High-substitution-degree CMC (Carboxy Methylated Cellulose) pretreatment slurry for digital printing of silk

Through the combination of high-substituted carboxymethylcellulose with non-ionic penetrant and tragacanth, combined with intermittent microwave etherification process, the prepared CMC pretreated slurry solved the printing point caused by sodium alginate slurry. The problem of thickening and poor pattern clarity has achieved efficient silk digital printing effect and improved product quality.

CN119083207APending Publication Date: 2024-12-06SHANGHAI QINGMU TEXTILE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411266979.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing sodium alginate pretreatment slurry in silk digital printing causes the printing points to become thicker, the pattern clarity is poor, and the color is low, which affects the product quality.

Method used

High-substituted carboxymethylcellulose is combined with non-ionic penetrant A-113 and tragacanth gum, and combined with the CMC pretreatment slurry prepared by intermittent microwave etherification process, and sodium bicarbonate, urea and sodium sulfate are added. , forming an efficient pretreatment slurry.

Benefits of technology

It improves the pattern clarity, color yield and friction resistance of the fabric after printing, replaces traditional sodium alginate slurry, enhances printing accuracy and softness, and meets higher consumer needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a high-substitution-degree CMC (Carboxymethyl Cellulose) pretreatment sizing agent for silk digital printing, the total mass of the pretreatment sizing agent is 100%, the pretreatment sizing agent comprises the following components in percentage content: 3-6% of carboxymethyl cellulose with the substitution degree of 1.2-2, 3-5% of a thickening agent, 1-2.5% of sodium bicarbonate, 6-8% of an auxiliary agent MIROPRINT MSU-01 and / or urea, 2-4% of sodium sulfate and the balance of water. When the pretreatment slurry is applied to silk digital printing, a silk fabric with high pattern definition, high color yield, good friction resistance and high hand feeling softness can be obtained, and the pretreatment slurry can be used as an effective substitute of the traditional sodium alginate digital printing pretreatment slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of digital printing, and more specifically to a high-substitution CMC pre-treatment slurry for silk digital printing. Background Art

[0002] In recent years, digital printing technology has been widely used in silk printed fabrics, especially silk scarves and other products, which are colorful and have a wide variety of patterns and colors, and are increasingly popular among consumers. Sizing is an indispensable pre-treatment process in the production of digital printing of silk fabrics. The existing pre-treatment slurries for digital printing of silk fabrics mainly include additives such as pastes, alkali agents, urea, and sodium sulfate. Among them, sodium alginate pre-treatment slurries are the most commonly used slurries. However, when it is applied to digital printing of silk fabrics, it will produce problems such as coarsening of the printing dots, poor pattern clarity, and low color yield after evaporation, which affects the product quality. Therefore, it is necessary to develop a new pre-treatment slurry that can replace sodium alginate pre-treatment slurries. Summary of the invention

[0003] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art and provide a high-substitution CMC pre-treatment slurry for silk digital printing.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A high-substitution CMC pretreatment slurry for silk digital printing comprises the following components in percentage based on 100% of the total mass of the pretreatment slurry: 3-6% of carboxymethyl cellulose with a substitution degree of 1.2-2, 3-5% of a thickener, 1-2.5% of sodium bicarbonate, 6-8% of an auxiliary agent MIROPRINT MSU-01 and / or urea, 2-4% of sodium sulfate, and the balance is water.

[0006] Furthermore, the thickener is a mixture of nonionic penetrant A-113 and tragacanth gum.

[0007] Furthermore, the mass ratio of the nonionic permeabilizing agent A-113 to tragacanth gum is 1:0.5-1.

[0008] Further, bagasse cellulose, sodium hydroxide and 95% ethanol-water solution are mixed and stirred at 35-40° C. for alkalization, and then sodium chloroacetate is added and etherification is carried out under intermittent microwave radiation. After the etherification is completed, the product is filtered and separated, and sodium hydroxide, sodium chloroacetate and 90% ethanol-water solution are added to the product again, mixed and etherification is carried out again under intermittent microwave radiation. After the reaction is completed, the product is separated by suction, washed and dried to obtain carboxymethyl cellulose with a degree of substitution of 1.2-2.

[0009] Furthermore, during the first etherification reaction, the mass ratio of bagasse cellulose, sodium hydroxide, 95% ethanol-water solution, and sodium chloroacetate is 1:(1.4-2.1):(3.5-5):(1-2).

[0010] Furthermore, during the second etherification reaction, the mass ratio of the added sodium hydroxide, 95% ethanol-water solution, sodium chloroacetate to the added bagasse cellulose during the first etherification reaction is 1:(1.5-2):(0.5-1):1.

[0011] Furthermore, during the first etherification reaction, the microwave power is 220-250 W, the microwave irradiation time is 2-4 min, and the microwave interval time is 2-4 min; during the second etherification reaction, the microwave power is 220-250 W, the microwave irradiation time is 2-3 min, and the microwave interval time is 2-3 min.

[0012] Furthermore, the preparation method of the pre-treated slurry is: disperse carboxymethyl cellulose in water, let it stand for 12 hours, add a thickener, sodium bicarbonate, urea, sodium sulfate and mix them evenly.

[0013] Furthermore, based on 100% of the total mass of the pre-treated slurry, the pre-treated slurry includes the following components in percentage: 3.3% carboxymethyl cellulose with a degree of substitution of 1.8, 4.5% thickener, 1.5% sodium bicarbonate, 7% auxiliary agent MIROPRINTMSU-01 and / or urea, 2.5% sodium sulfate, and the balance is water.

[0014] The beneficial effects of the present invention are:

[0015] By compounding highly substituted carboxymethyl cellulose with non-ionic penetrant A-113, tragacanth gum, etc., a pretreatment slurry for silk digital printing is formed. The fabric obtained after printing has high pattern clarity, high color yield, and good friction resistance. It can replace the traditional sodium alginate digital printing pretreatment slurry. The non-ionic penetrant A-113 and tragacanth gum have a synergistic effect, which can further improve the printing accuracy and softness of the hand to meet higher consumer demands. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] The preparation method of the high-substitution CMC pre-treatment slurry for silk digital printing of the present invention is as follows: dispersing carboxymethyl cellulose in water, standing for 12 hours, adding a thickener, sodium bicarbonate, urea, sodium sulfate and mixing evenly; based on 100% of the total mass of the pre-treatment slurry, the pre-treatment slurry includes the following percentage components: 3-6% of carboxymethyl cellulose with a substitution degree of 1.2-2, 3-5% of a thickener, 1-2.5% of sodium bicarbonate, 6-8% of an auxiliary agent MIROPRINT MSU-01 and / or urea, 2-4% of sodium sulfate, and the balance is water; the thickener is preferably a mixture of non-ionic penetrant A-113 (purchased from Suzhou Liansheng Chemical Co., Ltd.) and tragacanth gum, more preferably a mixture of non-ionic penetrant A-113 and tragacanth gum in a mass ratio of 1:0.5-1. The auxiliary agent MIROPRINT MSU-01 can be used as a urea substitute and is purchased from Guangdong Mingnuo Textile Industry Co., Ltd.

[0018] The carboxymethyl cellulose with a substitution degree of 1.2-2 is prepared by the following method: bagasse cellulose, sodium hydroxide and 95% ethanol-water solution are mixed and stirred at 35-40° C. for alkalization, and then sodium chloroacetate is added and etherified under intermittent microwave radiation. In the first etherification reaction, the mass ratio of bagasse cellulose, sodium hydroxide, 95% ethanol-water solution and sodium chloroacetate is 1: (1.4-2.1): (3.5-5): (1-2), the microwave power is 220-250 W, the microwave irradiation time is 2-4 min, and the microwave intermittent time is 2-4min; after the etherification is completed, filter and separate, add sodium hydroxide, sodium chloroacetate and 90% ethanol-water solution to the product again, mix well and etherify again under intermittent microwave radiation, the mass ratio of sodium hydroxide, 95% ethanol-water solution, sodium chloroacetate added in this stage to the bagasse cellulose added in the first etherification is 1: (1.5-2): (0.5-1): 1, the microwave power is 220-250W, the microwave irradiation time is 2-3min, and the microwave intermittent time is 2-3min; after the reaction is completed, filter and separate, wash and dry to obtain.

[0019] The preferred embodiments are as follows:

[0020] Example 1 Preparation of high-substitution CMC pre-treatment slurry for silk digital printing

[0021] (1) Bagasse cellulose, sodium hydroxide and 95% ethanol-water solution are mixed and stirred at 40°C for alkalization, and then sodium chloroacetate is added and etherification is carried out under intermittent microwave irradiation. In the first etherification reaction stage, the mass ratio of bagasse cellulose, sodium hydroxide, 95% ethanol-water solution and sodium chloroacetate is 1:1.8:4.2:1.5, the microwave power is 230W, the microwave irradiation time is 3min, and the microwave intermittent time is 3min. After the etherification is completed, the product is filtered and separated, and sodium hydroxide, sodium chloroacetate and 90% ethanol-water solution are added to the product again. After mixing, the product is etherified again under intermittent microwave irradiation. The mass ratio of sodium hydroxide, 95% ethanol-water solution and sodium chloroacetate added in this stage to the bagasse cellulose added in the first etherification is 1:2:0.8:1, the microwave power is 230W, the microwave irradiation time is 2min, and the microwave intermittent time is 2min. After the reaction is completed, the product is filtered and separated, washed and dried to obtain carboxymethyl cellulose with a degree of substitution of 1.8.

[0022] (2) dispersing the obtained carboxymethyl cellulose in water, letting it stand for 12 hours, and then adding a thickener, sodium bicarbonate, urea, and sodium sulfate and mixing them evenly; based on the total mass of the pre-treated slurry of 100%, the pre-treated slurry includes 3.3% of carboxymethyl cellulose with a degree of substitution of 1.8, 4.5% of a thickener (mixed by a non-ionic penetrant A-113 and tragacanth gum in a mass ratio of 1:0.5), 1.5% of sodium bicarbonate, 7% of urea, 2.5% of sodium sulfate, and the balance is water.

[0023] Example 2

[0024] A high-substitution CMC pretreatment slurry for silk digital printing was prepared according to Example 1, except that urea was replaced by the auxiliary agent MIROPRINT MSU-01.

[0025] Comparative Example 1

[0026] Commercially available carboxymethyl cellulose with a degree of substitution of 0.8 was used to prepare a pre-treated slurry according to the method of Example 1.

[0027] Comparative Example 2

[0028] The pre-treated slurry was prepared according to the method of Example 2, except that the 4.1% thickener was all non-ionic penetrant A-113.

[0029] Comparative Example 3

[0030] The pre-treated slurry was prepared according to the method of Example 2, except that the 4.1% thickener was all tragacanth gum.

[0031] The dye active yellow K-6G was used as the printing dye, and the pre-treatment slurries of Example 1 and Comparative Examples 1-3 were used for digital printing of silk fabrics, respectively. The printing process was as follows: the silk fabric was placed in the pre-treatment slurry for one dip and one roll, with a roll-off rate of 90%; after dipping and rolling, it was dried at 95°C, and then digital printing was performed. After printing, the fabric was dried at 85°C, steamed at 105°C for 30 minutes, washed with hot water at 40°C, and dried at 85°C. The performance test results are shown in the following table:

[0032]

[0033]

[0034] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A high-substitution CMC pre-treatment slurry for silk digital printing, characterized in that: Based on 100% of the total mass of the pre-treated slurry, the pre-treated slurry includes the following components in percentage: 3-6% of carboxymethyl cellulose with a degree of substitution of 1.2-2, 3-5% of a thickener, 1-2.5% of sodium bicarbonate, 6-8% of an auxiliary agent MIROPRINT MSU-01 and / or urea, 2-4% of sodium sulfate, and the balance is water.

2. According to claim 1, a high-substitution CMC pre-treatment slurry for silk digital printing is characterized in that: The thickener is a mixture of nonionic penetrant A-113 and tragacanth gum.

3. The high-substitution CMC pretreatment slurry for silk digital printing according to claim 2, characterized in that: The mass ratio of the nonionic permeabilizing agent A-113 to tragacanth gum is 1:0.5-1.

4. The high-substitution CMC pretreatment slurry for silk digital printing according to claim 1, characterized in that: Bagasse cellulose, sodium hydroxide and 95% ethanol-water solution are mixed and stirred at 35-40° C. for alkalization, and then sodium chloroacetate is added to carry out etherification under intermittent microwave radiation. After the etherification is completed, the product is filtered and separated, and sodium hydroxide, sodium chloroacetate and 90% ethanol-water solution are added to the product again, mixed and etherified again under intermittent microwave radiation. After the reaction is completed, the product is filtered and separated, washed and dried to obtain carboxymethyl cellulose with a degree of substitution of 1.2-2.

5. The high-substitution CMC pre-treatment slurry for silk digital printing according to claim 4, characterized in that: In the first etherification reaction, the mass ratio of bagasse cellulose, sodium hydroxide, 95% ethanol-water solution and sodium chloroacetate is 1:(1.4-2.1):(3.5-5):(1-2).

6. The high-substitution CMC pre-treatment slurry for silk digital printing according to claim 4, characterized in that: During the second etherification reaction, the mass ratio of the added sodium hydroxide, 95% ethanol-water solution, sodium chloroacetate and the added bagasse cellulose during the first etherification reaction is 1:(1.5-2):(0.5-1):

1.

7. The high-substitution CMC pretreatment slurry for silk digital printing according to claim 4, characterized in that: During the first etherification reaction, the microwave power is 220-250W, the microwave irradiation time is 2-4min, and the microwave interval time is 2-4min; during the second etherification reaction, the microwave power is 220-250W, the microwave irradiation time is 2-3min, and the microwave interval time is 2-3min.

8. The high-substitution CMC pre-treatment slurry for silk digital printing according to claim 1, characterized in that: The preparation method of the pre-treated slurry is as follows: dispersing carboxymethyl cellulose in water, leaving it to stand for 12 hours, and then adding a thickener, sodium bicarbonate, urea, and sodium sulfate and mixing them evenly.

9. The high-substituted CMC pre-treatment slurry for silk digital printing according to claim 1, characterized in that: Based on 100% of the total mass of the pre-treated slurry, the pre-treated slurry includes the following components in percentage: 3.3% carboxymethyl cellulose with a degree of substitution of 1.8, 4.1% thickener, 1.5% sodium bicarbonate, 7% auxiliary agent MIROPRINT MSU-01 and / or urea, 2.5% sodium sulfate, and the balance is water.