Preparation method and application of catalyst for preparing acetaldehyde through methane electric coupling
By preparing NiCo2O4-Vo vertical porous nanosheet catalyst, the problem of low catalyst activity in the prior art was solved, and efficient methane electric coupling to produce acetaldehyde was achieved, which improved catalytic activity and stability, simplified the process and reduced costs. .
Patent Information
- Application Number
- CN202411204361.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The catalyst activity in the existing methane electrocatalytic oxidation technology is low, resulting in low methane conversion efficiency. The complex catalyst components and electrooxidation mechanism hinder the further development of CH4 electrocatalytic conversion.
NiCo2O4-Vo vertical porous nanosheets are used as catalysts and prepared by ultrasonic dissolution, hydrothermal reaction, radio frequency plasma treatment and other methods to regulate the oxygen vacancy and active sites on the surface of the catalyst, and improve the selectivity and stability of CH4 electric coupling to make acetaldehyde sex.
The catalytic activity of methane electrocoupling to produce acetaldehyde was significantly improved, the Faraday efficiency reached 74%, and remained stable within 120 hours. The process was simple and the cost was low, which effectively inhibited the oxygen evolution reaction.
Smart Images

Figure CN119082774A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy utilization, in particular to a preparation method and application of a catalyst for preparing acetaldehyde by electric coupling of methane. Background Art
[0002] CH4, as the main component of natural gas, is one of the most abundant fossil fuels and carbon-based raw materials. With the extensive use of natural gas and shale gas, the environmental problems caused by CH4 emissions have received great attention. If CH4 can be directly converted into value-added chemicals, this will effectively utilize renewable energy to significantly reduce emissions and store energy. However, due to the fully stable symmetrical tetrahedral structure, the conversion of CH4 needs to overcome the low polarizability and high CH bond energy (439 kJ / mol), resulting in huge challenges in CH4 activation and CH bond breaking. Therefore, CH4 conversion is usually a high-energy input process accompanied by high temperature and pressure, and is considered the "holy grail" in the field of catalysis. Although various CH4 direct conversion methods have been developed to produce C1-C3 hydrocarbons or liquid fuels, including CH4 oxidation, oxidative coupling and non-oxidative coupling, their efficacy is largely limited by the specific conditions of the reaction environment.
[0003] Methane electrocatalytic oxidation (MEO) technology is attempted to solve the high temperature and high pressure problems. It is considered to be the most powerful technology to control the reaction route and final product by changing the electrode potential and electrocatalyst. For CH4 activation, a series of precious metal-based, nickel-based oxide catalysts and metal alloys have been shown to improve the selectivity of MEO products. Transition metal nickel-based catalysts have been widely studied due to their advantages of being cheap and non-toxic. For example, NiO / Ni interfacial catalysts can effectively activate CH bonds and promote the CC coupling of methanol and ethanol (Y. Song, et al. Appl Catal B-Environ 270 (2020) 118888). In addition, Ni on Fe-Ni-OH nanosheet catalysts II OOH also has excellent CH4 electrocatalytic activity as an active site (J. Li et al. Appl Catal B-Environ 316 (2022) 121657). However, the complex catalyst composition and electrooxidation mechanism will hinder the further development of CH4 electrocatalytic conversion to a certain extent. Therefore, the development of a simple and efficient electrocatalyst is the key to achieve CH4 electrooxidation. Summary of the invention
[0004] In view of the problem of low catalytic activity of the current catalyst for preparing acetaldehyde by electrocatalytic oxidation of methane, the present invention provides a method for preparing a catalyst for preparing acetaldehyde by electrocoupling of methane. The prepared catalyst is a NiCo2O4-Vo vertical porous nanosheet, which has both high selectivity and stabilizer, and significantly improves the catalytic activity of preparing acetaldehyde by electrocoupling of methane.
[0005] The preparation method of the catalyst for preparing acetaldehyde by electric coupling of methane provided by the present invention comprises the following steps:
[0006] (1) dissolving and dispersing equimolar amounts of nickel salt and cobalt salt in a mixed solvent of anhydrous ethanol and ethylene glycol by ultrasonication to obtain a reddish brown solution A; dissolving polyvinyl pyrrolidone (PVP) in deionized water to obtain a colorless transparent solution B;
[0007] (2) adding solution B dropwise to solution A and stirring for 30 min to obtain a mixed solution; transferring the mixed solution to a Teflon-lined stainless steel hydrothermal reactor, performing a constant temperature hydrothermal reaction at 150-200° C. for 8-14 h, and cooling naturally after the reaction to obtain a dark green slurry; centrifuging the dark green slurry, washing and collecting the dark green precipitate, and drying to obtain a dark green powder;
[0008] (3) calcining the dark green powder at 600°C for 6 h and cooling to obtain a black powder;
[0009] (4) The black powder was subjected to radio frequency plasma treatment at 50°C and 200W in a H2 atmosphere for 2 h to obtain the target catalyst NiCo2O4-V o .
[0010] Preferably, in step (1), anhydrous ethanol and ethylene glycol are mixed in equal volume ratios in the mixed solvent.
[0011] Preferably, the nickel salt is Ni(NO3)2·6H2O, and the cobalt salt is Co(NO3)3·6H2O. The concentrations of Ni(NO3)2·6H2O and Co(NO3)3·6H2O in the mixed solvent are both 0.12 mol / L.
[0012] It is further preferred that in step (1), the molar ratio of Ni(NO3)2·6H2O to polyvinyl pyrrolidone is 2:1.
[0013] Preferably, in step (2), the hydrothermal reaction is carried out at a constant temperature of 180° C. for 12 hours, the drying temperature is 80° C., and the drying time is 12 hours.
[0014] Compared with the prior art, the present invention is beneficial in that:
[0015] (1) Plasma bombardment of the catalyst surface modulates the concentration of oxygen vacancies on the catalyst surface, thereby regulating the d-band center of the active sites Ni and Co, strengthening the adsorption and CC coupling of the intermediate states *CH2 and *CH3 in the CH4 electrical coupling process, and improving the selectivity of methane electrical coupling to acetaldehyde.
[0016] (2) By optimizing the template, the vertically standing two-dimensional nanosheets are opened to suppress the in-plane curling and stacking problems of NiCo2O4 two-dimensional layered nanosheets.
[0017] (3) The vertical porous ultra-thin nanosheet Ni-based catalyst rich in oxygen vacancies prepared by the present invention is used for the electrocoupling of methane (CH4) to produce acetaldehyde. Specifically, it is a catalyst for converting abundant fossil fuel and carbon-based raw material methane into value-added chemicals (acetaldehyde). The catalytic activity of the catalyst is significantly improved compared with that of the pure nanosheet Ni-based catalyst. At a voltage of 1.5V vs.RHE, the Faraday efficiency reaches 74%, and can remain stable within 120h. At the same time, the oxygen evolution reaction is effectively inhibited by combining with oxygen vacancies.
[0018] (4) The present invention prepares NiCo2O4-V o Vertical porous nanosheet catalyst, in the preparation method, RF plasma is used to activate Ni-based catalyst in a green and efficient manner, the process is simple, the cost is low, and the catalytic activity for the electrocatalytic oxidation of methane to acetaldehyde is high.
[0019] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 XRD spectra of NiCo2O4 catalysts prepared under different template content conditions.
[0021] Figure 2 The XRD spectra of the catalyst of Example 1 and the catalyst of Example 7 after plasma treatment.
[0022] Figure 3 The catalyst prepared in Example 7 is NiCo2O4-V at different potentials. o Faradaic efficiency of electrocatalytic methane production.
[0023] Figure 4 This is a stability test chart of the electrocatalytic methane to acetaldehyde reaction of the catalyst prepared in Example 7. DETAILED DESCRIPTION
[0024] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0025] Example 1
[0026] A method for preparing a catalyst comprises the following steps:
[0027] 1.7448g Ni(NO3)2·6H2O and 1.7463g Co(NO3)3·6H2O were dispersed in a mixed solvent of 25mL anhydrous ethanol and 25mL ethylene glycol, and ultrasonically treated for 2h until completely dissolved and marked as solution A; 0.3964g PVP was weighed and dissolved in 50mL deionized water and marked as solution B; under strong stirring, solution B was slowly added dropwise to solution A and stirred continuously for 30min to obtain a mixed solution; the mixed solution was transferred to a Teflon-lined hydrothermal autoclave and hydrothermally reacted at 180℃ for 12h; after naturally cooling to room temperature, the precipitate was collected by centrifugal washing; then dried in an oven at 80℃ for 12h; the dried powder was calcined at 600℃ in an air atmosphere in a muffle furnace for 3h to obtain a NiCo2O4 vertical porous nanosheet catalyst.
[0028] Embodiment 2-4
[0029] The preparation method is different from that in Example 1 except for the PVP content, and the other processes are the same as those in Example 1. The PVP contents in Examples 2, 3, and 4 are 0.1982 g, 0.7928 g, and 1.5856 g, respectively.
[0030] Example 5
[0031] A method for preparing a catalyst comprises the following steps:
[0032] 1.7448g Ni(NO3)2·6H2O and 1.7463g Co(NO3)3·6H2O were weighed and dispersed in a mixed solvent of 25mL anhydrous ethanol and 25mL ethylene glycol, and ultrasonically treated for 2h until completely dissolved and marked as solution A; solution A was transferred to a Teflon-lined hydrothermal kettle and hydrothermally reacted at 180°C for 12h; after naturally cooling to room temperature, the precipitate was collected by centrifugal washing; it was then dried in an oven at 80°C for 12h; the dried powder was calcined at 600°C for 3h in an air atmosphere in a muffle furnace; the calcined product was plasma treated by radio frequency plasma treatment for 2h in a H2 atmosphere at a power of 200W and a temperature of 50°C to obtain a catalyst.
[0033] Embodiment 6-8
[0034] The NiCo2O4 vertical porous nanosheet catalyst prepared in Example 1 was treated with radio frequency plasma for different times in a H2 atmosphere at a power of 200 W and a temperature of 50°C to obtain NiCo2O4-V o Vertical porous nanosheet catalyst The plasma treatment time of Examples 6, 7, and 8 is 1 h, 2 h, and 2.5 h, respectively.
[0035] Examples 9-10
[0036] The NiCo2O4 vertical porous nanosheet catalyst prepared in Example 1 was treated with radio frequency plasma for 2 h in a H2 atmosphere at a temperature of 50°C, except that the treatment power was different, i.e., a NiCo2O4-Vo vertical porous nanosheet catalyst rich in oxygen vacancies was obtained. The plasma treatment time of Examples 9 and 10 was 150 W and 250 W, respectively.
[0037] The preparation parameter conditions of each embodiment are shown in Table 1. The performance tests of the catalyst are as follows:
[0038] (1) The catalytic performance of the catalysts prepared in the above examples was evaluated as follows:
[0039] MEO experiments were carried out in a standard three-electrode system with 0.1M NaOH solution (298K, pH=13) as electrolyte in a closed two-chamber H-type electrochemical cell (Nafion-212 membrane separation). The system consists of a glassy carbon electrode as a working electrode, a platinum electrode as a counter electrode, and a calomel electrode as a reference electrode. First, the catalyst, isopropanol, and Nafion solution (5wt%, Dupont) were mixed and ultrasonicated for 20min to obtain a slurry. Then, 5μmL of the slurry was deposited on the surface of the glassy carbon electrode (area=0.07cm2) to prepare the working electrode. When the electrochemical measurement was carried out under a CH4 atmosphere, CH4 (99.9999%) was bubbled in the electrolyte for 30 minutes to form a CH4 saturated electrolyte. The catalytic activity of the samples for MEO was evaluated by cyclic voltammetry (CV) and linear sweep voltammetry (LSV) on a CHI 660E electrochemical workstation. The stability of the catalyst was analyzed by time-varying analysis. The electrochemical impedance spectroscopy (EIS) of the catalyst was performed at 1.5 V vs. RHE, 0.1 to 10 6 Hz frequency range. RHE =E Hg / HgO+0.059×pH+0.2415, all potentials are calibrated to reversible hydrogen electrode (RHE). The activity evaluation of each catalyst is shown in Table 1. From the starting potential values of the catalysts of each embodiment in Table 1, it can be seen that the starting potentials of the catalysts after plasma treatment are all lower than those of the catalysts of Embodiments 1-4 that have not been treated with plasma, indicating that plasma treatment can reduce the starting potential of the catalyst, that is, improve the catalytic activity of the catalyst. Further, from the current density, the current density of the catalyst of Embodiment 7 is the largest, indicating that the catalytic activity of the catalyst is the best.
[0040] Table 1. Conditions and parameters for preparing catalysts in Examples 1-11 and evaluation of catalyst activity
[0041]
[0042]
[0043] (2) XRD characterization
[0044] The XRD spectra of NiCo2O4 catalysts prepared under different template content conditions are shown in Figure 2. Figure 1 As shown, the XRD patterns of all samples show four characteristic peaks at 2θ=31.2, 36.7, 44.6 and 64.9°, corresponding to the (220), (311), (400) and (440) planes of NiCo2O4 (PDF 20-0781), respectively. The XRD spectra of the catalyst of Example 1 and the plasma-treated catalyst of Example 7 are shown in FIG. Figure 2 As shown, it can be seen that after the plasma treatment, the XRD spectrum has almost no change, indicating that the plasma treatment method used in the present invention does not affect the crystal phase.
[0045] (3) Stability evaluation of catalyst NiCo2O4-Vo
[0046] The gaseous products of the electrocatalytic oxidation of methane were analyzed by a gas chromatograph (SC3000B) equipped with a TDX01 molecular sieve column, and the liquid products were analyzed and quantified by nuclear magnetic resonance (NMR) spectroscopy. When measuring the nuclear magnetic resonance spectrum, 0.1 mL of reaction electrolyte and 0.1 mL of internal standard substance solution (50% dimethyl sulfoxide in D2O) were used. According to the measurement results of the product, the Faraday efficiency (FE) was calculated by measuring the product and current value of the reaction for 6 hours at a constant potential. The Faraday efficiency of the NiCo2O4-Vo electrocatalytic methane product prepared in Example 7 at different potentials is shown in Figure 3As shown. The product Faraday efficiency and stability evaluation results of the catalysts prepared in Example 1 and Example 7 at 1.5V vs.RHE are shown in Table 2. "—" in Table 2 represents data that has not been tested. It can be seen from the test value of the starting potential in Table 1 that the starting potential of Example 7 is less than that of Example 1, indicating that the catalytic performance of Example 7 is better than that of Example 1. Therefore, there is no need to test the stability of the catalyst in Example 1. Under the condition of 1.5V vs.RHE, after the catalyst prepared in Example 7 reacted continuously for 120h, the Faraday efficiency of the acetaldehyde product was still maintained at 68.5%, which was only 7.4% lower than the Faraday efficiency of the acetaldehyde product in the initial reaction. Figure 4 shown.
[0047] Table 2. Product Faraday efficiency and stability results of the catalysts of Example 1 and Example 7 at 1.5 V vs. RHE
[0048] Example Catalyst name <![CDATA[O2]]> CO <![CDATA[CO2]]> <![CDATA[CH3OH]]> <![CDATA[CH3CH2OH]]> <![CDATA[CH3CHO]]> stability 1 <![CDATA[NiCo2O4]]> 2.8 1.4 11.4 21.7 30.2 31 — 7 <![CDATA[NiCo2O4-Vo]]> 2.1 1.6 2.3 7.7 13.2 74 120h
[0049] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a catalyst for preparing acetaldehyde by electric coupling of methane, characterized in that: The following steps are involved: (1) dissolving and dispersing equimolar amounts of nickel salt and cobalt salt in a mixed solvent of anhydrous ethanol and ethylene glycol by ultrasonic dissolution to obtain a reddish brown solution A; dissolving polyvinyl pyrrolidone in deionized water to obtain a colorless transparent solution B; (2) adding solution B dropwise to solution A and stirring for 30 min to obtain a mixed solution; transferring the mixed solution to a Teflon-lined stainless steel hydrothermal reactor, performing a constant temperature hydrothermal reaction at 150-200° C. for 8-14 h, and cooling naturally after the reaction to obtain a dark green slurry; centrifuging the dark green slurry, washing and collecting the dark green precipitate, and drying to obtain a dark green powder; (3) calcining the dark green powder at 600°C for 6 h and cooling to obtain a black powder; (4) The black powder was subjected to radio frequency plasma treatment in a H2 atmosphere at a temperature of 50°C and a power of 200 W for 2 h to obtain the target catalyst.
2. The method for preparing a catalyst for producing acetaldehyde by electric coupling of methane as claimed in claim 1, characterized in that: In step (1), anhydrous ethanol and ethylene glycol are mixed in equal volume ratio in the mixed solvent.
3. The method for preparing a catalyst for producing acetaldehyde by electric coupling of methane as claimed in claim 1, characterized in that: The nickel salt is Ni(NO3)2·6H2O, and the cobalt salt is Co(NO3)3·6H2O.
4. The method for preparing a catalyst for producing acetaldehyde by electric coupling of methane as claimed in claim 3, characterized in that: The concentrations of Ni(NO3)2·6H2O and Co(NO3)3·6H2O in the mixed solvent are both 0.12 mol / L.
5. The method for preparing a catalyst for producing acetaldehyde by electric coupling of methane as claimed in claim 3, characterized in that: In step (1), the molar ratio of Ni(NO3)2·6H2O to polyvinyl pyrrolidone is 2:
1.
6. The method for preparing a catalyst for producing acetaldehyde by electric coupling of methane as claimed in claim 1, characterized in that: In step (2), the hydrothermal reaction is carried out at a constant temperature of 180° C. for 12 h.
7. The method for preparing a catalyst for producing acetaldehyde by electric coupling of methane according to claim 1, characterized in that: In step (2), the drying temperature is 80° C. and the drying time is 12 h.
8. A catalyst for preparing acetaldehyde by electric coupling of methane, characterized in that: The method is prepared according to any one of claims 1 to 7.
9. An application of the catalyst for preparing acetaldehyde by electric coupling of methane as claimed in claim 8, characterized in that: Used as a catalyst for the electric coupling of methane to acetaldehyde.