Semiconductor structure, solar cell and manufacturing method thereof, and photovoltaic module

By adjusting the refractive indices and extinction coefficients of N-type and P-type doped polysilicon layers in solar cells, the balance of electron and hole collection is improved, enhancing the efficiency and reducing manufacturing challenges.

CN119092581APending Publication Date: 2024-12-06LONGI GREEN ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411155282.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing solar cells face challenges in balancing the refraction effects of N-type and P-type doped polysilicon layers, which affects the efficiency of electron and hole collection, leading to suboptimal performance.

Method used

The refractive indices and extinction coefficients of the N-type and P-type doped polysilicon layers are adjusted to be within specific ranges, ensuring balanced light refraction and improved electron-hole balance, with the P-type layer being denser to resist etching and enhance passivation, and the N-type layer having a higher extinction coefficient to prevent electrode penetration.

Benefits of technology

This adjustment enhances the efficiency of electron-hole pair generation, reduces carrier recombination, and improves the overall performance of the solar cell by optimizing the electrode contact and reducing manufacturing difficulties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092581A_ABST
    Figure CN119092581A_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor structure, a solar cell, a manufacturing method of the solar cell and a photovoltaic module, relates to the technical field of photovoltaics, and is used for improving the working performance of the solar cell. The solar cell comprises a semiconductor substrate, a P-type doped polycrystalline silicon layer and an N-type doped polycrystalline silicon layer. The semiconductor substrate includes a first region and a second region. The P-type doped polysilicon layer is at least formed on the first region. The N-type doped polysilicon layer is at least formed on the second region. And at least partial region of the N-type doped polycrystalline silicon layer and at least partial region of the P-type doped polycrystalline silicon layer are arranged at intervals. The ratio of the refractive index n of the N-type doped polycrystalline silicon layer to the refractive index n of the P-type doped polycrystalline silicon layer is greater than or equal to 0.9 and less than or equal to 1.1; and / or the absolute value of the difference between the refractive index n of the P-type doped polycrystalline silicon layer and the refractive index n of the N-type doped polycrystalline silicon layer is greater than or equal to 0 and less than or equal to 0.1.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the application number 202410684958.0, and the invention title is "A semiconductor structure, a solar cell and a method for manufacturing the same, and a photovoltaic module". The application date of the patent application with application number 202410684958.0 is May 30, 2024. Technical Field

[0002] The present invention relates to the field of photovoltaic technology, and in particular to a semiconductor structure, a solar cell and a manufacturing method thereof, and a photovoltaic module. Background Art

[0003] A solar cell is a device that can convert sunlight into electrical energy. Specifically, when a solar cell is in operation, sunlight shines on the semiconductor pn junction of the solar cell, forming new hole-electron pairs. Under the action of the built-in electric field of the pn junction, photogenerated holes flow to the p region and photogenerated electrons flow to the n region. When the circuit is connected, current can be generated.

[0004] However, in existing solar cells, the N-type doped polysilicon layer and the P-type doped polysilicon layer have different refraction effects on light, which makes it difficult to ensure the balance of electrons and holes, and is not conducive to improving the working efficiency of solar cells. Summary of the invention

[0005] The object of the present invention is to provide a semiconductor structure, a solar cell and a method for manufacturing the same, and a photovoltaic module, so that the refraction effects of the N-type doped polysilicon layer and the P-type doped polysilicon layer on light are roughly the same, which is beneficial to ensure the balance of electrons and holes and improve the working efficiency of the solar cell.

[0006] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a solar cell, which comprises: a semiconductor substrate, a P-type doped polysilicon layer and an N-type doped polysilicon layer. The semiconductor substrate has a first region and a second region. The first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate, respectively. The P-type doped polysilicon layer is formed at least on the first region. The N-type doped polysilicon layer is formed at least on the second region. At least a portion of the N-type doped polysilicon layer and at least a portion of the P-type doped polysilicon layer are arranged at intervals from each other. Wherein, the ratio between the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer is greater than or equal to 0.9 and less than or equal to 1.1; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.1.

[0007] When the above technical solution is adopted, one of the P-type doped polysilicon layer and the N-type doped polysilicon layer can form a high-low junction with the semiconductor substrate, and the other can form a PN junction with the semiconductor substrate. Based on this, when the solar cell is in a working state, the semiconductor substrate can form new hole-electron pairs after absorbing photons. Under the action of the built-in electric field of the above-mentioned PN junction and high-low junction, the photogenerated holes flow to the P-type doped polysilicon layer, and the photogenerated electrons flow to the N-type doped polysilicon layer, and current can be generated after the circuit is connected. Secondly, in addition to being able to collect and transmit the electrons and holes generated in the semiconductor substrate respectively, the N-type doped polysilicon layer and the P-type doped polysilicon layer can also generate a part of the electron-hole pairs after absorbing photons for power generation. Moreover, after the light enters the semiconductor substrate from the light-facing side of the solar cell corresponding to the semiconductor substrate, part of the light will pass through the semiconductor substrate to reach the interface between the semiconductor substrate and the N-type doped polysilicon layer, or the interface between the semiconductor substrate and the P-type doped polysilicon layer. At this time, the N-type doped polysilicon layer and the P-type doped polysilicon layer can reflect part of the light, so that the semiconductor substrate absorbs light energy for a second time, generates more electron and hole pairs, and improves the utilization rate of the semiconductor substrate for light. In the above case, when the ratio between the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer is within the above range, the refractive index n of the two is approximately equal, so that the refractive effect of the N-type doped polysilicon layer and the P-type doped polysilicon layer on the light is approximately the same, which is conducive to ensuring the balance of electrons and holes and improving the working efficiency of the solar cell. In addition, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.1. The beneficial effects in this case can refer to the beneficial effects when the ratio of the refractive index n between the N-type doped polysilicon layer and the P-type doped polysilicon layer is greater than or equal to 0.9 and less than or equal to 1.1 as mentioned above, and will not be repeated here.

[0008] As a possible implementation solution, the extinction coefficient k of the N-type doped polysilicon layer is greater than the extinction coefficient k of the P-type doped polysilicon layer.

[0009] In the case of adopting the above technical solution, due to the different conductivity types of the carriers to be collected by the P-type doped polysilicon layer and the N-type doped polysilicon layer, the corresponding electrode slurry for manufacturing the positive electrode electrically connected to the P-type doped polysilicon layer and the electrode slurry for manufacturing the negative electrode electrically connected to the N-type doped polysilicon layer usually have different compositions to ensure that the positive electrode has a higher hole transfer rate and that the negative electrode has a higher electron transfer rate. However, the film etching ability of the positive electrode and the negative electrode with different conventional slurry compositions is different. The etching depth of the positive electrode of the film layer with the same density is much deeper than that of the negative electrode, and the positive electrode has a greater risk of burn-through. By adjusting the density of the P-type doped polysilicon layer and the N-type doped polysilicon layer, the P-type doped polysilicon layer is made denser, the etching resistance of the positive electrode is increased, thereby reducing the etching depth of the positive electrode, and the positive electrode stays at a suitable depth. The extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer are related to the density of the film layer itself. Within a certain range, the extinction coefficient k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is inversely proportional to the density of the film layer itself. Based on this, the film density of the N-type doped polysilicon layer and the P-type doped polysilicon layer can be regulated by adjusting the magnitude relationship of the extinction coefficient k values ​​of the above two film layers, and the extinction coefficient k of the N-type doped polysilicon layer is set to be greater than the extinction coefficient k of the P-type doped polysilicon layer, so that the P-type doped polysilicon layer has a relatively high density, and then the P-type doped polysilicon layer has a relatively high ability to resist electrode slurry etching, preventing the manufactured positive electrode from penetrating the P-type doped polysilicon layer, improving the matching between the electrode slurry corresponding to the P-type doped polysilicon layer and the positive electrode, and ensuring that the P-type doped polysilicon layer has a high field passivation effect, reducing the carrier recombination rate on the backlight side, and improving the working performance of the solar cell.

[0010] As a possible implementation scheme, the solar cell further includes a surface passivation layer. The surface passivation layer covers at least one side of the P-type doped polysilicon layer away from the semiconductor substrate and one side of the N-type doped polysilicon layer away from the semiconductor substrate. In addition, the ratio of the extinction coefficient k of the N-type doped polysilicon layer to the extinction coefficient k of the P-type doped polysilicon layer is greater than or equal to 1.5 and less than or equal to 2.5; and / or the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer is greater than or equal to 0.2 and less than or equal to 0.5.

[0011] When the above technical solution is adopted, the ratio of the extinction coefficient k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is within the above range, so as to prevent the film layer of the N-type doped polysilicon layer from being too loose due to the large ratio, so that the negative electrode can easily penetrate the N-type doped polysilicon layer, and ensure that the N-type doped polysilicon layer has a high field passivation effect. In addition, when the first region and the second region are located on the same surface or the first region is located in a part of a certain surface, it can also prevent the film layer of the P-type doped polysilicon layer from being too dense due to the large ratio, so that the etching difficulty of the entire deposited P-type doped polysilicon layer during patterning is large and the etching efficiency is low, thereby reducing the difficulty of manufacturing solar cells and improving the manufacturing efficiency of solar cells. At the same time, it can also prevent the contact area between the positive electrode and the P-type doped polysilicon layer from being small due to the P-type doped polysilicon layer being too dense, so as to ensure that the positive electrode and the negative electrode have a small contact resistance. In addition, when the ratio of the extinction coefficients k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is within the above range, it can also prevent the density of the P-type doped polysilicon layer from being improved to a small extent due to the small ratio, thereby ensuring that the positive electrode does not penetrate the P-type doped polysilicon layer, and at the same time, it is beneficial to reduce the metal composite loss between the positive electrode and the P-type doped polysilicon layer, thereby ensuring that the solar cell has a higher working performance.

[0012] As a possible implementation scheme, the solar cell further includes a positive electrode in ohmic contact with the P-type doped polysilicon layer, and a negative electrode in ohmic contact with the N-type doped polysilicon layer. Moreover, along the thickness direction of the semiconductor substrate, at least part of the positive electrode extends to a depth greater than or equal to a depth at least part of the negative electrode extends to the N-type doped polysilicon layer. In this case, when at least part of the positive electrode extends to a depth greater than or equal to a depth at least part of the negative electrode extends to the N-type doped polysilicon layer, it is beneficial to increase the contact area between the positive electrode and the P-type doped polysilicon layer, thereby making the positive electrode and the P-type doped polysilicon layer have a smaller contact resistance, which is beneficial to reducing the transmission loss of holes from the P-type doped polysilicon layer to the positive electrode, and is beneficial to improving the working performance of the solar cell. In addition, in actual application, due to factors such as the limitation of doping solid concentration, the impurity doping concentration in the P-type doped polysilicon layer is often lower than the impurity doping concentration in the N-type doped polysilicon layer. Therefore, when at least part of the positive electrode extends to a depth greater than or equal to a depth of at least part of the negative electrode extending to the N-type doped polysilicon layer, it is also beneficial to prevent a large metal composite area between the N-type doped polysilicon layer and the negative electrode due to a large contact area between the two, thereby ensuring a small composite loss between the N-type doped polysilicon layer and the negative electrode.

[0013] As a possible implementation scheme, in the case where the above-mentioned solar cell also includes a positive electrode in ohmic contact with the P-type doped polycrystalline silicon layer, and a negative electrode in ohmic contact with the N-type doped polycrystalline silicon layer, along the thickness direction of the semiconductor substrate, at least a portion of the positive electrode extends into the P-type doped polycrystalline silicon layer to a depth greater than or equal to 80nm and less than or equal to 100nm.

[0014] When the above technical solution is adopted, along the thickness direction of the semiconductor substrate, at least part of the positive electrode extends to a depth within the P-type doped polysilicon layer within the above range, which is beneficial to prevent the contact area between the positive electrode and the P-type doped polysilicon layer from being small due to the small depth, and is beneficial to reducing the contact resistance between the positive electrode and the P-type doped polysilicon layer. In addition, it is also beneficial to prevent the contact area between the positive electrode and the P-type doped polysilicon layer from being too large due to the large depth, and is beneficial to reducing the metal composite loss between the positive electrode and the P-type doped polysilicon layer. In summary, the depth of the positive electrode extending into the P-type doped polysilicon layer is within the above range, which is beneficial to balance the contact resistance and metal composite loss between the positive electrode and the P-type doped polysilicon layer, and ensure that the solar cell has a high working performance.

[0015] As a possible implementation scheme, in the case where the solar cell further includes a positive electrode in ohmic contact with the P-type doped polysilicon layer and a negative electrode in ohmic contact with the N-type doped polysilicon layer, along the thickness direction of the semiconductor substrate, at least a portion of the negative electrode extends to a depth greater than or equal to 50 nm and less than or equal to 80 nm in the N-type doped polysilicon layer. The beneficial effects in this case are similar to the beneficial effects of at least a portion of the positive electrode extending to a depth greater than or equal to 80 nm and less than or equal to 100 nm in the P-type doped polysilicon layer as described above, and are not described in detail here.

[0016] As a possible implementation scheme, the solar cell further includes a first tunneling passivation layer, and the first tunneling passivation layer is located between the P-type doped polysilicon layer and the semiconductor substrate.

[0017] When the above-mentioned technical solution is adopted, the first tunneling passivation layer and the P-type doped polysilicon layer can constitute a tunneling passivation contact structure to achieve chemical passivation of the first region of the semiconductor substrate and selective collection of holes, thereby reducing the carrier recombination rate on the side of the semiconductor substrate where the first tunneling passivation layer is formed, which is beneficial to improving the photoelectric conversion efficiency of the solar cell.

[0018] As a possible implementation scheme, the solar cell further includes a second tunneling passivation layer, and the second tunneling passivation layer is at least located between the N-type doped polysilicon layer and the semiconductor substrate.

[0019] When the above-mentioned technical solution is adopted, the second tunneling passivation layer and the N-type doped polysilicon layer can constitute a tunneling passivation contact structure to achieve chemical passivation of the second region of the semiconductor substrate and selective collection of electrons, thereby reducing the carrier recombination rate on the side of the semiconductor substrate where the second tunneling passivation layer is formed, which is beneficial to improving the photoelectric conversion efficiency of the solar cell.

[0020] As a possible implementation scheme, the solar cell is a back contact cell. In this case, the first region and the second region are located on the same surface of the semiconductor substrate. Compared with double-sided contact solar cells, the technical solution of the present invention has a higher application advantage in back contact cells. The technology of the present invention can effectively control the height difference between the two regions of the back contact cell, improve the interconnection yield, improve the patterning efficiency, and improve the production efficiency.

[0021] In a second aspect, the present invention provides a semiconductor structure, which includes: a semiconductor substrate, a P-type doped polysilicon layer and an N-type doped polysilicon layer. The semiconductor substrate includes a first region and a second region. The first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate. The P-type doped polysilicon layer is formed at least on the first region. The N-type doped polysilicon layer is formed at least on the second region. At least part of the N-type doped polysilicon layer and at least part of the P-type doped polysilicon layer are arranged at intervals. Wherein, the ratio between the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer is greater than or equal to 0.8 and less than or equal to 1.2; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.2.

[0022] When the above technical solution is adopted, it is beneficial to make the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer in the solar cell manufactured based on the semiconductor structure provided by the present invention approximately equal. The beneficial effect of the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer in the solar cell being approximately equal can be referred to in the previous text, and will not be repeated here.

[0023] As a possible implementation scheme, the ratio between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer is greater than 1 and less than or equal to 2.6; and / or the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer is greater than 0 and less than or equal to 0.2.

[0024] In the case of adopting the above technical solution, it can be understood that the semiconductor structure provided by the present invention is an intermediate structure or semi-finished product for manufacturing solar cells. Based on this, when the ratio between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer in the semiconductor structure provided by the present invention is greater than 1 and less than or equal to 2.6, the extinction coefficient k of the N-type doped polysilicon layer is greater than the extinction coefficient k of the P-type doped polysilicon layer, which is beneficial to make the extinction coefficient k of the N-type doped polysilicon layer in the solar cell manufactured based on the semiconductor structure provided by the present invention also greater than the extinction coefficient k of the P-type doped polysilicon layer. The beneficial effect that the extinction coefficient k of the N-type doped polysilicon layer in the solar cell is also greater than the extinction coefficient k of the P-type doped polysilicon layer can be referred to the previous text and will not be repeated here. Similarly, the beneficial effect when the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer is greater than 0 and less than or equal to 0.2 can be analyzed by referring to the beneficial effect analysis of the extinction coefficient k of the N-type doped polysilicon layer in the solar cell described above being greater than the extinction coefficient k of the P-type doped polysilicon layer.

[0025] In a third aspect, the present invention provides a method for manufacturing a solar cell, the method for manufacturing a solar cell comprising: first, providing a semiconductor substrate. The semiconductor substrate comprises a first region and a second region. The first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate, respectively. Next, a P-type doped polysilicon layer is formed at least on the first region. Next, an N-type doped polysilicon layer is formed at least on the second region. At least a portion of the N-type doped polysilicon layer and at least a portion of the P-type doped polysilicon layer are arranged at intervals. Wherein, the ratio between the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer is greater than or equal to 0.9 and less than or equal to 1.1; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.1.

[0026] The beneficial effects of the third aspect of the present invention can be analyzed by referring to the beneficial effects of the first aspect and its various implementations, and will not be repeated here.

[0027] As a possible implementation scheme, when the first region and the second region are located on the same surface of the semiconductor substrate, the forming of the P-type doped polysilicon layer at least on the first region includes: forming a first intrinsic polysilicon layer covering the first region and the second region; then, performing a diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer; then, selectively removing the portion of the P-type doped polysilicon layer located at least on a portion of the second region. Furthermore, the forming of the N-type doped polysilicon layer at least on the second region includes: forming a second intrinsic polysilicon layer covering at least the P-type doped polysilicon layer and the second region; then, performing a diffusion treatment on the second intrinsic polysilicon layer so that the second intrinsic polysilicon layer forms an N-type doped polysilicon layer; then, selectively removing the portion of the N-type doped polysilicon layer located on at least a portion of the P-type doped polysilicon layer;

[0028] Alternatively, the above-mentioned forming of an N-type doped polysilicon layer at least on the second region includes: forming a second intrinsic polysilicon layer covering the first region and the second region; then, performing a diffusion treatment on the second intrinsic polysilicon layer so that the second intrinsic polysilicon layer forms an N-type doped polysilicon layer; then, selectively removing a portion of the N-type doped polysilicon layer located at least on a portion of the first region. Furthermore, forming a P-type doped polysilicon layer at least on the first region includes: forming a first intrinsic polysilicon layer covering at least the N-type doped polysilicon layer and the first region; then, performing a diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer; then, selectively removing a portion of the P-type doped polysilicon layer located on at least a portion of the N-type doped polysilicon layer.

[0029] As a possible implementation scheme, in the case where the first region and the second region are respectively located on two opposite sides of the semiconductor substrate, the forming of the P-type doped polysilicon layer at least on the first region includes: forming a first intrinsic polysilicon layer at least covering the first region; then, performing a diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer. Furthermore, the forming of the N-type doped polysilicon layer at least on the second region includes: forming a second intrinsic polysilicon layer at least covering the second region; then, performing a diffusion treatment on the second intrinsic polysilicon layer so that the second intrinsic polysilicon layer forms an N-type doped polysilicon layer.

[0030] As a possible implementation scheme, the extinction coefficient k of the first intrinsic polysilicon layer is smaller than the extinction coefficient k of the P-type doped polysilicon layer. In this case, the first intrinsic polysilicon layer has a higher density than the P-type doped polysilicon layer, which is beneficial to prevent the impurities from passing through the first intrinsic polysilicon layer and entering the semiconductor substrate when the first intrinsic polysilicon layer is diffused, thereby preventing the problem of easy penetration or large internal diffusion range, thereby ensuring that the solar cell has a higher open circuit voltage and fill factor.

[0031] As a possible implementation scheme, the refractive index n of the first intrinsic polysilicon layer is greater than or equal to the refractive index n of the P-type doped polysilicon layer.

[0032] When the above technical solution is adopted, the refractive index n of the first intrinsic polysilicon layer and the refractive index n of the P-type doped polysilicon layer are related to the compactness of the film layer itself. Within a certain range, the refractive index n of the first intrinsic polysilicon layer and the P-type doped polysilicon layer is proportional to the compactness of the film layer. Based on this, when the refractive index n of the first intrinsic polysilicon layer is greater than or equal to the refractive index n of the P-type doped polysilicon layer, the first intrinsic polysilicon layer is relatively dense, which is conducive to preventing impurities from passing through the first intrinsic polysilicon layer and entering the semiconductor substrate when the first intrinsic polysilicon layer is diffused, resulting in easy penetration or a large internal expansion range, ensuring that the solar cell has a higher open circuit voltage and fill factor.

[0033] As a possible implementation scheme, the refractive index n of the second intrinsic polysilicon layer is smaller than the refractive index n of the N-type doped polysilicon layer.

[0034] In the case of adopting the above technical solution, the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the N-type doped polysilicon layer are also related to the compactness of the film layer itself. Within a certain range, the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the N-type doped polysilicon layer are proportional to the compactness of the film layer. In this case, when the refractive index n of the second intrinsic polysilicon layer is less than the refractive index n of the N-type doped polysilicon layer, before the diffusion treatment, the compactness of the second intrinsic polysilicon layer is low, which is conducive to doping N-type impurities into the second intrinsic polysilicon layer. After the diffusion treatment, the compactness of the N-type doped polysilicon layer becomes higher, which is conducive to preventing the electrode slurry for manufacturing the negative electrode from penetrating the N-type doped polysilicon layer, and is conducive to reducing the metal composite area between the N-type doped polysilicon layer and the negative electrode, thereby reducing the metal composite loss.

[0035] As a possible implementation scheme, the extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the N-type doped polysilicon layer. In this case, as mentioned above, within a certain range, the extinction coefficient k of the film layer is inversely proportional to its own density. Based on this, when the extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the N-type doped polysilicon layer, the density of the second intrinsic polysilicon layer is lower than the density of the N-type doped polysilicon layer. The beneficial effect of the density of the second intrinsic polysilicon layer being lower than the density of the N-type doped polysilicon layer can be referred to the above, and will not be repeated here.

[0036] As a possible implementation solution, the thickness of the second intrinsic polysilicon layer is smaller than the thickness of the first intrinsic polysilicon layer.

[0037] When the above technical solution is adopted, as mentioned above, the etching ability of the electrode slurry for manufacturing the positive electrode on the film layer is greater than the etching ability of the electrode slurry for manufacturing the negative electrode on the film layer. The first intrinsic polysilicon layer is used to manufacture the P-type doped polysilicon layer, and the second intrinsic polysilicon layer is used to manufacture the N-type doped polysilicon layer. In the above case, when the thickness of the second intrinsic polysilicon layer is less than the thickness of the first intrinsic polysilicon layer, it is beneficial to increase the thickness of the P-type doped polysilicon layer formed based on the first intrinsic polysilicon layer with a larger thickness, further reduce the risk of the electrode slurry for manufacturing the positive electrode penetrating the P-type doped polysilicon layer, ensure that the P-type polysilicon layer has a higher field passivation effect, and prevent the electrode slurry for manufacturing the positive electrode from damaging the semiconductor substrate.

[0038] As a possible implementation scheme, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is greater than or equal to 0.55 and less than or equal to 0.8; and / or the difference between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is greater than or equal to -140nm and less than or equal to -100nm.

[0039] In the case of adopting the above technical solution, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is within the above range, which can prevent the second intrinsic polysilicon layer from being too small and / or the first intrinsic polysilicon layer from being too large due to the smaller ratio; secondly, it can also prevent the second intrinsic polysilicon layer from being too large and / or the first intrinsic polysilicon layer from being too small due to the larger ratio. In summary, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is within the above range, which is conducive to reasonably setting the thickness of the first intrinsic polysilicon layer and the second intrinsic polysilicon layer, ensuring that there will be no problems of penetration and large internal expansion after diffusion treatment, and at the same time, the P-type doped polysilicon layer and the N-type doped polysilicon layer have a high matching with the electrode slurry used to manufacture the positive electrode and the negative electrode, respectively, ensuring that the P-type doped polysilicon layer and the N-type doped polysilicon layer both have a high field passivation effect.

[0040] As a possible implementation scheme, the refractive index n of the second intrinsic polysilicon layer is smaller than the refractive index n of the first intrinsic polysilicon layer.

[0041] When the above technical solution is adopted, as mentioned above, within a certain range, the refractive index n of the film layer is proportional to its own density. Based on this, when the refractive index n of the second intrinsic polysilicon layer is less than the refractive index n of the first intrinsic polysilicon layer, the first intrinsic polysilicon layer has a relatively high film density, which is conducive to preventing P-type impurities such as smaller boron atoms from diffusing through the first intrinsic polysilicon layer. In addition, larger N-type impurities such as phosphorus are doped into the second intrinsic polysilicon layer by substitutional diffusion. Since the substitutional diffusion method is that impurity atoms replace the positions of semiconductor atoms to form doped regions, when the density of the second intrinsic polysilicon layer is relatively low, it is conducive to the diffusion of larger N-type impurities such as phosphorus, reducing the difficulty of diffusion, and helping to increase the impurity doping concentration in the N-type doped polysilicon layer.

[0042] As a possible implementation scheme, the difference between the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the first intrinsic polysilicon layer is greater than or equal to -0.12 and less than or equal to -0.1.

[0043] As a possible implementation scheme, the extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the first intrinsic polysilicon layer. In this case, the density of the second intrinsic polysilicon layer is lower than the density of the first intrinsic polysilicon layer. The beneficial effects at this time can refer to the beneficial effects of the refractive index n of the second intrinsic polysilicon layer being lower than the refractive index n of the first intrinsic polysilicon layer as described above, which will not be repeated here.

[0044] As a possible implementation scheme, the difference between the extinction coefficients k of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is greater than or equal to 0.02 and less than or equal to 0.3.

[0045] As a possible implementation scheme, the formation temperature of the second intrinsic polysilicon layer is greater than the formation temperature of the first intrinsic polysilicon layer. In this case, when other factors are the same, the higher the formation temperature, the faster the deposition rate. Based on this, when the formation temperature of the second intrinsic polysilicon layer is greater than the formation temperature of the first intrinsic polysilicon layer, the material deposition rate of the second intrinsic polysilicon layer is faster, and the corresponding film layer density is lower, which is conducive to obtaining a second intrinsic polysilicon layer with a loose structure and a first intrinsic polysilicon layer with a dense structure, thereby reducing the size of N-type impurities such as phosphorus that are larger in size and are doped into the second intrinsic polysilicon layer in a substitutional diffusion manner, and at the same time, it is conducive to preventing the problem of penetration or a large internal expansion range after the P-type impurities such as boron atoms that are smaller in size are doped into the first intrinsic polysilicon layer in a gap diffusion manner.

[0046] As a possible implementation scheme, the formation time of the second intrinsic polysilicon layer is shorter than the formation time of the first intrinsic polysilicon layer.

[0047] When the above technical solution is adopted, under the condition that other factors are the same, the longer the formation time is, the thicker the film layer is. Based on this, when the formation time of the second intrinsic polysilicon layer is less than the formation time of the first intrinsic polysilicon layer, the greater the film thickness of the first intrinsic polysilicon layer is, the problem of penetration or a larger inward expansion range after diffusion is further prevented.

[0048] As a possible implementation scheme, the temperature when the first intrinsic polysilicon layer is diffused is higher than the temperature when the second intrinsic polysilicon layer is diffused.

[0049] As a possible implementation scheme, after forming a P-type doped polysilicon layer at least on the first region and forming an N-type doped polysilicon layer at least on the second region, the method for manufacturing a solar cell further includes: performing a passivation treatment on at least one side of the P-type doped polysilicon layer away from the semiconductor substrate and one side of the N-type doped polysilicon layer away from the semiconductor substrate to form a surface passivation layer covering at least one side of the P-type doped polysilicon layer away from the semiconductor substrate and one side of the N-type doped polysilicon layer away from the semiconductor substrate. After the passivation treatment, the ratio of the extinction coefficients k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is greater than or equal to 1.5 and less than or equal to 2.5.

[0050] As a possible implementation scheme, the ratio of the thickness of the P-type doped polysilicon layer after passivation treatment to the thickness of the P-type doped polysilicon layer before passivation treatment is greater than or equal to 0.95 and less than or equal to 1; and / or, the ratio of the refractive index n of the P-type doped polysilicon layer after passivation treatment to the refractive index n of the P-type doped polysilicon layer before passivation treatment is greater than or equal to 1 and less than or equal to 1.05; and / or, the ratio of the extinction coefficient k of the P-type doped polysilicon layer after passivation treatment to the extinction coefficient k of the P-type doped polysilicon layer before passivation treatment is greater than or equal to 0.95 and less than or equal to 1.

[0051] In the case of adopting the above technical solution, the thickness of the P-type doped polysilicon layer before and after the passivation treatment is roughly the same, which is beneficial to prevent the thickness of the P-type doped polysilicon layer from being greatly reduced after the passivation treatment, which causes the electrode slurry for manufacturing the negative electrode to easily penetrate the P-type doped polysilicon layer, ensuring that the P-type doped polysilicon layer has a higher passivation effect. In addition, when the ratio of the refractive index n of the P-type doped polysilicon layer after the passivation treatment to the refractive index n of the P-type doped polysilicon layer before the passivation treatment is greater than or equal to 1 and less than or equal to 1.05; and / or, when the ratio of the extinction coefficient k of the P-type doped polysilicon layer after the passivation treatment to the extinction coefficient k of the P-type doped polysilicon layer before the passivation treatment is greater than or equal to 0.95 and less than or equal to 1, the film density of the P-type doped polysilicon layer after the passivation treatment becomes larger, which is further beneficial to prevent the electrode slurry for manufacturing the negative electrode from penetrating the P-type doped polysilicon layer, ensuring that the P-type doped polysilicon layer has a higher passivation effect.

[0052] As a possible implementation scheme, the ratio between the thickness of the N-type doped polysilicon layer after passivation treatment and the thickness of the N-type doped polysilicon layer before passivation treatment is greater than or equal to 0.85 and less than or equal to 0.9; and / or, the ratio between the refractive index n of the N-type doped polysilicon layer after passivation treatment and the refractive index n of the N-type doped polysilicon layer before passivation treatment is greater than or equal to 0.3 and less than or equal to 1.1; and / or, the ratio between the extinction coefficient k of the N-type doped polysilicon layer after passivation treatment and the extinction coefficient k of the N-type doped polysilicon layer before passivation treatment is greater than or equal to 1.9 and less than or equal to 2.1.

[0053] When the above technical solution is adopted, the film thickness of the N-type doped polysilicon layer becomes smaller after the passivation treatment, which is beneficial to improve its own compactness, prevent the electrode slurry for manufacturing the positive electrode from penetrating the N-type doped polysilicon layer, and ensure that the N-type doped polysilicon layer has a high passivation effect. The beneficial effect of the ratio between the refractive index n of the N-type doped polysilicon layer after the passivation treatment and the refractive index n of the N-type doped polysilicon layer before the passivation treatment being greater than or equal to 0.3 and less than or equal to 1.1 is similar to the beneficial effect of the ratio between the thickness of the N-type doped polysilicon layer after the passivation treatment and the thickness of the N-type doped polysilicon layer before the passivation treatment being greater than or equal to 0.85 and less than or equal to 0.9, which will not be repeated here.

[0054] In a fourth aspect, the present invention provides a photovoltaic module, which includes the solar cell provided by the first aspect and various implementations thereof.

[0055] The beneficial effects of the fourth aspect of the present invention and its various implementations can be analyzed by referring to the beneficial effects of the first aspect and its various implementations, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0057] Figure 1 A schematic longitudinal cross-sectional view of a first structure of a solar cell provided by an embodiment of the present invention;

[0058] Figure 2 A schematic longitudinal cross-sectional view of a second structure of a solar cell provided by an embodiment of the present invention;

[0059] Figure 3 A schematic longitudinal cross-sectional view of a third structure of a solar cell provided by an embodiment of the present invention;

[0060] Figure 4 A schematic longitudinal cross-sectional view of a fourth structure of a solar cell provided by an embodiment of the present invention;

[0061] Figure 5 A schematic longitudinal cross-sectional view of a first structure of a semiconductor structure provided by an embodiment of the present invention;

[0062] Figure 6 A schematic longitudinal cross-sectional view of a second structure of a semiconductor structure provided by an embodiment of the present invention;

[0063] Figure 7 A schematic diagram of the structure of a semiconductor structure provided in an embodiment of the present invention during the manufacturing process Figure 1 ;

[0064] Figure 8 A schematic diagram of the structure of a semiconductor structure provided in an embodiment of the present invention during the manufacturing process Figure 2 ;

[0065] Fig. 9 A schematic diagram of the structure of a semiconductor structure provided in an embodiment of the present invention during the manufacturing process Figure 3 ;

[0066] Fig.10 A schematic diagram of the structure of a semiconductor structure provided in an embodiment of the present invention during the manufacturing process Figure 4 ;

[0067] Fig.11 A schematic diagram of the structure of a semiconductor structure provided in an embodiment of the present invention during the manufacturing process Figure 5 ;

[0068] Fig.12 A schematic diagram of the structure of a semiconductor structure provided in an embodiment of the present invention during the manufacturing process Figure 6 ;

[0069] Fig.13 A schematic diagram of a structure of a solar cell provided by an embodiment of the present invention during a manufacturing process;

[0070] Fig.14 A schematic longitudinal cross-sectional view of a fifth structure of a solar cell provided by an embodiment of the present invention.

[0071] Figure numerals: 11 is a semiconductor substrate, 12 is a P-type doped polysilicon layer, 13 is an N-type doped polysilicon layer, 14 is a surface passivation layer, 15 is a positive electrode, 16 is a negative electrode, 17 is a first tunneling passivation layer, 18 is a second tunneling passivation layer, 19 is a first intrinsic polysilicon layer, and 20 is a second intrinsic polysilicon layer. DETAILED DESCRIPTION

[0072] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.

[0073] Various structural schematic diagrams according to embodiments of the present disclosure are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may further design regions / layers with different shapes, sizes, and relative positions according to actual needs.

[0074] In the context of the present disclosure, when a layer / element is referred to as being "on" another layer / element, the layer / element may be directly on the other layer / element, or there may be an intermediate layer / element between them. In addition, if a layer / element is "on" another layer / element in one orientation, then when the orientation is reversed, the layer / element may be "under" the other layer / element. In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0075] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0076] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0077] A solar cell is a device that can convert sunlight into electrical energy. Specifically, when a solar cell is in operation, sunlight shines on the semiconductor pn junction of the solar cell, forming new hole-electron pairs. Under the action of the built-in electric field of the pn junction, photogenerated holes flow to the p region and photogenerated electrons flow to the n region. When the circuit is connected, current can be generated.

[0078] However, in existing solar cells, the N-type doped polysilicon layer and the P-type doped polysilicon layer have different refraction effects on light, which makes it difficult to ensure the balance of electrons and holes, and is not conducive to improving the working efficiency of solar cells.

[0079] In order to solve the above technical problems, in a first aspect, an embodiment of the present invention provides a solar cell. Figures 1 to 4 ,as well as Fig.14 As shown, the solar cell provided by the embodiment of the present invention includes: a semiconductor substrate 11, a P-type doped polysilicon layer 12 and an N-type doped polysilicon layer 13. The semiconductor substrate 11 includes a first region and a second region. The first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate respectively. The N-type doped polysilicon layer 13 is formed at least on the second region. At least a portion of the N-type doped polysilicon layer 13 and at least a portion of the P-type doped polysilicon layer 12 are arranged at intervals from each other. Among them, the ratio between the refractive index n of the N-type doped polysilicon layer 13 and the refractive index n of the P-type doped polysilicon layer 12 is greater than or equal to 0.9 and less than or equal to 1.1; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer 12 and the refractive index n of the N-type doped polysilicon layer 13 is greater than or equal to 0 and less than or equal to 0.1.

[0080] Specifically, in actual application, the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer can be measured and obtained by testing instruments such as an ellipsometer. In the process of testing the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer, it is necessary to remove other film layers (such as doped silicon glass layer and / or surface passivation layer, etc.) located on the side of the N-type doped polysilicon layer away from the semiconductor substrate and located on the side of the P-type doped polysilicon layer away from the semiconductor substrate; and it is also necessary to measure under the same test conditions, especially different film layers that need to be compared need to be measured under the same test conditions to improve the accuracy of the measurement results and the accuracy of the comparison results.

[0081] When the above technical solution is adopted, Figures 1 to 4As shown, one of the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13 can form a high-low junction with the semiconductor substrate 11, and the other can form a PN junction with the semiconductor substrate 11. Based on this, when the solar cell is in a working state, the semiconductor substrate 11 can form new hole-electron pairs after absorbing photons. Under the action of the built-in electric field of the above-mentioned PN junction and the high-low junction, the photogenerated holes flow to the P-type doped polysilicon layer 12, and the photogenerated electrons flow to the N-type doped polysilicon layer 13, and current can be generated after the circuit is connected. Secondly, in addition to being able to collect and transmit the electrons and holes generated in the semiconductor substrate 11 respectively, the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 can also generate a part of the electron-hole pairs after absorbing photons for power generation. Furthermore, after the light enters the semiconductor substrate 11 from the light-facing side of the solar cell corresponding to the semiconductor substrate 11, part of the light will pass through the semiconductor substrate 11 and reach the interface between the semiconductor substrate 11 and the N-type doped polysilicon layer 13, or the interface between the semiconductor substrate 11 and the P-type doped polysilicon layer 12. At this time, the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 can reflect part of the light, so that the semiconductor substrate 11 absorbs light energy for a second time, generates more electron and hole pairs, and improves the utilization rate of the light by the semiconductor substrate 11. In the above case, when the ratio between the refractive index n of the N-type doped polysilicon layer 13 and the refractive index n of the P-type doped polysilicon layer 12 is within the above range, the refractive indexes n of the two are approximately equal, so that the refractive effects of the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 on the light are approximately the same, which is conducive to ensuring the balance of electrons and holes and improving the working efficiency of the solar cell. In addition, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer 12 and the refractive index n of the N-type doped polysilicon layer 13 is greater than or equal to 0 and less than or equal to 0.1. The beneficial effects in this case can refer to the beneficial effects when the ratio of the refractive index n of the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 is greater than or equal to 0.9 and less than or equal to 1.1 as described above, and will not be repeated here.

[0082] Specifically, if Fig.14 As shown, the solar cell provided in the embodiment of the present invention may be a double-sided contact solar cell, in which case the positive electrode 15 and the negative electrode 16 included in the solar cell are respectively arranged on the light-facing side and the backlight side of the solar cell. Figures 1 to 4 As shown, the solar cell provided in the embodiment of the present invention may also be a back contact cell, in which case the positive electrode 15 and the negative electrode 16 included in the solar cell are spaced apart and arranged on the backlight side of the solar cell.

[0083] As for the semiconductor substrate, the semiconductor substrate may be any semiconductor substrate such as a silicon substrate, a silicon germanium substrate, a germanium substrate or a gallium arsenide substrate.

[0084] Secondly, because the P-type doped polysilicon layer is formed at least on the first region and the N-type doped polysilicon layer is formed at least on the second region, the relative positional relationship between the first region and the second region will affect the relative positional relationship between the P-type doped polysilicon layer and the N-type doped polysilicon layer. Based on this, the relative positional relationship between the first region and the second region included in the semiconductor substrate can be determined according to the type of solar cell.

[0085] For example: Fig.14 As shown, when the solar cell provided by the embodiment of the present invention is a double-sided contact cell, the first region and the second region are respectively located on two opposite sides of the semiconductor substrate (i.e., the first side and the second side); specifically, the first side of the semiconductor substrate corresponds to the backlight side of the solar cell, and the second side of the semiconductor substrate corresponds to the light-facing side of the solar cell. In this case, the first region may be located on the first side of the semiconductor substrate, and the second region may be located on the second side of the semiconductor substrate; or, the first region may be located on the second side of the semiconductor substrate, and the second region may be located on the first side of the semiconductor substrate. Specifically, the first region and / or the second region may be distributed on the entire surface of the corresponding surface of the semiconductor substrate, or may be distributed locally on the corresponding surface, for example, there are multiple first regions and / or second regions, and intervals are set between adjacent first regions or adjacent second regions.

[0086] For another example, when the solar cell provided by the embodiment of the present invention is a back contact cell, the first region and the second region are located on the same side of the semiconductor substrate, that is, on the side of the semiconductor substrate corresponding to the backlight surface of the solar cell. In this case, the boundary between the first region and the second region included in the semiconductor substrate is a virtual boundary. The embodiment of the present invention does not specifically limit the distribution manner between the first region and the second region, as long as it can be applied to the solar cell provided by the embodiment of the present invention. For example: the first region and the second region may be alternately distributed. For another example: one of the first region and the second region may surround the other. For another example: the first region and the second region are respectively in a shape similar to a Chinese character 'feng' with alternately distributed finger-like parts. Secondly, since the P-type doped polysilicon layer is formed on the first region, the range of the first region in the corresponding surface can be determined according to the formation range of the P-type doped polysilicon layer included in the solar cell in the actual application scenario. Since the N-type doped polysilicon layer is at least formed on the second region, the range of the second region in the corresponding surface can be determined according to the range of the part of the N-type doped polysilicon layer included in the solar cell corresponding to the semiconductor substrate in the actual application scenario. Specifically, the corresponding surface of the semiconductor substrate may only include the first region and the second region; or, in addition to the first region and the second region, the corresponding surface of the semiconductor substrate may further include a spacer region, and the spacer region is located between the first region and the adjacent second region. The embodiment of the present invention does not specifically limit the width of the spacer region, as long as it can be applied to the solar cell provided by the embodiment of the present invention.

[0087] For the above-mentioned P-type doped polysilicon layer and N-type doped polysilicon layer, in terms of the formation position, as Figure 1 shown, the P-type doped polysilicon layer 12 can be directly formed on the first region included in the semiconductor substrate 11. Or, as Figure 2 shown, the above-mentioned solar cell may further include a first tunneling passivation layer 17, and the first tunneling passivation layer 17 is located between the P-type doped polysilicon layer 12 and the semiconductor substrate 11. In this case, the first tunneling passivation layer 17 and the P-type doped polysilicon layer 12 can form a tunneling passivation contact structure to chemically passivate the first region of the semiconductor substrate 11 and selectively collect holes, reduce the carrier recombination rate on the side of the semiconductor substrate where the first tunneling passivation layer 17 is formed, and is beneficial to improving the photoelectric conversion efficiency of the solar cell. Among them, the embodiment of the present invention does not specifically limit the material and thickness of the first tunneling passivation layer 17. Exemplarily, the material of the first tunneling passivation layer 17 may include one or more of silicon oxide, aluminum oxide, titanium oxide, hafnium dioxide, gallium oxide, tantalum pentoxide, niobium pentoxide, silicon nitride, silicon carbonitride, aluminum nitride, titanium nitride, titanium carbonitride. The thickness of the first tunneling passivation layer 17 may be greater than or equal to 0.5 nm and less than or equal to 5 nm.

[0088] As for the N-type doped polysilicon layer, Figure 1 As shown, the N-type doped polysilicon layer 13 can be directly formed on at least the second region included in the semiconductor substrate 11 (e.g., the N-type doped polysilicon layer 13 can be formed only on the second region, or the N-type doped polysilicon layer 13 can be formed on the second region and a portion of the first region, or the N-type doped polysilicon layer 13 can be formed on the second region and a portion of the P-type doped polysilicon layer 12. The specific formation range of the N-type doped polysilicon layer 13 is described in detail below and will not be repeated here). Or, Figure 2 As shown, the solar cell may further include a second tunneling passivation layer 18, which is at least located between the N-type doped polysilicon layer 13 and the semiconductor substrate 11. In this case, the second tunneling passivation layer 18 and the N-type doped polysilicon layer 13 may constitute a tunneling passivation contact structure to chemically passivate the second region included in the semiconductor substrate 11 and selectively collect electrons, thereby reducing the carrier recombination rate on the side of the semiconductor substrate where the second tunneling passivation layer 18 is formed, and is beneficial to improving the photoelectric conversion efficiency of the solar cell. It can be understood that the formation range of the second tunneling passivation layer changes with the change of the formation range of the N-type doped polysilicon layer 13, and the second tunneling passivation layer 18 is arranged on the side of the N-type doped polysilicon layer 13 close to the semiconductor substrate. Specifically, the second tunneling passivation layer 18 is arranged between the N-type doped polysilicon layer 13 and the structure in contact with itself. Secondly, the material and thickness of the second tunneling passivation layer 18 may refer to the material and thickness of the first tunneling passivation layer 17 mentioned above. Specifically, the material of the second tunnel passivation layer 18 may be the same as or different from the material of the first tunnel passivation layer 17. The thickness of the second tunnel passivation layer 18 may be the same as or different from the thickness of the first tunnel passivation layer 17.

[0089] In terms of the formation range, when the first region and the second region are located on opposite sides of the semiconductor substrate, the P-type doped polysilicon layer can be distributed with the N-type doped polysilicon layer through the side of the semiconductor substrate. The P-type doped polysilicon layer can be formed only on the first region, and the N-type doped polysilicon layer can be formed only on the second region. In special cases, the P-type doped polysilicon layer and the N-type doped polysilicon layer can be formed by contacting at a local preset position on the side of the semiconductor substrate, and distributed at intervals outside the local preset position on the side of the semiconductor substrate; forming a local leakage point effectively reduces the reverse breakdown voltage of the battery cell and enhances the solar cell's ability to resist hot spot risks.

[0090] In the case where the first region and the second region are located on the same surface of the semiconductor substrate, the P-type doped polysilicon layer can be formed only on the first region; or, the P-type doped polysilicon layer is not only formed on the first region, but also can be formed on part of the second region (in the case where the corresponding surface of the semiconductor substrate includes the first region, the second region and the spacing region, the P-type doped polysilicon layer can be formed not only on the first region, but also on part of the spacing region and / or part of the second region). Wherein, when the P-type doped polysilicon layer is also formed on part of the second region, the relative positional relationship between the portion of the P-type doped polysilicon layer corresponding to the second region and the N-type doped polysilicon layer can be determined according to the actual manufacturing process. For example: when the formation sequence of the P-type doped polysilicon layer is after the N-type doped polysilicon layer, the portion of the P-type doped polysilicon layer corresponding to the second region is located on the N-type doped polysilicon layer; when the formation sequence of the P-type doped polysilicon layer is before the N-type doped polysilicon layer, the portion of the P-type doped polysilicon layer corresponding to the second region is located below the N-type doped polysilicon layer.

[0091] As for the N-type doped polysilicon layer in the case where the first region and the second region are located on the same surface of the semiconductor substrate, the N-type doped polysilicon layer can be formed only on the second region; or, the N-type doped polysilicon layer is not only located on the second region, but can also be formed on part of the first region (in the case where the corresponding surface of the semiconductor substrate includes the first region, the second region and the spacing region, the N-type doped polysilicon layer can be formed not only on the second region, but also on part of the spacing region and / or part of the first region). The portion of the N-type doped polysilicon layer corresponding to the first region can be located above the portion of the P-type doped polysilicon layer facing away from the semiconductor substrate, or the portion of the N-type doped polysilicon layer corresponding to the first region can also be located below the P-type doped polysilicon layer, and the relative position between the two can be determined according to the actual manufacturing process.

[0092] Secondly, when the first region and the second region are located on the same surface of the semiconductor substrate, the entire region of the N-type doped polysilicon layer and the entire region of the P-type doped polysilicon layer may be spaced apart from each other; or, only a portion of the N-type doped polysilicon layer and only a portion of the P-type doped polysilicon layer may be spaced apart from each other, so as to reduce the risk of hot spots through the local electrical contact between the N-type doped polysilicon layer and the P-type doped polysilicon layer, and improve the working reliability of the photovoltaic module including the solar cell provided by the embodiment of the present invention. Specifically, when only a portion of the N-type doped polysilicon layer and only a portion of the P-type doped polysilicon layer are spaced apart from each other, the range, position and distribution of the local electrical contact between the N-type doped polysilicon layer and the P-type doped polysilicon layer may be set according to actual needs, and are not specifically limited here. In addition, the portions of the N-type doped polysilicon layer and the P-type doped polysilicon layer that need to be spaced apart may be separated by the spacing region described above, or may be separated by an insulating material or an intrinsic semiconductor material.

[0093] In terms of film thickness, the embodiment of the present invention does not specifically limit the thickness of the P-type doped polysilicon layer and the N-type doped polysilicon layer. Preferably, the thickness of the N-type doped polysilicon layer is less than the thickness of the P-type doped polysilicon layer. In this case, the first intrinsic polysilicon layer used to manufacture the P-type doped polysilicon layer is usually subjected to boron diffusion to form the P-type doped polysilicon layer, and the size of the boron atoms is relatively small, and the corresponding diffusion method is gap diffusion. Therefore, when the thickness of the P-type doped polysilicon layer is large, it is helpful to reduce the problem of large expansion or internal expansion of the P-type doped polysilicon layer after the diffusion treatment. Secondly, in the case where the solar cell also includes a first tunneling passivation layer, the first tunneling passivation layer can also be prevented from being affected by the expansion, ensuring that the first tunneling passivation layer has good passivation performance.

[0094] The difference or ratio between the thickness of the N-type doped polysilicon layer and the thickness of the P-type doped polysilicon layer, as well as the specific values ​​of the thicknesses of the two layers can be determined according to actual application scenarios.

[0095] Exemplarily, the difference between the thickness of the N-type doped polysilicon layer and the thickness of the P-type doped polysilicon layer may be greater than or equal to -140nm, and less than or equal to -100nm. For example, the difference between the thickness of the N-type doped polysilicon layer and the thickness of the P-type doped polysilicon layer may be -140nm, -130nm, -120nm, -110nm, -105nm or -100nm, etc.

[0096] Exemplarily, the thickness of the N-type doped polysilicon layer may be greater than or equal to 100 nm and less than or equal to 240 nm. For example, the thickness of the N-type doped polysilicon layer may be 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm nm or 240 nm.

[0097] Exemplarily, the thickness of the P-type doped polysilicon layer may be greater than or equal to 150 nm and less than or equal to 340 nm. For example, the thickness of the P-type doped polysilicon layer may be 150 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm or 340 nm.

[0098] From the doping aspect, the embodiment of the present invention does not specifically limit the doping type, doping concentration and doping depth of impurities in the P-type doped polysilicon layer and the N-type doped polysilicon layer, as long as they can be applied to the solar cell provided by the embodiment of the present invention.

[0099] Preferably, the impurities in the N-type doped polysilicon layer may include phosphorus, and the impurities in the P-type doped polysilicon layer may include boron. The size of phosphorus atoms is relatively large, and they are usually doped into the second intrinsic polysilicon layer used to manufacture the N-type doped polysilicon layer by substitutional diffusion. The size of boron atoms is relatively small, and they are usually doped into the first intrinsic polysilicon layer used to manufacture the P-type doped polysilicon layer by interstitial diffusion.

[0100] Preferably, the doping concentration of impurities in the N-type doped polysilicon layer can be greater than the doping concentration of impurities in the P-type doped polysilicon layer. It can be understood that, under the limitation of factors such as doping solid concentration, the doping concentration of impurities in the P-type doped polysilicon layer is limited. Therefore, when the doping concentration of impurities in the N-type doped polysilicon layer is greater than the doping concentration of impurities in the P-type doped polysilicon layer, it is beneficial to reduce the doping difficulty of the P-type doped polysilicon layer, while ensuring that the N-type doped polysilicon layer has a higher field passivation effect and a lower contact resistance between itself and the negative electrode. Specifically, when the doping concentration of impurities in the N-type doped polysilicon layer is greater than the doping concentration of impurities in the P-type doped polysilicon layer, the ratio or difference of the doping concentrations between the two can be determined according to the actual application scenario.

[0101] For example, the ratio between the doping concentration of the impurities in the N-type doped polysilicon layer and the doping concentration of the impurities in the P-type doped polysilicon layer may be greater than or equal to 5 and less than or equal to 10.

[0102] Preferably, the impurity doping depth corresponding to the P-type doped polysilicon layer may be greater than the impurity doping depth corresponding to the N-type doped polysilicon layer. In this case, the contact area between the two can be increased by increasing the etching depth of the electrode slurry corresponding to the positive electrode on the P-type doped polysilicon layer, thereby reducing the contact resistance between the two.

[0103] From the perspective of the optical parameters of the film layer, the numerical values ​​of the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer are not specifically limited, as long as they can be applied to the solar cell provided in the embodiment of the present invention. Specifically, as described in the text, the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer are related to the compactness of the film layer itself, thereby affecting its own resistance to etching of the electrode slurry. In addition, operations such as passivation treatment during the manufacturing process of the solar cell will affect the compactness and extinction coefficient k of the film layer. Based on this, the difference and ratio between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer, as well as the specific sizes of the two can be determined according to the specific structure of the solar cell and the etching ability of the electrode slurry corresponding to the positive electrode and the negative electrode in the actual application scenario.

[0104] Exemplarily, the extinction coefficient k of the N-type doped polysilicon layer may be greater than the extinction coefficient k of the P-type doped polysilicon layer.

[0105] Specifically, in actual application, the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer can be measured and obtained by testing instruments such as ellipsometers. In the process of testing the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer, it is necessary to remove other film layers (such as doped silicon glass layer and / or surface passivation layer, etc.) located on the side of the N-type doped polysilicon layer away from the semiconductor substrate and located on the side of the P-type doped polysilicon layer away from the semiconductor substrate; and it is also necessary to measure under the same test conditions, especially different film layers that need to be compared need to be measured under the same test conditions to improve the accuracy of the measurement results and the accuracy of the comparison results.

[0106] When the above technical solution is adopted, Figures 1 to 4As shown, due to the different conductivity types of the carriers to be collected by the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13, the corresponding electrode paste for manufacturing the positive electrode 15 electrically connected to the P-type doped polysilicon layer 12 and the electrode paste for manufacturing the negative electrode 16 electrically connected to the N-type doped polysilicon layer 13 usually have different compositions (wherein, the different compositions of the electrode paste corresponding to the positive electrode 15 and the electrode paste corresponding to the negative electrode 16 may refer to that the composition and / or content of the additives in the paste are not completely the same. For example, the content of the glass body in the electrode paste corresponding to the positive electrode 15 is different from the content of the glass body in the electrode paste corresponding to the negative electrode 16; or the conductive components in the paste are not completely the same, for example: the conductive components in the electrode paste corresponding to the positive electrode 15 may be silver and aluminum, while the component of the electrode paste corresponding to the negative electrode 16 is silver), so as to ensure that the positive electrode 15 has a higher hole transfer rate and the negative electrode 16 has a higher electron transfer rate. However, the film etching capabilities of the positive electrode 15 and the negative electrode 16 with different conventional slurry compositions are different. The etching depth of the positive electrode 15 of the film with the same density is much deeper than that of the negative electrode 16, and the positive electrode 15 has a greater risk of burn-through. By adjusting the density of the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13, the P-type doped polysilicon layer 12 is made denser, the etching resistance of the positive electrode is increased, and the etching depth of the positive electrode is reduced, so that the positive electrode stays at a suitable depth. In addition, the extinction coefficient k of the N-type doped polysilicon layer 13 and the extinction coefficient k of the P-type doped polysilicon layer 12 are related to the density of the film itself. Within a certain range, the extinction coefficient k of the N-type doped polysilicon layer 13 and the extinction coefficient k of the P-type doped polysilicon layer 12 are inversely proportional to the density of the film itself. Based on this, the density of the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 can be controlled by adjusting the size relationship of the extinction coefficient k values ​​of the above two film layers, and the extinction coefficient k of the N-type doped polysilicon layer 13 is set to be greater than the extinction coefficient k of the P-type doped polysilicon layer 12, so that the P-type doped polysilicon layer 12 has a relatively high density, and then the P-type doped polysilicon layer 12 has a relatively high ability to resist electrode slurry etching, preventing the manufactured positive electrode 15 from penetrating the P-type doped polysilicon layer 12, improving the matching between the electrode slurries corresponding to the P-type doped polysilicon layer 12 and the positive electrode 15, and ensuring that the P-type doped polysilicon layer 12 has a high field passivation effect, reducing the carrier recombination rate on the backlight side, and improving the working performance of the solar cell.

[0107] For example, Figure 1 and Figure 2As shown, in the case where the solar cell further includes a surface passivation layer 14, and the surface passivation layer 14 covers at least the side of the P-type doped polysilicon layer 12 away from the semiconductor substrate 11, and the side of the N-type doped polysilicon layer 13 away from the semiconductor substrate 11, the ratio between the extinction coefficient k of the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 can be greater than or equal to 1.5 and less than or equal to 2.5; and / or, the difference between the extinction coefficient k of the N-type doped polysilicon layer 13 and the extinction coefficient k of the P-type doped polysilicon layer 12 can be greater than or equal to 0.2 and less than or equal to 0.5.

[0108] For example, when the solar cell further includes a surface passivation layer, the ratio of the extinction coefficient k of the N-type doped polysilicon layer to the extinction coefficient k of the P-type doped polysilicon layer may be 1.5, 1.8, 1.85, 1.9, 1.95, 2.0, 2.05, 2.1, 2.2, 2.3, 2.4 or 2.5, etc. For example, when the solar cell further includes a surface passivation layer, the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer may be 0.2, 0.3, 0.32, 0.34, 0.36, 0.38, 0.4, 0.45 or 0.5, etc.

[0109] When the above technical solution is adopted, the ratio of the extinction coefficient k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is within the above range, so as to prevent the film layer of the N-type doped polysilicon layer from being too loose due to the large ratio, so that the negative electrode can easily penetrate the N-type doped polysilicon layer, and ensure that the N-type doped polysilicon layer has a high field passivation effect. In addition, when the first region and the second region are located on the same surface or the first region is located in a part of a certain surface, it can also prevent the film layer of the P-type doped polysilicon layer from being too dense due to the large ratio, so that the etching difficulty of the entire deposited P-type doped polysilicon layer during patterning is large and the etching efficiency is low, thereby reducing the difficulty of manufacturing solar cells and improving the manufacturing efficiency of solar cells. At the same time, it can also prevent the contact area between the positive electrode and the P-type doped polysilicon layer from being small due to the P-type doped polysilicon layer being too dense, so as to ensure that the positive electrode and the negative electrode have a small contact resistance. In addition, when the ratio of the extinction coefficients k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is within the above range, it can also prevent the density of the P-type doped polysilicon layer from being improved to a small extent due to the small ratio, thereby ensuring that the positive electrode does not penetrate the P-type doped polysilicon layer, and at the same time, it is beneficial to reduce the metal composite loss between the positive electrode and the P-type doped polysilicon layer, thereby ensuring that the solar cell has a higher working performance.

[0110] Exemplarily, the extinction coefficient k of the P-type doped polysilicon layer may be greater than or equal to 0.20 and less than or equal to 0.40. For example, the extinction coefficient k of the P-type doped polysilicon layer may be 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39 or 0.40, etc.

[0111] Exemplarily, the extinction coefficient k of the N-type doped polysilicon layer may be greater than or equal to 0.50 and less than or equal to 0.74. For example, the extinction coefficient k of the N-type doped polysilicon layer may be 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73 or 0.74, etc.

[0112] It should be noted that, as mentioned above, when other film layers are formed on the side of the P-type doped polysilicon layer away from the semiconductor substrate and the side of the N-type doped polysilicon layer away from the semiconductor substrate, it is necessary to remove the other film layers formed on the side of the P-type doped polysilicon layer away from the semiconductor substrate and the side of the N-type doped polysilicon layer away from the semiconductor substrate; then, under the same test conditions, the extinction coefficient k of the P-type doped polysilicon layer and the N-type doped polysilicon layer is measured by a test instrument such as an ellipsometer to improve the accuracy of the comparison result. For example: when the above-mentioned surface passivation layer is formed on the side of the P-type doped polysilicon layer away from the semiconductor substrate and the side of the N-type doped polysilicon layer away from the semiconductor substrate, it is necessary to remove the surface passivation layer, and then test the extinction coefficient k of the P-type doped polysilicon layer and the N-type doped polysilicon layer under the same test conditions.

[0113] In addition, in the actual application process, the optical parameters corresponding to the N-type doped polysilicon layer and the P-type doped polysilicon layer include not only the extinction coefficient k, but also the refractive index n and other parameters. Among them, the refractive index n value of the N-type doped polysilicon layer and the P-type doped polysilicon layer is also related to the density of the film layer; specifically, within a certain range, the refractive index n value corresponding to the N-type doped polysilicon layer and the P-type doped polysilicon layer is proportional to the density of the film layer. Secondly, as mentioned above, in addition to being able to collect and transmit electrons and holes generated in the semiconductor substrate respectively, the N-type doped polysilicon layer and the P-type doped polysilicon layer can also generate a part of electron-hole pairs after absorbing photons for power generation. Moreover, after the light enters the semiconductor substrate from the semiconductor substrate and the side corresponding to the light-facing surface of the solar cell, part of the light will pass through the semiconductor substrate to reach the interface between the semiconductor substrate and the N-type doped polysilicon layer, or the interface between the semiconductor substrate and the P-type doped polysilicon layer. At this time, the N-type doped polysilicon layer and the P-type doped polysilicon layer can reflect part of the light, so that the semiconductor substrate absorbs light energy for a second time, generates more electron and hole pairs, and improves the utilization rate of the semiconductor substrate for light. Based on this, the refractive index n of the N-type doped polysilicon layer and the P-type doped polysilicon layer reflects the refractive ability of the two film layers to light, thereby affecting the amount of light reflected back into the semiconductor substrate through the two film layers. In the above case, the specific size of the refractive index of the two can be determined according to the compactness of the N-type doped polysilicon layer and the P-type doped polysilicon layer in the actual application scenario, as well as the requirements for the reflection and refraction of light.

[0114] Wherein, the ratio between the refractive index n of the N-type doped polysilicon layer and the P-type doped polysilicon layer can be any value greater than or equal to 0.9 and less than or equal to 1.1. For example, the ratio between the refractive index n of the N-type doped polysilicon layer and the P-type doped polysilicon layer can be 0.9, 0.92, 0.94, 0.96, 0.98, 1.0, 1.02, 1.04, 1.06 or 1.1, etc. In the above case, when the ratio between the refractive index n of the N-type doped polysilicon layer and the P-type doped polysilicon layer is within the above range, the refractive index n of the two is approximately equal, so that the refraction effect of the N-type doped polysilicon layer and the P-type doped polysilicon layer on light is approximately the same, which is conducive to ensuring the balance of electrons and holes and improving the working efficiency of solar cells.

[0115] The absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer can be any value greater than or equal to 0 and less than or equal to 0.1. For example, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer can be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1. In the above case, when the ratio between the refractive index n of the N-type doped polysilicon layer and the P-type doped polysilicon layer is within the above range, the refractive index n of the two is approximately equal, so that the refractive effect of the N-type doped polysilicon layer and the P-type doped polysilicon layer on light is approximately the same, which is conducive to ensuring the balance of electrons and holes and improving the working efficiency of the solar cell. The smaller the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer, the better the effect. In addition, by adjusting the extinction coefficient k, the difference in thickness between the P-type doped polysilicon layer and the N-type doped polysilicon layer is reduced. The smaller the difference in thickness between the P-type doped polysilicon layer and the N-type doped polysilicon layer, the smaller the absolute value of the difference between the actual refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer, and the higher the battery efficiency.

[0116] Exemplarily, the refractive index n of the P-type doped polysilicon layer may be greater than or equal to 1 and less than or equal to 3.96. For example, the refractive index n of the P-type doped polysilicon layer may be 1, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 3.9, 3.91, 3.92, 3.93, 3.94, 3.95 or 3.96, etc.

[0117] Exemplarily, the refractive index n of the N-type doped polysilicon layer may be greater than or equal to 1 and less than or equal to 4. For example, the refractive index n of the N-type doped polysilicon layer may be 1, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 3.9, 3.98, 3.982, 3.984, 3.986, 3.988, 3.990, 3.995 or 4, etc.

[0118] In actual application, Figure 3 and Figure 4As shown, the solar cell also includes a positive electrode 15 in ohmic contact with the P-type doped polysilicon layer 12, and a negative electrode 16 in ohmic contact with the N-type doped polysilicon layer 13. The materials of the positive electrode 15 and the negative electrode 16 may include any conductive material such as silver, aluminum, copper, titanium or nickel. Specifically, in the actual manufacturing process, because the electrode slurry for manufacturing the positive electrode 15 and the negative electrode 16 has certain etching characteristics, after the positive electrode 15 and the negative electrode 16 are formed, the two will extend along the thickness of the semiconductor substrate 11 to a certain depth in the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13. The size of the depth is not only related to the etching characteristics of the electrode slurry, but also to factors such as the film density of the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13. At the same time, the size of the depth will also affect the contact area between the positive electrode 15 and the negative electrode 16 and the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13, respectively, and thus affect the contact resistance. Based on this, the depth to which the positive electrode 15 extends into the P-type doped polysilicon layer 12 and the depth to which the negative electrode 16 extends into the N-type doped polysilicon layer 13 can be determined according to the ability of the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13 to resist electrode slurry etching in the actual application scenario and the requirements for contact resistance.

[0119] For example, Figure 3 and Figure 4 As shown, along the thickness of the semiconductor substrate 11, the depth to which at least a portion of the positive electrode 15 extends into the P-type doped polysilicon layer 12 may be greater than or equal to the depth to which at least a portion of the negative electrode 16 extends into the N-type doped polysilicon layer 13. In this case, when the depth to which at least a portion of the positive electrode 15 extends into the P-type doped polysilicon layer 12 is greater than or equal to the depth to which at least a portion of the negative electrode 16 extends into the N-type doped polysilicon layer 13, it is beneficial to increase the contact area corresponding to the portion of the positive electrode 15 extending into the P-type doped polysilicon layer 12 to which the depth is greater, thereby facilitating a smaller contact resistance between the positive electrode 15 and the P-type doped polysilicon layer 12, facilitating a reduction in the transmission loss of holes from the P-type doped polysilicon layer 12 to the positive electrode 15, and further improving the working performance of the solar cell. In addition, in actual application, due to factors such as the limitation of doping solid concentration, the impurity doping concentration in the P-type doped polysilicon layer 12 is often lower than the impurity doping concentration in the N-type doped polysilicon layer 13. Therefore, when at least part of the positive electrode 15 extends to a depth greater than or equal to a depth of at least part of the negative electrode 16 extending to the N-type doped polysilicon layer 13, it is also beneficial to prevent the metal composite area between the N-type doped polysilicon layer 13 and the negative electrode 16 from being larger due to the larger contact area between the two, thereby ensuring that there is a smaller composite loss between the N-type doped polysilicon layer 13 and the negative electrode 16.

[0120] Exemplarily, along the thickness direction of the semiconductor substrate, the depth to which at least part of the positive electrode extends into the P-type doped polysilicon layer may be greater than or equal to 80 nm and less than or equal to 100 nm. For example: along the thickness direction of the semiconductor substrate, the depth to which at least part of the positive electrode extends into the P-type doped polysilicon layer may be 80 nm, 85 nm, 90 nm, 95 nm or 100 nm, etc. In this case, along the thickness direction of the semiconductor substrate, the depth to which at least part of the positive electrode extends into the P-type doped polysilicon layer is within the above range, which is conducive to preventing the contact area between the positive electrode and the P-type doped polysilicon layer from being small due to the small depth, and is conducive to reducing the contact resistance between the positive electrode and the P-type doped polysilicon layer. In addition, it is also conducive to preventing the contact area between the positive electrode and the P-type doped polysilicon layer from being too large due to the large depth, and is conducive to reducing the metal composite loss between the positive electrode and the P-type doped polysilicon layer. In summary, the depth of the positive electrode extending into the P-type doped polysilicon layer is within the above range, which is conducive to balancing the contact resistance and metal composite loss between the positive electrode and the P-type doped polysilicon layer, ensuring that the solar cell has high working performance.

[0121] Exemplarily, along the thickness direction of the semiconductor substrate, the depth to which at least part of the negative electrode extends into the N-type doped polysilicon layer may be greater than or equal to 50 nm and less than or equal to 80 nm. For example, the depth to which at least part of the negative electrode extends into the N-type doped polysilicon layer may be 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm or 80 nm, etc. The beneficial effects in this case are similar to the beneficial effects described above that at least part of the positive electrode extends into the P-type doped polysilicon layer to a depth greater than or equal to 80 nm and less than or equal to 100 nm, and will not be described in detail herein.

[0122] In a second aspect, an embodiment of the present invention provides a semiconductor structure. Figure 5 and Figure 6 As shown, the semiconductor structure includes: a semiconductor substrate 11, a P-type doped polysilicon layer 12 and an N-type doped polysilicon layer 13. The semiconductor substrate 11 includes a first region and a second region. The first region and the second region can be located on the same surface of the semiconductor substrate, or can be located on two opposite surfaces of the semiconductor substrate. Figure 5 and Figure 6 is a schematic diagram of a structure in which the first region and the second region are located on the same surface of a semiconductor substrate, Fig.14Schematic diagram of a structure in which the first region and the second region are located on opposite sides of the semiconductor substrate. The P-type doped polysilicon layer 12 is formed at least on the first region. The N-type doped polysilicon layer 13 is formed at least on the second region. At least a portion of the N-type doped polysilicon layer 13 and at least a portion of the P-type doped polysilicon layer 12 are arranged at intervals from each other. Among them, the ratio between the refractive index n of the N-type doped polysilicon layer and the P-type doped polysilicon layer can be greater than or equal to 0.8 and less than or equal to 1.2; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer can be greater than or equal to 0 and less than or equal to 0.2. In this case, it is beneficial to make the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer in the solar cell manufactured based on the semiconductor structure provided in the embodiment of the present invention substantially equal. The beneficial effect of the refractive index n of the N-type doped polysilicon layer and the refractive index n of the P-type doped polysilicon layer in the solar cell being substantially equal can be referred to the above, and will not be repeated here.

[0123] As for the ratio or difference of the refractive index n of the above-mentioned N-type doped polysilicon layer and the P-type doped polysilicon layer, as well as the specific sizes of the refractive indices n of the two, they can be determined based on the requirements of the actual application scenarios for the refraction effect of the N-type doped polysilicon layer and the P-type doped polysilicon layer on light, as well as the requirements for the density of the film layers of the two.

[0124] For example, the ratio of the refractive index n of the N-type doped polysilicon layer to the refractive index n of the P-type doped polysilicon layer is 0.8, 0.85, 0.9, 0.95, 1, 1.05, 1.1, 1.15 or 1.2, etc. For example, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer can be 0.01, 0.02, 0.06, 0.08, 0.1, 0.12, 0.14, 0.18 or 0.2, etc.

[0125] Exemplarily, the refractive index n of the P-type doped polysilicon layer may be greater than or equal to 3.8 and less than or equal to 4. For example, the refractive index n of the P-type doped polysilicon layer may be 3.8, 3.82, 3.85, 3.88, 3.9, 3.95 or 4.

[0126] Exemplarily, the refractive index n of the N-type doped polysilicon layer may be greater than or equal to 3.7 and less than or equal to 3.95. For example, the refractive index n of the N-type doped polysilicon layer may be 3.7, 3.75, 3.8, 3.85, 3.88, 3.9, 3.92, 3.94 or 3.95.

[0127] As for the ratio or difference of the extinction coefficients k of the above-mentioned N-type doped polysilicon layer and the P-type doped polysilicon layer, as well as the specific sizes of the extinction coefficients k of the two, they can be determined according to the requirements for the film density of the N-type doped polysilicon layer and the P-type doped polysilicon layer in the actual application scenario.

[0128] Exemplarily, the ratio of the extinction coefficient k of the N-type doped polysilicon layer 13 to the extinction coefficient k of the P-type doped polysilicon layer 12 is greater than 1 and less than or equal to 1.2; and / or, the difference between the extinction coefficient k of the N-type doped polysilicon layer 13 and the extinction coefficient k of the P-type doped polysilicon layer 12 is greater than 0 and less than or equal to 0.1.

[0129] Specifically, the ratio of the extinction coefficient k of the N-type doped polysilicon layer to the extinction coefficient k of the P-type doped polysilicon layer may be greater than 1 and less than or equal to any value of 2.6. For example, the ratio of the extinction coefficient k of the N-type doped polysilicon layer to the extinction coefficient k of the P-type doped polysilicon layer may be 1.01, 1.02, 1.06, 1.08, 1.1, 1.12, 1.16, 1.18, 1.2, 1.3, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4 or 2.6, etc.

[0130] The difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer can be any value greater than 0 and less than or equal to 0.2. For example, the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer can be 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.2, etc. As for the specific values ​​of the extinction coefficient k of the N-type doped polysilicon layer and the P-type doped polysilicon layer, they can be determined according to the actual application scenario and are not specifically limited here.

[0131] Exemplarily, the extinction coefficient k of the N-type doped polysilicon layer may be greater than or equal to 0.27 and less than or equal to 0.41. For example, the extinction coefficient k of the N-type doped polysilicon layer may be 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40 or 0.41, etc.

[0132] Exemplarily, the extinction coefficient k of the P-type doped polysilicon layer may be greater than or equal to 0.1 and less than or equal to 0.38. For example, the extinction coefficient k of the P-type doped polysilicon layer may be 0.1, 0.12, 0.14, 0.16, 0.18, 0.2, 0.22, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37 or 0.38, etc.

[0133] It can be understood that the semiconductor structure provided in the embodiment of the present invention is an intermediate structure or semi-finished product for manufacturing the solar cell described above. Based on this, when the ratio between the extinction coefficient k of the N-type doped polysilicon layer and the P-type doped polysilicon layer in the semiconductor structure provided in the embodiment of the present invention is greater than 1 and less than or equal to 2.6; and / or, the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer is greater than 0 and less than or equal to 0.2, the extinction coefficient k of the N-type doped polysilicon layer is greater than the extinction coefficient k of the P-type doped polysilicon layer, thereby facilitating that the extinction coefficient k of the N-type doped polysilicon layer in the solar cell manufactured based on the semiconductor structure provided in the embodiment of the present invention is also greater than the extinction coefficient k of the P-type doped polysilicon layer. The beneficial effect that the extinction coefficient k of the N-type doped polysilicon layer in the solar cell is also greater than the extinction coefficient k of the P-type doped polysilicon layer can be referred to the above and will not be repeated here.

[0134] The beneficial effects of the second aspect and its various implementations in the embodiments of the present invention can be analyzed by referring to the beneficial effects of the first aspect and its various implementations, and will not be repeated here.

[0135] In a third aspect, an embodiment of the present invention provides a method for manufacturing a solar cell. The method for manufacturing a solar cell comprises the following steps: first, providing a semiconductor substrate. The semiconductor substrate comprises a first region and a second region. The first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate. Next, Fig. 9 As shown in FIG. 1 , a P-type doped polysilicon layer 12 is formed at least on the first region. Next, as shown in FIG. Fig.12 As shown, an N-type doped polysilicon layer 13 is formed at least on the second region. At least a portion of the N-type doped polysilicon layer 13 and at least a portion of the P-type doped polysilicon layer 12 are arranged at intervals. The ratio of the refractive index n of the N-type doped polysilicon layer 13 to the refractive index n of the P-type doped polysilicon layer 12 is greater than or equal to 0.9 and less than or equal to 1.1; and / or the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer 12 and the refractive index n of the N-type doped polysilicon layer 13 is greater than or equal to 0 and less than or equal to 0.1.

[0136] The beneficial effects of the third aspect in the embodiments of the present invention can be analyzed by referring to the beneficial effects of the first aspect and its various implementations, and will not be described in detail here.

[0137] In the actual application process, the material of the semiconductor substrate, the range of the first region and the second region, the N-type doped polysilicon layer and the P-type doped polysilicon layer can be referred to the above text, and will not be repeated here. As for the formation process of the P-type doped polysilicon layer and the N-type doped polysilicon layer, it can be determined according to the type of solar cell manufactured.

[0138] Exemplarily, in the case where the first region and the second region are located on the same surface of the semiconductor substrate, when the formation sequence of the N-type doped polysilicon layer is after the formation sequence of the P-type doped polysilicon layer, the forming of the P-type doped polysilicon layer at least on the first region may include the following steps: Figure 7 As shown, a first intrinsic polysilicon layer 19 is formed covering the first region and the second region. Figure 8 As shown in FIG. 1 , the first intrinsic polysilicon layer is diffused to form a P-type doped polysilicon layer 12. Fig. 9 As shown, the portion of the P-type doped polysilicon layer 12 at least located on a portion of the second region is selectively removed.

[0139] Specifically, in the actual application process, chemical vapor deposition and other processes can be used to form the above-mentioned first intrinsic polysilicon layer. Then, after the first intrinsic polysilicon layer is subjected to a diffusion treatment of P-type impurities such as boron atoms to obtain a whole layer of P-type doped polysilicon layer, the doped silicon glass layer formed on the P-type doped polysilicon layer can be selectively heat-treated by laser irradiation or other methods, so that the structure of the part of the doped silicon glass layer located on the second area is looser. Next, under the masking effect of the part of the doped silicon glass layer located on the first area, the part of the P-type doped polysilicon layer located at least on part of the second area can be selectively removed. Among them, in the case where the corresponding surface of the semiconductor substrate has only the first area and the second area, the part of the P-type doped polysilicon layer located on the second area can be completely removed, or in order to reduce the risk of hot spots in the manufactured solar cell, only the part of the P-type doped polysilicon layer located on part of the second area can be removed. In addition, when the corresponding surface of the semiconductor substrate includes a first region, a second region and a spacing region, the portion of the P-type doped polysilicon layer located on the second region and the spacing region may be completely removed, or, in order to reduce the risk of hot spots in the manufactured solar cell, only the portion of the P-type doped polysilicon layer located on part of the second region and / or part of the spacing region may be removed.

[0140] Secondly, in the actual manufacturing process, when the first region and the second region are located on the same surface of the semiconductor substrate, when the formation order of the N-type doped polysilicon layer is before the formation order of the P-type doped polysilicon layer, the above-mentioned formation of the P-type doped polysilicon layer at least on the first region may include the steps of: forming a first intrinsic polysilicon layer covering at least the N-type doped polysilicon layer and the first region; next, performing diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer; then, selectively removing the portion of the P-type doped polysilicon layer located on at least part of the N-type doped polysilicon layer. In this case, the specific formation process of the P-type doped polysilicon layer can refer to the specific formation process of the P-type doped polysilicon layer when the formation order of the N-type doped polysilicon layer is after the formation order of the P-type doped polysilicon layer as described above, and will not be repeated here.

[0141] Exemplarily, in the case where the first region and the second region are respectively located on two opposite sides of the semiconductor substrate, the above-mentioned formation of a P-type doped polysilicon layer at least on the first region may include the steps of: forming a first intrinsic polysilicon layer covering at least the first region. Next, the first intrinsic polysilicon layer is diffused to form a P-type doped polysilicon layer in the first intrinsic polysilicon layer. Specifically, the above-mentioned first intrinsic polysilicon layer may be formed by a process such as chemical vapor deposition. Next, the first intrinsic polysilicon layer is diffused with P-type impurities such as boron atoms to obtain a whole layer of P-type doped polysilicon layer.

[0142] Specifically, in the actual manufacturing process, whether the first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate, a P-type doped polysilicon layer located at least on the first region can usually be formed by diffusing boron impurities into the first intrinsic polysilicon layer. The size of boron atoms is small, and the corresponding diffusion method is gap diffusion. Compared with the substitution diffusion method, gap diffusion is more difficult to control. The thickness, extinction coefficient k and refractive index n of the first intrinsic polysilicon layer will affect the doping depth of impurities in the first intrinsic polysilicon layer, as well as the difficulty of doping. Based on this, the thickness, extinction coefficient k and refractive index n of the first intrinsic polysilicon layer can be determined according to the doping condition of the P-type doped polysilicon layer in the actual application scenario.

[0143] Preferably, the ratio between the thickness of the first intrinsic polysilicon layer and the thickness of the P-type doped polysilicon layer may be greater than or equal to 1.4 and less than or equal to 1.5. For example, the ratio between the thickness of the first intrinsic polysilicon layer and the thickness of the P-type doped polysilicon layer may be 1.4, 1.42, 1.44, 1.46, 1.48 or 1.5, etc.

[0144] Preferably, the difference between the thickness of the first intrinsic polysilicon layer and the P-type doped polysilicon layer may be greater than or equal to 100 nm and less than or equal to 130 nm. For example, the difference between the thickness of the first intrinsic polysilicon layer and the P-type doped polysilicon layer may be 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm or 130 nm.

[0145] Preferably, the extinction coefficient k of the first intrinsic polysilicon layer may be smaller than the extinction coefficient k of the P-type doped polysilicon layer. In this case, the first intrinsic polysilicon layer has a higher density than the P-type doped polysilicon layer, which helps prevent the impurities from passing through the first intrinsic polysilicon layer and entering the semiconductor substrate during the diffusion treatment of the first intrinsic polysilicon layer, thereby preventing the problem of easy penetration or large internal diffusion range, thereby ensuring that the solar cell has a higher open circuit voltage and fill factor.

[0146] For example, the absolute value of the difference between the extinction coefficients k of the first intrinsic polysilicon layer and the P-type doped polysilicon layer may be greater than or equal to 0.05, 0.055, 0.06, 0.065, 0.07, 0.075 or 0.08, etc.

[0147] Preferably, the refractive index n of the first intrinsic polysilicon layer can be greater than or equal to the refractive index n of the P-type doped polysilicon layer. In this case, the magnitude of the refractive index n of the first intrinsic polysilicon layer and the refractive index n of the P-type doped polysilicon layer is related to the compactness of the film layer itself. Within a certain range, the refractive index n of the first intrinsic polysilicon layer and the P-type doped polysilicon layer is proportional to the compactness of the film layer. Based on this, when the refractive index n of the first intrinsic polysilicon layer is greater than or equal to the refractive index n of the P-type doped polysilicon layer, the first intrinsic polysilicon layer is relatively dense, which is conducive to preventing impurities from passing through the first intrinsic polysilicon layer and entering the semiconductor substrate when the first intrinsic polysilicon layer is diffused, resulting in easy penetration or a large internal expansion range, thereby ensuring that the solar cell has a higher open circuit voltage and fill factor.

[0148] Exemplarily, the difference between the refractive index n of the first intrinsic polysilicon layer and the P-type doped polysilicon layer may be greater than or equal to 0 and less than or equal to 0.1. For example, the difference between the refractive index n of the first intrinsic polysilicon layer and the P-type doped polysilicon layer may be 0, 0.01, 0.02, 0.04, 0.06, 0.08 or 0.1, etc.

[0149] In addition, in an actual manufacturing process, when the first region and the second region are located on the same surface of the semiconductor substrate, when the formation sequence of the N-type doped polysilicon layer is after the formation sequence of the P-type doped polysilicon layer, the above-mentioned forming of the N-type doped polysilicon layer at least on the second region may include: Fig.10As shown in FIG. 1 , a second intrinsic polysilicon layer 20 is formed to cover at least the P-type doped polysilicon layer and the second region. Next, as shown in FIG. Fig.11 As shown in FIG. 1 , the second intrinsic polysilicon layer is diffused to form an N-type doped polysilicon layer 13. Next, as shown in FIG. Fig.12 As shown, the portion of the N-type doped polysilicon layer 13 at least located on a portion of the P-type doped polysilicon layer is selectively removed.

[0150] Exemplarily, the second intrinsic polysilicon layer may be formed by a process such as chemical vapor deposition. When the corresponding surface of the semiconductor substrate includes only the first region and the second region, the second intrinsic polysilicon layer only covers the P-type doped polysilicon layer and the second region. When the corresponding surface of the semiconductor substrate includes not only the first region and the second region but also the spacing region, the second intrinsic polysilicon layer covers the P-type doped polysilicon layer, the second region and the spacing region. Next, the second intrinsic polysilicon layer is subjected to a diffusion treatment of N-type impurities such as phosphorus atoms to form an N-type doped polysilicon layer. Then, the doped silicon glass layer formed on the N-type doped polysilicon layer can be selectively heat-treated by laser irradiation or the like, so that the portion of the doped silicon glass layer located on at least part of the P-type doped polysilicon layer (it can be the portion of the doped silicon glass layer located on each region of the P-type doped polysilicon layer, or in order to reduce the risk of hot spots of the manufactured solar cell, it can also be the portion of the doped silicon glass layer located on part of the P-type doped polysilicon layer. And, in the case where the corresponding surface of the semiconductor substrate also includes a spacing region, it can also be the portion of the doped silicon glass layer located on each region and the spacing region of the P-type doped polysilicon layer, or in order to reduce the risk of hot spots of the manufactured solar cell, it can also be the portion of the doped silicon glass layer located on part of the P-type doped polysilicon layer and / or part of the spacing region) has a looser structure. Next, the portion of the N-type doped polysilicon layer located on at least part of the P-type doped polysilicon layer can be selectively removed under the masking effect of the portion of the doped silicon glass layer located at least on the second region.

[0151] Secondly, in the actual manufacturing process, when the first region and the second region are located on the same surface of the semiconductor substrate, when the formation order of the N-type doped polysilicon layer is before the formation order of the P-type doped polysilicon layer, the above-mentioned formation of the N-type doped polysilicon layer at least on the second region may include the steps of: forming a second intrinsic polysilicon layer covering the first region and the second region; next, performing diffusion treatment on the second intrinsic polysilicon layer so that the second intrinsic polysilicon layer forms an N-type doped polysilicon layer; then, selectively removing the portion of the N-type doped polysilicon layer located at least on part of the first region. In this case, the formation process of the N-type doped polysilicon layer can refer to the formation process of the N-type doped polysilicon layer when the formation order of the N-type doped polysilicon layer is after the formation order of the P-type doped polysilicon layer as described above, and will not be repeated here.

[0152] In the case where the first region and the second region are located on opposite sides of the semiconductor substrate, the formation of the N-type doped polysilicon layer at least on the second region may include: forming a second intrinsic polysilicon layer covering at least the first region and the second region. Next, the second intrinsic polysilicon layer is diffused to form an N-type doped polysilicon layer. Specifically, the second intrinsic polysilicon layer may be formed by a process such as chemical vapor deposition. Next, the second intrinsic polysilicon layer is diffused with N-type impurities such as phosphorus atoms to form an N-type doped polysilicon layer.

[0153] Specifically, in the actual manufacturing process, when the first region and the second region are respectively located on two opposite sides of the semiconductor substrate, the formation order of the N-type doped polysilicon layer can be before the formation order of the P-type doped polysilicon layer, or it can be after the formation order of the P-type doped polysilicon layer. The embodiment of the present invention does not specifically limit the formation order of the N-type doped polysilicon layer and the P-type doped polysilicon layer. Among them, when the first region and the second region are respectively located on two opposite sides of the semiconductor substrate, the formation process of the N-type doped polysilicon layer and the P-type doped polysilicon layer can refer to the above. In this case, if at least one of the N-type doped polysilicon layer and the P-type doped polysilicon layer is partially formed on the corresponding surface, after the doped semiconductor layer of the corresponding conductive type is formed, it is also necessary to form a mask layer (such as a doped silicon glass layer) on the local area of ​​the doped semiconductor layer by laser and etching process, and then the doped semiconductor layer is patterned under the protection of the mask layer, so as to obtain a doped semiconductor layer located only on the local area of ​​the corresponding surface.

[0154] In addition, the thickness, extinction coefficient k and refractive index n of the second intrinsic polysilicon layer will affect the doping depth of impurities in the second intrinsic polysilicon layer and the difficulty of doping. Based on this, the thickness, extinction coefficient k and refractive index n of the second intrinsic polysilicon layer can be determined according to the doping conditions of the N-type doped polysilicon layer in the actual application scenario.

[0155] Exemplarily, the ratio between the thickness of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be greater than or equal to 1.1 and less than or equal to 1.3. For example, the ratio between the thickness of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be 1.1, 1.12, 1.15, 1.19, 1.2, 1.25, 1.28 or 1.3, etc.

[0156] Exemplarily, the difference between the thickness of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be greater than or equal to 40 nm and less than or equal to 60 nm. For example, the difference between the thickness of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be 40 nm, 45 nm, 50 nm, 55 nm, 58 nm or 60 nm.

[0157] Preferably, the refractive index n of the second intrinsic polysilicon layer can be less than the refractive index n of the N-type doped polysilicon layer. In this case, the magnitude of the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the N-type doped polysilicon layer is also related to the compactness of the film layer itself. Within a certain range, the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the N-type doped polysilicon layer are proportional to the compactness of the film layer. In this case, when the refractive index n of the second intrinsic polysilicon layer is less than the refractive index n of the N-type doped polysilicon layer, before the diffusion treatment, the compactness of the second intrinsic polysilicon layer is low, which is conducive to doping N-type impurities into the second intrinsic polysilicon layer. After the diffusion treatment, the compactness of the N-type doped polysilicon layer becomes higher, which is conducive to preventing the electrode slurry for manufacturing the negative electrode from penetrating the N-type doped polysilicon layer, and is conducive to reducing the metal composite area between the N-type doped polysilicon layer and the negative electrode, thereby reducing the metal composite loss.

[0158] Exemplarily, the difference between the refractive index n of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be greater than or equal to -0.09 and less than or equal to -0.05. For example, the difference between the refractive index n of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be -0.09, -0.086, -0.08, -0.07, -0.065, -0.06 or -0.05, etc.

[0159] Exemplarily, the extinction coefficient k of the second intrinsic polysilicon layer may be greater than the extinction coefficient k of the N-type doped polysilicon layer. In this case, as described above, within a certain range, the extinction coefficient k of the film layer is inversely proportional to its own compactness. Based on this, when the extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the N-type doped polysilicon layer, the compactness of the second intrinsic polysilicon layer is lower than the compactness of the N-type doped polysilicon layer. The beneficial effect of the compactness of the second intrinsic polysilicon layer being lower than the compactness of the N-type doped polysilicon layer can be referred to the above, and will not be repeated here.

[0160] Exemplarily, the difference between the extinction coefficient k of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be greater than or equal to 0.08 and less than or equal to 0.23. For example, the difference between the extinction coefficient k of the second intrinsic polysilicon layer and the N-type doped polysilicon layer may be 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22 or 0.23, etc.

[0161] As for the relationship between the thickness, extinction coefficient k and refractive index n of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer, it can be determined based on the relationship between the thickness, refractive index n and extinction coefficient k between the P-type doped polysilicon layer and the N-type doped polysilicon layer, between the first intrinsic polysilicon layer and the P-type doped polysilicon layer, and between the second intrinsic polysilicon layer and the N-type doped polysilicon layer, and no specific limitation is made here.

[0162] Exemplarily, the thickness of the second intrinsic polysilicon layer can be less than the thickness of the first intrinsic polysilicon layer. In this case, as described above, the etching ability of the electrode slurry for manufacturing the positive electrode on the film layer is greater than the etching ability of the electrode slurry for manufacturing the negative electrode on the film layer. The first intrinsic polysilicon layer is used to manufacture the P-type doped polysilicon layer, and the second intrinsic polysilicon layer is used to manufacture the N-type doped polysilicon layer. In the above case, when the thickness of the second intrinsic polysilicon layer is less than the thickness of the first intrinsic polysilicon layer, it is beneficial to increase the thickness of the P-type doped polysilicon layer formed based on the first intrinsic polysilicon layer with a larger thickness, further reduce the risk of the electrode slurry for manufacturing the positive electrode penetrating the P-type doped polysilicon layer, ensure that the P-type polysilicon layer has a higher field passivation effect, and prevent the electrode slurry for manufacturing the positive electrode from damaging the semiconductor substrate.

[0163] Exemplarily, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be greater than or equal to 0.55 and less than or equal to 0.8; and / or, the difference between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be greater than or equal to -140nm and less than or equal to -100nm.

[0164] For example, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be 0.55, 0.56, 0.58, 0.6, 0.65, 0.7, 0.75 or 0.8, etc. For example, the difference between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be -140nm, -135nm, -130nm, -125nm, -120nm, -110nm or -100nm, etc.

[0165] In the case of adopting the above technical solution, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is within the above range, which can prevent the second intrinsic polysilicon layer from being too small and / or the first intrinsic polysilicon layer from being too large due to the smaller ratio; secondly, it can also prevent the second intrinsic polysilicon layer from being too large and / or the first intrinsic polysilicon layer from being too small due to the larger ratio. In summary, the ratio between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is within the above range, which is conducive to reasonably setting the thickness of the first intrinsic polysilicon layer and the second intrinsic polysilicon layer, ensuring that there will be no problems of penetration and large internal expansion after diffusion treatment, and at the same time, the P-type doped polysilicon layer and the N-type doped polysilicon layer have a high matching with the electrode slurry used to manufacture the positive electrode and the negative electrode, respectively, ensuring that the P-type doped polysilicon layer and the N-type doped polysilicon layer both have a high field passivation effect.

[0166] Exemplarily, the refractive index n of the second intrinsic polysilicon layer can be less than the refractive index n of the first intrinsic polysilicon layer. In this case, as mentioned above, within a certain range, the refractive index n of the film layer is proportional to its own density. Based on this, when the refractive index n of the second intrinsic polysilicon layer is less than the refractive index n of the first intrinsic polysilicon layer, the first intrinsic polysilicon layer has a relatively high film density, which is conducive to preventing P-type impurities such as smaller boron atoms from diffusing through the first intrinsic polysilicon layer. In addition, larger N-type impurities such as phosphorus are doped into the second intrinsic polysilicon layer in a substitutional diffusion manner. Because the substitutional diffusion manner is that impurity atoms replace the positions of semiconductor atoms to form doped regions, when the density of the second intrinsic polysilicon layer is relatively low, it is conducive to the diffusion of larger N-type impurities such as phosphorus, reducing the difficulty of diffusion, and helping to increase the impurity doping concentration in the N-type doped polysilicon layer.

[0167] Exemplarily, the difference between the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the first intrinsic polysilicon layer may be greater than or equal to -0.12 and less than or equal to -0.1. For example, the ratio between the refractive index n of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be -0.12, -0.118, -0.116, -0.114, -0.112 or -0.1, etc.

[0168] Exemplarily, the extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the first intrinsic polysilicon layer. In this case, the compactness of the second intrinsic polysilicon layer is lower than the compactness of the first intrinsic polysilicon layer. The beneficial effects at this time can refer to the beneficial effects of the refractive index n of the second intrinsic polysilicon layer being lower than the refractive index n of the first intrinsic polysilicon layer as described above, which will not be repeated here.

[0169] Exemplarily, the difference between the extinction coefficient k of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be greater than or equal to 0.02 and less than or equal to 0.3. For example, the difference between the extinction coefficient k of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer may be 0.02, 0.022, 0.024, 0.026, 0.028, 0.03, 0.034, 0.038, 0.04, 0.08, 0.1, 0.12, 0.15, 0.18, 0.2, 0.22, 0.25, 0.28 or 0.3, etc.

[0170] In addition, in the actual manufacturing process, the formation temperature, formation time, and diffusion temperature of the film layer will affect the density and formation thickness of the film layer. Therefore, the film layer characteristics of the first intrinsic polysilicon layer and the second intrinsic polysilicon layer, as well as the P-type doped polysilicon layer and the N-type doped polysilicon layer can be controlled by adjusting the above parameters.

[0171] Exemplarily, the formation temperature of the second intrinsic polysilicon layer may be greater than the formation temperature of the first intrinsic polysilicon layer. In this case, when other factors are the same, the higher the formation temperature, the faster the deposition rate. Based on this, when the formation temperature of the second intrinsic polysilicon layer is greater than the formation temperature of the first intrinsic polysilicon layer, the material deposition rate of the second intrinsic polysilicon layer is faster, and the corresponding film layer density is lower, which is conducive to obtaining a second intrinsic polysilicon layer with a loose structure and a first intrinsic polysilicon layer with a dense structure, thereby reducing the size of N-type impurities such as phosphorus that are larger in size and are doped into the second intrinsic polysilicon layer in a substitutional diffusion manner, and at the same time, it is conducive to preventing the problem of penetration or a large internal expansion range after the P-type impurities such as boron atoms that are smaller in size are doped into the first intrinsic polysilicon layer in a gap diffusion manner.

[0172] Exemplarily, the formation time of the second intrinsic polysilicon layer may be less than the formation time of the first intrinsic polysilicon layer. In this case, when other factors are the same, the longer the formation time, the thicker the film layer. Based on this, when the formation time of the second intrinsic polysilicon layer is less than the formation time of the first intrinsic polysilicon layer, the greater the film thickness of the first intrinsic polysilicon layer, the problem of penetration or a larger inward expansion range after diffusion is further prevented.

[0173] For example, the temperature of the diffusion treatment of the first intrinsic polysilicon layer may be greater than the temperature of the diffusion treatment of the second intrinsic polysilicon layer. In this case, the P-type impurities of boron atoms are diffused into the first intrinsic polysilicon layer in a manner that facilitates diffusion through gaps, reduces the diffusion difficulty, and helps to increase the impurity doping concentration in the P-type doped polysilicon layer.

[0174] The specific values ​​of the process parameters for forming the first intrinsic polysilicon layer and the second intrinsic polysilicon layer and the diffusion process can be determined according to the actual application scenario and are not specifically limited here.

[0175] It should be noted that, in the case where the first region and the second region are located on the same surface of the semiconductor substrate, when the formation order of the P-type doped polysilicon layer is before the formation order of the N-type doped polysilicon layer. The step of forming the first intrinsic polysilicon layer covering the first region and the second region specifically includes at least the following two cases: the first case, the first intrinsic polysilicon layer used to manufacture the P-type doped polysilicon layer is directly formed on the surface where the first region and the second region of the semiconductor substrate are located; or, the second case, in the case where the manufactured solar cell also includes a first tunneling passivation layer, the first tunneling passivation layer is formed on the surface where the first region and the second region of the semiconductor substrate are located, or the surface where the first region and the second region of the semiconductor substrate are located is oxidized to form the first tunneling passivation layer, and then the first intrinsic polysilicon layer is formed on the first tunneling passivation layer. In this case, after the first intrinsic polysilicon layer is formed, the first tunneling passivation layer and the first intrinsic polysilicon layer are stacked on the first region and the second region along the thickness direction of the semiconductor substrate. Furthermore, the entire first tunnel passivation layer can be patterned before forming the first intrinsic polysilicon layer, or the entire first tunnel passivation layer can be patterned after forming the P-type doped polysilicon layer and selectively removing the P-type doped polysilicon layer, leaving only the portion of the first tunnel passivation layer between the P-type doped polysilicon layer and the semiconductor substrate. Specifically, the first tunnel passivation layer can be formed on the first region and the second region of the semiconductor substrate by processes such as chemical vapor deposition or thermal oxidation.In addition, the step of forming a second intrinsic polysilicon layer covering at least the P-type doped polysilicon layer and the second region may specifically include at least the following situations: first, the second intrinsic polysilicon layer used to manufacture the N-type doped polysilicon layer may be directly formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate; or, second, in the case where the manufactured solar cell also includes a second tunneling passivation layer or an insulating mask layer, an insulating mask layer or a second tunneling passivation layer is formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate, and a second intrinsic polysilicon layer is formed on the surface of the second tunneling passivation layer or the insulating mask layer away from the semiconductor substrate; after the second intrinsic polysilicon layer is formed, the insulating mask layer or the second tunneling passivation layer is formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate. The passivation layer and the second intrinsic polysilicon layer are stacked on the P-type doped polysilicon layer and the second region along the thickness direction of the semiconductor substrate; or, in the third case, when the manufactured solar cell also includes an insulating mask layer and a second tunnel passivation layer, an insulating mask layer and a second tunnel passivation layer are sequentially formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate, the second tunnel passivation layer is formed on the side of the insulating mask layer away from the semiconductor substrate, and a second intrinsic polysilicon layer is formed on the surface of the second tunnel passivation layer away from the semiconductor substrate; after the second intrinsic polysilicon layer is formed, the insulating mask layer, the second tunnel passivation layer, and the second intrinsic polysilicon layer are stacked on the P-type doped polysilicon layer and the second region along the thickness direction of the semiconductor substrate. Among them, the insulating mask layer can be prepared separately, or it can be formed when the P-type doped polysilicon layer is diffused, and is obtained by laser irradiation and etching process. The formation process of the second tunnel passivation layer can refer to the formation process of the first tunnel passivation layer described above, which will not be repeated here.

[0176] The following is an example of a solar cell further including a first tunnel passivation layer: before forming the first intrinsic polysilicon layer, a first tunnel passivation layer needs to be formed on the first region and the second region; then, a first intrinsic polysilicon layer is formed on the side of the first tunnel passivation layer away from the semiconductor substrate; in this case, after forming the first intrinsic polysilicon layer, the first tunnel passivation layer and the first intrinsic polysilicon layer are stacked on the first region and the second region along the thickness direction of the semiconductor substrate. Specifically, the first tunnel passivation layer can be formed on the first region and the second region of the semiconductor substrate by processes such as chemical vapor deposition or thermal oxidation.

[0177] In the case where the first region and the second region are located on the same surface of the semiconductor substrate, when the formation order of the N-type doped polysilicon layer is before the formation order of the P-type doped polysilicon layer, the step of forming the second intrinsic polysilicon layer covering the first region and the second region specifically includes at least the following two cases: the first case, the second intrinsic polysilicon layer used to manufacture the N-type doped polysilicon layer is directly formed on the surface where the first region and the second region of the semiconductor substrate are located; or, the second case, in the case where the manufactured solar cell also includes a second tunneling passivation layer, the second tunneling passivation layer is formed on the surface where the first region and the second region of the semiconductor substrate are located or the surface where the first region and the second region of the semiconductor substrate are located is oxidized to form the second tunneling passivation layer, and then the second intrinsic polysilicon layer is formed on the second tunneling passivation layer. In this case, after the second intrinsic polysilicon layer is formed, the second tunneling passivation layer and the second intrinsic polysilicon layer are stacked on the first region and the second region along the thickness direction of the semiconductor substrate. Furthermore, the entire second tunnel passivation layer can be patterned before forming the second intrinsic polysilicon layer, or the entire second tunnel passivation layer can be patterned after forming the N-type doped polysilicon layer and selectively removing the N-type doped polysilicon layer, leaving only the portion of the second tunnel passivation layer between the N-type doped polysilicon layer and the semiconductor substrate. Specifically, the second tunnel passivation layer can be formed on the first region and the second region of the semiconductor substrate by processes such as chemical vapor deposition or thermal oxidation. In addition, the step of forming a second intrinsic polysilicon layer covering at least the P-type doped polysilicon layer and the second region may specifically include at least the following three situations: first, the second intrinsic polysilicon layer used to manufacture the N-type doped polysilicon layer may be directly formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate; or, second, in the case where the manufactured solar cell also includes a second tunneling passivation layer or an insulating mask layer, an insulating mask layer or a second tunneling passivation layer is formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate; then, a second intrinsic polysilicon layer is formed on the surface of the second tunneling passivation layer or the insulating mask layer away from the semiconductor substrate, in which case, after the second intrinsic polysilicon layer is formed, the insulating mask layer or the second tunneling passivation layer and the second intrinsic polysilicon layer are stacked along the thickness direction of the semiconductor substrate on the P-type doped polysilicon layer and the second region of the semiconductor substrate.Alternatively, in the third case, when the manufactured solar cell also includes an insulating mask layer and a second tunneling passivation layer, an insulating mask layer and a second tunneling passivation layer are sequentially formed on the surface of the second region of the semiconductor substrate and on the surface of the P-type doped polysilicon layer away from the semiconductor substrate, and the second tunneling passivation layer is formed on the side of the insulating mask layer away from the semiconductor substrate; then, a second intrinsic polysilicon layer is formed on the surface of the second tunneling passivation layer away from the semiconductor substrate, and after the second intrinsic polysilicon layer is formed, the insulating mask layer, the second tunneling passivation layer, and the first intrinsic polysilicon layer are stacked on the P-type doped polysilicon layer and the second region along the thickness direction of the semiconductor substrate.

[0178] The following is an example in which the solar cell also includes a second tunneling passivation layer: before forming the second intrinsic polysilicon layer, a second tunneling passivation layer needs to be formed on the second region and the P-type doped polysilicon layer; then, a second intrinsic polysilicon layer is formed on the second tunneling passivation layer. In this case, after forming the second intrinsic polysilicon layer, the second tunneling passivation layer and the second intrinsic polysilicon layer are stacked on the second region and the P-type doped polysilicon layer along the thickness direction of the semiconductor substrate. Specifically, the second tunneling passivation layer can be formed on the second region and the P-type doped polysilicon layer of the semiconductor substrate by processes such as chemical vapor deposition or thermal oxidation.

[0179] As for the case where the first region and the second region are located on two opposite surfaces of the semiconductor substrate, the step of forming the first intrinsic polycrystalline silicon layer on the first region specifically includes at least the following cases: first, the first intrinsic polycrystalline silicon layer for manufacturing the P-type doped polycrystalline silicon layer is directly formed on the surface where the first region of the semiconductor substrate is located, and / or the second intrinsic polycrystalline silicon layer for manufacturing the N-type doped polycrystalline silicon layer is directly formed on the surface where the second region of the semiconductor substrate is located; or, second, when the manufactured solar cell also includes a first tunneling passivation layer, the first tunneling passivation layer is formed on the surface where the first region of the semiconductor substrate is located or the surface where the first region of the semiconductor substrate is located is oxidized to form the first tunneling passivation layer, and then the first intrinsic polycrystalline silicon layer is formed on the first tunneling passivation layer, and / or when the manufactured solar cell also includes a second tunneling passivation layer, the second tunneling passivation layer is formed on the surface where the second region of the semiconductor substrate is located or the surface where the second region of the semiconductor substrate is located is oxidized to form the second tunneling passivation layer, and then the second intrinsic polycrystalline silicon layer is formed on the second tunneling passivation layer. In the above case, when there is a first tunneling passivation layer, after the first intrinsic polysilicon layer is formed, the first tunneling passivation layer and the first intrinsic polysilicon layer are stacked on the first region along the thickness direction of the semiconductor substrate; when there is a second tunneling passivation layer, after the second intrinsic polysilicon layer is formed, the second tunneling passivation layer and the second intrinsic polysilicon layer are stacked on the second region along the thickness direction of the semiconductor substrate.

[0180] In one example, after forming a P-type doped polysilicon layer at least on the first region and forming an N-type doped polysilicon layer at least on the second region (i.e., after forming the semiconductor structure), the method for manufacturing the solar cell further includes the following steps: Fig.13 As shown, at least one side of the P-type doped polysilicon layer 12 facing away from the semiconductor substrate 11 and one side of the N-type doped polysilicon layer 13 facing away from the semiconductor substrate 11 are passivated to form a surface passivation layer 14 covering at least one side of the P-type doped polysilicon layer 12 facing away from the semiconductor substrate 11 and one side of the N-type doped polysilicon layer 13 facing away from the semiconductor substrate 11. After the passivation treatment, the ratio of the extinction coefficients k of the N-type doped polysilicon layer 13 and the P-type doped polysilicon layer 12 is greater than or equal to 1.5 and less than or equal to 2.5.

[0181] Among them, in the case where the first region and the second region are located on opposite sides of the semiconductor substrate, when the first region and the second region leveling layers are arranged on the corresponding surfaces, only the side of the P-type doped polysilicon layer facing away from the semiconductor substrate and the side of the N-type doped polysilicon layer facing away from the semiconductor substrate can be passivated; when the first region and / or the second region are only partially arranged on the corresponding surface, the side of the P-type doped polysilicon layer facing away from the semiconductor substrate and the side of the N-type doped polysilicon layer facing away from the semiconductor substrate can be passivated, and the corresponding surface of the semiconductor substrate exposed outside the P-type doped polysilicon layer or the N-type doped polysilicon layer can also be passivated. In the case where a region and a second region are located on the same surface of a semiconductor substrate, when the corresponding surface has only the first region and the second region, only the side of the P-type doped polysilicon layer facing away from the semiconductor substrate and the side of the N-type doped polysilicon layer facing away from the semiconductor substrate can be passivated; when the corresponding surface has the first region, the second region and the spacing region, the side of the P-type doped polysilicon layer facing away from the semiconductor substrate and the side of the N-type doped polysilicon layer facing away from the semiconductor substrate can be passivated, and the surface of the spacing region can also be passivated. Secondly, after the passivation treatment, the extinction coefficient k, refractive index n and thickness of the N-type doped polysilicon layer and the P-type doped polysilicon layer can refer to the previous text and will not be repeated here.

[0182] In addition, the thickness of the P-type doped polysilicon layer after passivation treatment and the thickness of the P-type doped polysilicon layer before passivation treatment, the relationship between the extinction coefficient k and the refractive index n, as well as the thickness of the N-type doped polysilicon layer after passivation treatment and the thickness of the N-type doped polysilicon layer before passivation treatment, the relationship between the extinction coefficient k and the refractive index n can be determined according to the process conditions of the passivation treatment, the density of the P-type doped polysilicon layer and the N-type doped polysilicon layer before passivation treatment, and the etching characteristics of the electrode slurry for subsequently forming the positive electrode and the negative electrode, and are not specifically limited here.

[0183] Exemplarily, the ratio of the thickness of the P-type doped polysilicon layer after the passivation treatment to the thickness of the P-type doped polysilicon layer before the passivation treatment may be greater than or equal to 0.95 and less than or equal to 1. For example, the ratio of the thickness of the P-type doped polysilicon layer after the passivation treatment to the thickness of the P-type doped polysilicon layer before the passivation treatment may be 0.95, 0.96, 0.97, 0.98, 0.99 or 1, etc. In this case, the thickness of the P-type doped polysilicon layer before and after the passivation treatment is substantially the same, which helps to prevent the electrode slurry for manufacturing the negative electrode from easily penetrating the P-type doped polysilicon layer due to a large reduction in the thickness of the P-type doped polysilicon layer after the passivation treatment, thereby ensuring that the P-type doped polysilicon layer has a high passivation effect.

[0184] Exemplarily, the ratio of the refractive index n of the P-type doped polysilicon layer after the passivation treatment to the refractive index n of the P-type doped polysilicon layer before the passivation treatment may be greater than or equal to 1 and less than or equal to 1.05. For example, the ratio of the refractive index n of the P-type doped polysilicon layer after the passivation treatment to the refractive index n of the P-type doped polysilicon layer before the passivation treatment may be 1, 1.01, 1.02, 1.03, 1.04 or 1.05, etc.

[0185] Exemplarily, the ratio of the extinction coefficient k of the P-type doped polysilicon layer after the passivation treatment to the extinction coefficient k of the P-type doped polysilicon layer before the passivation treatment may be greater than or equal to 0.95 and less than or equal to 1. For example, the ratio of the extinction coefficient k of the P-type doped polysilicon layer after the passivation treatment to the extinction coefficient k of the P-type doped polysilicon layer before the passivation treatment may be 0.95, 0.96, 0.97, 0.98, 0.99 or 1, etc.

[0186] When the above technical solution is adopted, the ratio of the refractive index n of the P-type doped polysilicon layer after passivation treatment to the refractive index n of the P-type doped polysilicon layer before passivation treatment is greater than or equal to 1 and less than or equal to 1.05; and / or, when the ratio of the extinction coefficient k of the P-type doped polysilicon layer after passivation treatment to the extinction coefficient k of the P-type doped polysilicon layer before passivation treatment is greater than or equal to 0.95 and less than or equal to 1, the film density of the P-type doped polysilicon layer after passivation treatment becomes greater, which is further beneficial to prevent the electrode slurry for manufacturing the negative electrode from penetrating the P-type doped polysilicon layer, ensuring that the P-type doped polysilicon layer has a higher passivation effect.

[0187] Exemplarily, the ratio between the thickness of the N-type doped polysilicon layer after the passivation treatment and the thickness of the N-type doped polysilicon layer before the passivation treatment can be greater than or equal to 0.85 and less than or equal to 0.9. For example, the ratio between the thickness of the N-type doped polysilicon layer after the passivation treatment and the thickness of the N-type doped polysilicon layer before the passivation treatment can be 0.85, 0.86, 0.87, 0.88, 0.89 or 0.9, etc. In this case, the film thickness of the N-type doped polysilicon layer itself becomes smaller after the passivation treatment, which is conducive to improving its own compactness, preventing the electrode slurry for manufacturing the positive electrode from penetrating the N-type doped polysilicon layer, and ensuring that the N-type doped polysilicon layer has a higher passivation effect.

[0188] Exemplarily, the ratio of the refractive index n of the N-type doped polysilicon layer after the passivation treatment to the refractive index n of the N-type doped polysilicon layer before the passivation treatment may be greater than or equal to 0.3 and less than or equal to 1.1. For example, the ratio of the refractive index n of the N-type doped polysilicon layer after the passivation treatment to the refractive index n of the N-type doped polysilicon layer before the passivation treatment may be 0.3, 0.5, 0.8, 1, 1.02, 1.03, 1.04, 1.06, 1.08 or 1.1, etc.

[0189] Exemplarily, the ratio of the extinction coefficient k of the N-type doped polysilicon layer after the passivation treatment to the extinction coefficient k of the N-type doped polysilicon layer before the passivation treatment may be greater than or equal to 1.9 and less than or equal to 2.1. For example, the ratio of the extinction coefficient k of the N-type doped polysilicon layer after the passivation treatment to the extinction coefficient k of the N-type doped polysilicon layer before the passivation treatment may be 1.9, 1.92, 1.94, 1.96, 1.98, 2.0, 2.2, 2.4, 2.6, 2.8 or 2.1, etc.

[0190] When the above technical solution is adopted, the ratio of the refractive index n of the N-type doped polysilicon layer after passivation treatment to the refractive index n of the N-type doped polysilicon layer before passivation treatment is greater than or equal to 0.3 and less than or equal to 1.1, and the ratio of the extinction coefficient k of the N-type doped polysilicon layer after passivation treatment to the extinction coefficient k of the N-type doped polysilicon layer before passivation treatment can be greater than or equal to 1.9 and less than or equal to 2.1. The beneficial effects are similar to the beneficial effects of the ratio of the thickness of the N-type doped polysilicon layer after passivation treatment to the thickness of the N-type doped polysilicon layer before passivation treatment being greater than or equal to 0.85 and less than or equal to 0.9, which will not be repeated here.

[0191] Exemplarily, after forming the surface passivation layer, as Fig.13As shown, a process such as screen printing can be used to form a positive electrode 15 located on the side of the P-type doped polysilicon layer 12 away from the semiconductor substrate 11, and a negative electrode 16 located on the side of the N-type doped polysilicon layer 13 away from the semiconductor substrate 11. The depths to which the positive electrode 15 and the negative electrode 16 extend into the P-type doped polysilicon layer 12 and the N-type doped polysilicon layer 13, respectively, along the thickness direction of the semiconductor substrate 11 can refer to the above.

[0192] It should be noted that, as mentioned above, whether it is the test of the extinction coefficient k and the refractive index n of the first intrinsic polysilicon layer and the second intrinsic polysilicon layer, or the test of the extinction coefficient k and the refractive index n of the P-type doped polysilicon layer and the N-type doped polysilicon layer, it is necessary to expose the side of the film layer to be tested away from the semiconductor substrate, and then under the same test conditions, measure the extinction coefficient k and the refractive index n of the film layer to be tested by testing instruments such as an ellipsometer to improve the accuracy of the test results.

[0193] The embodiment of the present invention also provides the following specific examples, taking the manufacture of back-contact cells as an example to specifically illustrate the process of manufacturing solar cells:

[0194] Example 1

[0195] The first step is to place the cleaned and polished crystalline silicon wafers in a quartz boat in sequence, and to uniformly transport the quartz boat filled with crystalline silicon wafers from the bottom of the reaction furnace to the inner furnace chamber at a certain speed. Each crystalline silicon wafer includes a first surface and a second surface that are arranged oppositely.

[0196] The second step is to raise the temperature in the inner and outer furnace chambers to 607±5°C, and introduce oxygen into the inner furnace chamber to oxidize the surface of the crystalline silicon wafer, so as to form a first interface passivation layer on at least the first surface of the crystalline silicon wafer. The oxidation time is 15 minutes, and the pressure in the inner and outer furnace chambers is maintained within the range of 300±50mTorr.

[0197] Step 3: The temperature in the inner and outer furnace chambers was stabilized within the range of 572±5°C, SiH4 was introduced into the inner furnace chamber, and the first intrinsic polysilicon layer was formed on the first interface passivation layer to obtain sample A. The polysilicon film deposition time was 155 min, and the pressure in the inner and outer furnace chambers was maintained within the range of 300±50 mTorr.

[0198] Step 4: Place the boat containing sample A into a diffusion furnace tube, the temperature of which is 800°C.

[0199] Step 5: Boron source / oxygen / nitrogen are introduced for diffusion. The pressure in the furnace tube is 100mbar-200mbar and the temperature is 860-870°C.

[0200] Step 6: Nitrogen is introduced to carry out oxygen-free advancement, so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer. The temperature is 910°C-920°C. Then, high oxygen and low oxygen are introduced at the same time, the temperature in the furnace tube is raised to 930°C, and the pressure in the furnace tube is increased to 300mbar-500mbar, and the oxidation process is carried out. Then, the introduction of high oxygen is stopped, the temperature in the furnace tube is lowered, and the boat is taken out to obtain sample B.

[0201] Step 7: Perform a wet process on sample B to remove the P-type doped polysilicon layer and the first interface passivation layer located on the partial area of ​​the first surface.

[0202] Step 8: The quartz boat filled with sample B processed by the wet process is uniformly transported from the bottom of the reaction furnace to the inner furnace chamber at a certain speed. Then, a second interface passivation layer is formed on one side of the first surface of sample B. The temperature is 600±5℃, the time is 7min, and the pressure in the inner and outer furnace chambers is maintained within the range of 300±50mTorr.

[0203] Step 9: Form a second intrinsic polysilicon layer on the second interface passivation layer to obtain sample C. The temperature is 580±5° C., the time is 42 min, and the pressure in the inner and outer furnace chambers is maintained in the range of 300±50 mTorr.

[0204] Step 10. Place the boat containing sample C into the furnace tube, the temperature inside the furnace tube is 800°C.

[0205] Step 11: introduce phosphorus source / oxygen / nitrogen for diffusion, the pressure in the furnace tube is 650 mbar, and the temperature is 860°C. Then, introduce high oxygen and low oxygen at the same time, raise the temperature in the furnace tube to 865°C, and increase the pressure in the furnace tube to 950 mbar, and perform an oxidation process to form an N-type doped polysilicon layer from the second intrinsic polysilicon layer. Then, stop introducing high oxygen, cool the furnace tube, and remove the boat to obtain sample D.

[0206] Step 12: Perform a wet process on sample D to remove the N-type doped polysilicon layer and the second interface passivation layer at least partially located on the P-type doped polysilicon layer.

[0207] Step 13: Place the sample D processed by the wet process into the process chamber, and form a vacuum constant temperature environment in the process chamber with a target temperature of 400°C-450°C.

[0208] Step 14: Introduce H2O vapor into the process chamber to deposit on the SiO2 surface to form a passivation interface.

[0209] Step 15: TMA and H2O vapor are alternately introduced into the process chamber to grow a highly passivated Al2O3 film. The vacuum is then purged to complete the process and sample E is obtained.

[0210] Table 1 Related parameters of the first intrinsic polysilicon layer and the P-type doped polysilicon layer

[0211]

[0212] Table 2 Related parameters of the second intrinsic polysilicon layer and the N-type doped polysilicon layer

[0213]

[0214] It can be seen from the data shown in Table 1 that the extinction coefficient k of the P-type doped polysilicon layer in sample B is smaller than the extinction coefficient k of the N-type doped polysilicon layer in sample D, and the extinction coefficient k of the P-type doped polysilicon layer in sample E is smaller than the extinction coefficient k of the N-type doped polysilicon layer in sample E, so as to prevent the manufactured positive electrode from penetrating the P-type doped polysilicon layer, improve the matching between the electrode slurry corresponding to the P-type doped polysilicon layer and the positive electrode, and ensure that the P-type doped polysilicon layer has a higher field passivation effect, and reduce the carrier recombination rate on the backlight side. The embodiment of the present invention only provides a specific example of the manufacturing method when the extinction coefficient k of the P-type doped polysilicon layer and the N-type doped polysilicon layer included in the solar cell is in the table, which does not mean that the extinction coefficient k of the P-type doped polysilicon layer and the N-type doped polysilicon layer included in the solar cell is only the specific value in the table, nor does it mean that only the above-mentioned manufacturing parameters can be used to manufacture the solar cell provided by the embodiment of the present invention. As for when the extinction coefficient k of the P-type doped polysilicon layer and the N-type doped polysilicon layer included in the solar cell is other reasonable values, the corresponding manufacturing conditions can be reasonably adjusted according to the above examples. For example: the extinction coefficient k and the density of the doped polysilicon layer formed based on the intrinsic polysilicon layer can be adjusted by adjusting the formation time and / or formation temperature of the intrinsic polysilicon layer. Specifically, within a certain range, the longer the corresponding formation time and the lower the temperature of the intrinsic polysilicon layer, the smaller the extinction coefficient k of the doped polysilicon layer formed by the intrinsic polysilicon layer, and the denser the film layer.

[0215] In a fourth aspect, an embodiment of the present invention provides a photovoltaic module, which includes the solar cell provided by the first aspect and various implementations thereof.

[0216] The beneficial effects of the fourth aspect and its various implementations in the embodiments of the present invention can be analyzed with reference to the beneficial effects of the first aspect and its various implementations, and will not be repeated here.

[0217] In the above description, the technical details of the patterning and etching of each layer are not described in detail. However, those skilled in the art should understand that various technical means can be used to form layers, regions, etc. of desired shapes. In addition, in order to form the same structure, those skilled in the art can also design methods that are not completely the same as the methods described above. In addition, although the various embodiments are described above separately, this does not mean that the measures in the various embodiments cannot be used in combination to advantage.

[0218] The embodiments of the present disclosure are described above. However, these embodiments are for illustrative purposes only and are not intended to limit the scope of the present disclosure. The scope of the present disclosure is defined by the appended claims and their equivalents. Without departing from the scope of the present disclosure, a person skilled in the art may make a variety of substitutions and modifications, which should all fall within the scope of the present disclosure.

Claims

1. A solar cell, characterized in that: include: A semiconductor substrate, wherein the semiconductor substrate comprises a first region and a second region; the first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate; A P-type doped polysilicon layer is formed at least on the first region; An N-type doped polysilicon layer is formed at least on the second region; at least a portion of the N-type doped polysilicon layer and at least a portion of the P-type doped polysilicon layer are spaced apart from each other; Wherein, the ratio of the refractive index n of the N-type doped polysilicon layer to the refractive index n of the P-type doped polysilicon layer is greater than or equal to 0.9 and less than or equal to 1.1; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.

1.

2. The solar cell according to claim 1, characterized in that The solar cell further comprises a surface passivation layer; the surface passivation layer at least covers a side of the P-type doped polysilicon layer away from the semiconductor substrate and a side of the N-type doped polysilicon layer away from the semiconductor substrate; The ratio of the extinction coefficient k of the N-type doped polysilicon layer to the extinction coefficient k of the P-type doped polysilicon layer is greater than or equal to 1.5 and less than or equal to 2.5; and / or the difference between the extinction coefficient k of the N-type doped polysilicon layer and the extinction coefficient k of the P-type doped polysilicon layer is greater than or equal to 0.2 and less than or equal to 0.

5.

3. The solar cell according to claim 1, characterized in that The solar cell further comprises a positive electrode in ohmic contact with the P-type doped polysilicon layer, and a negative electrode in ohmic contact with the N-type doped polysilicon layer; Along the thickness direction of the semiconductor substrate, a depth to which at least a portion of the positive electrode extends into the P-type doped polysilicon layer is greater than or equal to a depth to which at least a portion of the negative electrode extends into the N-type doped polysilicon layer.

4. The solar cell according to claim 1, characterized in that The solar cell further comprises a positive electrode in ohmic contact with the P-type doped polysilicon layer, and a negative electrode in ohmic contact with the N-type doped polysilicon layer; Along the thickness direction of the semiconductor substrate, at least part of the positive electrode extends to a depth greater than or equal to 80nm and less than or equal to 100nm in the P-type doped polysilicon layer; and / or, along the thickness direction of the semiconductor substrate, at least part of the negative electrode extends to a depth greater than or equal to 50nm and less than or equal to 80nm in the N-type doped polysilicon layer.

5. The solar cell according to any one of claims 1 to 4, characterized in that: The solar cell further comprises a first tunnel passivation layer, wherein the first tunnel passivation layer is located between the P-type doped polysilicon layer and the semiconductor substrate; and / or, The solar cell further comprises a second tunneling passivation layer, wherein the second tunneling passivation layer is at least located between the N-type doped polysilicon layer and the semiconductor substrate; and or, The solar cell is a back contact cell.

6. A semiconductor structure, characterized in that: The semiconductor structure is applied to a solar cell, and the semiconductor structure comprises: A semiconductor substrate, wherein the semiconductor substrate comprises a first region and a second region; the first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate; A P-type doped polysilicon layer is formed at least on the first region; An N-type doped polysilicon layer is formed at least on the second region; at least a portion of the N-type doped polysilicon layer and at least a portion of the P-type doped polysilicon layer are spaced apart from each other; Wherein, the ratio of the refractive index n of the N-type doped polysilicon layer to the refractive index n of the P-type doped polysilicon layer is greater than or equal to 0.8 and less than or equal to 1.2; and / or; the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.

2.

7. A method for manufacturing a solar cell, characterized in that: include: Providing a semiconductor substrate; The semiconductor substrate includes a first region and a second region; the first region and the second region are located on the same surface of the semiconductor substrate, or the first region and the second region are located on two opposite surfaces of the semiconductor substrate respectively; forming a P-type doped polysilicon layer at least on the first region; An N-type doped polysilicon layer is formed at least on the second region; at least a portion of the N-type doped polysilicon layer and at least a portion of the P-type doped polysilicon layer are arranged at intervals; Wherein, the ratio of the refractive index n of the N-type doped polysilicon layer to the refractive index n of the P-type doped polysilicon layer is greater than or equal to 0.9 and less than or equal to 1.1; and / or, the absolute value of the difference between the refractive index n of the P-type doped polysilicon layer and the refractive index n of the N-type doped polysilicon layer is greater than or equal to 0 and less than or equal to 0.

1.

8. The method for manufacturing a solar cell according to claim 7, characterized in that: When the first region and the second region are located on the same surface of the semiconductor substrate, The forming of the P-type doped polysilicon layer at least on the first region includes: forming a first intrinsic polysilicon layer covering the first region and the second region; performing diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer; selectively removing a portion of the P-type doped polysilicon layer located at least on a portion of the second region; and the forming of the N-type doped polysilicon layer at least on the second region includes: forming a second intrinsic polysilicon layer covering at least the P-type doped polysilicon layer and the second region; performing diffusion treatment on the second intrinsic polysilicon layer so that the second intrinsic polysilicon layer forms an N-type doped polysilicon layer; selectively removing a portion of the N-type doped polysilicon layer located on at least a portion of the P-type doped polysilicon layer; Or, the forming of an N-type doped polysilicon layer at least on the second region includes: forming a second intrinsic polysilicon layer covering the first region and the second region; performing diffusion treatment on the second intrinsic polysilicon layer so that the second intrinsic polysilicon layer forms an N-type doped polysilicon layer; selectively removing a portion of the N-type doped polysilicon layer located at least on a portion of the first region; and, the forming of the P-type doped polysilicon layer at least on the first region includes: forming a first intrinsic polysilicon layer covering at least the N-type doped polysilicon layer and the first region; performing diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer; and selectively removing a portion of the P-type doped polysilicon layer located on at least a portion of the N-type doped polysilicon layer.

9. The method for manufacturing a solar cell according to claim 7, characterized in that: In the case where the first region and the second region are located on two opposite sides of the semiconductor substrate, The forming of the P-type doped polysilicon layer at least on the first region comprises: forming a first intrinsic polysilicon layer covering at least the first region; performing diffusion treatment on the first intrinsic polysilicon layer so that the first intrinsic polysilicon layer forms a P-type doped polysilicon layer; The forming of an N-type doped polysilicon layer at least on the second region includes: forming a second intrinsic polysilicon layer covering at least the second region; and performing diffusion treatment on the second intrinsic polysilicon layer to form an N-type doped polysilicon layer.

10. The method for manufacturing a solar cell according to claim 8 or 9, characterized in that: The extinction coefficient k of the first intrinsic polysilicon layer is smaller than the extinction coefficient k of the P-type doped polysilicon layer; and / or, The refractive index n of the first intrinsic polysilicon layer is greater than or equal to the refractive index n of the P-type doped polysilicon layer.

11. The method for manufacturing a solar cell according to claim 8 or 9, characterized in that: The refractive index n of the second intrinsic polysilicon layer is less than the refractive index n of the N-type doped polysilicon layer; and / or, The extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the N-type doped polysilicon layer.

12. The method for manufacturing a solar cell according to claim 8 or 9, characterized in that: The thickness of the second intrinsic polysilicon layer is less than the thickness of the first intrinsic polysilicon layer; and / or, The ratio of the thickness of the second intrinsic polysilicon layer to the thickness of the first intrinsic polysilicon layer is greater than or equal to 0.55 and less than or equal to 0.8; and / or, The difference between the thickness of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is greater than or equal to -140 nm and less than or equal to -100 nm; and / or, The refractive index n of the second intrinsic polysilicon layer is less than the refractive index n of the first intrinsic polysilicon layer; and / or, The difference between the refractive index n of the second intrinsic polysilicon layer and the refractive index n of the first intrinsic polysilicon layer is greater than or equal to -0.12 and less than or equal to -0.1; and / or, The extinction coefficient k of the second intrinsic polysilicon layer is greater than the extinction coefficient k of the first intrinsic polysilicon layer; and / or, A difference between the extinction coefficients k of the second intrinsic polysilicon layer and the first intrinsic polysilicon layer is greater than or equal to 0.02 and less than or equal to 0.

3.

13. The method for manufacturing a solar cell according to claim 8 or 9, characterized in that: The formation temperature of the second intrinsic polysilicon layer is greater than the formation temperature of the first intrinsic polysilicon layer; and / or, The formation time of the second intrinsic polysilicon layer is shorter than the formation time of the first intrinsic polysilicon layer; and / or, The temperature when the first intrinsic polysilicon layer is diffused is higher than the temperature when the second intrinsic polysilicon layer is diffused.

14. The method for manufacturing a solar cell according to claim 8 or 9, characterized in that: After forming the P-type doped polysilicon layer at least on the first region and forming the N-type doped polysilicon layer at least on the second region, the method for manufacturing a solar cell further includes: At least one side of the P-type doped polysilicon layer facing away from the semiconductor substrate and one side of the N-type doped polysilicon layer facing away from the semiconductor substrate are passivated to form a surface passivation layer covering at least one side of the P-type doped polysilicon layer facing away from the semiconductor substrate and one side of the N-type doped polysilicon layer facing away from the semiconductor substrate; after the passivation treatment, the ratio between the extinction coefficients k of the N-type doped polysilicon layer and the P-type doped polysilicon layer is greater than or equal to 1.5 and less than or equal to 2.

5.

15. The method for manufacturing a solar cell according to claim 14, characterized in that: The ratio of the thickness of the P-type doped polysilicon layer after the passivation treatment to the thickness of the P-type doped polysilicon layer before the passivation treatment is greater than or equal to 0.95 and less than or equal to 1; and / or, The ratio of the refractive index n of the P-type doped polysilicon layer after the passivation treatment to the refractive index n of the P-type doped polysilicon layer before the passivation treatment is greater than or equal to 1 and less than or equal to 1.05; and / or, A ratio of an extinction coefficient k of the P-type doped polysilicon layer after the passivation treatment to an extinction coefficient k of the P-type doped polysilicon layer before the passivation treatment is greater than or equal to 0.95 and less than or equal to 1.

16. The method for manufacturing a solar cell according to claim 14, characterized in that: The ratio of the thickness of the N-type doped polysilicon layer after the passivation treatment to the thickness of the N-type doped polysilicon layer before the passivation treatment is greater than or equal to 0.85 and less than or equal to 0.9; and / or, The ratio of the refractive index n of the N-type doped polysilicon layer after the passivation treatment to the refractive index n of the N-type doped polysilicon layer before the passivation treatment is greater than or equal to 0.3 and less than or equal to 1.1; and / or, A ratio of an extinction coefficient k of the N-type doped polysilicon layer after the passivation treatment to an extinction coefficient k of the N-type doped polysilicon layer before the passivation treatment is greater than or equal to 1.9 and less than or equal to 2.

1.

17. A photovoltaic module, characterized in that: The invention comprises a solar cell as claimed in any one of claims 1 to 5.