Method for judging manufacturability of plate bent pipe

By identifying the characteristics of the parts and combining the rolling direction of the material for bending tests, the crack problem of sheet material during bending forming is solved, accurate prediction of metal sheet parts is achieved, manufacturing accuracy is improved, and suitable for the application of high-strength materials.

CN119089582AActive Publication Date: 2024-12-06ANGANG STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411199119.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

In the manufacturing process of automotive parts, the sheet is prone to cracks during bending and forming, resulting in a decrease in the strength and stiffness of the parts. Traditional empirical methods are difficult to meet the manufacturing requirements of high-strength steel materials.

Method used

By identifying the cross-section and overall profile characteristics of the part, determining the minimum bending radius and maximum bending angle, combining the rolling direction and tensile test of the material, scientifically predicting the bending deformation characteristics of the sheet, and determining whether the sheet meets the manufacturing of bent parts. Require.

Benefits of technology

It has achieved scientific and accurate prediction of metal sheet pipe parts, overcomes the technical difficulties of traditional empirical methods that cannot determine high-strength materials, greatly improves the accuracy of bending deformation prediction of parts, and is suitable for the manufacturing of various bent characteristics of parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119089582A_ABST
    Figure CN119089582A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of automobile parts, in particular to a method for judging manufacturability of a plate bent pipe. On the basis of a material bending deformation mechanism, bending deformation characteristics of a material are associated with bending deformation characteristic parameters of a part, and the bending characteristics of the part are accurately predicted by utilizing a micro deformation mechanism in the bending process. The method can scientifically and accurately predict the bending crack of the metal plate pipe part, overcomes the technical problem that a traditional experience method cannot judge a high-strength material, greatly improves the bending deformation prediction precision of the part, is very suitable for the occasion of judging the part with a plurality of different bent pipe characteristics, and has a wide application prospect. And the application requirements of engineering practice and scientific research work are widely met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile parts, and in particular to a method for determining the manufacturability of a plate tube bend. Background Art

[0002] In the manufacturing process of automotive parts, after the sheet metal is made into square tubes or round tubes, the bending process is usually used to bend the tube parts into different angles to meet the application requirements of the parts. However, the sheet metal will experience various types of deformation states such as stretching and compression to varying degrees during the bending process, which can easily cause cracks and thus cause parts to crack. After cracks occur in the parts, the stiffness and strength will drop significantly, and thus cannot meet the use requirements of the parts.

[0003] At present, the existing technical means in the industry mainly rely on empirical methods to select low-strength materials with higher elongation at break as much as possible to avoid cracking during the bending process of the material. However, due to the relatively low elongation at break of high-strength steel materials, cracking often occurs during the process of using high-strength steel to make pipe parts. The traditional empirical judgment method can no longer meet the actual requirements of the project. Therefore, it is very important to develop a method for determining the manufacturability of sheet metal bending. Summary of the invention

[0004] In order to overcome the shortcomings of the prior art, the present invention provides a method for determining the manufacturability of sheet metal pipe bending, which can scientifically and accurately predict the bending cracks of metal sheet metal pipe parts and determine whether the sheet metal can meet the manufacturing requirements of the bending parts.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for determining the manufacturability of a plate tube bend comprises the following steps:

[0007] 1) Identify the cross-sectional features of the part and measure the minimum bending radius inside the cross-sectional area of ​​the part as R 截面内弯min , unit: mm; the minimum bending radius of the outer side of the part section is R 截面外弯min , unit: mm; the maximum bending angle of the part section is α 截面max , unit: °;

[0008] 2) Identify the overall contour of the part and measure the minimum bending radius of the inner side of the part’s bend as R 整体内弯min , unit: mm; the minimum bending radius of the outer side of the part is R 整体外弯min , unit: mm; the maximum bending angle of the part is α 整体max , unit: °;

[0009] 3) If R 截面内弯min <R 整体内弯min, the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius;

[0010] If R 截面内弯min >R 整体内弯min , the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is parallel to the center line of the bending radius;

[0011] Punch radius and R 截面内弯min To adapt, the sheet material is α 截面max °Bending test, the limit strain at the outer bending radius of the sheet is measured as ε;

[0012] 4) Process the uniaxial tensile specimen in the direction of the rectangular sheet material in step 3), and the width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen satisfies:

[0013] L w ≥2.5×(R 整体内弯min +t);

[0014] Where: L w is the width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen, mm;

[0015] R 整体内弯min The minimum bending radius of the inner side of the part bend, mm;

[0016] t is the thickness of the part, mm;

[0017] The tensile test specimen is stretched to the limit strain measured in step 3) and then the stretching is stopped;

[0018] 5) Process the deformed area of ​​the tensile specimen in step 4) into a rectangular sheet. The extension direction of the bending radius center of the sheet is opposite to that in step 3). The punch radius is equal to R 整体内弯min To adapt, the sheet material is α 整体max °Bending test;

[0019] 6) If cracks appear in the sheet during the bending test in step 3) or step 5), the current sheet cannot meet the use requirements and needs to be replaced with a material with better bending performance;

[0020] If no cracks occur in the sheet material during the bending tests in step 3) and step 5), the current sheet material can meet the manufacturing requirements of the bent part.

[0021] Furthermore, in the step 1), the part is a bent tube with a rectangular cross-section.

[0022] Furthermore, in step 3), if R 截面内弯min >R 整体内弯min , the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is parallel to the center line of the bending radius.

[0023] Furthermore, in the step 3), the sheet material is a metal sheet material.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention discloses a method for determining the manufacturability of sheet metal tube bending. Based on the bending deformation mechanism of materials, the bending deformation characteristics of materials are associated with the bending deformation characteristic parameters of parts, and the bending characteristics of parts are accurately predicted using the microscopic deformation mechanism in the bending process. The present invention can scientifically and accurately predict the bending cracks of metal sheet tube parts, overcomes the technical difficulty that the traditional empirical method cannot determine high-strength materials, greatly improves the prediction accuracy of the bending deformation of parts, and is very suitable for determining the occasions of parts with multiple different bending characteristics, and widely meets the application requirements of engineering practice and scientific research work. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the three-dimensional structure of an embodiment of the present invention.

[0027] Figure 2 It is a cross-sectional characteristic diagram of an embodiment of the present invention.

[0028] Figure 3 It is a contour feature diagram of an embodiment of the present invention.

[0029] Figure 4 It is a cross-sectional bending specimen diagram of an embodiment of the present invention.

[0030] Figure 5 It is a characteristic diagram of the tensile specimen of the embodiment of the present invention.

[0031] Figure 6 It is a schematic diagram of a profile bending test according to an embodiment of the present invention. DETAILED DESCRIPTION

[0032] The present invention discloses a method for determining the manufacturability of a plate bending tube. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0033] A method for determining the manufacturability of sheet metal bending is based on the bending deformation mechanism of the material, associates the bending deformation characteristics of the material with the bending deformation characteristic parameters of the part, and uses the microscopic deformation mechanism in the bending process to accurately predict the bending characteristics of the part. The specific steps are as follows:

[0034] 1. Identify the cross-sectional features of the parts, measure the inner and outer bending radius and bending angle at the locations with typical cross-sectional features, and determine the minimum bending radius and maximum bending angle in the typical cross-sectional features of the parts. The minimum bending radius inside the part cross section is measured as R 截面内弯min , unit: mm; the minimum bending radius of the outer side of the part section is R 截面外弯min , unit: mm; the maximum bending angle of the part section is α 截面max , unit: °.

[0035] 2. Identify the overall contour features of the part, measure the inner and outer bending radius and bending angle of the part with bending features, and determine the minimum bending radius and maximum bending angle of the overall bending features of the part. The minimum bending radius of the inner side of the part bending is measured as R 整体内弯min , unit: mm; the minimum bending radius of the outer side of the part is R 整体外弯min , unit: mm; the maximum bending angle of the part is α 整体max , unit: °.

[0036] 3. If the minimum bending radius in the cross-sectional feature is smaller than the minimum bending radius in the contour feature, a rectangular sheet is manufactured in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius. If the minimum bending radius in the cross-sectional feature is larger than the minimum bending radius in the contour feature, a rectangular sheet is manufactured in such a way that the rolling direction of the sheet is parallel to the center line of the bending radius. The punch radius is selected according to the inner minimum bending radius determined in step 1. The sheet is subjected to a bending test at the maximum bending angle determined in step 1, and the limit strain at the outer bending radius of the sheet is determined.

[0037] If R 截面内弯min <R 整体内弯min , the rectangular sheet is made in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius; if R 截面内弯min >R 整体内弯min , the rectangular sheet is made in such a way that the rolling direction of the sheet is parallel to the center line of the bending radius. 截面内弯min To adapt, the sheet material is α 截面max °Bending test, the limit strain at the outer bending radius of the sheet is measured as ε.

[0038] 4. Process the uniaxial tensile specimen in the direction of the rectangular sheet material in step 3. The width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen needs to meet the requirement of Lw ≥ 2.5 × (R min轮廓 +t), that is, the width must be greater than 2.5 times the minimum bending radius determined in step 2 plus 2 times the material thickness. The tensile specimen is stretched to the limit strain measured in step 3 and then stopped.

[0039] That is, the uniaxial tensile specimen is processed according to the rectangular sheet manufacturing direction of step 3, and the width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen satisfies:

[0040] L w ≥2.5×(R 整体内弯min +t);

[0041] Where: L w is the width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen, mm;

[0042] R 整体内弯min The minimum bending radius of the inner side of the part bend, mm;

[0043] t is the thickness of the part, mm;

[0044] The tensile specimen is stretched to the limit strain measured in step 3) and then the stretching is stopped. 整体内弯min Equal to R min轮廓 .

[0045] 5. Process the deformed area of ​​the tensile specimen in step 4 into a rectangular sheet. The direction of the extension line of the bending radius center of the sheet is opposite to that of step 3. Select the punch radius according to the minimum inner bending radius determined in step 2. Perform a bending test on the sheet according to the maximum bending angle determined in step 2. Process the deformed area of ​​the tensile specimen in step 4 into a rectangular sheet. The direction of the extension line of the bending radius center of the sheet is opposite to that of step 3. Select the punch radius according to the minimum inner bending radius determined in step 2. Perform a bending test on the sheet according to the maximum bending angle determined in step 2. 整体内弯min To adapt, the sheet material is α 整体max °Bending test;

[0046] 6. If cracks appear in the sheet during the bending test in step 3 or step 5, the current sheet cannot meet the use requirements and needs to be replaced with a material with better bending performance. If no cracks appear in the bending tests in step 3 and step 5, the current sheet can meet the manufacturing requirements of the bent part.

[0047] [Example 1]

[0048] like Figure 1-6 As shown in the figure, a method for determining the manufacturability of sheet metal bending is Figure 1 Take the bent pipe parts as an example to illustrate, which specifically includes the following steps:

[0049] 1. If Figure 2 As shown, the cross-sectional features of the part are identified, and the inner and outer bending radii and bending angles are measured for the locations with typical cross-sectional features. The minimum bending radius of the typical cross-sectional features of the part is determined to be 5 mm and the maximum bending angle is 90 degrees. 截面内弯min =5mm, the minimum bending radius of the outer side of the part section is R 截面外弯min=6mm, maximum bending angle of part section α 截面max =90°.

[0050] 2. If Figure 3 As shown, the overall contour features of the part are identified, and the inner and outer bending radii and bending angles of the bending feature positions of the part are measured to determine that the minimum bending radius of the overall bending feature of the part is 24 mm and the maximum bending angle is 90 degrees. 整体内弯min =24mm, R 整体外弯min =51mm, α 整体max =90°.

[0051] 3. If Figure 4 As shown in the figure, since the minimum bending radius in the cross-section feature is smaller than the minimum bending radius in the profile feature, the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius, as shown in the figure. Figure 4 As shown, according to the minimum inner bending radius determined in step 1, the punch radius is selected to be 5 mm, and a 90-degree bending test is performed on the sheet material according to the maximum bending angle determined in step 1. The ultimate strain at the outer bending radius of the sheet material is measured to be 2.68%.

[0052] 4. Process the uniaxial tensile specimen in the direction of the rectangular sheet material in step 3. The width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen needs to meet the requirement of Lw ≥ 2.5 × (R min轮廓 +t), that is, the width must be greater than 2.5 times the minimum bending radius determined in step 2 plus 2 times the material thickness, such as Figure 5 As shown, the tensile test specimen is stretched to the ultimate strain of 2.68% measured in step 3 and then the stretching is stopped. The ultimate strain ε at the outer bending radius of the sheet is 2.68%.

[0053] 5. Process the deformed area of ​​the tensile specimen in step 4 into a rectangular sheet. The direction of the extension line of the bending radius center of the sheet is opposite to that in step 3, such as Figure 6 As shown, according to the minimum inner bending radius determined in step 2, the punch radius is selected to be 24 mm, and the sheet is subjected to a bending test at the maximum bending angle of 90 degrees determined in step 2.

[0054] 6. If no cracks appear on the current sheet in the bending tests in step 3 and step 5, the current sheet can meet the manufacturing requirements of the bent part.

[0055] [Example 2]

[0056] like Figure 1-6 As shown in the figure, a method for determining the manufacturability of sheet metal bending is Figure 1 Take the bent pipe parts as an example to illustrate, which specifically includes the following steps:

[0057] 1. If Figure 2As shown, the cross-sectional features of the part are identified, and the inner and outer bending radii and bending angles are measured for the positions with typical cross-sectional features. The minimum bending radius of the typical cross-sectional features of the part is determined to be 20 mm and the maximum bending angle is 120 degrees. 截面内弯min =20mm, the minimum bending radius of the outer side of the part section is R 截面外弯min =25mm, maximum bending angle of part section α 截面max =120°.

[0058] 2. If Figure 3 As shown, the overall contour features of the part are identified, and the inner and outer bending radii and bending angles of the bending feature positions of the part are measured, and the minimum bending radius of the overall bending features of the part is determined to be 18 mm and the maximum bending angle is 135 degrees. 整体内弯min =26mm, R 整体外弯min =36mm, α 整体max =135°.

[0059] 3. If Figure 4 As shown in the figure, since the minimum bending radius in the cross-section feature is smaller than the minimum bending radius in the profile feature, the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius, as shown in the figure. Figure 4 As shown, according to the minimum inner bending radius determined in step 1, the punch radius is selected to be 20 mm, and the sheet is subjected to a 120-degree bending test according to the maximum bending angle determined in step 1. The ultimate strain at the outer bending radius of the sheet is measured to be 5.66%.

[0060] 4. Process the uniaxial tensile specimen in the direction of the rectangular sheet material in step 3. The width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen needs to meet the requirement of Lw ≥ 2.5 × (R min轮廓 +t), that is, the width must be greater than 2.5 times the minimum bending radius determined in step 2 plus 2 times the material thickness, such as Figure 5 As shown, the tensile test specimen is stretched to the ultimate strain of 5.66% measured in step 3 and then the stretching is stopped. The ultimate strain ε at the outer bending radius of the sheet is 5.66%.

[0061] 5. Process the deformed area of ​​the tensile specimen in step 4 into a rectangular sheet. The direction of the extension line of the bending radius center of the sheet is opposite to that in step 3, such as Figure 6 As shown, according to the minimum inner bending radius determined in step 2, the punch radius is selected to be 26 mm, and the sheet is subjected to a bending test at the maximum bending angle of 135 degrees determined in step 2.

[0062] 6. If no cracks appear on the current sheet in the bending tests in step 3 and step 5, the current sheet can meet the manufacturing requirements of the bent part.

[0063] [Example 3]

[0064] like Figure 1-6 As shown in the figure, a method for determining the manufacturability of sheet metal bending is Figure 1 Take the bent pipe parts as an example to illustrate, which specifically includes the following steps:

[0065] 1. If Figure 2 As shown, the cross-sectional features of the part are identified, and the inner and outer bending radii and bending angles are measured for the positions with typical cross-sectional features. The minimum bending radius of the typical cross-sectional features of the part is determined to be 10 mm and the maximum bending angle is 110 degrees. 截面内弯min =10mm, the minimum bending radius of the outer side of the part section is R 截面外弯min =12mm, maximum bending angle of part section α 截面max =110°.

[0066] 2. If Figure 3 As shown, the contour features of the whole part are identified, and the inner and outer bending radii and bending angles of the bending feature positions of the part are measured, and the minimum bending radius of the whole bending feature of the part is determined to be 20 mm and the maximum bending angle is 100 degrees. 整体内弯min =20mm, R 整体外弯min =40mm, α 整体max =100°.

[0067] 3. If Figure 4 As shown in the figure, since the minimum bending radius in the cross-section feature is smaller than the minimum bending radius in the profile feature, the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius, as shown in the figure. Figure 4 As shown, according to the minimum inner bending radius determined in step 1, the punch radius is selected to be 10 mm, and the sheet is subjected to a 110-degree bending test according to the maximum bending angle determined in step 1. The ultimate strain at the outer bending radius of the sheet is measured to be 3.67%.

[0068] 4. Process the uniaxial tensile specimen in the direction of the rectangular sheet material in step 3. The width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen needs to meet the requirement of Lw ≥ 2.5 × (R min轮廓 +t), that is, the width must be greater than 2.5 times the minimum bending radius determined in step 2 plus 2 times the material thickness, such as Figure 5 As shown, the tensile test specimen is stretched to the ultimate strain of 3.67% measured in step 3 and then the stretching is stopped. The ultimate strain ε at the outer bending radius of the sheet is 3.67%.

[0069] 5. Process the deformed area of ​​the tensile specimen in step 4 into a rectangular sheet. The direction of the extension line of the bending radius center of the sheet is opposite to that in step 3, such as Figure 6As shown, according to the minimum inner bending radius determined in step 2, the punch radius is selected to be 20 mm, and the sheet is subjected to a bending test at the maximum bending angle of 100 degrees determined in step 2.

[0070] 6. If no cracks appear on the current sheet in the bending tests in step 3 and step 5, the current sheet can meet the manufacturing requirements of the bent part.

[0071] The present invention is based on the bending deformation mechanism of materials, associates the bending deformation characteristics of materials with the bending deformation characteristic parameters of parts, and uses the microscopic deformation mechanism in the bending process to accurately predict the bending characteristics of parts. The present invention can scientifically and accurately predict the bending cracks of metal sheet and tube parts, overcomes the technical difficulty that the traditional empirical method cannot determine high-strength materials, greatly improves the prediction accuracy of the bending deformation of parts, and is very suitable for determining parts with multiple different bending characteristics, and widely meets the application requirements of engineering practice and scientific research work.

[0072] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for determining the manufacturability of a plate tube bend, characterized in that: The specific steps include: 1) Identify the cross-sectional features of the part and measure the minimum bending radius inside the cross-sectional area of ​​the part as R 截面内弯min , unit: mm; the minimum bending radius of the outer side of the part section is R 截面外弯min , unit: mm; the maximum bending angle of the part section is α 截面max , unit: °; 2) Identify the overall contour of the part and measure the minimum bending radius of the inner side of the part’s bend as R 整体内弯min , unit: mm; the minimum bending radius of the outer side of the part is R 整体外弯min , unit: mm; the maximum bending angle of the part is α 整体max , unit: °; 3) If R 截面内弯min <R 整体内弯min , the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is perpendicular to the center line of the bending radius; Punch radius and R 截面内弯min To adapt, the sheet is α 截面max °Bending test, the limit strain at the outer bending radius of the sheet is measured as ε; 4) Process the uniaxial tensile specimen in the direction of the rectangular sheet material in step 3), and the width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen satisfies: L w ≥2.5×(R 整体内弯min +t); Where: L w is the width of the deformation area in the middle of the dumbbell-shaped uniaxial tensile specimen, mm; R 整体内弯min The minimum bending radius of the inner side of the part bend, mm; t is the thickness of the part, mm; The tensile test specimen is stretched to the limit strain measured in step 3) and then the stretching is stopped; 5) Process the deformed area of ​​the tensile specimen in step 4) into a rectangular sheet. The extension direction of the bending radius center of the sheet is opposite to that in step 3). The punch radius is equal to R 整体内弯min To adapt, the sheet is α 整体max °Bending test; 6) If cracks appear in the sheet during the bending test in step 3) or step 5), the current sheet cannot meet the use requirements and needs to be replaced with a material with better bending performance; If no cracks occur in the sheet material during the bending tests in step 3) and step 5), the current sheet material can meet the manufacturing requirements of the bent part.

2. A method for determining the manufacturability of a plate tube bend according to claim 1, characterized in that: In the step 1), the part is a bent tube with a rectangular cross section.

3. The method for determining the manufacturability of a plate tube bend according to claim 1, characterized in that: In step 3), if R 截面内弯min >R 整体内弯min , the rectangular sheet is manufactured in such a way that the rolling direction of the sheet is parallel to the center line of the bending radius.

4. The method for determining the manufacturability of a plate tube bend according to claim 1, characterized in that: In the step 3), the sheet material is a metal sheet material.

Citation Information

Patent Citations

  • Vehicle collision energy absorbing member excellent in energy absorbing performance and manufacturing method therefor

    CA2835153A1

  • Metal sheet edge limit strain test method

    CN115165562A

  • Method for evaluating three-dimensional threshold hydrogen-induced cracks of roll-formed high-strength steel

    CN116893255A

  • Deformation limit evaluation method, crack prediction method and press metal mold design method

    JP2020040111A

  • Metal sheet bending fracture determination method and recording medium

    US20160161382A1