Efficient one-way water guiding and quick-drying single-layer nanofiber membrane and preparation method thereof
The continuous gradient-grade porous single-layer nanofiber membrane was prepared through electrospinning technology, and combined with asymmetric gradient wetting, it solved the problems of cumbersome preparation of existing fabrics and insufficient moisture separation rate, and achieved efficient one-way water guidance and quick drying Performance improves the comfort of the material.
Patent Information
- Application Number
- CN202411375313.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The preparation steps for existing one-way guide wet fabrics are cumbersome, the hydrophilic side is easy to absorb and saturate, and the moisture separation rate is not enough to cope with high sweating conditions, and it is impossible to achieve efficient water guidance and quick drying performance.
A single-layer nanofiber membrane with continuous gradient gradation and porous layered porous monolayer nanofiber membrane was prepared by one-step electrospinning technology. Combined with asymmetric gradient wetting, the perfusion speed and hydrophobic modification were controlled by microcomputer to form a local gradient water conduit channel to accelerate moisture transmission.
The high-efficiency rate of moisture disengages from the surface of the fabric in the form of droplets is achieved, which is much greater than the evaporation rate and human sweat rate of ordinary Janus fabrics, significantly improving the comfort of the material.
Smart Images

Figure CN119083043A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-efficiency, one-way water-conducting, quick-drying single-layer nanofiber membrane and a preparation method thereof, belonging to the technical field of textile materials. Background Art
[0002] Existing high-comfort outdoor textiles are mainly commercial polyester fabrics Dry-FIT and Cool-max. Both use the ultra-high capillary force between shaped fibers to enhance perspiration and evaporation efficiency, which can significantly accelerate the rate of sweat extraction. However, this water transfer process is bidirectional and cannot prevent the invasion of external rain.
[0003] In recent years, textiles with unidirectional water transport properties have attracted much attention. "Advanced Functional Materials" 2021, Vol. 31, No. 14, No. 2008705 reported a four-layer composite nanofiber membrane made of different proportions of polyurethane and boron nitride nanosheets, with a graded porous structure that gradually decreases from bottom to top, and a low unidirectional water transport index of 1072%. "ACS Applied Materials & Interfaces" 2022, Vol. 14, No. 16, pp. 18944-18953 reported a three-layer composite unidirectional moisture-conducting fabric with gradient wettability, whose unidirectional transport index is 1522%. This type of fabric has an asymmetric pore size or asymmetric wettability along the thickness direction, which can make liquid spontaneously transfer from the hydrophobic side to the hydrophilic side or penetrate the fabric in a directional manner along the direction of decreasing pore size, and prevent water transmission in the opposite direction. This type of textile that allows liquid to flow in one direction plays a key role in maintaining human physiological and psychological comfort because it can effectively manage skin dryness and microclimate temperature and humidity. However, its characteristics are cumbersome preparation steps, easy saturation of the hydrophilic side, low rate of water detachment from the fabric surface, and the accumulated water makes the human body feel stuffy and uncomfortable, and even causes stress response. Summary of the invention
[0004] [Technical issues]
[0005] Among the existing unidirectional moisture-conducting fabrics, most are multi-layer composite fabrics. The preparation steps of such fabrics are cumbersome and easy to peel off. In high sweating or high humidity environments, the hydrophilic side of the fabric is easily saturated with moisture. The rate at which moisture leaves the fabric surface in the form of water vapor is much lower than the sweating rate of the human body under strenuous exercise (1.5 L h -1 ), which cannot meet the human body's demand for textile fabrics with both high water conductivity and quick-drying properties.
[0006] To this end, the present invention innovatively uses a one-step electrospinning technology to prepare a single-layer nanofiber membrane with continuous gradient graded porosity, and combines it with asymmetric gradient wettability. The two work together to achieve efficient unidirectional water conduction and quick-drying performance of the material. The single-layer nanofiber membrane is different from ordinary unidirectional moisture-conducting fabrics. The nanofiber membrane can make water gather in the form of droplets on one side of the membrane and then detach from the fabric surface. The water detachment rate is much higher than the evaporation rate of water on the surface of ordinary Janus fabrics after spreading (0.735gh -1 ), and at the same time, it is much greater than the maximum sweating rate of the human body under high temperature, high humidity and high-intensity exercise scenes (1.5×10 3 g / (m 2 h)) greatly improves the overall comfort of the human microenvironment.
[0007] [Technical solution]
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] The present invention provides a highly efficient one-way water-conducting, quick-drying single-layer nanofiber membrane and a preparation method thereof. The perfusion speed of the nanofiber membrane in the spinning process is controlled in real time by a microcomputer, so that it increases linearly within a set range, so that the prepared single-layer nanofiber membrane has a continuous gradient graded porous structure. The graded porous structure enables the nanofiber membrane to have a gradually enhanced differential capillary effect. Under the action of the capillary driving force, the liquid tends to transport water in the direction of smaller pore size and hinders its reverse transport. Subsequently, the continuously gradient graded porous nanofiber membrane is hydrophobically modified, and a patterned template is used to locally hydrophilically modify it, so that it locally has a gradually wettable water-conducting channel along the thickness direction. Due to the synergistic effect of the pore size difference and the wettability difference in the channel, the transmission efficiency of water in the water-conducting channel can be accelerated, and the water is gathered into droplets on the surface of the membrane, which can drip with the body swinging. The detachment rate of the droplets from the fabric surface is much greater than the water evaporation rate of ordinary Janus fabrics.
[0010] The specific technical solutions are as follows:
[0011] The present invention provides a method for preparing a single-layer nanofiber membrane with high efficiency, unidirectional water conduction and quick drying, the method comprising the following steps:
[0012] (1) Prepare a polymer spinning solution and use electrospinning technology to prepare a single-layer nanofiber membrane with continuous gradient porosity: electrospinning parameters: voltage of 10 to 35 kV, perfusion speed of 0 ml h -1 Increases linearly to 1-5 ml h -1 The perfusion rate increment is 0.1 to 10 μL s -1, receiving distance is 10-30cm, spinning environment temperature is 25-50℃; humidity is 20-70%;
[0013] (2) placing the single-layer nanofiber membrane with continuous gradient graded porosity obtained in step (1) in a hydrophobic modifier for local hydrophobic modification;
[0014] (3) Taking the patterned hollow template, placing it on one side of the single-layer nanofiber membrane after the hydrophobic modification in step (2), and performing hydrophilic modification, thereby obtaining a single-layer nanofiber membrane with high efficiency, unidirectional water conduction and quick drying.
[0015] In one embodiment, the concentration of the polymer spinning solution in step (1) is 5 to 20 wt%.
[0016] In one embodiment, the polymer used in the polymer spinning solution in step (1) is one or more of polymers such as polycaprolactone, polypropylene, polyacrylonitrile, polyvinyl alcohol, polyethylene glycol, sodium polyacrylate, etc.
[0017] In one embodiment, the solvent used in the polymer spinning solution in step (1) is one or more of water, toluene, xylene, acetone, cyclohexanone, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide and the like.
[0018] In one embodiment, the electrospinning parameters of step (1) are: voltage of 10 to 35 kV, perfusion speed of 0 ml h -1 Increases linearly to 1-3 ml h -1 The perfusion rate increment is 0.1 to 5 μL s -1 , the receiving distance is 10-30cm, the spinning environment temperature is 25-50℃; the humidity is 20-70%.
[0019] In one embodiment, the electrospinning parameters of step (1) are: voltage of 10 to 35 kV, perfusion speed of 0 ml h -1 Increased linearly to 2 ml h -1 The perfusion rate increment is 1 to 1.5 μL s -1 , the receiving distance is 10-30cm, the spinning environment temperature is 25-50℃; the humidity is 20-70%.
[0020] In one embodiment, the electrospinning parameters of step (1) are: voltage of 10 to 35 kV, perfusion speed of 0 ml h -1 Increased linearly to 4 ml h -1 The perfusion rate increment is 1 to 1.5 μL s -1 , the receiving distance is 10-30cm, the spinning environment temperature is 25-50℃; the humidity is 20-70%.
[0021] In one embodiment, the electrospinning parameters of step (1) are: voltage of 15 kV, perfusion speed of 0 ml / h -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1.2 μL s -1 , the receiving distance is 15 cm, the spinning environment temperature is 30°C, and the humidity is 50%.
[0022] In one embodiment, the pore size of the single-layer nanofiber membrane with continuous gradient graded porosity in step (1) ranges from 50 nm to 50 μm.
[0023] In one embodiment, the hydrophobic modifier in step (2) is any one of polyurethane, silane coupling agent or commercial hydrophobic modifier.
[0024] In one embodiment, the polyurethanes include one or more of silicone-modified polyurethanes, fluorinated polyurethanes, and nanomaterial-modified polyurethanes.
[0025] In one embodiment, the silane coupling agent includes one or more of vinyl silane, amino silane, epoxy silane, mercapto silane and methacryloxy silane.
[0026] In one embodiment, the hydrophobic modification in step (2) is specifically to place the continuously gradient graded porous nanofiber membrane in a hydrophobic modifier for immersion and rolling, and then dry it for use.
[0027] In one embodiment, the patterned hollow template in step (3) has a hollow aperture of 0.5 to 5 mm, and a hollow dot matrix spacing of 5 to 20 mm.
[0028] In one embodiment, the patterned hollow template in step (3) has a hollow aperture of 1 to 3 mm, and a hollow dot matrix spacing of 7 to 9 mm.
[0029] In one embodiment, the patterned hollow cellulose paper template in step (3) is any one of punchable cellulose paper, tape, tin foil, and plastic board.
[0030] In one embodiment, the local hydrophilic modification in step (3) is carried out by plasma treatment or light-induced polymerization.
[0031] In one embodiment, the plasma treatment is to place the sample to be treated in a plasma treatment machine, set the cleaning time to 10-600s, the air flow rate to 100-200ml / min, and the power to 40-300W.
[0032] In one embodiment, the light-induced polymerization method is to immerse the sample to be treated in a mixture of a hydrophilic modifier and a photoinitiator, wherein the concentration of the hydrophilic modifier is 5 to 50 wt %, and the mass ratio of the hydrophilic modifier to the photoinitiator is 10:1 to 1:1, and then place it under a light source with a wavelength corresponding to the photoinitiator, the wavelength of the light source is 250 to 420 nm, and the illumination time is 30 to 300 s. After the illumination is completed, it is cleaned and dried.
[0033] In one embodiment, the hydrophilic modifier is an oligomer, and the concentration of the oligomer is 10 to 60 wt %, wherein the oligomer is one or more of hydroxyethyl methacrylate, polyethylene glycol diacrylate, and acrylates.
[0034] In one embodiment, the photoinitiator is one or more of 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, 4,4-dimethylphenyldi(4-methylphenyl)carbonyl ammonium bromide, distyrylbenzidine, and benzophenone.
[0035] The present invention also provides a high-efficiency, one-way water-conducting, quick-drying single-layer nanofiber membrane prepared by the above-mentioned method.
[0036] In one embodiment, the water contact angle of the exposed part of the efficient unidirectional water-conducting, quick-drying single-layer nanofiber membrane is 0-40°, the water contact angle of the covered part is 100-130°, the water contact angle of the bottom of the exposed part is 110-140°, and the water contact angle of the bottom of the covered part is 130-150°.
[0037] In one embodiment, the one-way water conduction rate of the high-efficiency one-way water conduction and quick-drying single-layer nanofiber membrane is (1.5-2.5)×10 5 g / (m 2 ·h); the maximum one-way water conduction rate is 2.5×10 5 g / (m 2 h).
[0038] The present invention also provides the application of the above-mentioned high-efficiency, one-way water-conducting, quick-drying single-layer nanofiber membrane in functional clothing, medical health, filtration separation, and flow control.
[0039] Beneficial effects:
[0040] (1) The present invention adopts microcomputer control so that the perfusion speed of the nanofiber membrane during the spinning process increases linearly within a set range, so that the prepared single-layer nanofiber membrane has a continuously gradient graded porous structure. The graded porous structure enables the nanofiber membrane to have a gradually enhanced differential capillary effect. Under the action of the capillary driving force, the liquid tends to transport water in the direction of smaller pore size and hinders its reverse transport.
[0041] (2) The present invention combines asymmetric gradual wettability with pore asymmetry. The two work together to accelerate the unidirectional water conduction rate, greatly improving the transmission efficiency of tiny droplets. (The water contact angle of the exposed part of the single-layer nanofiber membrane is 0-40°, the water contact angle of the covered part is 100-130°, the water contact angle of the exposed bottom is 110-140°, and the water contact angle of the covered bottom is 130-150°; the unidirectional water conduction rate of the membrane is 1.5-2.5×10 5 g / (m 2 h));
[0042] (3) The highly efficient one-way water-conducting and quick-drying single-layer nanofiber membrane prepared by the present invention can continuously conduct water in the water-conducting channel to the surface of the nanofiber membrane and then gather into droplets. When wearing, the water can slide down with the swing of the arm. The water is separated from the surface of the fabric in the form of water droplets, and the water separation rate is (1.5-2.5)×10 5 g / (m 2 ·h), which is much greater than the rate at which moisture on the surface of ordinary Janus fabric escapes in the form of steam (0.735gh -1 ). BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a schematic diagram of the structure of the high-efficiency unidirectional moisture-conducting nanofiber membrane of the present invention;
[0044] Figure 2 This is a schematic SEM diagram of the bottom layer of the single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying in Example 1;
[0045] Figure 3 This is a top SEM schematic diagram of the highly efficient, unidirectional water-conducting, quick-drying single-layer nanofiber membrane in Example 1. DETAILED DESCRIPTION
[0046] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention. The following specific implementation methods further describe the present invention.
[0047] The test method involved in the present invention is:
[0048] 1. Water contact angle, water rolling angle
[0049] The wettability of the samples was characterized using a water feeler.
[0050] 2. Moisture transfer rate
[0051] The propulsion speed is set by the propeller to test the maximum water transmission rate of the fabric to be tested.
[0052] The raw material sources involved in the present invention are:
[0053] Commercial silane coupling agent, brand is DASU NANO / Dashu, model is S500, manufacturer is Shanghai Huaxia Jiahe New Material Technology Co., Ltd.
[0054] Example 1
[0055] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0056] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The solution was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was controlled by a microcomputer in real time, and the perfusion speed was set from 0 ml h to 100 ml h. -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1 μL s per second. -1 , the receiving distance is 15 cm; the spinning environment temperature is controlled to be 30°C and the humidity is 50%; a graded porous PAN single-layer nanofiber membrane is obtained; the water contact angle of the fiber membrane is 60°;
[0057] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with a commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0058] (3) A cellulose paper template with a patterned template hollow aperture of 1 mm and a hollow dot matrix spacing of 9 mm was placed on one side of the hydrophobically modified graded porous PAN nanofiber membrane, and a plasma treatment machine was used to perform unilateral hydrophilic modification on one side of the patterned template. The cleaning time was set to 90 s, the air flow rate was 170 ml / min, and the power was 100 W; a single-layer nanofiber membrane with high efficiency, unidirectional water conduction, and quick drying was obtained.
[0059] Example 2
[0060] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0061] (1) Polypropylene (PP) powder was placed in a vacuum oven at 60°C and dried for 12 h. An appropriate amount of PP powder was then weighed and dissolved in a toluene solution. The solution was heated and stirred in an oil bath at 110°C for 6 h to prepare a uniform electrospinning solution with a concentration of 12 wt%. The electrospinning parameters were as follows: voltage was 25 kV; microcomputer controlled the perfusion speed in real time, and the perfusion speed was set from 0 ml / h to 10 ml / h. -1 Increased linearly to 4 ml h -1 ; The perfusion rate increment was 1.5 μL s -1 ; The receiving distance is 20 cm; The spinning environment temperature is controlled to be 40°C; The humidity is 60%; A graded porous PP single-layer nanofiber membrane is obtained, and the water contact angle of the fiber membrane is 80°;
[0062] (2) using commercial silane coupling agent M190 to repeatedly roll the hierarchical porous PP nanofiber membrane for 3 times at a rolling pressure of 1 MPa, and then transferring it to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PP nanofiber membrane;
[0063] (3) Polyethylene glycol diacrylate was used as a hydrophilic modifier and mixed with 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone in a ratio of 10:1 to prepare a mixed aqueous solution with a concentration of 20 wt%. The hydrophobically modified graded porous PP nanofiber membrane was immersed in the mixed solution. After being taken out, one side of the membrane was covered with a patterned hollow tin foil template with a pore size of 1.5 mm and a hollow lattice spacing of 7 mm. The membrane was polymerized under ultraviolet light with a wavelength of 365 nm for 120 s. The membrane was washed three times and dried in an oven at 60°C to obtain a single-layer nanofiber membrane with high efficiency, unidirectional water conduction and quick drying.
[0064] Example 3
[0065] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0066] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The solution was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was controlled by a microcomputer in real time, and the perfusion speed was set from 0 ml h to 100 ml h. -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1 μL s per second. -1 , the receiving distance is 15 cm; the spinning environment temperature is controlled to be 30°C and the humidity is 50%; a graded porous PAN single-layer nanofiber membrane is obtained; the water contact angle of the fiber membrane is 60°;
[0067] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with a commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0068] (3) A cellulose paper template with a patterned template hollow aperture of 2 mm and a hollow dot matrix spacing of 8 mm was placed on one side of the hydrophobically modified graded porous PAN nanofiber membrane, and a plasma treatment machine was used to perform unilateral hydrophilic modification on one side of the patterned template. The cleaning time was set to 90 s, the air flow rate was 170 ml / min, and the power was 100 W; a single-layer nanofiber membrane with high efficiency, unidirectional water conduction, and quick drying was obtained.
[0069] Example 4
[0070] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0071] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The solution was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was controlled by a microcomputer in real time, and the perfusion speed was set from 0 ml h to 100 ml h. -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1 μL s per second. -1 , receiving distance is 15cm; the spinning environment temperature is controlled to be 30℃ and the humidity is 50%; graded porous PAN single-layer nanofiber membrane; the water contact angle of the fiber membrane is 60°;
[0072] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with a commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0073] (3) A cellulose paper template with a patterned template hollow aperture of 3 mm and a hollow dot matrix spacing of 7 mm was placed on one side of the hydrophobically modified graded porous PAN nanofiber membrane, and a plasma treatment machine was used to perform unilateral hydrophilic modification on one side of the patterned template. The cleaning time was set to 90 s, the air flow rate was 170 ml / min, and the power was 100 W; a single-layer nanofiber membrane with high efficiency, unidirectional water conduction, and quick drying was obtained.
[0074] Example 5
[0075] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0076] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The solution was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was controlled by a microcomputer in real time, and the perfusion speed was set from 0 ml h to 100 ml h. -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1.2 μL s -1 , receiving distance is 15cm; the spinning environment temperature is controlled to be 30℃ and the humidity is 50%; graded porous PAN single-layer nanofiber membrane; the water contact angle of the fiber membrane is 60°;
[0077] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with a commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0078] (3) A cellulose paper template with a patterned template hollow aperture of 1 mm and a hollow dot matrix spacing of 9 mm was placed on one side of the hydrophobically modified graded porous PAN nanofiber membrane, and a plasma treatment machine was used to perform unilateral hydrophilic modification on one side of the patterned template. The cleaning time was set to 90 s, the air flow rate was 170 ml / min, and the power was 100 W; a single-layer nanofiber membrane with high efficiency, unidirectional water conduction, and quick drying was obtained.
[0079] Example 6
[0080] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0081] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The solution was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was controlled by a microcomputer in real time, and the perfusion speed was set from 0 ml h to 100 ml h. -1 Increased linearly to 3 ml h -1 The perfusion rate increment was 1 μL s per second. -1 , receiving distance is 15cm; the spinning environment temperature is controlled to be 30℃ and the humidity is 50%; graded porous PAN single-layer nanofiber membrane; the water contact angle of the fiber membrane is 60°;
[0082] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with a commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0083] (3) A cellulose paper template with a patterned template hollow aperture of 1 mm and a hollow dot matrix spacing of 9 mm was placed on one side of the hydrophobically modified graded porous PAN nanofiber membrane, and a plasma treatment machine was used to perform unilateral hydrophilic modification on one side of the patterned template. The cleaning time was set to 90 s, the air flow rate was 170 ml / min, and the power was 100 W; a single-layer nanofiber membrane with high efficiency, unidirectional water conduction, and quick drying was obtained.
[0084] Comparative Example 1
[0085] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0086] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The mixture was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was manually set to 0.5 ml h in multiple times. -1 1ml h -1 , 2ml h -1 , so that it changes from 0.5ml h -1 Increase to 2 ml h in three stages -1 , keep the total spinning time the same, the receiving distance is 15cm; control the spinning environment temperature to 30℃, the humidity to 50%; obtain the graded porous PAN single-layer nanofiber membrane; the water contact angle of the fiber membrane is 60°;
[0087] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0088] (3) A cellulose paper template with a patterned template hollow aperture of 1 mm and a hollow dot matrix spacing of 9 mm was placed on one side of the hydrophobically modified graded porous PAN nanofiber membrane, and a plasma treatment machine was used to perform unilateral hydrophilic modification on one side of the patterned template. The cleaning time was set to 90 s, the air flow rate was 170 ml / min, and the power was 100 W; a single-layer nanofiber membrane with high efficiency, unidirectional water conduction, and quick drying was obtained.
[0089] Comparative Example 2
[0090] A method for preparing a single-layer nanofiber membrane with high efficiency, one-way water conduction and quick drying, specifically comprising the following steps:
[0091] (1) Polyacrylonitrile (PAN) powder was placed in a vacuum oven at 60°C and dried for 20 h. Then, an appropriate amount of PAN powder was weighed and dissolved in N,N-dimethylformamide. The mixture was heated and stirred in a water bath at 60°C for 12 h to prepare a uniform electrospinning solution with a concentration of 14 wt%. The electrospinning parameters were as follows: the voltage was 15 kV; the perfusion speed was set from 0 ml h -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1 μL s per second. -1 , receiving distance is 15cm; the spinning environment temperature is controlled to be 30℃ and the humidity is 50%; graded porous PAN single-layer nanofiber membrane; the water contact angle of the fiber membrane is 60°;
[0092] (2) The hierarchical porous PAN nanofiber membrane was repeatedly impregnated 3 times with a commercial silane coupling agent S500 at a pressure of 1 MPa, and then transferred to a 60°C oven for 4 hours to obtain a hydrophobically modified hierarchical porous PAN nanofiber membrane;
[0093] (3) A plasma treatment machine is used to directly perform unilateral hydrophilic modification on one side without a template, and the cleaning time is set to 90 s, the air flow rate is 170 ml / min, and the power is 100 W; a single-layer nanofiber membrane with unidirectional water conduction and quick-drying functions is obtained.
[0094] Results Analysis
[0095] The single-layer nanofiber membranes prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested for performance indicators, and the results are shown in Table 1:
[0096] Table 1 Test indexes of water conduction performance of nanofiber membranes in the embodiments and control examples
[0097]
[0098] Note: The exposed part refers to the hollow exposed part after the patterned hollow template covers the top layer of the fabric when the fabric is hydrophilically modified; the covered part refers to the part of the fabric covered by the patterned hollow template; the bottom of the exposed part refers to the bottom side of the fabric corresponding to the hollow exposed part of the patterned hollow template; the bottom of the covered part refers to the bottom side of the fabric corresponding to the part of the fabric covered by the patterned hollow template.
[0099] From the data in Table 1, it can be seen that the single-layer nanofiber membrane obtained by the technical solution of the present invention has a large water conductivity. For example, in Examples 1 to 6, the water conductivity reaches 1.5 to 2.5×10 5g / (m 2 ·h); compared with comparative examples 1 and 2, the maximum water conductivity rate is increased by an order of magnitude; and it can be seen from Examples 1, 3 and 4 that the change in the patterned template parameters also has an impact on the maximum water conductivity rate of the single-layer fiber membrane. In Examples 3 and 4, the diameter of the hollow points becomes larger, so the hydrophilic points become larger, and after the water-conducting channels are formed, the water droplets converge at the top and are easy to reverse osmosis, and the maximum water conductivity rate decreases; the large hydrophilic points have greater adhesion to water, and the rolling angle becomes larger.
[0100] Compared with Example 1, the perfusion speed range of Example 5 remains unchanged, but the increment of the perfusion rate per second is increased from 1 μL s -1 Increase to 1.2 μL s -1 , the faster the change speed becomes, the thinner the fiber membrane thickness becomes, the water conduction path becomes shorter, and the maximum water conduction rate increases; since the injection speed range does not change, the pore size difference between the surface and bottom layers is not much.
[0101] Compared with Example 1, the perfusion rate increment per second in Example 6 is unchanged, but the perfusion interval is increased from 0 to 2 ml h -1 Changes to 0~3ml h -1 , the interval becomes larger, the fiber membrane thickness becomes thicker, the water conduction path becomes longer, and the maximum water conduction rate decreases; due to the change in the perfusion speed interval, the maximum pore size of the surface layer increases.
[0102] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A method for preparing a single-layer nanofiber membrane with high efficiency, unidirectional water conduction and quick drying, characterized in that: The method comprises the following: (1) Prepare a polymer spinning solution and use electrospinning technology to prepare a single-layer nanofiber membrane with continuous gradient porosity: electrospinning parameters: voltage of 10 to 35 kV, perfusion speed of 0 ml h -1 Increases linearly to 1-5 ml h -1 The perfusion rate increment is 0.1 to 10 μL s -1 , receiving distance is 10-30cm, spinning environment temperature is 25-50℃; humidity is 20-70%; (2) placing the single-layer nanofiber membrane with continuous gradient graded porosity obtained in step (1) in a hydrophobic modifier for local hydrophobic modification; (3) Taking the patterned hollow template, placing it on one side of the single-layer nanofiber membrane after the hydrophobic modification in step (2), and performing hydrophilic modification, thereby obtaining a single-layer nanofiber membrane with high efficiency, unidirectional water conduction and quick drying.
2. The preparation method according to claim 1, characterized in that: The concentration of the polymer spinning solution in step (1) is 5 to 20 wt%.
3. The preparation method according to claim 1, characterized in that: The polymer used in the polymer spinning solution in step (1) is one or more of polymers such as polycaprolactone, polypropylene, polyacrylonitrile, polyvinyl alcohol, polyethylene glycol, sodium polyacrylate, etc.
4. The preparation method according to claim 1, characterized in that: The solvent used in the polymer spinning solution in step (1) is one or more of water, toluene, xylene, acetone, cyclohexanone, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide and the like.
5. The preparation method according to claim 1, characterized in that: The electrospinning parameters of step (1) are: voltage of 10-35 kV, perfusion speed of 0 ml h -1 Increases linearly to 1-3 ml h -1 The perfusion rate increment is 0.1 to 5 μLs per second. -1 , the receiving distance is 10-30cm, the spinning environment temperature is 25-50℃; the humidity is 20-70%.
6. The preparation method according to claim 1, characterized in that: The electrospinning parameters of step (1) are: voltage of 10-35 kV, perfusion speed of 0 ml h -1 Increased linearly to 2 ml h -1 The perfusion rate increment is 1 to 1.5 μL s -1 , the receiving distance is 10-30cm, the spinning environment temperature is 25-50℃; the humidity is 20-70%.
7. The preparation method according to claim 1, characterized in that: The electrospinning parameters of step (1) are: voltage of 10-35 kV, perfusion speed of 0 ml h -1 Increased linearly to 4 ml h -1 The perfusion rate increment is 1 to 1.5 μL s -1 , the receiving distance is 10-30cm, the spinning environment temperature is 25-50℃; the humidity is 20-70%.
8. The preparation method according to claim 1, characterized in that: The electrospinning parameters of step (1) are: voltage of 15 kV, perfusion speed of 0 ml h -1 Increased linearly to 2 ml h -1 The perfusion rate increment was 1.2 μL s -1 , the receiving distance is 15 cm, the spinning environment temperature is 30°C, and the humidity is 50%.
9. The preparation method according to claim 1, characterized in that: The hydrophobic modifier in step (2) is any one of polyurethane, silane coupling agent or commercial hydrophobic modifier.
10. The preparation method according to claim 1, characterized in that: The patterned hollow template in step (3) has a hollow aperture of 0.5 to 5 mm, and a hollow dot matrix spacing of 5 to 20 mm.
11. The preparation method according to claim 1, characterized in that: The patterned hollow template in step (3) has a hollow aperture of 1 to 3 mm, and a hollow dot matrix spacing of 7 to 9 mm.
12. The preparation method according to claim 1, characterized in that: The patterned hollow cellulose paper template in step (3) is any one of punchable cellulose paper, tape, tin foil, and plastic board.
13. The preparation method according to claim 1, characterized in that: The local hydrophilic modification method in step (3) is any one of plasma treatment and light-induced polymerization.
14. The preparation method according to claim 13, characterized in that: The plasma treatment is to place the sample to be treated in a plasma treatment machine, set the cleaning time to 10-600s, the air flow rate to 100-200ml / min, and the power to 40-300W.
15. The preparation method according to claim 13, characterized in that: The light-induced polymerization method is to immerse the sample to be treated in a mixed solution of a hydrophilic modifier and a photoinitiator, wherein the concentration of the hydrophilic modifier is 5 to 50 wt %, and the mass ratio of the hydrophilic modifier to the photoinitiator is 10:1 to 1:1, and then place it under a light source with a wavelength corresponding to the photoinitiator, wherein the wavelength of the light source is 250 to 420 nm, and the illumination time is 30 to 300 s. After the illumination is completed, it is cleaned and dried.
16. The preparation method according to claim 15, characterized in that: The hydrophilic modifier is an oligomer, and the concentration of the oligomer is 10-60 wt %, wherein the oligomer is one or more of hydroxyethyl methacrylate, polyethylene glycol diacrylate, and acrylates.
17. The preparation method according to claim 15, characterized in that: The photoinitiator is one or more of 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, 4,4-dimethylphenyl di(4-methylphenyl)carbonyl ammonium bromide, distyryl benzidine, and benzophenone.
18. A high-efficiency, one-way, water-conducting, quick-drying single-layer nanofiber membrane prepared by the method according to any one of claims 1 to 17.
19. The high-efficiency one-way water-conducting, quick-drying single-layer nanofiber membrane according to claim 18, characterized in that: The one-way water conduction rate of the high-efficiency one-way water conduction and quick-drying single-layer nanofiber membrane is (1.5-2.5)×10 5 g / (m 2 h).
20. Application of the highly efficient, one-way water-conducting, quick-drying single-layer nanofiber membrane according to any one of claims 18 or 19 in functional clothing, medical health, filtration separation, and flow control.
Citation Information
Patent Citations
Preparation method of constant-hydrophilic graft-modified chlorinated polymer micro / nano fiber film
CN103924384A
Method for realizing liquid drop directional transportation on super-hydrophobic substrate
CN105566666A
High-tensile strain piezoelectric sensor and preparation method thereof
CN105928452A
One-way moisture-conducting micronano fiber membrane with multistage communicating hole structure and preparation method thereof
CN111111458A
Submillimeter-micrometer-nanometer cross-scale three-dimensional patterned super-wetting surface electrochemical processing method
CN111593382A
Cited By
Body surface sweat in-situ detection sensor based on composite nanofibers and preparation method
CN119498836A