Cathode active material for lithium secondary battery and method for preparing same

By forming an organic polyphosphate or organic polyphosphate ester coating on the surface of lithium metal oxide particles of lithium secondary batteries and doping elements, the structural unevenness and difficulty in removing impurities caused by lithium precipitation in lithium secondary batteries are solved. Problem, improving the stability and electrical performance of the battery.

CN119092659APending Publication Date: 2024-12-06SK ON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991827.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-11-26
Filing Date
2019-11-22
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When lithium metal oxides in lithium secondary batteries are used as positive electrode active materials, they are prone to uneven chemical structure due to lithium precipitation, and the structure is deformed or damaged after repeated charging and discharge, resulting in a decrease in life stability and capacity retention rate. The existing washing methods cannot be sufficient. Removal of impurities and may damage the surface of the particles.

Method used

The organic polyphosphate or organic polyphosphate ester coating is formed on the surface of lithium metal oxide particles, and impurities are removed by washing with a specific washing solution and structural stability is enhanced. Nickel-based lithium oxide is used and elements such as Co, Mn, Al, Zr, Ti to improve chemical and mechanical stability.

Benefits of technology

It significantly improves the operating stability and electrical performance of lithium secondary batteries, extends the battery life, enhances the capacity retention rate and power output, avoids lithium ion side reactions, and improves the stability of the crystal structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092659A_ABST
    Figure CN119092659A_ABST
Patent Text Reader

Abstract

A positive electrode active material for a lithium secondary battery includes: lithium metal oxide particles; and an organic polyphosphate ester or an organic polyphosphonate ester formed on at least a portion of the surface of the lithium metal oxide particles. By means of the organic polyphosphate or the organic polyphosphonate, the chemical stability of the lithium metal oxide particles can be improved and surface residues can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the patent application with application number 201911157506.2, application date November 22, 2019, and invention name “Positive electrode active material for lithium secondary battery and preparation method thereof”. Cross-references to related applications and priority claims

[0002] This application claims the benefit of Korean Patent Application No. 10-2018-0147722 filed on November 26, 2018 in the Korean Intellectual Property Office (KIPO), the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0003] The present invention relates to a positive electrode active material for a lithium secondary battery and a method for preparing the same. More specifically, the present invention relates to a lithium metal oxide positive electrode active material for a lithium secondary battery and a method for preparing the same. Background Art

[0004] With the development of information and display technology, secondary batteries that can be repeatedly charged and discharged have been widely used as power sources for mobile electronic devices such as camcorders, mobile phones, laptop computers, etc. Recently, secondary batteries or battery packs including the secondary batteries are being developed and used as environmentally friendly power sources for electric vehicles such as hybrid vehicles.

[0005] The secondary battery includes, for example, a lithium secondary battery, a nickel-cadmium battery, a nickel-hydrogen battery, etc. The lithium secondary battery stands out due to high operating voltage and high energy density per unit weight, high charging rate, compact size, and the like.

[0006] For example, a lithium secondary battery may include: an electrode assembly including a positive electrode, a negative electrode, and a separator; and an electrolyte that immerses the electrode assembly. The lithium secondary battery may also include a case having, for example, a pouch shape.

[0007] Lithium metal oxide may be used as a positive electrode active material of a lithium secondary battery, and nickel-based lithium metal oxide may be used as the lithium metal oxide.

[0008] As the application range of lithium secondary batteries expands, the demand for more improved life, capacity and operational stability increases. In lithium metal oxides used as positive electrode active materials, chemical structure inhomogeneity due to lithium precipitation may occur, and lithium secondary batteries with desired capacity and life may not be obtained. In addition, when charging and discharging operations are repeated, the structure of lithium metal oxides may be deformed or damaged, resulting in reduced life stability and capacity retention.

[0009] For example, Korean Patent Application No. 10-0821523 discloses a method of removing lithium salt impurities by washing lithium complex metal oxide with water. However, impurities may not be sufficiently removed by this method, and surface damage of positive electrode active material particles may be caused during the washing process. Summary of the invention

[0010] According to one aspect of the present invention, a positive electrode active material for a lithium secondary battery having improved operational stability and electrical properties and a method for preparing the same are provided.

[0011] According to one aspect of the present invention, a lithium secondary battery having improved operational stability and electrical performance is provided.

[0012] According to an exemplary embodiment of the present invention, a positive electrode active material for a lithium secondary battery includes: lithium metal oxide particles; and an organic polyphosphate or organic polyphosphonate formed on at least a portion of a surface of the lithium metal oxide particles.

[0013] In some embodiments, the organic polyphosphate is obtained from an organic polyphosphate compound represented by the following structural formula 1 or an organic polyphosphate salt thereof, and the organic polyphosphonate is obtained from an organic polyphosphonate compound represented by the following structural formula 2 or an organic polyphosphonate salt thereof.

[0014] [Structural Formula 1]

[0015]

[0016] [Structural Formula 2]

[0017]

[0018] In the above structural formula 1 and structural formula 2, m may be an integer from 2 to 20, R1 may represent a C1-C10 hydrocarbon group that can be substituted by a substituent, and the substituent may include a halogen, a cyano group, a hydroxyl group, a phosphoric acid group, a carboxyl group or a salt thereof.

[0019] In some embodiments, the hydrocarbon group included in R1 can be selected from the group consisting of carbon-carbon double bonds, -O-, -S-, -CO-, -OCO-, -SO-, -CO-O-, -O-CO-O-, -S-CO-, -S-CO-O-, -CO-NH-, -NH-CO-O-, -NR'-, At least one of the group consisting of -R'OH-, -SS- and -SO2- is substituted or linked, and R' is hydrogen or a C1-C8 alkyl group.

[0020] In some embodiments, the organic polyphosphate compound or the organic polyphosphonate compound may include at least one of the compounds represented by Chemical Formula 1 to Chemical Formula 3 below.

[0021] [Chemical formula 1]

[0022]

[0023] [Chemical formula 2]

[0024]

[0025] [Chemical formula 3]

[0026]

[0027] In some embodiments, the organic polyphosphate or organic polyphosphonate includes a compound represented by Chemical Formula 4 below.

[0028] [Chemical formula 4]

[0029]

[0030] In the above Chemical Formula 4, n may be an integer of 2 to 10.

[0031] In some embodiments, the lithium metal oxide particles include a nickel-based lithium oxide represented by the following Formula 1.

[0032] [General formula 1]

[0033] Li x Ni y M 1-y O2

[0034] In the above General Formula 1, 0.95≤x≤1.08, y≥0.5, and M may be at least one element selected from the group consisting of Co, Mn, Al, Zr, Ti, B, Mg, and Ba.

[0035] In some embodiments, in Formula 1, 0.8≤y≤0.93.

[0036] In some embodiments, in Formula 1, M may include Co and Mn.

[0037] In some embodiments, the lithium metal oxide particles may include a dopant or coating including at least one of Al, Zr, and Ti.

[0038] In some embodiments, the organopolyphosphate or organopolyphosphonate may form a coating, a ligand bond, or a complex bond on the surface of the lithium metal oxide particle.

[0039] In some embodiments, the lithium metal oxide particles have a layer structure, and grain boundaries at a surface portion of the lithium metal oxide particles may be coated with an organic polyphosphate or an organic polyphosphonate.

[0040] According to an exemplary embodiment of the present invention, in a method of preparing a positive electrode active material for a lithium secondary battery, lithium metal oxide particles are prepared and washed with a washing solution containing an organic polyphosphate compound or an organic polyphosphonate compound.

[0041] In some embodiments, the organic polyphosphate compound or the organic polyphosphonate compound may be added in an amount ranging from 0.1 wt % to 2 wt % based on the total weight of the lithium metal oxide particles.

[0042] In some embodiments, the organic polyphosphate compound or the organic polyphosphonate compound may be added in an amount ranging from 0.2 wt % to 1 wt % based on the total weight of the lithium metal oxide particles.

[0043] In some embodiments, the lithium metal oxide particles may be mixed with at least one of Al 2 O 3 , ZrO 2 , and TiO 2 and annealed before washing the lithium metal oxide particles.

[0044] According to an exemplary embodiment of the present invention, a lithium secondary battery includes: a positive electrode including lithium metal oxide particles and an organic polyphosphate or organic polyphosphonate formed on at least a portion of a surface of the lithium metal oxide particles; a negative electrode; and a separator layer interposed between the positive electrode and the negative electrode.

[0045] According to an exemplary embodiment of the present invention, an organic polyphosphate or organic polyphosphonate may be formed on the surface of the lithium metal oxide particles so that a metal ion complex may be formed when the layer structure of the lithium metal oxide particles is damaged. Therefore, compared with the case where inorganic phosphoric acid or inorganic phosphate may be used, the stability of the structure or crystal may be enhanced, and the stability and capacity / power output of the positive electrode active material may also be improved.

[0046] In an exemplary embodiment, the organic polyphosphate or organic polyphosphonate may be introduced through a washing process using a washing solution. Thus, impurities such as lithium salt precipitates remaining on the surface of the lithium metal oxide particles may be removed while the organic polyphosphate or organic polyphosphonate is formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 is a graph showing capacity retention rates of battery cells according to Example 3-3, Comparative Example 4, Comparative Example 5, and Comparative Example 7 during repeated charge / discharge operations.

[0048] Figure 2 is a TOF-SIMS analysis image of the surface of the lithium metal oxide particle according to Example 3-3. DETAILED DESCRIPTION

[0049] <Positive electrode active material and preparation method thereof>

[0050] A positive electrode active material for a lithium secondary battery according to an exemplary embodiment (hereinafter, simply referred to as a positive electrode active material) may include lithium metal oxide particles and an organic polyphosphate coating or an organic polyphosphonate coating (hereinafter, also abbreviated as an organic polyphosphate / phosphonate coating) formed on surfaces of the lithium metal oxide particles.

[0051] The term "lithium metal oxide" used herein refers to a composite oxide including lithium and at least one metal other than lithium. In an exemplary embodiment, the lithium metal oxide may include a nickel-based lithium oxide.

[0052] For example, the nickel-based lithium oxide may be represented by the following General Formula 1.

[0053] [General formula 1]

[0054] Li x Ni y M 1-y O2

[0055] In the above General Formula 1, 0.95≤x≤1.08, y≥0.5, and M may be at least one element selected from Co, Mn, Al, Zr, Ti, B, Mg, and Ba.

[0056] For example, nickel (Ni) may be an element related to the capacity of a lithium secondary battery in the lithium metal oxide of Formula 1. For example, as the amount of nickel increases, the capacity and power output of the lithium secondary battery may be improved.

[0057] In one embodiment, in Formula 1, 0.8≤y≤0.93, so that a positive electrode active material providing high capacity and high power output can be easily obtained.

[0058] M may include cobalt (Co) and manganese (Mn), so that conductivity and chemical stability can be added to high Ni compounds. For example, cobalt (Co) may be an element related to the conductivity and resistance of a lithium secondary battery. In one embodiment, M may include manganese (Mn), and Mn may be an element related to the mechanical stability and electrical stability of a lithium secondary battery.

[0059] Therefore, the lithium metal oxide particles may include a nickel-cobalt-manganese-based compound, and may provide a positive active material having improved capacity, power output, low resistance, and lifespan.

[0060] In some embodiments, the lithium metal oxide particles may further include a doping element or a coating element in addition to Ni, Co, and Mn. For example, the doping element or the coating element may include Al, Zr, and / or Ti, and may preferably include Al, Zr, and Ti.

[0061] In the nickel-cobalt-manganese-based lithium oxide, the amount of the doping element may be in the range of about 0.1 mol % to about 1 mol %, preferably in the range of about 0.5 mol % to about 1 mol %, based on the total molar number of Ni, Co, Mn and the doping element (e.g., Al, Zr and / or Ti). Within the above range, the chemical stability and structural stability of the lithium metal oxide particles may be enhanced without excessively reducing the activity of the positive electrode active material.

[0062] The coating element may be derived from a coating metal oxide such as Al2O3, ZrO2 and / or TiO2. The coating metal oxide may be added in an amount ranging from about 0.5 wt% to about 1 wt% based on the total weight of the nickel-cobalt-manganese-based lithium oxide.

[0063] In some embodiments, the lithium metal oxide particles may have a layer structure. For example, primary particles of lithium metal oxide may be aggregated into a layer structure to form lithium metal oxide particles as a positive electrode active material. The particle structure may facilitate the mobility of lithium ions generated from the positive electrode active material.

[0064] In some embodiments, an organopolyphosphate / phosphonate coating may be formed on the surface of the lithium metal oxide particles.

[0065] The term "organopolyphosphate / phosphonate coating" used herein may include a coating formed on substantially the entire surface of a lithium metal oxide particle, as well as a coating or an island layer formed on a portion of the surface of a lithium metal oxide particle.

[0066] In some embodiments, the organopolyphosphate / phosphonate coating may include organic ligand bonds attached to the surface of the lithium metal oxide particles, or organometallic complexes that bind to metal ions exposed on the surface of the lithium metal oxide particles.

[0067] In some embodiments, the grain boundaries at the surface portion of the lithium metal oxide particles may be coated by an organopolyphosphate / phosphonate coating.

[0068] In an exemplary embodiment, the organic polyphosphate coating may be derived from an organic polyphosphate compound or an organic polyphosphate salt.The organic polyphosphonate coating may be derived from an organic polyphosphonate compound or an organic polyphosphonate salt.

[0069] In the present specification, an organic polyphosphate compound may also mean an organic polyphosphate salt, and an organic polyphosphonate compound may also mean an organic polyphosphonate salt.

[0070] In some embodiments, the organic polyphosphate compound may include a compound represented by the following Structural Formula 1.

[0071] [Structural Formula 1]

[0072]

[0073] In some embodiments, the organic polyphosphonate compound may include a compound represented by the following Structural Formula 2.

[0074] [Structural Formula 2]

[0075]

[0076] In the above structural formula 1 and structural formula 2, m may be an integer of 2 to 20, and R1 may represent a C1-C10 hydrocarbon group that can be substituted with a substituent. The substituent may include a halogen, a cyano group, a hydroxyl group, a phosphoric acid group, a carboxyl group, or a salt thereof.

[0077] The term "hydrocarbyl" as used herein may include cyclic aliphatic groups, straight chain aliphatic groups, aromatic groups or combinations thereof. For example, the hydrocarbyl may include alkyl, alcohol, alkoxy, aryl (e.g., C6-C10), arylalkoxy (e.g., C6-C10), cycloalkyl (e.g., C3-C10) or polycyclic groups (e.g., C5-C10).

[0078] In some embodiments, the hydrocarbon group included in R1 can be selected from carbon-carbon double bonds, -O-, -S-, -CO-, -OCO-, -SO-, -CO-O-, -O-CO-O-, -S-CO-, -S-CO-O-, -CO-NH-, -NH-CO-O-, -NR'-, -R'OH-, At least one of the group consisting of -SS- and -SO2- is substituted or linked. R' may be hydrogen or a C1-C8 alkyl group.

[0079] In some embodiments, the organic polyphosphate compound or the organic polyphosphonate compound may include at least one of the compounds represented by Chemical Formula 1 (inositol hexaphosphate or phytic acid), Chemical Formula 2 (etidronic acid), and Chemical Formula 3 (nitrilotris(methylene)triphosphonic acid).

[0080] [Chemical formula 1]

[0081]

[0082] [Chemical formula 2]

[0083]

[0084] [Chemical formula 3]

[0085]

[0086] In some embodiments, the organic polyphosphate or organic polyphosphonate may include a compound represented by Chemical Formula 4 below.

[0087] [Chemical formula 4]

[0088]

[0089] In the above Chemical Formula 4, n may be an integer of 2 to 10.

[0090] The above-mentioned organic polyphosphate compound or organic polyphosphonate compound (hereinafter abbreviated as organic polyphosphate / phosphonate compound) can form a ligand bond or a complex bond on the surface of the lithium metal oxide particles, so that a large number of stable bonds can be formed with the metal ions exposed on the surface of the lithium metal oxide particles. Therefore, compared with when phosphoric acid or an inorganic phosphate can be added, the surface of the lithium metal oxide particles can be effectively protected from, for example, side reactions with the electrolyte.

[0091] For example, when phytic acid of Chemical Formula 1 can be used as an organic polyphosphate / phosphonate compound, one molecule of phytic acid can simultaneously form bonds with monovalent ions (e.g., lithium ions), divalent ions (e.g., nickel ions), and trivalent ions (e.g., cobalt ions or aluminum ions), as shown in Structural Formula 3.

[0092] [Structural Formula 3]

[0093]

[0094] Therefore, even when the layer structure of the lithium metal oxide particles may be deformed or damaged due to repeated charge / discharge operations, multiple bonds or multiple complexes can be formed with the exposed or released metal ions through the organic polyphosphate / phosphonate, so that byproducts caused by the side reactions of the metal ions can be prevented or reduced.

[0095] Furthermore, if the lithium metal oxide particles include an additional dopant or coating, the organic polyphosphate / phosphonate compound may be combined with the dopant or coating to further improve the chemical stability of the positive electrode active material.

[0096] Hereinafter, a method of preparing a positive electrode active material will be described in more detail.

[0097] In an exemplary embodiment, the lithium precursor and the nickel precursor may react with each other to form lithium metal oxide particles. The lithium precursor and the nickel precursor may include oxides or hydroxides of lithium and nickel, respectively. For example, the lithium precursor and the nickel precursor may react in a solution to form a primary lithium metal oxide by a precipitation reaction such as coprecipitation.

[0098] In some embodiments, in addition to the lithium precursor and the nickel precursor, another metal precursor (e.g., a cobalt precursor, a manganese precursor, etc.) may be reacted. In some embodiments, a nickel-cobalt-manganese precursor (e.g., Ni-Co-Mn hydroxide) may be used together with the lithium precursor.

[0099] In consideration of forming doping, another metal precursor may include a precursor of Al, Zr, and / or Ti in addition to the cobalt precursor and the manganese precursor.

[0100] In some embodiments, after preparing the lithium metal oxide, a firing process (or calcination process) may be further performed. For example, the firing process may be performed at a temperature range of about 600° C. to about 1000° C. The layer structure of the lithium metal oxide particles may be stabilized by the firing process and the doping elements may be fixed.

[0101] In some embodiments, the lithium metal oxide particles may be mixed with a metal oxide (eg, Al 2 O 3 , ZrO 2 , and / or TiO 2 ) for forming a coating layer, and then an additional annealing process may be further performed to form the coating layer.

[0102] In an exemplary embodiment, the lithium metal oxide particles may be washed or cleaned using a washing solution including an organic polyphosphate / phosphonate compound.

[0103] Unreacted precursors may remain or precipitate on the surface of lithium metal oxide particles synthesized by the precursor reaction as described above. In addition, during the synthesis, impurities and solution molecules may remain on the lithium metal oxide particles.

[0104] In some embodiments, an excess of lithium precursor may be used for production efficiency and synthesis stability of lithium metal oxide particles. In this case, lithium salt impurities including, for example, lithium hydroxide (LiOH) and lithium carbonate (Li2CO3) may remain on the surface of the lithium metal oxide particles.

[0105] The lithium salt impurities can be captured and removed by the organic polyphosphate / phosphonate compound contained in the washing solution. In the comparative example, when water is used in the washing solution, the lithium salt impurities can also be removed. However, oxidation of the surface of the lithium metal oxide particles and side reactions caused by water may occur, thereby causing destruction of the layer structure in the positive electrode active material.

[0106] However, according to an exemplary embodiment, the washing process may be performed using a washing solution including an organic compound, so that lithium salt impurities may be effectively removed by the multivalent structure of the organic polyphosphate / phosphonate compound while preventing oxidation of the particle surface and layer structure damage.

[0107] Additionally, as described above, an organic polyphosphate / phosphonate coating may be formed during the washing process, thereby achieving both impurity removal and passivation of the particle surface.

[0108] In some embodiments, the amount of the organic polyphosphate / phosphonate compound may be in the range of about 0.1 wt % to about 2 wt % based on the total weight of the lithium metal oxide particles. Within this range, sufficient coating and passivation may be achieved without excessively reducing the activity of the metal contained in the positive electrode active material.

[0109] Preferably, the amount of the organic polyphosphate / phosphonate compound may be in the range of about 0.2 wt % to about 1 wt % based on the total weight of the lithium metal oxide particles.

[0110] In some embodiments, the wash solution may be prepared by dissolving the organopolyphosphate / phosphonate compound in water. In one embodiment, an organic solvent, such as an alcohol solvent, may be used in the wash solution.

[0111] In some embodiments, a drying process may be further performed after the washing process. The organic polyphosphate / phosphonate coating may be fixed or stabilized on the particle surface through the drying process.

[0112] <Lithium Secondary Battery>

[0113] According to example embodiments, a lithium secondary battery may include: a positive electrode including lithium metal oxide particles, on which an organic polyphosphate / phosphonate coating may be formed; a negative electrode; and a separator.

[0114] The positive electrode may include a positive electrode active material layer formed by coating a positive electrode active material, which may include lithium metal oxide particles, on a positive electrode collector.

[0115] For example, lithium metal oxide particles may be mixed with a binder, a conductive agent and / or a dispersant in a solvent and stirred to form a slurry. The slurry may be coated on a positive electrode collector, and pressed and dried to obtain a positive electrode.

[0116] The positive electrode current collector may include stainless steel, nickel, aluminum, titanium, copper or an alloy thereof. Preferably, aluminum or an alloy thereof may be used.

[0117] The adhesive may include: an organic adhesive such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, etc.; or an aqueous adhesive such as styrene-butadiene rubber (SBR), which may be used together with a thickener such as carboxymethyl cellulose (CMC).

[0118] For example, a PVDF-based binder can be used as a positive electrode binder. In this case, the amount of the binder used to form the positive electrode active material layer can be reduced, and the amount of the positive electrode active material can be relatively increased. Therefore, the capacity and power output of the lithium secondary battery can be further improved.

[0119] Conductive agents may be added to promote electron mobility between active material particles. For example, conductive additives may include: carbon-based materials such as graphite, carbon black, graphene, carbon nanotubes, etc.; and / or metal-based materials such as tin, tin oxide, titanium oxide, perovskite materials (e.g., LaSrCoO3 or LaSrMnO3).

[0120] The negative electrode may include a negative electrode collector and a negative electrode active material layer formed by coating a negative electrode active material on the negative electrode collector.

[0121] The negative electrode active material may include a material capable of absorbing and discharging lithium ions. For example, carbon-based materials (such as crystalline carbon, amorphous carbon, carbon complex or carbon fiber), lithium alloys, silicon, tin, etc. may be used. Amorphous carbon may include hard carbon, coke, mesophase carbon microbeads (MCMB) calcined at 1500°C or lower, mesophase pitch-based carbon fibers (MPCF), etc. Crystalline carbon may include graphite-based materials, such as natural graphite, graphitized coke, graphitized MCMB, graphitized MPCF, etc. Lithium alloys may also include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium or indium.

[0122] The negative electrode current collector may include gold, stainless steel, nickel, aluminum, titanium, copper or an alloy thereof, and preferably may include copper or a copper alloy.

[0123] In some embodiments, the negative electrode active material may be mixed with a binder, a conductive agent and / or a dispersant in a solvent and stirred to form a slurry. The slurry may be coated on a negative electrode collector, and pressed and dried to obtain a negative electrode.

[0124] A binder and a conductive agent substantially the same or similar to those described above may be used. In some embodiments, the binder for the negative electrode may include an aqueous binder such as styrene-butadiene rubber (SBR), which may be used together with a thickener such as carboxymethyl cellulose (CMC) to improve compatibility with the carbon-based active material.

[0125] The separator may be between the positive electrode and the negative electrode. The separator may include a porous polymer film prepared from, for example, a polyolefin polymer (e.g., ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, ethylene / methacrylate copolymer, etc.). The separator may also be formed from a non-woven fabric including high melting point glass fiber, polyethylene terephthalate fiber, etc.

[0126] In an exemplary embodiment, an electrode unit may be defined by a positive electrode, a negative electrode and a separator, and a plurality of electrode units may be stacked to form an electrode assembly having, for example, a jelly roll shape. For example, the electrode assembly may be formed by winding, laminating or folding a separator.

[0127] The electrode assembly may be housed in a case together with an electrolyte to form a lithium secondary battery. In an exemplary embodiment, the electrolyte may include a nonaqueous electrolyte solution.

[0128] The non-aqueous electrolyte solution may include a lithium salt and an organic solvent. The lithium salt may be Li + X - Indicates that the anion X of the lithium salt - This may include, for example, F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - 、 CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - 、(CF3CF2SO2)2N - wait.

[0129] The organic solvent may include propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, γ-butyrolactone, propylene sulfite, tetrahydrofuran, etc. These may be used alone or in combination thereof.

[0130] The electrode tab may be formed by each of the positive electrode collector and the negative electrode collector to extend to one end of the case. The electrode tab may be welded with one end of the case to form an electrode lead exposed to the outside of the case.

[0131] The lithium secondary battery can be manufactured in a cylindrical shape using a can, a prismatic shape, a pouch shape, a button shape, or the like.

[0132] According to exemplary embodiments, the chemical stability of the positive electrode active material may be enhanced by the organic polyphosphate / phosphonate coating, so that the lifespan and long-term stability of the lithium secondary battery may be improved while suppressing the decrease in capacity and average voltage.

[0133] Hereinafter, preferred embodiments are proposed to more specifically describe the present invention. However, the following embodiments are provided only to illustrate the present invention, and those skilled in the relevant art will clearly understand that various changes and modifications can be made within the scope and spirit of the present invention. Such changes and modifications are appropriately included in the appended claims.

[0134] Examples and Comparative Examples

[0135] In the examples and comparative examples, lithium metal oxide particles (Li[Ni 0.88 Co 0.09 Mn 0.03 ]O2 or Li[Ni 0.8 Co 0.1 Mn 0.1 ]O2).

[0136] Specifically, lithium hydroxide as a lithium precursor and nickel-cobalt-manganese hydroxide as a composite metal precursor having a molar ratio corresponding to that shown in Table 1 were uniformly mixed at a molar ratio of 1.05:1 to form a mixture. The mixture was placed in a firing chamber, oxygen was supplied at a flow rate of 10 mL / min, and simultaneously heated to a temperature between 700°C and 800°C at a rate of 2°C / min, and the mixture was kept in the firing chamber at this temperature for 10 hours. After firing, the mixture was cooled to room temperature, and then ground and dispersed to obtain lithium metal oxide particles as a positive electrode active material.

[0137] Example

[0138] The organic polyphosphate / phosphonate compound listed in Table 1 was placed in 100 mL of pure water having a resistivity of 20 MΩcm or less to prepare a washing solution. The lithium metal oxide particles were placed in the washing solution, stirred for 10 minutes and filtered. The filtered lithium metal oxide particles were vacuum dried at a temperature of 250° C. for 12 hours to obtain the desired lithium metal oxide.

[0139] Comparative Example

[0140] In Comparative Example 1-4, the same process as in Example was performed except that only pure water having a resistivity of 20 MΩcm or less was used as a washing solution.

[0141] In Comparative Examples 5 and 6, the same process as in Example was performed except that phosphoric acid or an inorganic phosphate was used instead of the organic polyphosphate / phosphonate compound.

[0142] In Comparative Example 7, the same process as in Example 1 was performed except that carbon-free ammonium polyphosphate was used instead of the organic polyphosphate / phosphonate compound.

[0143] [Table 1]

[0144]

[0145]

[0146] Experimental example

[0147] (1) Measurement of residual lithium salt impurities

[0148] 5.0 g of each lithium metal oxide particle according to the embodiment and the comparative example was quantitatively added in a 250 mL flask with 100 g of deionized water, and then a magnetic bar was placed and stirred at a rate of 4 rpm for 10 minutes. A reduced pressure flask was used to filter the mixture, and 50 g of the mixture was collected. The collected mixture was automatically titrated with 0.1 N HCl in an automatic titrator to measure the amount of LiOH and Li2CO3, as shown in Table 2 below.

[0149] (2) Evaluation of battery performance

[0150] 2-1) Manufacturing of secondary battery cells

[0151] The lithium metal oxide particles of the embodiments and comparative examples, carbon black as a conductive additive, and PVDF as a binder are mixed in a weight ratio of 92:5:3 to form a slurry. The slurry is uniformly coated on an aluminum foil having a thickness of 15 μm and vacuum dried at 130°C to form a positive electrode for a lithium secondary battery. An electrode assembly is formed using a positive electrode, a lithium foil as a counter electrode, and a porous polyethylene layer (thickness: 21 μm) as a separator. Using an electrode assembly and an electrolyte solution (formed by dissolving 1.0 M LiPF6 in a solution containing ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7), a battery cell having a button half-cell shape is manufactured by a generally known method.

[0152] 2-2) Measurement of initial charge / discharge capacity

[0153] The battery cells of the examples and comparative examples were subjected to one cycle of charge (CC / CV 0.1C 4.3V 0.05CA cutoff) and discharge (CC 0.1C 3.0V cutoff), and the initial charge capacity and discharge capacity (CC: constant current, CV: constant voltage) were measured.

[0154] 2-3) Measurement of initial efficiency

[0155] The initial discharge capacity measured in the above 2-2) was divided by the initial charge capacity to measure the initial efficiency as a percentage value.

[0156] 2-4) Measurement of capacity retention rate

[0157] Using the battery cells of the examples and comparative examples, 300 cycles of charge (CC / CV 0.5C 4.3V 0.05CA cutoff) and discharge (CC 1.0C 3.0V cutoff) were repeated. The discharge capacity of the 300th cycle was divided by the discharge capacity of the 1st cycle to determine the capacity retention rate as a percentage.

[0158] The results are shown in Table 2 below.

[0159] [Table 2]

[0160]

[0161] Referring to Table 2 above, when the washing process using the organic polyphosphate / phosphonate compound was performed, the amount of lithium impurities was reduced and improved charge / discharge efficiency and capacity retention were obtained.

[0162] In Comparative Examples 1 to 4, in which only water was used in the washing process, lithium impurities were effectively removed, but efficiency and capacity retention were reduced due to oxidation of the particle structure.

[0163] Figure 1is a graph showing discharge capacity retention ratios of battery cells according to Example 3-3, Comparative Example 4, Comparative Example 5, and Comparative Example 7 during repeated charge / discharge operations.

[0164] refer to Figure 1 , compared with the comparative example, a significantly improved capacity retention rate was obtained according to Example 3-3 (in which a washing process using an organic polyphosphate / phosphonate compound was performed).

[0165] (3) Surface analysis

[0166] The surface of the lithium metal oxide particles prepared by Example 3-3 (in which the washing process using the organic polyphosphate / phosphonate compound was performed) was analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS). 3+ The ion gun was used by a TOF-SIMS V (ION-TOF GmbH, Germany) instrument equipped with a Bi ion gun, and the analysis area was 50×50 μm 2 .

[0167] Figure 2 is a TOF-SIMS analysis image of the surface of the lithium metal oxide particle according to Example 3-3.

[0168] like Figure 2 As shown, ion fragment peaks (such as C x H y PO3+ and PO+ peaks) are evenly distributed on the particle surface of Example 3-3.

Claims

1. A positive electrode active material for a lithium secondary battery, comprising: Lithium metal oxide particles; and an organic polyphosphate or an organic polyphosphonate formed on at least a portion of the surface of the lithium metal oxide particle, wherein the lithium metal oxide particles include a dopant or coating containing at least one of Al, Zr and Ti, Wherein, on the surface of the lithium metal oxide particle, the ion fragment peaks generated by the organic polyphosphate or the organic polyphosphonate are detected by time-of-flight secondary ion mass spectrometry (TOF-SIMS) analysis.

2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein The organic polyphosphate is obtained by an organic polyphosphate compound represented by the following structural formula 1 or an organic polyphosphate salt thereof, and the organic polyphosphonate is obtained by an organic polyphosphonate compound represented by the following structural formula 2 or an organic polyphosphonate salt thereof: [Structural Formula 1] [Structural Formula 2] Wherein, in the above structural formula 1 and structural formula 2, m is an integer from 2 to 20, R1 represents a C1-C10 hydrocarbon group that can be substituted by a substituent, and the substituent includes a halogen, a cyano group, a hydroxyl group, a phosphate group, a carboxyl group or a salt thereof.

3. The positive electrode active material for a lithium secondary battery according to claim 2, wherein: The hydrocarbon group contained in R1 is selected from the group consisting of carbon-carbon double bonds, -O-, -S-, -CO-, -OCO-, -SO-, -CO-O-, -O-CO-O-, -S-CO-, -S-CO-O-, -CO-NH-, -NH-CO-O-, -NR'-, The alkyl group is substituted or connected with at least one of the group consisting of -R'OH-, -SS- and -SO2-, and R' is hydrogen or a C1-C8 alkyl group.

4. The positive electrode active material for a lithium secondary battery according to claim 2, wherein: The organic polyphosphate compound or the organic polyphosphonate compound includes at least one of the compounds represented by the following Chemical Formulas 1 to 3: [Chemical formula 1] [Chemical formula 2] [Chemical formula 3] 5. The positive electrode active material for a lithium secondary battery according to claim 2, wherein: The organic polyphosphate or the organic polyphosphonate includes a compound represented by the following Chemical Formula 4: [Chemical formula 4] In the above Chemical Formula 4, n is an integer of 2 to 10.

6. The positive electrode active material for a lithium secondary battery according to claim 1, wherein The lithium metal oxide particles include a nickel-based lithium oxide represented by the following general formula 1: [General formula 1] Li x Ni y M 1-y O2 In the above general formula 1, 0.95≤x≤1.08, y≥0.5, and M is at least one element selected from the group consisting of Co, Mn, Al, Zr, Ti, B, Mg and Ba.

7. The positive electrode active material for a lithium secondary battery according to claim 6, wherein In the general formula 1, 0.8≤y≤0.

93.

8. The positive electrode active material for a lithium secondary battery according to claim 6, wherein In the general formula 1, M includes Co and Mn.

9. The positive electrode active material for a lithium secondary battery according to claim 1, wherein The organic polyphosphate or the organic polyphosphonate forms a coating, a ligand bond, or a complex bond on the surface of the lithium metal oxide particle.

10. The positive electrode active material for a lithium secondary battery according to claim 1, wherein The lithium metal oxide particles have a layer structure, and grain boundaries of surface portions of the lithium metal oxide particles are coated with the organic polyphosphate or the organic polyphosphonate.

11. A lithium secondary battery comprising: A positive electrode, the positive electrode comprising the positive electrode active material according to claim 1; negative electrode; and A separator layer is disposed between the positive electrode and the negative electrode.