046] After obtaining the laser cladding nickel-based single crystal alloy, the critical temperature between no recrystallization and recrystallization during solution heat treatment of the laser cladding nickel-based single crystal alloy can be determined as the first-level solution temperature. This critical temperature can also be called the highest temperature at which no recrystallization occurs.

[0047] Reference below Figure 4 The process of determining the first-stage solution temperature is explained.

[0048] In step S402, the temperature at which the laser-clad nickel-based single crystal alloy γ′ phase begins to dissolve is determined as the first intermediate temperature. Specifically, a differential scanning calorimetry (DSC) experiment can be performed on the laser-clad nickel-based single crystal alloy, and the temperature at which the laser-clad nickel-based single crystal alloy γ′ phase begins to dissolve is determined based on the DSC experiment results.

[0049] In step S404, the laser cladding nickel-based single crystal alloy is subjected to solution heat treatment at the first intermediate temperature to obtain a first intermediate alloy. For example, the temperature can be raised to the first intermediate temperature at a heating rate of 10°C / min to 15°C / min, kept at the temperature for 0.5h to 1h, and then air-cooled to room temperature.

[0050] In step S406, the first master alloy may be subjected to morphological detection. Specifically, a sample may be cut from the first master alloy using electric spark wire cutting, and the sample may be embedded into a hot embedding material using an embedding machine to prepare a metallographic sample. Then, the surface of the sample to be observed is polished on an automatic grinder, for example, using 600#, 800#, 1000#, 1500#, 2000# sandpaper for polishing, observing the polished surface, and stopping polishing until the scratches on the surface of the sample are small and uniform. Subsequently, the sample is polished with a flannel cloth on an automatic grinder, and polished with abrasive pastes with a particle size of 1μm and 0.5μm step by step until the surface of the sample is as smooth as a mirror. The sample is pried out of the embedding material with a hot melt gun and placed in anhydrous ethanol for cleaning. After cleaning, the sample surface is electrolytically corroded with a concentrated phosphoric acid electrochemical etching solution (H3PO4), and the corrosion time is 2s. The corroded sample is observed by a scanning electron microscope (SEM).

[0051] In step S408, it is determined whether recrystallization occurs by observing the morphology. If recrystallization occurs, step S410 is performed. If recrystallization does not occur, step S412 is performed.

[0052] In step S410, the first intermediate temperature is lowered by the first temperature to obtain a new first intermediate temperature, and the process returns to step S404. The first temperature may be preset, for example, 5°C, 10°C, 20°C, etc., which is not limited in the present disclosure.

[0053] In step S412, the first intermediate temperature is determined as the first-stage solid solution temperature.

[0054] S34. Determine the temperature at which the γ′ phase is completely dissolved during solution heat treatment of laser cladding nickel-based single crystal alloy as the final solution temperature.

[0055] After obtaining the laser-clad nickel-based single crystal alloy, the temperature at which the γ′ phase is completely dissolved during the solution heat treatment of the laser-clad nickel-based single crystal alloy can also be determined as the final solution temperature.

[0056] Reference below Figure 5 The process of determining the final solution temperature is explained.

[0057] In step S502, the temperature at which the laser clad nickel-based single crystal alloy γ′ phase completely dissolves is determined as the second intermediate temperature. Specifically, a differential scanning calorimetry (DSC) experiment can be performed on the laser clad nickel-based single crystal alloy, and the temperature at which the laser clad nickel-based single crystal alloy γ′ phase completely dissolves is determined based on the DSC experiment results.

[0058] In step S504, the laser cladding nickel-based single crystal alloy is subjected to solution heat treatment at the second intermediate temperature to obtain a second intermediate alloy. For example, the temperature can be raised to the second intermediate temperature at a heating rate of 10°C / min to 15°C / min, kept at the temperature for 0.5h to 1h, and then air-cooled to room temperature.

[0059] In step S506, the second master alloy can be subjected to morphological detection. Similarly, a sample can be cut out from the second master alloy using electric spark wire cutting, and the sample can be embedded into the hot embedding material using an embedding machine to prepare a metallographic sample. Then, the surface of the sample to be observed is polished on an automatic grinder, for example, using 600#, 800#, 1000#, 1500#, 2000# sandpaper for polishing, observing the polished surface, and stopping polishing until the scratches on the surface of the sample are small and uniform. Subsequently, the sample is polished with flannel on an automatic grinder, and polished with grinding pastes with particle sizes of 1μm and 0.5μm step by step until the surface of the sample is as smooth as a mirror. The sample is pried out of the embedding material with a hot melt gun and placed in anhydrous ethanol for cleaning. After cleaning, the surface of the sample is electrolytically corroded with concentrated phosphoric acid electrochemical etching solution (H3PO4), and the corrosion time is 2s. The corroded sample is observed by a scanning electron microscope.

[0060] In step S508, it is determined by morphological observation whether the γ′ phase is completely dissolved. If the γ′ phase is not completely dissolved, step S510 is performed. If the γ′ phase is completely dissolved, step S512 is performed.

[0061] In step S510, the second intermediate temperature is increased by a second temperature to obtain a new second intermediate temperature, and the process returns to step S504. The second temperature may be preset, for example, 5°C, 10°C, 20°C, etc., which is not limited in the present disclosure.

[0062] In step S512, the second intermediate temperature is determined as the final stage solid solution temperature.

[0063] S36. Determine the multi-stage solution temperature based on the first-stage solution temperature and the last-stage solution temperature.

[0064] According to some embodiments of the present disclosure, the solid solution temperature range consisting of the first-stage solid solution temperature and the last-stage solid solution temperature may be equally divided to determine a multi-stage solid solution temperature.

[0065] For example, the first solution temperature is recorded as T1 and the last solution temperature is recorded as T n , then you can use T1 and T n The operations are performed equally between them to obtain T1, T2, T3, ..., T n-1 , T n Multi-stage solution temperature.

[0066] In addition, each stage of solid solution temperature can be increased by 10°C compared with the previous stage, that is, T2 is 10°C higher than T1. It should be noted that the above difference of 10°C is only an exemplary description, and can also be a difference of 5°C, 15°C, 20°C, etc., which is not limited in the present disclosure.

[0067] It is understandable that the above steps S32 to S36 may be pre-configured processes for the purpose of determining the multi-stage solution temperature. When the multi-stage solution temperature is determined, the laser cladding nickel-based single crystal alloy to be heat treated may be processed.

[0068] S38. Heat treatment of current laser clad nickel-based single crystal alloy using multi-stage solution temperature.

[0069] In an exemplary embodiment of the present disclosure, a plurality of solution heat treatment processes to be performed step by step are determined using multi-stage solution temperatures, and the above-mentioned solution heat treatment processes are performed step by step on the current laser cladding nickel-based single crystal alloy.

[0070] According to some embodiments of the present disclosure, the heating rate and / or holding time of each solution heat treatment process are consistent. The above-mentioned multiple solution heat treatment processes are performed on the current laser cladding nickel-based single crystal alloy. Among them, the heating rate of each solution heat treatment process can be, for example, 3°C / min to 5°C / min, and the holding time can be, for example, 0.5h to 1h.

[0071] According to other embodiments of the present disclosure, the heating rate and / or holding time of each solution heat treatment process may also be inconsistent. For example, the heating rate of the first solution heat treatment process is 10°C / min to 15°C / min, and the heating rate of the second solution heat treatment process is 3°C / min to 5°C / min, and so on. The present disclosure does not impose any restrictions on this.

[0072] After performing multiple solution heat treatment processes based on multi-stage solution temperatures, aging heat treatment can also be performed. Specifically, the current laser cladding nickel-based single crystal alloy is heat treated using multi-stage solution temperatures to obtain a third master alloy, and the third master alloy is subjected to aging heat treatment.

[0073] Specifically, the third master alloy is subjected to a first aging heat treatment, and air-cooled after the first aging heat treatment to obtain a fourth master alloy. The fourth master alloy is then subjected to a second aging heat treatment to obtain a target nickel-based single crystal alloy. It is understood that the target nickel-based single crystal alloy is the alloy finally obtained by the heat treatment.

[0074] The temperature of the first aging heat treatment is higher than that of the second aging heat treatment. For example, the temperature of the first aging heat treatment is 1050°C to 1150°C, and the temperature of the second aging heat treatment is 850°C to 950°C. In addition, the holding time of the first aging heat treatment is 6h to 10h, and the heating rate is 10°C / min to 15°C / min; the holding time of the second aging heat treatment is 20h to 25h, and the heating rate is 10°C / min to 15°C / min.

[0075] Figure 6 The figure shows the morphology of the γ′ strengthening phase in the repaired area of ​​the laser cladding nickel-based single crystal alloy after the heat treatment process of the embodiment of the present disclosure. Figure 6 Through the heat treatment recrystallization control scheme of the embodiment of the present disclosure, it is possible to maintain a good single crystal structure without cracks while promoting the growth of the γ′ strengthening phase, which helps to restore the mechanical properties of the material.

[0076] Furthermore, the present disclosure also provides a nickel-based single crystal alloy, which is obtained by processing based on the above-mentioned laser cladding nickel-based single crystal alloy heat treatment recrystallization control method.

[0077] It should be noted that although the steps of the method in the present disclosure are described in a specific order in the drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.

[0078] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0079] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing what is disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and embodiments are to be considered merely as exemplary, and the true scope and spirit of the present disclosure are indicated by the claims.

[0080] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A method for regulating recrystallization of laser cladding nickel-based single crystal alloy heat treatment, It is characterized in that include: The critical temperature between no recrystallization and recrystallization during solution heat treatment of laser cladding nickel-based single crystal alloy is determined as the first-stage solution temperature. Determine the temperature at which the γ′ phase is completely dissolved during the solution heat treatment of the laser cladding nickel-based single crystal alloy as the last stage solution temperature; Determining a multi-stage solution temperature based on the first-stage solution temperature and the last-stage solution temperature; The multi-stage solution temperature is used to perform heat treatment on the current laser cladding nickel-based single crystal alloy.

2. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 1, It is characterized in that Determining the critical temperature between no recrystallization and recrystallization during solution heat treatment of laser cladding nickel-based single crystal alloy as the first-stage solution temperature includes: Performing a differential scanning calorimetry (DSC) experiment on the laser-clad nickel-based single crystal alloy to determine the temperature at which the γ′ phase of the laser-clad nickel-based single crystal alloy begins to dissolve as the first intermediate temperature; performing a solution heat treatment on the laser cladding nickel-based single crystal alloy using the first intermediate temperature to obtain a first intermediate alloy; When recrystallization of the first master alloy is determined through the morphology of the first master alloy, lowering the first intermediate temperature by a first temperature to obtain a new first intermediate temperature; When it is determined through the morphology of the first master alloy that the first master alloy has not been recrystallized, the first intermediate temperature is determined as a first-stage solid solution temperature.

3. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 1, It is characterized in that Determining the temperature at which the γ′ phase is completely dissolved during the solution heat treatment of the laser cladding nickel-based single crystal alloy as the last stage solution temperature includes: Performing a differential scanning calorimetry (DSC) experiment on the laser-clad nickel-based single crystal alloy to determine the temperature at which the γ′ phase of the laser-clad nickel-based single crystal alloy is completely dissolved as the second intermediate temperature; performing a solution heat treatment on the laser cladding nickel-based single crystal alloy at the second intermediate temperature to obtain a second intermediate alloy; When it is determined through the morphology of the second master alloy that the γ′ phase is not completely dissolved, raising the second intermediate temperature by a second temperature to obtain a new second intermediate temperature; When it is determined through the morphology of the second master alloy that the γ′ phase is completely dissolved, the second intermediate temperature is determined as the final solid solution temperature.

4. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 1, It is characterized in that Determining the multi-stage solution temperature based on the first-stage solution temperature and the last-stage solution temperature includes: The solid solution temperature range consisting of the first-stage solid solution temperature and the last-stage solid solution temperature is equally divided to determine a multi-stage solid solution temperature.

5. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 1, It is characterized in that The heat treatment of the current laser cladding nickel-based single crystal alloy using the multi-stage solution temperature includes: Using the multi-stage solution temperature, a plurality of solution heat treatment processes to be performed step by step are determined, and the heating rate and / or holding time of each solution heat treatment process are consistent; The plurality of solid solution heat treatment processes are performed on the current laser cladding nickel-based single crystal alloy.

6. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 1, It is characterized in that The control method further comprises: The original nickel-based single crystal alloy is subjected to surface grinding and polishing, cleaning and drying in sequence; Obtaining spherical single crystal alloy powder as raw material for laser cladding forming; Under a protective gas atmosphere, the spherical single crystal alloy powder is transported to each layer of the laser forming molten pool to obtain the laser cladding nickel-based single crystal alloy.

7. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 6, It is characterized in that The spherical single crystal alloy powder is transported into each layer of laser forming molten pool to obtain the laser cladding nickel-based single crystal alloy, comprising: delivering the spherical single crystal alloy powder into each layer of laser forming molten pool to obtain a candidate alloy; Performing structural testing on the candidate alloy; When it is determined that the structural detection result of the candidate alloy is a single crystal structure and the candidate alloy has no cracks, the candidate alloy is determined to be the laser cladding nickel-based single crystal alloy.

8. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to any one of claims 1 to 7, It is characterized in that The heat treatment of the current laser cladding nickel-based single crystal alloy using the multi-stage solution temperature includes: Using the multi-stage solution temperature to heat treat the current laser cladding nickel-based single crystal alloy to obtain a third master alloy; The third master alloy is subjected to aging heat treatment.

9. The method for controlling recrystallization of laser cladding nickel-based single crystal alloy during heat treatment according to claim 8, It is characterized in that Performing aging heat treatment on the third master alloy comprises: performing a first aging heat treatment on the third master alloy, and air cooling after the first aging heat treatment, so as to obtain a fourth master alloy; Performing a second aging heat treatment on the fourth master alloy to obtain a target nickel-based single crystal alloy; Wherein, the temperature of the first aging heat treatment is higher than the temperature of the second aging heat treatment.

10. A nickel-based single crystal alloy, It is characterized in that The nickel-based single crystal alloy is obtained by processing according to any one of claims 1 to 9 of the method for regulating and controlling heat treatment recrystallization of a laser cladding nickel-based single crystal alloy.

Citation Information

Patent Citations

  • Heat treatment method of nickel-based single-crystal superalloy

    CN113528993A

  • Solid solution heat treatment method for reducing solid solution hole content of high-rhenium nickel-based single crystal superalloy

    CN114250519A

  • Remelting heat treatment process of second-generation nickel-based single-crystal high-temperature alloy

    CN115537694A

  • Recovery heat treatment method of nickel-based single crystal superalloy

    CN115584455A

  • Continuous heating heat treatment process for second-generation nickel-based single-crystal high-temperature alloy