Composite current collector

By alternately setting the brittle layer and the metal layer in the conductive layer of the composite fluid collection to form a multi-layer structure, the risk of thermal runaway in the case of puncture and other situations is solved, and higher safety performance is achieved.

CN119092715AActive Publication Date: 2024-12-06JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD

Patent Information

Application Number
CN202411203542.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The composite fluid collector has a risk of thermal runaway when subjected to puncture or other external impacts, affecting the safety performance of lithium-ion batteries.

Method used

A composite fluid collector is designed, and its conductive layer consists of multiple alternately arranged brittle layers and metal layers. The thickness ratio of each metal layer to the adjacent brittle layers is 3.5 to 15:1, and the elongation ratio of break is 6.8. ~12.2:1, the thickness of the brittle layer is 1 to 15 nm and the thickness of the metal layer is 10 to 100 nm. The conductive layer is formed by magnetron sputtering deposition, and the surface of the support layer is roughened to improve the bonding force.

Benefits of technology

It effectively reduces the risk of internal short-circuit thermal runaway in lithium-ion batteries when subjected to extrusion, collision or puncture. It forms a circuit breaker through the fracture of brittle materials, increases the short-circuit point and improves the thermal safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092715A_ABST
    Figure CN119092715A_ABST
Patent Text Reader

Abstract

The invention discloses a composite current collector, which comprises a support layer made of a polymer material; the conductive layer is arranged on the supporting layer; the conductive layer comprises a plurality of brittle layers and metal layers which are alternately arranged; the thickness ratio of each metal layer to the adjacent brittle layer is (3.5-15): 1; and the ratio of the elongation at break of the metal layer to the elongation at break of the brittle layer is 6.8-12.2: 1. The brittle material with low elongation at break and good brittleness is arranged on the surface of the metal layer of the conductive layer, and when the conductive layer is driven to stretch under the external action of puncture and the like, the metal layer can be directly broken and broken to form an open circuit due to the action of the brittle material; and the risk of internal short-circuit thermal runaway when the lithium ion battery is extruded, collided or punctured and the like is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a composite current collector. Background Art

[0002] With the rapid development of new energy and electronic technology, the cycle life, safety performance, energy density, etc. of batteries have become top priorities. The current collector is a very important part of the battery. It is used to collect the current generated by the active materials of the battery in order to form a larger current output. Its performance will directly affect the cycle life, energy density, safety, etc. of the battery. At present, the positive and negative electrodes in lithium batteries and sodium batteries mostly use copper foil and aluminum foil as current collectors. This type of current collector has high cost and quality, which is not conducive to controlling battery costs and improving energy density.

[0003] Composite current collectors have obvious advantages over traditional foil current collectors. Composite current collectors are usually "sandwich" structures, with a polymer layer on the inner layer and metal conductive layers on both sides. Since the metal layer on the surface of the composite current collector is thinner and the polymer layer inside is lighter, it can greatly reduce the overall weight of the current collector, thereby increasing the energy density of lithium-ion batteries.

[0004] Lithium-ion batteries are prone to internal short circuits when squeezed, collided or punctured, causing the battery to catch fire or even explode. The current composite current collector has an insulating polymer support layer, which can play a certain role in blocking electron transmission during puncture. However, when nailing or internal puncture occurs, the metal layer on the surface of the polymer support layer still retains a certain conductivity, and the battery temperature still tends to rise, with a certain risk of thermal runaway. Therefore, it is necessary to further improve the structure of the composite current collector to improve its thermal safety performance. Summary of the invention

[0005] In order to improve the thermal safety performance of a composite current collector, the present invention proposes a composite current collector. The above object can be achieved by implementing the following technical solution:

[0006] A composite current collector, comprising:

[0007] a support layer, the support layer comprising a polymer material;

[0008] A conductive layer, the conductive layer is arranged on the support layer; the conductive layer comprises a plurality of brittle layers and metal layers arranged alternately;

[0009] The thickness ratio of each metal layer to the adjacent brittle layer is 3.5 to 15:1;

[0010] The ratio of the elongation at break of each metal layer to the adjacent brittle layer is 6.8 to 12.2:1.

[0011] Optionally, the thickness of each brittle layer is 1 to 15 nm; the thickness of each metal layer is 10 to 100 nm.

[0012] Preferably, the conductive layer comprises at least 3 brittle layers and at least 3 metal layers.

[0013] Optionally, the tensile strength of the supporting layer is smaller than the tensile strength of the conductive layer.

[0014] Optionally, the bonding force between each metal layer and the adjacent brittle layer is greater than the bonding force between the support layer and the conductive layer.

[0015] Optionally, the thickness of each brittle layer increases sequentially as the distance between the brittle layer and the support layer increases.

[0016] Optionally, the surface of the conductive layer in contact with the supporting layer is a brittle layer.

[0017] Optionally, a surface of the conductive layer away from the supporting layer is a brittle layer.

[0018] Optionally, the brittle layer has a hardness greater than that of the metal layer.

[0019] Optionally, the metal layer is made of at least one of aluminum, lithium and nickel.

[0020] Optionally, the brittle material is a ceramic inorganic material.

[0021] Optionally, the brittle layer is made of at least one of aluminum oxide, silicon oxide, titanium oxide, silicon carbide, aluminum nitride, and silicon nitride.

[0022] Optionally, the support layer is made of at least one of PP, PET, and PI.

[0023] The preparation method of the composite current collector comprises the following steps:

[0024] A plurality of brittle metal layers are alternately deposited on the support layer by magnetron sputtering to form a conductive layer.

[0025] The deposition method is magnetron sputtering, and can also be at least one of evaporation, PVD, and CVD.

[0026] Optionally, before depositing the brittle metal layer, the surface of the support layer is roughened to improve the bonding force between the support layer and the conductive layer.

[0027] Optionally, the conditions for magnetron sputtering deposition are: moving the tape from the metal target to the brittle material target, the magnetron sputtering power density is 50W / cm2, the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the deposition time for each time is 4.5s.

[0028] Optionally, the present invention also proposes the use of the above composite current collector in preparing a battery.

[0029] The technical solution of the present invention has the following advantages:

[0030] The present invention arranges a brittle material layer on the surface of the metal layer of the conductive layer. When the metal layer is stretched by external forces such as puncture, the metal layer can be directly fractured and broken due to the action of the brittle material, forming a short circuit. This greatly reduces the risk of internal short circuit thermal runaway of the lithium-ion battery when it is squeezed, collided or punctured.

[0031] In order to meet the current capacity of the current collector, the conductive layer needs to reach a certain thickness. A thicker thickness makes it more difficult to produce cracks due to tensile deformation. Therefore, this solution designs the conductive layer as a multi-layer structure, in which the metal layer and the brittle layer are both multi-layer and alternately arranged. When each brittle layer breaks and shatters, it only needs to act on the adjacent metal layer to drive it to break together to achieve a point short circuit. By alternating multiple layers, the short-circuit points can exist not only in the two-dimensional direction of the plane, but also increase the short-circuit points in the thickness direction, forming a multi-point circuit break in three-dimensional space, further reducing the risk of internal short-circuit thermal runaway when the battery is impacted by external forces. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 It is a schematic diagram of the puncture experiment.

[0034] Markings in the figure: negative electrode plate 1; diaphragm 2; positive electrode plate 3; nail 4. DETAILED DESCRIPTION

[0035] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0036] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0037] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0038] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0039] A composite current collector in the present invention comprises:

[0040] A supporting layer, wherein the supporting layer is made of a polymer material;

[0041] A conductive layer, the conductive layer is arranged on the support layer; the conductive layer comprises a plurality of brittle metal layers arranged alternately;

[0042] The thickness ratio of each metal layer to the adjacent brittle layer is 3.5 to 15:1;

[0043] The ratio of the elongation at break of the metal layer to that of the brittle layer is 6.8 to 12.2:1.

[0044] The thickness of the brittle layer is 1-15 nm; the thickness of the metal layer is 10-100 nm.

[0045] The conductive layer comprises at least 3 brittle layers and at least 3 metal layers.

[0046] When the battery is impacted by external force, the current collector may be punctured, stretched, etc. Since the composite current collector contains a polymer support layer with good ductility and high toughness, when it is stretched and punctured, the surface conductive layer can be deformed synchronously due to the stretched and deformed polymer support layer. The ductility of the conductive layer is relatively weak, and cracks may be generated due to stretching. These cracks can break the circuit and reduce the risk of thermal runaway of the battery. However, since the polymer support layer has good toughness, even if the metal layer on the surface cracks, it cannot be completely disconnected. Therefore, this solution sets a brittle material with low elongation at break and good brittleness on the surface of the metal layer. When it is driven to stretch, due to the effect of the brittle material, the metal layer can not only be generated, but directly broken and shattered to form a short circuit; and in order to meet the current capacity of the collector, the conductive layer needs to reach a certain thickness. The thicker the thickness, the more difficult it is to produce cracks due to tensile deformation. Therefore, this solution designs the conductive layer as a multi-layer structure, in which the metal layer and the brittle layer are both multi-layer and alternately arranged, and the thickness of each metal layer is thin. When each brittle layer breaks and breaks, it only needs to act on the adjacent metal layer to drive it to break together to achieve a point short circuit. Not only that, through the alternating arrangement of multiple layers, the short-circuit point can exist not only in the two-dimensional direction of the plane, but also increase the short-circuit point in the thickness direction, forming a multi-point short circuit in three-dimensional space, further reducing the risk of internal short-circuit thermal runaway when the battery is impacted by external force.

[0047] The ratio of the elongation at break of the metal layer to the brittle layer must be greater than a certain value, so that the brittle layer is prone to fracture and open circuit, but it should not be too large. If the ratio is too large, the brittle layer will be too fragile to ensure the normal processing and use of the battery electrode, or the metal layer will be too ductile to break together with the brittle layer. Therefore, the ratio of the elongation at break of the metal layer to the brittle layer, especially the ratio of the elongation at break of the innermost metal layer close to the support layer to the innermost brittle layer, should be 6.8 to 12.2:1.

[0048] The thickness ratio of the metal layer and the adjacent brittle layer cannot be too small. If it is too small, the ductility of the conductive layer tends to be closer to the brittle layer, and the ductility difference with the supporting layer is too large. During the rolling process of the pole piece, a large number of wrinkles are easily generated at the junction of the slurry coating area and the empty foil area due to uneven stress, affecting the welding of the pole ear; the ratio cannot be too large either. If it is too large, the brittle layer is too thin, and microcracks are easily generated during the processing and use of the pole piece. Moreover, when the brittle layer is too thin and the metal layer is too thick, the fracture of the brittle layer may not lead to the fracture of the metal layer together.

[0049] The tensile strength of the support layer is less than the tensile strength of the conductive layer. The bonding force between each metal layer and the adjacent brittle layer is greater than the bonding force between the support layer and the conductive layer.

[0050] When the bonding force between the supporting layer and the conductive layer is large enough, the tensile deformation of the supporting layer can transfer the force to the conductive layer, driving the brittle layer therein to stretch and fracture. Otherwise, the supporting layer and the conductive layer may be directly peeled off due to uneven elongation, and the conductive layer cannot be disconnected. In addition, since the tensile tension is transferred from the supporting layer to the brittle layer, and then transferred to the adjacent metal layer on the outside after the brittle layer breaks, the bonding force between the metal layer and its adjacent inner brittle layer must be greater than the bonding force between the supporting layer and the conductive layer, so that when the brittle layer breaks, it can drive the adjacent outer metal layer to crack synchronously.

[0051] The bonding strength between the supporting layer and the conductive layer can be achieved by selecting a high adhesion coating method such as magnetron sputtering ion beam deposition, or by laser cleaning and roughening the surface of the supporting layer to control and improve it. Generally, ceramic materials have better adhesion to polymer base films than metal materials, so a ceramic brittle layer can be set in the innermost layer. The bonding strength between the brittle layer and the metal layer can be improved by one-step coating. The elongation at break of the metal layer can be controlled by selecting different types of metals or alloys. The elongation at break of the brittle layer can be controlled by selecting different types of ceramic substances or mixing multiple ceramic substances.

[0052] The hardness of the brittle layer is greater than that of the metal layer. The thickness of each brittle layer increases with the distance between the brittle layer and the support layer. First, when the composite current collector is impacted by an external force and undergoes deformation such as puncture and stretching, the tensile deformation of the support layer first causes the brittle layer closer to it to break and shatter, and then initiates a fracture reaction chain, generating force layer by layer to the brittle layer away from the support layer. The brittle layer closer to the support layer is thinner and more easily achieves step fracture;

[0053] Second, when the composite current collector is used in the battery, it will go through the electrode slurry coating and rolling process. The upper layer of the current collector is squeezed by the electrode particles. If the upper brittle layer is thinner than the lower layer and the hardness of the upper layer is not high enough, it is easy to cause fine cracks in the upper brittle layer during the rolling process. The cracks in the upper layer increase the contact area between the electrolyte and the current collector, increasing the risk of corrosion of the electrolyte to the current collector.

[0054] Preferably, the surface of the conductive layer in contact with the support layer is a brittle layer, that is, the brittle layer is in direct contact with the support layer and is more likely to initiate a rupture reaction chain.

[0055] Preferably, the surface of the conductive layer away from the support layer is a brittle layer. The uppermost brittle layer is the thickest and has a higher hardness, which can protect the thinner brittle layer below from cracking during the processing of pole piece rolling.

[0056] The metal layer is made of metal such as aluminum, lithium, and nickel.

[0057] The brittle layer is a ceramic inorganic material, and the maximum thickness of the brittle layer is not higher than 15nm. Ceramic inorganic materials have good brittleness, good chemical properties and temperature, are not easily corroded by electrolytes, and can also protect the base film. However, ceramic inorganic materials have poor electrical conductivity, so the thickness of the brittle layer needs to be set thinner, so that the current collector can still excite the electrons in the metal layer to move in a directional manner under the potential difference. The brittle layer cannot provide a large resistance due to its small thickness, and the conductivity will not change much, so as not to affect the conductivity of the current collector.

[0058] The brittle layer is a ceramic inorganic material, such as one or more of aluminum oxide, silicon oxide, titanium oxide, silicon carbide, aluminum nitride and silicon nitride.

[0059] The support layer is a high molecular polymer, such as PP, PET, and PI.

[0060] The test method for the elongation at break of the brittle layer metal layer in each embodiment is as follows:

[0061] Prepare a brittle layer test sample, select the same support layer as in the embodiment, select the same coating method, prepare the same brittle layer as the bottom layer (the layer closest to the support layer) in the embodiment on the upper and lower surfaces of the support layer, and obtain a brittle layer sample;

[0062] Prepare a metal layer test sample, select the same support layer as in the embodiment, select the same coating method, prepare the same metal layer as the bottom layer (the layer closest to the support layer) in the embodiment on the upper and lower surfaces of the support layer, and obtain a metal layer sample;

[0063] The brittle layer samples and metal layer samples were punched and cut into 10 mm wide samples to be tested; a universal tensile test machine was used for tensile testing at room temperature and pressure (25°C, 0.1 MPa), the initial position was set so that the sample length between the clamps was 50 mm, the tensile speed was 50 mm / min, and the equipment displacement y (mm) when cracks occurred in the brittle layer or the metal layer was recorded. Finally, the elongation at break was calculated as (y / 50)×100%

[0064] Example 1

[0065] This embodiment provides a composite current collector and a preparation method thereof, the composite current collector includes a support layer and a conductive layer, the conductive layer is arranged on the support layer, the conductive layer includes multiple brittle layer metal layers arranged alternately, wherein the support layer material is PET, the metal layer material is aluminum, and the brittle layer material is titanium oxide. The metal layer and the brittle layer each have five layers, the innermost layer (the layer where the conductive layer contacts the support layer) is the metal layer, and the outermost layer (the layer where the conductive layer is farthest from the support layer) is the brittle layer. The thickness of each metal layer is 30nm, and the thickness of each brittle layer is 3nm.

[0066] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0067] 1) The target arrangement is set to 8 aluminum targets plus one titanium oxide target (purity of each is 99.95%), the PET film is moved from the aluminum target to the titanium oxide target, the magnetron sputtering power density is 50 W / cm2, the vacuum degree is 0.1 Pa, the protective gas is argon, the flow rate is 50 mL / min, and the first deposition time is 4.5 s;

[0068] 2) Repeat the above steps 5 times, with each deposition time being 4.5 s.

[0069] According to the test, the elongation at break of the metal layer in Example 1 is 18.1%, and that of the brittle layer is 1.8%.

[0070] Example 2

[0071] This embodiment provides a composite current collector and a preparation method thereof. The composite current collector includes a support layer and a conductive layer. The conductive layer is arranged on the support layer. The conductive layer includes multiple brittle layer metal layers alternately arranged, wherein the support layer is PET, the metal layer is aluminum, and the brittle layer is titanium oxide.

[0072] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0073] 1) The target arrangement is set to 8 aluminum targets plus 1 titanium oxide target (purity of each is 99.95%), the PET film is moved from the aluminum target to the titanium oxide target, the magnetron sputtering power density is 50 W / cm2, the vacuum degree is 0.1 Pa, the protective gas is argon, the flow rate is 50 mL / min, and the first deposition time is 2.5 s;

[0074] 2) Repeat the above steps 5 times, with each deposition time being 0.5 s longer than the first.

[0075] Five metal layers and five brittle layers are obtained, the innermost is the metal layer, and the outermost is the brittle layer. The thickness of the metal layers from the inside to the outside are 15nm, 20nm, 25nm, 30nm, 35nm, and 40nm respectively; the thickness of the brittle layer from the inside to the outside are 1nm, 3nm, 5nm, 7nm, 9nm, and 11nm respectively. Compared with Example 1, the thickness of the metal layer and the brittle layer is increasing. After testing, the elongation at break of the metal layer of Example 2 is 14.5%, and that of the brittle layer is 1.3%.

[0076] Example 3

[0077] This embodiment provides a composite current collector and a preparation method thereof. The composite current collector includes a support layer and a conductive layer. The conductive layer is arranged on the support layer. The conductive layer includes multiple brittle layer metal layers alternately arranged, wherein the support layer is PET, the metal layer is aluminum, and the brittle layer is titanium oxide.

[0078] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0079] 1) The target arrangement is set to 1 titanium oxide target plus 8 aluminum targets (purity of 99.95%), and the PET film is moved from the titanium oxide target to the aluminum target. The magnetron sputtering power density is 50W / cm 2 , the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the first deposition time is 4.5s;

[0080] 2) Repeat the above steps 5 times, with each deposition time being 4.5 s.

[0081] Five metal layers and five brittle layers were obtained, the innermost layer was the brittle layer, and the outermost layer was the metal layer. The thickness of each metal layer was 30 nm, and the thickness of the brittle layer was 3 nm. After testing, the elongation at break of the metal layer of Example 3 was 18.2%, and that of the brittle layer was 1.7%.

[0082] Example 4

[0083] This embodiment provides a composite current collector and a preparation method thereof. The composite current collector includes a support layer and a conductive layer. The conductive layer is arranged on the support layer. The conductive layer includes multiple brittle layer metal layers alternately arranged, wherein the support layer is PET, the metal layer is aluminum, and the brittle layer is titanium oxide.

[0084] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0085] 1) Laser etching the PET surface to increase surface roughness and improve bonding strength.

[0086] 2) The target arrangement is set as one titanium oxide target, 8 aluminum targets, and one titanium oxide target (with a purity of 99.95%), and the PET film is moved from the aluminum target to the titanium oxide target. The magnetron sputtering power density is 50 W / cm2, the vacuum degree is 0.1 Pa, the protective gas is argon, the flow rate is 50 mL / min, and the first deposition time is 5 s; 3) Repeat the above steps 5 times, and the deposition time each time is 5 s.

[0087] Five metal layers and six brittle layers are obtained, and the innermost and outermost layers are both brittle layers. The thickness of each metal layer is 30nm, and the thickness of the brittle layer is 3nm. After testing, the elongation at break of the metal layer of Example 4 is 18%, and that of the brittle layer is 1.8%.

[0088] Example 5

[0089] This embodiment provides a composite current collector and a preparation method thereof. The composite current collector includes a support layer and a conductive layer. The conductive layer is arranged on the support layer. The conductive layer includes multiple layers of brittle layer metal layers alternately arranged, wherein the support layer is PET, the metal layer is copper, and the brittle layer is silicon carbide.

[0090] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0091] 3) The target arrangement is set to 1 silicon carbide target plus 8 copper targets (purity of 99.95%), the PET film is moved from the silicon carbide target to the copper target, the magnetron sputtering power density is 50 W / cm2, the vacuum degree is 0.1 Pa, the protective gas is argon, the flow rate is 50 mL / min, and the first deposition time is 4.5 s;

[0092] 4) Repeat the above steps 5 times, with each deposition time being 4.5 s.

[0093] Five metal layers and five brittle layers were obtained, the innermost layer was the brittle layer, and the outermost layer was the metal layer. The thickness of each metal layer was 30 nm, and the thickness of the brittle layer was 3 nm. After testing, the elongation at break of the metal layer in Example 5 was 13.7%, and that of the brittle layer was 2%.

[0094] Example 6

[0095] This embodiment provides a composite current collector and a preparation method thereof. The composite current collector includes a support layer and a conductive layer. The conductive layer is arranged on the support layer. The conductive layer includes multiple brittle layer metal layers alternately arranged. The support layer is PET, the metal layer is lithium, and the brittle layer is aluminum oxide.

[0096] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0097] 5) The target arrangement is set to 1 alumina target plus 8 lithium targets (purity of 99.95%), and the PET film is moved from the alumina target to the lithium target. The magnetron sputtering power density is 50W / cm 2, the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the first deposition time is 4.5s;

[0098] 6) Repeat the above steps 5 times, with each deposition time being 4.5 s.

[0099] Five metal layers and five brittle layers were obtained, the innermost layer was the brittle layer, and the outermost layer was the metal layer. The thickness of each metal layer was 30 nm, and the thickness of the brittle layer was 3 nm. After testing, the elongation at break of the metal layer of Example 6 was 20.7%, and that of the brittle layer was 1.7%.

[0100] Example 7

[0101] This embodiment provides a composite current collector and a preparation method thereof. The composite current collector includes a support layer and a conductive layer. The conductive layer is arranged on the support layer. The conductive layer includes multiple brittle layer metal layers alternately arranged, wherein the support layer is PP, the metal layer is aluminum, and the brittle layer is titanium oxide.

[0102] Preparation method: A PP film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the thickness direction of the PP film. The specific process conditions are:

[0103] 1) The target arrangement is set to 8 aluminum targets plus one titanium oxide target (purity of each is 99.95%). The PP film is moved from the aluminum target to the titanium oxide target. The magnetron sputtering power density is 50W / cm 2 , the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the first deposition time is 4.5s;

[0104] 2) Repeat the above steps 5 times, with each deposition time being 4.5 s.

[0105] Five metal layers and five brittle layers were obtained, the innermost layer was the metal layer, and the outermost layer was the brittle layer. The thickness of each metal layer was 30 nm, and the thickness of the brittle layer was 3 nm. After testing, the elongation at break of the metal layer of Example 7 was 18%, and that of the brittle layer was 1.8%.

[0106] Comparative Example 1

[0107] The support layer is PET, the metal layer is iron, and the brittle layer is zirconium oxide. In this comparative example, a metal layer with a lower elongation at break and a brittle layer with a higher elongation at break are used.

[0108] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0109] 1) The target arrangement is set to 8 iron targets plus one zirconium oxide target (purity of each is 99.95%). The PET film is moved from the iron target to the zirconium oxide target. The magnetron sputtering power density is 50W / cm 2 , the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the first deposition time is 4.5s;

[0110] 2) Repeat the above steps 5 times, with each deposition time being 4.5 s.

[0111] Five metal layers and five brittle layers were obtained, the innermost layer was the metal layer, and the outermost layer was the brittle layer. The thickness of each metal layer was 30 nm, and the thickness of the brittle layer was 3 nm. After testing, the elongation at break of the metal layer of comparative example 1 was 12.2%, and that of the brittle layer was 2.1%.

[0112] Comparative Example 2

[0113] The supporting layer is PET, the metal layer is aluminum, and the brittle layer is titanium oxide.

[0114] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0115] 1) In the first magnetron sputtering machine, the target arrangement is set to 9 aluminum targets (purity of 99.95%), the magnetron sputtering power density is 60 W / cm2, the vacuum degree is 0.1 Pa, the protective gas is argon, the flow rate is 50 mL / min, and the deposition time is 20 s;

[0116] 2) Transfer to the second magnetron sputtering machine, set the target arrangement to 1 titanium oxide target (purity 99.95%), and the magnetron sputtering power density to 50W / cm 2 , the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the deposition time is 1s;

[0117] A metal layer and a brittle layer are obtained, the inner side is the metal layer, and the outer side is the brittle layer. The thickness of the metal layer is 160nm, and the thickness of the brittle layer is 5nm. After testing, the elongation at break of the metal layer of comparative example 2 is 18.2%, and that of the brittle layer is 1.8%.

[0118] Comparative Example 3

[0119] The supporting layer is PET, the metal layer is aluminum, and the brittle layer is titanium oxide.

[0120] Preparation method: A PET film with a thickness of 6 μm is placed in a magnetron sputtering machine, and a brittle layer and a metal layer are alternately deposited on both sides of the PET film in the thickness direction. The specific process conditions are as follows:

[0121] 1) The target arrangement is set to 4 aluminum targets plus 4 titanium oxide targets (purity of each is 99.95%). The PET film is moved from the aluminum target to the titanium oxide target. The magnetron sputtering power density is 50W / cm 2 , the vacuum degree is 0.1Pa, the protective gas is argon, the flow rate is 50mL / min, and the first deposition time is 4.5s;

[0122] 2) Repeat the above steps 5 times, and the deposition time is 4.5s each time. Five layers of metal layer and brittle layer are obtained, the innermost layer is the metal layer, and the outermost layer is the brittle layer. The thickness of each metal layer is 16nm, and the thickness of the brittle layer is 14nm. Compared with Example 1, the thickness ratio of the metal layer and the brittle layer in this comparative example is too small, and the two are step-coated, and the bonding force is weak. After testing, the elongation at break of the metal layer of Comparative Example 3 is 18.1%, and that of the brittle layer is 1.8%.

[0123] Bonding strength test

[0124] The test method is as follows: select the above-mentioned composite current collector as the sample to be tested, the width h is 0.02m, use 3M double-sided tape at room temperature and pressure (25°C, 0.1MPa), one side is evenly attached to the stainless steel plate, and then the sample to be tested is evenly attached to the other side of the double-sided tape, and the sample to be tested is peeled off using a high-speed rail tensile machine. After peeling, the surface of one side of the support layer is tested for elements. If the proportion of the elements contained in the brittle layer on the surface of the support layer is less than 5%, it is considered that the bonding force between the metal layer and the brittle layer is greater than the bonding force between the brittle layer and the support layer. After testing, the bonding force between the metal layer and the brittle layer in each embodiment is greater than the bonding force between the brittle layer and the support layer.

[0125] Battery performance test:

[0126] Battery preparation method:

[0127] Preparation of pole pieces and batteries:

[0128] 1) Preparation of positive electrode

[0129] The ternary active material NCM811, conductive carbon black and binder PVDF were mixed in NMP at a weight ratio of 92:4:4 to obtain the positive electrode slurry. The positive electrode slurry was coated on the composite current collector sample, dried, rolled and die-cut to obtain the positive electrode sheet. The compaction density of the positive electrode active material layer was 3.3g / cm 3 .

[0130] 2) Preparation of negative electrode sheet

[0131] The negative electrode active material artificial graphite, binder SBR, dispersant CMC and conductive carbon black were mixed in water at a weight ratio of 96:2:1.2:0.8 to obtain the negative electrode slurry. The negative electrode slurry was coated on the composite current collector sample, dried and rolled, and then die-cut to obtain the negative electrode sheet. The compaction density of the negative electrode active material layer was 1.55g / cm 3 .

[0132] 3) Diaphragm

[0133] PE film is selected as the diaphragm.

[0134] 4) Preparation of electrolyte

[0135] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 4:6 as a solvent, and lithium salt LiPF6 was selected as the solute with a concentration of 1 mol / L.

[0136] 5) Preparation of batteries

[0137] The positive electrode sheet, separator and negative electrode sheet are stacked in order, and a battery cell is obtained after winding, which is placed in a battery casing, and the electrolyte is added. After packaging, standing, formation, capacity division and other processes, a sample lithium battery is obtained.

[0138] Puncture test method:

[0139] like Figure 1 As shown, in this application, a puncture test is used to simulate the abnormal condition of the battery and observe the changes in the battery after the nail is penetrated. Schematic diagram of a nail penetration test in this application. The figure shows that a nail 4 penetrates a layer of positive electrode sheet 3, a layer of separator 2 and a layer of negative electrode sheet 1 of the battery.

[0140] Mechanical piercing uses a steel needle with a diameter of 8mm to pierce the large surface of the experimental sample battery at a speed of 25mm / s. A temperature monitoring point is set on the large surface of the sample battery 1.5cm away from the puncture position. Real-time detection is performed through a temperature sensor to detect and read the battery temperature change within 2 hours after the steel needle contacts the battery.

[0141] Puncture displacement test method:

[0142] When the puncture displacement of the supporting layer material is lower, the deformation of the current collector, the corresponding pole piece and the battery when mechanical damage occurs is also smaller, the probability of thermal runaway caused by battery short circuit is also lower, and the battery is safer.

[0143] Use a tensile machine to test the puncture displacement. Fix the disc-shaped sample composite current collector with a diameter of 4 cm on the sample loading platform of the tensile machine, keep the horizontal plane of the sample perpendicular to the moving direction of the steel nail, and use a cross-section of 1mm 2A steel nail is inserted into the center of the sample at a speed of 50 mm / min. The displacement of the steel nail from the time the steel nail contacts the sample to the time the sample is pierced is measured and recorded, which is the puncture displacement of the sample.

[0144] Comparison of test results:

[0145] Table 1 Battery performance test results prepared using the composite current collectors of the embodiments and comparative examples

[0146] serial number Puncture displacement(mm) Maximum rate of temperature rise ℃ / min Temperature rise maximum temperature ℃ Example 1 4.2 0.01 25.9 Example 2 3.7 0 25.2 Example 3 3.8 0 25.1 Example 4 3.5 0 25.1 Example 5 3.2 0 25.1 Example 6 4.8 0.01 25.8 Example 7 3.7 0 25.2 Comparative Example 1 5.1 0.33 36.5 Comparative Example 2 6.3 0.41 38.6 Comparative Example 3 7.9 0.57 42.1

[0147] From the above experimental results, it can be seen that the battery prepared by the composite current collector of the present invention can effectively suppress the risk of internal short-circuit thermal runaway when abnormalities such as puncture occur. According to the effect comparison of each embodiment and comparative example, if the elongation at break of the brittle layer is too large or the brittle layer and the metal layer are not alternately arranged, the effect of suppressing short-circuit thermal runaway will be reduced.

[0148] Obviously, the above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.

Claims

1. A composite current collector, characterized in that: include: a support layer, the support layer comprising a polymer material; A conductive layer, the conductive layer is arranged on the support layer; the conductive layer comprises a plurality of brittle layers and metal layers arranged alternately; The thickness ratio of each metal layer to the adjacent brittle layer is 3.5 to 15:1; The ratio of the elongation at break of each metal layer to the adjacent brittle layer is 6.8 to 12.2:

1.

2. The composite current collector according to claim 1, characterized in that: The thickness of each brittle layer is 1 to 15 nm; the thickness of each metal layer is 10 to 100 nm; and / or, The conductive layer comprises at least 3 brittle layers and at least 3 metal layers.

3. The composite current collector according to claim 1, characterized in that: The tensile strength of the support layer is less than the tensile strength of the conductive layer.

4. The composite current collector according to claim 1, characterized in that: The bonding force between each metal layer and the adjacent brittle layer is greater than the bonding force between the support layer and the conductive layer.

5. The composite current collector according to claim 1, characterized in that: The thickness of each brittle layer increases successively with the increase of the distance between the brittle layer and the supporting layer.

6. The composite current collector according to claim 1, characterized in that: The surface of the conductive layer in contact with the supporting layer is a brittle layer.

7. The composite current collector according to claim 1, characterized in that: The surface of the conductive layer away from the supporting layer is a brittle layer.

8. The composite current collector according to claim 1, characterized in that: The metal layer is made of at least one of aluminum, lithium and nickel; and / or, The brittle material is a ceramic inorganic material; and / or, The brittle layer is made of at least one of aluminum oxide, silicon oxide, titanium oxide, silicon carbide, aluminum nitride and silicon nitride; and / or, The support layer is made of at least one of PP, PET and PI; and / or, The brittle layer has a harderness than that of the metal layer.

9. The method for preparing a composite current collector according to any one of claims 1 to 8, characterized in that: The steps include: Multiple brittle metal layers are alternately deposited on the support layer to form a conductive layer.

10. Use of the composite current collector according to any one of claims 1 to 8 in preparing a battery.

Citation Information

Patent Citations

  • Composite current collector, electrode plate and electrochemical device

    CN110943227A

  • Positive current collector, positive pole piece, electrochemical device, electric automobile and electronic product

    CN112290029A

  • Composite current collector, preparation method thereof, electrode plate, battery and electric device

    CN116581301A

  • Positive current collector, positive pole piece and secondary battery

    CN216145647U

  • Current collector, pole piece and battery

    CN219800916U

Cited By

  • Polymer composite film, composite current collector, preparation method of composite current collector, positive electrode and application of positive electrode

    CN119898103A

  • Thermal safety type functional current collector, preparation method thereof, pole piece and battery

    CN120164957A

  • A thermal safety type functional current collector, a preparation method thereof, a pole piece and a battery

    CN120164957B