Wood yield stress and compression stress relaxation process testing device and method

By designing a test device for yield stress and compression stress relaxation process of wood, using hot plate clamping and mechanical testing machine to determine the yield stress and stress relaxation process of wood, the problem of long time and poor accuracy of the existing detection methods is solved, and the correct The accurate determination of wood with different moisture content provides basic data for wood modification research and process design.

CN119086304APending Publication Date: 2024-12-06BEIJING FUTURE NOVEL SOLID WOOD TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311348762.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-10-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing wood glass transition temperature detection methods have problems such as long detection time, long environmental humidity equilibrium time, small samples and inaccurate detection, especially in materials with large water content changes, which are difficult to obtain accurate results.

Method used

A test device for wood yield stress and compression stress relaxation process is designed, including a hot plate clamping device, a mechanical testing machine and a hot plate sealing device. The wood is clamped through the hot plate clamping device, and the wood is measured by a mechanical testing machine. The yield stress and stress relaxation process are obtained by combining the data acquisition device to obtain stress-strain data, and judge the yield point and stress relaxation process.

Benefits of technology

The yield stress determination and compression stress relaxation process of wood with different moisture content at different temperatures is achieved, which simplifies operation, improves detection efficiency and accuracy, and provides basic data for wood modification research and process optimization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086304A_ABST
    Figure CN119086304A_ABST
Patent Text Reader

Abstract

The invention discloses a wood yield stress and compression stress relaxation process testing device and method.According to the testing device, a mature mechanical testing machine is adopted as a platform, then a hot plate clamping device and an inter-hot-plate sealing device are loaded and additionally installed to form a basic structure, the hot plate clamping device is adopted for clamping wood, and the wood yield stress and compression stress relaxation process testing method is adopted for testing the wood yield stress and compression stress relaxation process. A mechanical testing machine is used for testing the yield stress and the stress relaxation process of the wood, then stress-strain data in the testing process are obtained through a data acquisition device, the stress yield point and the yield stress are judged through curve changes, and in the long-time heat treatment process of the compressed wood, the stress-strain data are obtained. Or a stress release process in a gas pressure and high temperature environment. The testing device is simple in structure and low in cost, the testing method can be used for measuring the yield stress of the wood with different water contents at different temperatures and measuring the compression stress relaxation process of the compressed wood, and the testing device has the advantages of being easy and convenient to operate and accurate in result.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wood performance detection, in particular to a device for testing wood yield stress and compression stress relaxation process. Background Art

[0002] Wood is a natural polymer material with a porous structure. Dried wood has obvious characteristics of elastic materials, but because the cell wall components that constitute the porous structure skeleton of wood are plastic, they will expand when encountering polar inorganic or organic gases or liquids such as water, ammonia, low molecular alcohols, phenols, etc., which will reduce the elastic modulus of wood and lower the softening temperature, thus showing the characteristics of plastic materials. By utilizing the porous structure and plasticity of wood, wood can be subjected to compression densification, shaping compression, and single-dimensional and multi-dimensional bending and other wood plastic modification, which can not only improve the physical and mechanical properties of wood such as density, hardness, strength and modulus, and improve the processing properties of wood such as wear resistance and nail holding force, but also change the macro and micro structures of wood and the shape of wood products. Therefore, the plasticity of wood has always been a research hotspot in the field of wood science and technology for a long time.

[0003] When using the plasticity of wood to compress or bend wood, the wood must be fully softened before applying external force to ensure that the wood cell wall is not damaged. The glass transition temperature and the yield point of the stress-strain curve are the main methods for judging the softening of wood. At present, there are three main methods for detecting the glass transition temperature, namely differential scanning calorimetry, static thermomechanical analysis, and dynamic thermomechanical analysis. Differential scanning calorimetry measures the change of the specific heat capacity of the material with temperature, static thermomechanical analysis is based on the deformation change of the polymer at different temperatures under a certain external force, and dynamic thermomechanical analysis uses the change of viscoelasticity of the polymer during the glass transition process to judge the glass transition temperature of the material. These methods have certain requirements on the thermal effect of the material, the size and shape of the sample, and the preparation of the sample. Moreover, due to the small size of the test sample, the long test time, and the long humidity balance time of the test environment, it is difficult for these test methods to obtain accurate test results of the glass transition temperature for materials with large changes in moisture content.

[0004] The yield point is a commonly used parameter to characterize the softening state of wood, which is determined by the stress-strain curve of wood under stress. Since the stress-strain curve of wood under stress can scientifically reproduce the elastic-plastic transformation process of wood, and the stress-change curve after stopping the external force loading can also reproduce the stress relaxation process, the stress-strain process of wood with different moisture contents under stress at different temperatures is recorded using the measurement system of the mechanical testing machine, and the yield point is determined based on the stress-strain curve analysis, so that the yield stress and stress relaxation process of wood with different moisture contents and other materials can be obtained. The corresponding testing equipment developed based on this idea and method is of great value in the research of wood modification such as wood compression densification, plastic compression, and single-dimensional and multi-dimensional bending, as well as the corresponding product development and process optimization. Summary of the invention

[0005] The purpose of the present invention is to provide a device and method for testing the yield stress and compression stress relaxation process of wood. The testing device of the present invention has a simple structure and low cost. The testing method of the present invention can measure the yield stress of wood with different moisture contents at different temperatures, and can measure the compression stress relaxation process of compressed wood, and has the advantages of simple operation and accurate results.

[0006] The technical scheme of the present invention is as follows: a device for testing the yield stress and compressive stress relaxation process of wood, comprising a hot plate clamping device, a mechanical testing machine and a sealing device between hot plates, wherein the hot plate clamping device comprises an upper pressing plate, a lower pressing plate and a heating system; the heating system is connected to the upper pressing plate and the lower pressing plate respectively; the mechanical testing machine comprises a base, an external force loading device and a data acquisition device; the lower end of the external force loading device is connected to the upper pressing plate via the data acquisition device; the lower pressing plate is connected to the base;

[0007] The closed device between hot plates is used for stress relaxation measurement and is loaded on the upper pressure plate or the lower pressure plate; the closed device between hot plates includes a frame and a cavity, the end face of the opening side of the frame is grooved and a sealing strip is installed; the cavity is connected with an airflow control channel, a temperature measurement and control channel and a pressure measurement and control channel; the airflow control channel is used to introduce gas into the cavity or exhaust gas from the cavity to control the composition and pressure of the gas medium in the cavity; the temperature measurement and control channel is used to install a temperature sensor to monitor the temperature in the cavity; the gas pressure measurement and control channel is used to install a gas pressure gauge to monitor the gas pressure in the cavity.

[0008] The above-mentioned wood yield stress and compression stress relaxation process testing device is provided with a first connecting device on the upper part of the upper pressing plate, and a fixing device is provided on the lower part of the lower pressing plate; a second connecting device is provided at the lower end of the data acquisition device, and the second connecting device is connected to the first connecting device of the upper pressing plate; the lower pressing plate is connected to the base via the fixing device.

[0009] The above-mentioned wood yield stress and compression stress relaxation process testing device, the size of the upper and lower pressing plates are both 8cm-40cm square or circular with the above-mentioned square edge material as the diameter, the thickness is greater than 4cm, and the material is steel plate or high temperature and high pressure resistant material; the frame of the sealing device between the hot plates is made of a material that can withstand gas pressure and mechanical pressure.

[0010] The aforementioned wood yield stress and compressive stress relaxation process testing device, the format size of the sealed device between hot plates is consistent with the size of the upper pressing plate or the lower pressing plate or is smaller than the pressing plate size, and the cavity of the sealed device between hot plates is circular or elliptical.

[0011] In the aforementioned wood yield stress and compressive stress relaxation process testing device, the height of the frame is greater than 5 mm, and the wall thickness width of the frame is greater than 2 cm.

[0012] The testing method of the aforementioned wood yield stress and compression stress relaxation process testing device adopts a hot plate clamping device to clamp the wood, uses a mechanical testing machine to test the wood yield stress and stress relaxation process, and then obtains the stress-strain data in the test process through a data acquisition device, and judges the stress yield point and yield stress through the changes in the curve, as well as the stress release process of the compressed wood after a long period of heat treatment or under gas pressure and high temperature environment.

[0013] The test method of the aforementioned wood yield stress and compression stress relaxation process test device, the test process of the wood yield stress is as follows:

[0014] Step 1, process the wood into a square sample with a thickness of 3-50 mm and a length and width of 1-10 cm, and pretreat the sample to achieve the target moisture content;

[0015] Step 2, adjusting the temperature of the upper pressing plate and the lower pressing plate of the hot plate clamping device to the target temperature of the wood yield stress test;

[0016] Step 3, place the sample with adjusted moisture content at the center of the lower pressing plate, quickly close the press, apply load at a speed of 2-15 mm / min, stop loading when the strain reaches more than 30% of the total thickness of the sample, and observe, measure and record the stress-strain data of the loading process in real time through the data acquisition device;

[0017] Step 4: According to the intersection point P0 of the proportional limit strain of the stress-strain curve and the stress-strain curve, or the intersection point P0 of the straight line after the proportional limit strain is compensated by the strain compensation coefficient α and the stress-strain curve OFF , determined as the stress yield point of the wood. The stress corresponding to the stress yield point is the yield stress of the sample, that is, the yield stress of the wood at a specific moisture content and a specific temperature.

[0018] The test method of the aforementioned wood yield stress and compression stress relaxation process test device, the test of the wood compression stress relaxation process includes stress relaxation measurement under normal pressure development state, and the process is as follows:

[0019] Step a, processing the wood into a square sample with a thickness of 3-50 mm and a length and width of 1-10 cm, and pretreating the sample to achieve a target moisture content;

[0020] Step b, adjusting the temperature of the upper pressing plate and the lower pressing plate of the hot plate clamping device to the target temperature of the wood yield stress test;

[0021] Step c, placing the sample with adjusted moisture content at the center of the lower pressing plate, quickly closing the press, compressing it to the target thickness at a speed of 2-15 mm / min, stopping increasing the external force value, and completing the compression process;

[0022] Step d: adjust the temperature of the hot press plate according to the target temperature of the stress relaxation process, and heat the upper and lower press plates to the target temperature. Use a mechanical testing machine to record the process in which the compressive stress applied during the compression process is completely released, i.e., the stress relaxation process, and output the stress change process and time when the loaded pressure is reduced to 0.

[0023] The test method of the aforementioned wood yield stress and compression stress relaxation process test device, the test of the wood compression stress relaxation process includes stress relaxation measurement under a closed pressurized state, and the process is as follows:

[0024] Step A, cutting the length and width of the sample size to be smaller than the side length of the square closed cavity or the diameter of the circular closed cavity, with a thickness of 5-80 mm, and pre-treating the sample to achieve the target moisture content;

[0025] Step B, installing the hot plate sealing device on the hot pressing clamping device, and after the hot pressing clamping device is adjusted to the target temperature, placing the wetted wood sample at the position corresponding to the center of the closed cavity;

[0026] Step C, quickly closing the press, compressing to the target thickness at a speed of 2-15 mm / min, stopping increasing the external force value, at which time the sample is still under a constant external force loading state, and then performing steam pressure heating treatment in a closed state to release the stress generated by compression, inputting or exhausting steam through the air flow channel, regulating the steam pressure, or after exhausting water vapor through the air flow channel, introducing nitrogen, inert gas or air, and controlling the steam, nitrogen or inert gas or air pressure to be 0.05-1.2 MPa;

[0027] Step D: Output the stress change process and time when the loaded pressure is reduced to 0, which is the wood stress relaxation process.

[0028] The test method of the above-mentioned wood yield stress and compressive stress relaxation process test device, the target moisture content pretreatment of the sample is to dry the sample to an absolute dry state and then weigh it, and the obtained mass is W0; then the mass of water required to achieve the target is calculated according to the target moisture content MC ; Then put the wood sample into a sealed bag and drop a mass of W into the wood sample. MC After adding distilled water, the sample is sealed tightly and placed at room temperature until the moisture in the wood is evenly distributed. During this period, the sample is taken out and weighed every day. By adding distilled water to the sample, the total mass of the sample is equal to or close to the sum of the mass of the absolute dry sample and the mass of water required to reach the target moisture content W0+W MC , to achieve the target moisture content.

[0029] Compared with the prior art, the test device of the present invention uses a mature (universal) mechanical testing machine as a platform, and then carries and installs a hot plate clamping device to form a basic structure, uses the hot plate clamping device to clamp the wood, uses the mechanical testing machine to test the wood yield stress and stress relaxation process, and then obtains the stress-strain data during the test process through a data acquisition device, and judges the stress yield point and yield stress through the change of the curve, as well as the long-term heat treatment process of the compressed wood, or the stress release process under gas pressure and high temperature environment. The present invention can measure the yield stress of wood with different moisture contents at different temperatures, improve basic data for scientific and technological research such as wood compression, and can also provide basic data for the process design of compressed wood production. The present invention can measure the compressive stress relaxation process of compressed wood in water vapor, nitrogen, inert gas or air environment under different gas pressure and temperature conditions, and provide basic data for basic research on the shaping treatment of compressed wood and production process design. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a structural schematic diagram of the testing device of the present invention;

[0031] Figure 2 It is a schematic diagram of the structure of the closed device;

[0032] Figure 3 Schematic diagram of the method for determining yield point and yield stress based on stress-strain curve.

[0033] Reference numerals

[0034] 1-hot plate clamping device; 101-upper pressing plate; 102-lower pressing plate; 103-first connecting device; 104-fixing device; 105-heating system; 2-mechanical testing machine; 201-base; 202-data acquisition device; 203-second connecting device; 204-external force loading device; 3-wood sample; 4, sealing device between hot plates; 401-cavity; 402-sealing device frame; 403-sealing strip; 404-airflow control channel; 405-temperature measurement and control channel; 406-pressure measurement and control channel. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.

[0036] Embodiment 1: A device for testing the yield stress and compressive stress relaxation process of wood, such as Figure 1 As shown, it includes a hot plate clamping device 1, a mechanical testing machine 2 and a hot plate sealing device 4. The hot plate clamping device is equipped with an electric heating or thermal oil heating device, with or without a cooling system, and the temperature control range is room temperature-250°C. The pressure of the mechanical testing machine is greater than 1kN, and the deformation measurement range is 3-80mm. The hot plate clamping device 1 includes an upper pressing plate 101, a lower pressing plate 102 and a heating system 105; the size of the upper pressing plate 101 and the lower pressing plate 102 are both 8cm-40cm square or circular with the above square edge material as the diameter, with a thickness greater than 4cm, and the material is steel plate or other high temperature and high pressure resistant materials. The upper part of the upper pressing plate 101 is provided with a first connecting device 103, and the lower part of the lower pressing plate 102 is provided with a fixing device 104; the heating system 105 is connected to the upper pressing plate 101 and the lower pressing plate 102 respectively; the mechanical testing machine 2 includes a base 201, an external force loading device 204 and a data acquisition device 202; the lower end of the external force loading device 204 is connected to the data acquisition device 202, and the lower end of the data acquisition device 202 is provided with a second connecting device 203; the second connecting device 203 is connected to the first connecting device 103 of the upper pressing plate 101; the lower pressing plate 102 is connected to the base 201 via the fixing device 104;

[0037] like Figure 2As shown, the closed device 4 between hot plates is used for stress relaxation measurement and is loaded on the upper pressing plate 101 or the lower pressing plate 102; the closed device includes a frame 402, in which a cavity 401 is arranged, and the cavity 401 is circular or elliptical; the end surface of the opening side of the frame 402 is grooved and a sealing strip 403 is installed; the cavity 401 is connected with an airflow control channel 404, a temperature measurement and control channel 405 and a pressure measurement and control channel 406. The airflow control channel 404 is used to introduce gas into the cavity or discharge gas from the cavity to control the gas medium composition and pressure in the cavity; the temperature measurement and control channel 405 is used to install a temperature sensor to monitor the temperature in the cavity; the gas pressure measurement and control channel 406 is used to install a gas pressure gauge to monitor the gas pressure in the cavity. The closed device 4 can be hoisted on the upper pressing plate (the cavity opening faces downward), or installed above the lower pressing plate (the cavity opening faces upward). In other embodiments, the upper pressing plate or the lower pressing plate can be made into a closed device. The frame of the sealing device is made of materials that are resistant to gas pressure and mechanical pressure, including metal or non-metal materials. The size of the sealing device is consistent with or smaller than the size of the pressing plate, and the cavity of the sealing device is designed in a cylindrical shape. The frame height of the sealing device is required to be greater than 5mm, the width of the frame wall is greater than 2cm, and a groove is opened in the middle of the frame to embed the sealing strip 403 or any other method that can make the frame airtight when the wood is compressed to the target thickness.

[0038] Furthermore, the test device also includes auxiliary equipment: a steam generator, an air booster pump, a high-pressure nitrogen tank, a thermal oil or electric heating system, a temperature control system, and a gas pressure control system. The above auxiliary equipment is used to achieve corresponding experimental conditions.

[0039] Embodiment 2: This embodiment 1 is a method for testing the yield stress of wood based on the testing device of embodiment 1, comprising the following steps:

[0040] Step 1: Process the wood into a square sample with a thickness of 3-50 mm and a length and width of 1-10 cm, and pre-treat the sample to achieve the target moisture content; the target moisture content pre-treatment of the sample is to dry the sample to an absolute dry state and then weigh it, and the obtained mass is W0; then calculate the mass of water W required to achieve the target according to the target moisture content MC ; Then put the wood sample into a sealed bag and drop a mass of W into the wood sample. MC After adding distilled water, the sample is sealed tightly and placed at room temperature until the moisture in the wood is evenly distributed. During this period, the sample is taken out and weighed every day. By adding distilled water to the sample, the total mass of the sample is equal to or close to the sum of the mass of the absolute dry sample and the mass of water required to reach the target moisture content W0+W MC , to achieve the target moisture content.

[0041] Step 2, adjusting the temperature of the upper pressing plate and the lower pressing plate of the hot plate clamping device to the target temperature of the wood yield stress test;

[0042] Step 3, place the sample with adjusted moisture content at the center of the lower pressing plate, quickly close the press, apply load at a speed of 2-15 mm / min (preferably 3-10 mm / min, 5 mm / min is used in this embodiment), stop loading when the strain reaches more than 30% of the total thickness of the sample, and observe, measure and record the stress-strain data of the loading process in real time through a data acquisition device;

[0043] Step 4: Figure 3 As shown, according to the intersection point P0 of the proportional limit strain of the stress-strain curve and the stress-strain curve, or the intersection point P0 of the straight line after the proportional limit strain is strain compensated according to the compensation coefficient α (the value range of α is 0.2%-3%) and the stress-strain curve OFF , determined as the stress yield point of the wood. The stress corresponding to the stress yield point is the yield stress of the sample, that is, the yield stress of the wood at a specific moisture content and a specific temperature.

[0044] Embodiment 4: This embodiment 1 is based on the test device of embodiment 1 to carry out the compressive stress relaxation process of wood under normal pressure development state, including the following steps:

[0045] Step a, processing the wood into a square sample with a thickness of 3-50 mm and a length and width of 1-10 cm, and pretreating the sample to achieve a target moisture content; wherein the pretreatment is the same as the method in Example 2;

[0046] Step b, adjusting the temperature of the upper pressing plate and the lower pressing plate of the hot plate clamping device to the target temperature of the wood yield stress test;

[0047] Step c: Place the sample with adjusted moisture content at the center of the lower platen, quickly close the press, compress it to the target thickness at a speed of 2-15mm / min, stop increasing the external force value, and complete the compression process; at this time, the sample is still under a constant external force loading state, and the stress generated by compression is released through long-term continuous heating treatment. In this step, the sample thickness and target thickness are determined according to the target compression rate, and the strain value of the compression process is regulated.

[0048] Step d: adjust the temperature of the hot press plate according to the target temperature of the stress relaxation process, and heat the upper and lower press plates to the target temperature. Use a mechanical testing machine to record the process in which the compressive stress applied during the compression process is completely released, i.e., the stress relaxation process, and output the stress change process and time when the loaded pressure is reduced to 0.

[0049] Embodiment 5: This embodiment 1 is based on the test device of embodiment 1 to carry out the compressive stress relaxation process of wood in a closed development state, including the following steps:

[0050] Step A, cutting the length and width of the sample size to be smaller than the side length of the square closed cavity or the diameter of the circular closed cavity, with a thickness of 5-80 mm, and pretreating the sample to achieve the target moisture content; wherein the pretreatment is the same as the method in Example 2; or adopting softening treatment, water spraying, soaking in water and other wetting treatments.

[0051] Step B, installing the hot plate sealing device on the hot pressing clamping device, and after the hot pressing clamping device is adjusted to the target temperature, placing the wetted wood sample at the position corresponding to the center of the closed cavity;

[0052] Step C, quickly closing the press, compressing to the target thickness at a speed of 2-15 mm / min, stopping increasing the external force value, at which time the sample is still under a constant external force loading state, and then performing steam pressure heating treatment in a closed state to release the stress generated by compression, inputting or exhausting steam through the air flow channel, regulating the steam pressure, or after exhausting water vapor through the air flow channel, introducing nitrogen, inert gas or air, and controlling the steam, nitrogen or inert gas or air pressure to be 0.05-1.2 MPa;

[0053] Step D: Output the stress change process and time when the loaded pressure reaches 0, which is the wood stress relaxation process.

[0054] In summary, the testing device of the present invention uses a mature (universal) mechanical testing machine as a platform, and then carries and adds a hot plate clamping device to form a basic structure, uses the hot plate clamping device to clamp the wood, uses the mechanical testing machine to test the wood yield stress and stress relaxation process, and then obtains the stress-strain data during the test process through a data acquisition device, and judges the stress yield point and yield stress through the change of the curve, as well as the long-term heat treatment process of the compressed wood, or the stress release process under gas pressure and high temperature environment. The present invention can measure the yield stress of wood with different moisture contents at different temperatures, improve basic data for scientific and technological research such as wood compression, and can also provide basic data for the process design of compressed wood production. The present invention can measure the compressive stress relaxation process of compressed wood in water vapor, nitrogen, inert gas or air environment under different gas pressure and temperature conditions, and provide basic data for basic research on the shaping treatment of compressed wood and production process design.

Claims

1. A device for testing the yield stress and compressive stress relaxation process of wood, comprising a hot plate clamping device (1), a mechanical testing machine (2) and a sealing device between hot plates (4), characterized in that: The hot plate clamping device (1) comprises an upper pressing plate (101), a lower pressing plate (102) and a heating system (105); the heating system (105) is connected to the upper pressing plate (101) and the lower pressing plate (102) respectively; the mechanical testing machine (2) comprises a base (201), an external force loading device (204) and a data acquisition device (202); the lower end of the external force loading device (204) is connected to the upper pressing plate (101) via the data acquisition device (202); the lower pressing plate (102) is connected to the base (201); The closed device (4) between hot plates is used for stress relaxation measurement and is loaded on the upper pressing plate (101) or the lower pressing plate (102); the closed device (402) between hot plates comprises a frame (402) and a cavity (401); the end surface of the opening side of the frame (402) is grooved and a sealing strip (403) is installed; the cavity is connected with an airflow control channel (404), a temperature measurement and control channel (405) and a pressure measurement and control channel (406); the airflow control channel (404) is used to introduce gas into the cavity or exhaust gas from the cavity to control the gas medium composition and pressure in the cavity; the temperature measurement and control channel (405) is used to install a temperature sensor to monitor the temperature in the cavity; the gas pressure measurement and control channel (406) is used to install a gas pressure gauge to monitor the gas pressure in the cavity.

2. The device for testing wood yield stress and compressive stress relaxation process according to claim 1, characterized in that: The upper portion of the upper pressing plate (101) is provided with a first connecting device (103), and the lower portion of the lower pressing plate (102) is provided with a fixing device (104); the lower end of the data acquisition device (202) is provided with a second connecting device (203), and the second connecting device (203) is connected to the first connecting device (103) of the upper pressing plate (101); and the lower pressing plate (102) is connected to the base (201) via the fixing device (104).

3. The device for testing wood yield stress and compressive stress relaxation process according to claim 1, characterized in that: The upper pressing plate (101) and the lower pressing plate (102) are both 8cm-40cm square or circular with the square edge as the diameter, with a thickness greater than 4cm, and are made of steel plate or high temperature and high pressure resistant material; the frame (402) of the hot plate inter-enclosed device (4) is made of a material resistant to gas pressure and mechanical pressure.

4. The device for testing wood yield stress and compressive stress relaxation process according to claim 1, characterized in that: The size of the sealed device (4) between the hot plates is consistent with or smaller than the size of the upper pressing plate (101) or the lower pressing plate (102), and the cavity (401) of the sealed device (4) between the hot plates is circular or elliptical.

5. The device for testing wood yield stress and compressive stress relaxation process according to claim 1, characterized in that: The height of the frame (402) is greater than 5 mm, and the wall thickness width of the frame (402) is greater than 2 cm.

6. The testing method of the wood yield stress and compressive stress relaxation process testing device according to any one of claims 1 to 5, characterized in that: The wood is clamped by a hot plate clamping device, and the wood yield stress and stress relaxation process are tested using a mechanical testing machine. The stress-strain data during the test is obtained through a data acquisition device, and the stress yield point and yield stress are determined by the changes in the curve, as well as the stress release process of the compressed wood during a long period of heat treatment or under gas pressure and high temperature environment.

7. The testing method of the wood yield stress and compressive stress relaxation process testing device according to claim 6, characterized in that: The test process of the wood yield stress is as follows: Step 1, process the wood into a square sample with a thickness of 3-50 mm and a length and width of 1-10 cm, and pretreat the sample to achieve the target moisture content; Step 2, adjusting the temperature of the upper pressing plate and the lower pressing plate of the hot plate clamping device to the target temperature of the wood yield stress test; Step 3, place the sample with adjusted moisture content at the center of the lower pressing plate, quickly close the press, apply load at a speed of 2-15 mm / min, stop loading when the strain reaches more than 30% of the total thickness of the sample, and observe, measure and record the stress-strain data of the loading process in real time through the data acquisition device; Step 4: According to the intersection point P0 of the proportional limit strain of the stress-strain curve and the stress-strain curve, or the intersection point P0 of the straight line after the proportional limit strain is compensated by the strain compensation coefficient α and the stress-strain curve OFF , determined as the stress yield point of the wood. The stress corresponding to the stress yield point is the yield stress of the sample, that is, the yield stress of the wood at a specific moisture content and a specific temperature.

8. The testing method of the wood yield stress and compressive stress relaxation process testing device according to claim 6, characterized in that: The test of the wood compression stress relaxation process includes the stress relaxation measurement under normal pressure development state, and the process is as follows: Step a, processing the wood into a square sample with a thickness of 3-50 mm and a length and width of 1-10 cm, and pretreating the sample to achieve a target moisture content; Step b, adjusting the temperature of the upper pressing plate and the lower pressing plate of the hot plate clamping device to the target temperature of the wood yield stress test; Step c, placing the sample with adjusted moisture content at the center of the lower pressing plate, quickly closing the press, compressing it to the target thickness at a speed of 2-15 mm / min, stopping increasing the external force value, and completing the compression process; Step d: adjust the temperature of the hot press plate according to the target temperature of the stress relaxation process, and heat the upper and lower press plates to the target temperature. Use a mechanical testing machine to record the process in which the compressive stress applied during the compression process is completely released, i.e., the stress relaxation process, and output the stress change process and time when the loaded pressure is reduced to 0.

9. The testing method of the wood yield stress and compressive stress relaxation process testing device according to claim 6, characterized in that: The test of the wood compression stress relaxation process includes stress relaxation measurement under a closed pressurized state, and the process is as follows: Step A, cutting the length and width of the sample size to be smaller than the side length of the square closed cavity or the diameter of the circular closed cavity, with a thickness of 5-80 mm, and pre-treating the sample to achieve the target moisture content; Step B, installing the hot plate sealing device on the hot pressing clamping device, and after the hot pressing clamping device is adjusted to the target temperature, placing the wetted wood sample at the position corresponding to the center of the closed cavity; Step C, quickly closing the press, compressing to the target thickness at a speed of 2-15 mm / min, stopping increasing the external force value, at which time the sample is still under a constant external force loading state, and then performing steam pressure heating treatment in a closed state to release the stress generated by compression, inputting or discharging steam through the air flow control channel, regulating the steam pressure, or after discharging water vapor through the air flow channel, introducing nitrogen, inert gas or air, and controlling the steam, nitrogen or inert gas or air pressure to be 0.05-1.2 MPa; Step D: Output the stress change process and time when the loaded pressure is reduced to 0, which is the wood stress relaxation process.

10. The testing method of the wood yield stress and compressive stress relaxation process testing device according to any one of claims 7 to 9, characterized in that: The target moisture content pretreatment of the sample is to dry the sample to an absolute dry state and then weigh it, and the obtained mass is W0; then the mass of water required to achieve the target is calculated according to the target moisture content. MC ; Then put the wood sample into a sealed bag and drop a mass of W into the wood sample. MC After adding distilled water, the sample is sealed tightly and placed at room temperature until the moisture in the wood is evenly distributed. During this period, the sample is taken out and weighed every day. By adding distilled water to the sample, the total mass of the sample is equal to or close to the sum of the mass of the absolute dry sample and the mass of water required to reach the target moisture content W0+W MC , to achieve the target moisture content.