Resource recycling method for nickel-cobalt-manganese ternary positive electrode material
Through the three-stage adsorption treatment and the preferred adsorption characteristics of biochar materials, the problems of high energy consumption and low recovery in the pyrometallurgical treatment methods are solved, and efficient nickel, cobalt and manganese recycling is achieved, which improves recycling efficiency and environmental protection. .
Patent Information
- Application Number
- CN202410969572.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing pyrometallurgical treatment methods have high energy consumption and low recovery rate on the positive electrode materials of waste nickel, cobalt, manganese ternary lithium-ion batteries, resulting in low loss and recovery efficiency of valuable metals such as nickel, cobalt, and manganese.
The third-level adsorption treatment method is adopted to preferentially adsorb nickel, manganese and cobalt using biochar materials from different sources. Through the filtration and elution steps of the acid solution, nickel, manganese and cobalt are extracted and precipitated respectively to improve their recovery rate.
The recovery rates of nickel, cobalt and manganese are achieved exceeding 85%, reducing energy consumption and improving recycling efficiency. It also has a simple process, low cost, good environmental protection, and is suitable for industrial applications.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling waste lithium-ion battery positive electrode materials, and in particular to a method for recycling nickel-cobalt-manganese ternary positive electrode materials. Background Art
[0002] Nickel-cobalt-manganese ternary materials are a new type of lithium-ion battery cathode material developed in recent years. They have important advantages such as high capacity, good cycle stability, and moderate cost. Since this type of material can effectively overcome the problems of high cost of lithium cobalt oxide materials, low stability of lithium manganese oxide materials, and low capacity of lithium iron phosphate, it has been successfully applied in industries that require batteries such as new energy vehicles, and the scale of application has been rapidly developed. However, nickel, cobalt, and manganese elements are mainly distributed in the form of mineral resources in nature. Faced with the huge demand of current new energy vehicles and other industries, nickel, cobalt, and manganese resources are very limited. However, the content of valuable metals such as nickel, cobalt, and manganese in the nickel-cobalt-manganese cathode materials of waste ternary lithium-ion batteries is relatively high, far higher than that of natural ores. Therefore, faced with the huge demand of current new energy vehicles and other industries, it is necessary to recycle and reuse nickel-cobalt-manganese ternary cathode materials.
[0003] At present, the main method used to recycle waste nickel-cobalt-manganese (NCM) ternary lithium-ion battery positive electrode materials is pyrometallurgy. The pyrometallurgical treatment method mainly uses high temperature to treat waste positive electrode materials, and purifies the valuable metals through physical and chemical transformation, converting them into metal elements and metal oxides, so as to achieve the purpose of extracting and purifying valuable metals; however, the pyrometallurgical treatment method has the disadvantages of high energy consumption and low recovery rate of valuable metals such as nickel, cobalt, and manganese due to loss in the slag. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the shortcomings of the prior art, the present invention provides a method for resource recovery of nickel-cobalt-manganese ternary positive electrode materials, which solves the technical problems of high energy consumption of pyrometallurgical treatment methods and low recovery rate of valuable metals such as nickel, cobalt and manganese.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] In one aspect, the present invention provides a method for resource utilization of nickel-cobalt-manganese ternary positive electrode materials, comprising the following steps:
[0009] S1. Preparation of acid solution
[0010] The nickel-cobalt-manganese ternary positive electrode material is crushed, then immersed in an inorganic acid to dissolve to obtain a solution, the solution is filtered, and the filtrate is taken to obtain an acid hydrolysis solution; the inorganic acid is selected from any one of sulfuric acid, hydrochloric acid, and nitric acid, and an appropriate amount of H2O2 can also be added to the inorganic acid to improve the solubility of the nickel-cobalt-manganese ternary positive electrode material.
[0011] S2. Adsorption treatment of acid solution
[0012] The acid hydrolysis solution is subjected to a first-stage adsorption treatment to obtain a first support body loaded with nickel and a first filtrate, and then the first filtrate is subjected to a second-stage adsorption treatment to obtain a second support body loaded with manganese and a second filtrate, and then the second filtrate is subjected to a third-stage adsorption treatment to obtain a third support body loaded with cobalt and a third filtrate;
[0013] The adsorption medium of the first stage adsorption treatment is a first biochar material, and the first biochar material is obtained by modifying the biochar obtained by anaerobic pyrolysis of the first carbon-containing organic matter at 400-900°C;
[0014] The adsorption medium of the second stage adsorption treatment is a second biochar material, and the second biochar material is obtained by modifying the biochar obtained by anaerobic pyrolysis of the second carbon-containing organic matter at 400-900°C;
[0015] The adsorption medium of the third stage adsorption treatment is a third biochar material, and the third biochar material is obtained by modifying the biochar obtained by anaerobic pyrolysis of the third carbon-containing organic matter at 400-900°C;
[0016] S3, elution
[0017] The first support body, the second support body and the third support body are subjected to elution treatment respectively, and a first eluent containing nickel, a second eluent containing manganese and a third eluent containing cobalt are obtained accordingly;
[0018] S4. Precipitation
[0019] adjusting the pH of the first eluent to 10 to obtain nickel-containing precipitate nickel hydroxide;
[0020] adding sulfate to the second eluent to obtain a manganese dioxide precipitate;
[0021] The pH of the third eluent is adjusted to 10 to obtain cobalt hydroxide as a cobalt-containing precipitate.
[0022] Sodium carbonate is added to the third filtrate to obtain lithium carbonate precipitate.
[0023] Preferably, the first carbon-containing organic matter is selected from at least one of peanut shells and reed straws, and the biochar obtained by anaerobic pyrolysis of at least one of the peanut shells and reed straws is acid-washed and modified to obtain the first biochar material;
[0024] The second carbon-containing organic matter is selected from at least one of mangosteen shells and buckwheat shells, and the biochar obtained by anaerobic pyrolysis of at least one of mangosteen shells and buckwheat shells is acid-washed and modified to obtain a second biochar material;
[0025] The third carbon-containing organic matter is selected from at least one of rice straw and grapefruit peel. The biochar obtained by anaerobic pyrolysis of at least one of rice straw and grapefruit peel is modified by acid washing to obtain the third biochar material.
[0026] Preferably, the acid used for pickling modification includes an inorganic acid or an organic acid, the inorganic acid is selected from any one of sulfuric acid, hydrochloric acid, and nitric acid, and the organic acid is selected from any one of citric acid, oxalic acid, and formic acid. The acid used for pickling modification is recovered by filtration and used to dissolve the nickel-cobalt-manganese ternary positive electrode material in S1;
[0027] Preferably, the concentration of the organic acid or inorganic acid is 0.5-1 mol / L.
[0028] Preferably, the specific surface area of the first biochar material, the second biochar material, and the third biochar material is 200-400 m 2 / g.
[0029] Preferably, in the first stage adsorption treatment, the liquid-to-solid ratio of the acid hydrolyzate to the first biochar material is 1000 ml:(1-50) g, and the adsorption time is 10-60 min;
[0030] In the second stage adsorption treatment, the liquid-to-solid ratio of the first filtrate to the second biochar material is 1000 ml:(1-50) g, and the adsorption time is 10-60 min;
[0031] In the third stage adsorption treatment, the liquid-to-solid ratio of the second filtrate to the third biochar material is 1000 ml: (1-50) g, and the adsorption time is 10-60 min.
[0032] Preferably, in S2, the temperature of the acid hydrolysis solution is 25°C to 50°C, and the pH value is 5.5 to 7.0.
[0033] Preferably, the step S1 further comprises adding alkaline solution to the acid hydrolysis solution, adjusting the pH value of the acid hydrolysis solution to 4.0-4.5, and removing impurity ions and hydroxide ions.
[0034] Preferably, in S3, an acidic solution or an alkaline solution is selected for elution treatment.
[0035] Preferably, the chemical formula of the nickel-cobalt-manganese ternary positive electrode material is LiNi x Co y Mn 1-x-y O2, where x+y≤1.
[0036] (III) Beneficial effects
[0037] The present invention provides a method for recycling nickel-cobalt-manganese ternary positive electrode materials. Compared with the prior art, it has the following beneficial effects:
[0038] A method for recycling nickel-cobalt-manganese ternary positive electrode materials, comprising: performing a first-stage adsorption treatment on an acid hydrolysis solution using a first biochar material as an adsorption medium to obtain a first support body loaded with nickel and a first filtrate, then performing a second-stage adsorption treatment on the first filtrate using a second biochar material as an adsorption medium to obtain a second support body loaded with manganese and a second filtrate, and then performing a third-stage adsorption treatment on the second filtrate using a third biochar material as an adsorption medium to obtain a third support body loaded with cobalt and a third filtrate; wherein the first biochar material is at least one of peanut shells and reed straws, obtained by anaerobic pyrolysis at 400-900°C, and is modified by acid washing, and has preferential adsorption characteristics for nickel; the second biochar The material is at least one of mangosteen shell and buckwheat shell, which is pyrolyzed in the absence of oxygen at 400-900°C to obtain biochar, which is modified by acid washing and has preferential adsorption characteristics for manganese; the third biochar material is at least one of rice straw and grapefruit peel, which is pyrolyzed in the absence of oxygen at 400-900°C to obtain biochar, which is modified by acid washing and has preferential adsorption characteristics for cobalt; the recovery method of the present application utilizes the preferential adsorption characteristics of the first biochar material for nickel, the preferential adsorption characteristics of the second biochar material for manganese, and the preferential adsorption characteristics of the third biochar material for cobalt, and performs a three-stage adsorption treatment on the acid hydrolysis liquid of the nickel-cobalt-manganese ternary positive electrode material waste, so that the recovery rates of nickel, manganese and cobalt are all greater than 85%. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with specific implementation methods.
[0041] Example 1
[0042] This embodiment provides a method for recycling waste nickel-cobalt-manganese ternary positive electrode materials, comprising the following steps:
[0043] Preparation of biochar materials:
[0044] Peanut shells are pyrolyzed at 400° C. in a nitrogen atmosphere to obtain biochar, which is then soaked in hydrochloric acid, washed and dried to obtain a first biochar material;
[0045] Buckwheat husks are pyrolyzed at 400°C in a nitrogen atmosphere to obtain biochar, which is then soaked in hydrochloric acid, washed and dried to obtain a second biochar material;
[0046] The rice straw is pyrolyzed at 400°C in a nitrogen atmosphere to obtain biochar, which is then soaked in hydrochloric acid, washed and dried to obtain a third biochar material;
[0047] The specific surface area of the first biochar material, the second biochar material, and the third biochar material is 200m 2 / g.
[0048] Preparation of acid solution:
[0049] A waste nickel-cobalt-manganese ternary material is crushed to a particle size D50≤4μm, and then immersed in sufficient hydrochloric acid to dissolve to obtain a solution, the solution is filtered, and the filtrate is taken to obtain an acid solution; sodium hydroxide solution is added to the acid solution to adjust its pH value to 4.0-4.5, and the impurity ions in the acid solution are combined with hydroxide ions to form a precipitate to remove impurities, and then the contents of lithium, nickel, cobalt, and manganese in the acid solution are determined to be: Li 0.85mg / l, Ni 1.63mg / l, Co 0.24mg / l, Mn0.44mg / l, respectively;
[0050] Three-stage adsorption treatment of acid hydrolysate
[0051] The pH value of the acid hydrolyzate was adjusted to 5.5, heated to 25°C, and then immersed in an adsorption stirring tank containing the first biochar material, the liquid-solid ratio of the acid hydrolyzate to the first biochar material was 1000ml:1g, and the adsorption was stirred for 10 minutes to obtain a first support body loaded with nickel and a first filtrate;
[0052] The first filtrate is immersed in an adsorption stirring tank containing a second biochar material, the liquid-to-solid ratio of the first filtrate to the second biochar material is 1000 ml:1 g, and the adsorption is stirred for 10 minutes to obtain a second support body loaded with manganese and a second filtrate;
[0053] The second filtrate was immersed in an adsorption stirring tank containing a third biochar material, the liquid-to-solid ratio of the second filtrate to the third biochar material was 1000ml:1g, and the mixture was stirred and adsorbed for 10 minutes to obtain a third carrier loaded with cobalt and a third filtrate. The test was performed using ICP (inductively coupled plasma spectrometer), and the contents of nickel, cobalt, and manganese in the third filtrate were measured to be Ni 0.06mg / l, Co 0.02mg / l, and Mn 0.01mg / l, respectively; the calculated recovery rates of nickel, cobalt, and manganese were 96.3%, 91.7%, and 97.7%, respectively.
[0054] Elution:
[0055] The first carrier, the second carrier, and the third carrier are eluted with 1 mol / L dilute hydrochloric acid respectively, and a first eluent containing nickel, a second eluent containing manganese, and a third eluent containing cobalt are obtained after elution. The first carrier, the second carrier, and the third carrier are eluted to obtain a first biochar material, a second biochar material, and a third biochar material, which are washed, dried, and reused;
[0056] S4. Precipitation
[0057] Sodium hydroxide was added dropwise to the first eluate to adjust the pH to 10, thereby obtaining nickel-containing precipitate nickel hydroxide.
[0058] adding sodium sulfate to the second eluate to obtain manganese dioxide;
[0059] Potassium hydroxide solution was added dropwise to the third eluate to adjust the pH to 10, thereby obtaining cobalt hydroxide as a cobalt-containing precipitate.
[0060] Sodium carbonate is added to the third filtrate to obtain lithium carbonate precipitate, and the lithium carbonate precipitate is removed by filtration to obtain a fourth filtrate.
[0061] The recovery rates of nickel, cobalt and manganese are calculated according to the following formula:
[0062] Nickel recovery rate = (nickel content in acid solution - nickel content in the third filtrate) / nickel content in acid solution;
[0063] Cobalt recovery rate = (cobalt content in acid solution - cobalt content in the third filtrate) / cobalt content in acid solution;
[0064] The recovery rate of manganese = (the content of manganese in the acid hydrolysis solution - the content of manganese in the third filtrate) / the content of manganese in the acid hydrolysis solution.
[0065] Example 2
[0066] This embodiment provides a method for recycling waste nickel-cobalt-manganese ternary positive electrode materials, comprising the following steps:
[0067] The biochar used is selected from the regenerated biochar after elution in Example 1.
[0068] Preparation of acid solution:
[0069] A waste nickel-cobalt-manganese ternary material was crushed to a particle size of D50≤3μm, and then immersed in sufficient hydrochloric acid to dissolve to obtain a solution, the solution was filtered, and the filtrate was taken to obtain an acid solution; potassium hydroxide solution was added to the acid solution to adjust its pH value to 4.0-4.5, and the impurity ions in the acid solution were combined with hydroxide ions to form a precipitate to remove impurities, and then the contents of lithium, nickel, cobalt, and manganese in the acid solution were determined to be: Li 0.76mg / l, Ni 1.33mg / l, Co 0.2mg / l, Mn 0.34mg / l, respectively;
[0070] Three-stage adsorption treatment of acid hydrolysate
[0071] The pH value of the acid hydrolyzate was adjusted to 6.0, heated to 40°C, and then immersed in an adsorption column containing the first biochar material, the liquid-solid ratio of the acid hydrolyzate to the first biochar material was 1000ml:10g, and the adsorption was stirred for 40 minutes to obtain a first support body loaded with nickel and a first filtrate;
[0072] The first filtrate is immersed in an adsorption column containing a second biochar material, the liquid-to-solid ratio of the first filtrate to the second biochar material is 1000 ml:10 g, and adsorbed by stirring for 40 minutes to obtain a second support body loaded with manganese and a second filtrate;
[0073] The second filtrate was immersed in an adsorption column containing the third biochar material, the liquid-to-solid ratio of the second filtrate to the third biochar material was 1000ml:10g, and the adsorption was stirred for 40 minutes to obtain a third carrier loaded with cobalt and a third filtrate. The contents of nickel, cobalt and manganese in the third filtrate were measured to be Ni 0.07mg / l, Co 0.03mg / l, and Mn 0.03mg / l, respectively; after calculation, the recovery rates of nickel were 94.7%, cobalt 85.0%, and manganese 91.2%.
[0074] Elution:
[0075] The first carrier, the second carrier and the third carrier are eluted with dilute hydrochloric acid respectively, and a first eluent containing nickel, a second eluent containing manganese and a third eluent containing cobalt are obtained after elution. The first carrier, the second carrier and the third carrier are eluted to obtain a first biochar material, a second biochar material and a third biochar material, which are washed, dried and reused;
[0076] S4. Precipitation
[0077] Adding ammonia water dropwise to the first eluate to adjust the pH to 10, to obtain nickel-containing precipitate nickel hydroxide;
[0078] adding sodium sulfate to the second eluate to obtain manganese dioxide;
[0079] adjusting the pH of the third eluent to 10 to obtain cobalt hydroxide as a cobalt-containing precipitate;
[0080] Example 3
[0081] This embodiment provides a method for recycling waste nickel-cobalt-manganese ternary positive electrode materials, comprising the following steps:
[0082] Preparation of biochar materials:
[0083] Peanut shells are pyrolyzed at 900° C. in a nitrogen atmosphere to obtain biochar, which is then soaked in hydrochloric acid, washed and dried to obtain a first biochar material;
[0084] The mangosteen shell is pyrolyzed at 900°C in a nitrogen atmosphere to obtain biochar, which is then soaked in hydrochloric acid, washed and dried to obtain a second biochar material;
[0085] The rice straw is pyrolyzed at 900°C in a nitrogen atmosphere to obtain biochar, which is then soaked in hydrochloric acid, washed and dried to obtain a third biochar material;
[0086] The specific surface area of the first biochar material, the second biochar material, and the third biochar material is 400m 2 / g.
[0087] Preparation of acid solution:
[0088] A waste nickel-cobalt-manganese ternary material was crushed to a particle size of D50≤3μm, and then immersed in sufficient hydrochloric acid to dissolve to obtain a solution, the solution was filtered, and the filtrate was taken to obtain an acid solution; ammonia water was added to the acid solution to adjust its pH value to 4.0-4.5, and the impurity ions in the acid solution were combined with hydroxide ions to form a precipitate to remove impurities, and then the contents of lithium, nickel, cobalt, and manganese in the acid solution were determined to be: Li 0.83mg / l, Ni 1.27mg / l, Co 0.28mg / l, Mn 0.37mg / l, respectively;
[0089] Three-stage adsorption treatment of acid hydrolysate
[0090] The pH value of the acid hydrolyzate was adjusted to 7.0, heated to 50° C., and then immersed in an adsorption stirring tank containing the first biochar material, the liquid-solid ratio of the acid hydrolyzate to the first biochar material was 1000 ml:50 g, and stirred and adsorbed for 60 minutes to obtain a first support body loaded with nickel and a first filtrate;
[0091] The first filtrate is immersed in an adsorption stirring tank containing a second biochar material, the liquid-to-solid ratio of the first filtrate to the second biochar material is 1000 ml:50 g, and the adsorption is stirred for 60 minutes to obtain a second support body loaded with manganese and a second filtrate;
[0092] The second filtrate was immersed in an adsorption stirring tank containing a third biochar material. The liquid-to-solid ratio of the second filtrate to the third biochar material was 1000ml:50g. The mixture was stirred and adsorbed for 60 minutes to obtain a third cobalt-loaded carrier and a third filtrate. The contents of nickel, cobalt and manganese in the third filtrate were measured to be Ni 0.03mg / l, Co 0.008mg / l and Mn 0.015mg / l, respectively. After calculation, the recovery rates of nickel, cobalt and manganese were 97.6%, 97.1% and 95.9%, respectively.
[0093] Elution:
[0094] The first carrier, the second carrier, and the third carrier are respectively eluted with 0.5 mol / L dilute hydrochloric acid to obtain a first eluent containing nickel, a second eluent containing manganese, and a third eluent containing cobalt. The first carrier, the second carrier, and the third carrier are eluted to obtain a first biochar material, a second biochar material, and a third biochar material, which are washed, dried, and reused;
[0095] S4. Precipitation
[0096] adjusting the pH of the first eluent to 10 to obtain nickel-containing precipitate nickel hydroxide;
[0097] adding sodium sulfate to the second eluate to obtain manganese dioxide;
[0098] The pH of the third eluate was adjusted to 10 to obtain cobalt hydroxide as a cobalt-containing precipitate.
[0099] Comparative Example 1
[0100] The difference between this comparative example and Example 1 is that the third stage adsorption treatment step is omitted, and only the first stage adsorption treatment and the second stage adsorption treatment are performed on the acid hydrolyzed liquid, and the rest is the same as Example 1. The second filtrate is tested, and the contents of nickel, cobalt and manganese in the second filtrate are respectively: Ni 0.07mg / l, Co 0.23mg / l, and Mn 0.04mg / l; the calculated recovery rates of nickel are 95.7%, cobalt 4.2%, and manganese 90.9%.
[0101] Comparative Example 2
[0102] The difference between this comparative example and Example 1 is that the second stage adsorption treatment step is omitted, and only the first stage adsorption treatment and the third stage adsorption treatment are performed on the acid hydrolyzed liquid, and the rest is the same as Example 1. The third filtrate is tested, and the contents of nickel, cobalt and manganese in the third filtrate are respectively: Ni 0.05mg / l, Co 0.03mg / l, and Mn 0.43mg / l; the calculated recovery rates of nickel are 96.9%, cobalt 87.5%, and manganese 2.3%.
[0103] Comparative Example 3
[0104] The difference between this comparative example and Example 1 is that the first stage adsorption treatment step is omitted, and only the second stage adsorption treatment and the third stage adsorption treatment are performed on the acid hydrolyzed liquid, and the rest is the same as Example 1. The third filtrate is tested, and the contents of nickel, cobalt and manganese in the third filtrate are: Ni 1.60mg / l, Co 0.03mg / l, Mn 0.02mg / l respectively; the recovery rate of nickel is calculated to be 1.8%, the recovery rate of cobalt is 87.5%, and the recovery rate of manganese is 95.5%.
[0105] Comparative Example 4
[0106] The difference between this comparative example and Example 1 is that the adsorption treatment process is different. Specifically, the first biochar material, the second biochar material, and the third biochar material are first mixed evenly and placed in an adsorption stirring tank, and then the acid hydrolyzed liquid is immersed in the adsorption stirring tank containing the first biochar material, the second biochar material, and the third biochar material for adsorption treatment, so as to replace the three-stage adsorption treatment method, and the rest is the same as Example 1. The filtrate after adsorption was tested, and the contents of nickel, cobalt, and manganese in the filtrate were: Ni 1.50mg / l, Co 0.19mg / l, Mn 0.30mg / l, respectively; the recovery rate of nickel was 20.2%, the recovery rate of cobalt was 20.8%, and the recovery rate of manganese was 31.8%.
[0107] In summary, compared with the prior art, the present invention has the following beneficial effects:
[0108] 1. A method for recycling nickel-cobalt-manganese ternary positive electrode materials, comprising: performing a first-stage adsorption treatment on an acid hydrolysis solution using a first biochar material as an adsorption medium to obtain a first support body loaded with nickel and a first filtrate, then performing a second-stage adsorption treatment on the first filtrate using a second biochar material as an adsorption medium to obtain a second support body loaded with manganese and a second filtrate, and then performing a third-stage adsorption treatment on the second filtrate using a third biochar material as an adsorption medium to obtain a third support body loaded with cobalt and a third filtrate; wherein the first biochar material is at least one of peanut shells and reed straws, obtained by anaerobic pyrolysis at 400-900°C, and is modified by acid washing, and has a preferential adsorption characteristic for nickel; the second biochar The material is at least one of mangosteen shell and buckwheat shell, which is pyrolyzed in the absence of oxygen at 400-900°C to obtain biochar, which is modified by acid washing and has preferential adsorption characteristics for manganese; the third biochar material is at least one of rice straw and grapefruit peel, which is pyrolyzed in the absence of oxygen at 400-900°C to obtain biochar, which is modified by acid washing and has specific adsorption characteristics for cobalt; the recovery method of the present application utilizes the preferential adsorption characteristics of the first biochar material for nickel, the preferential adsorption characteristics of the second biochar material for manganese, and the preferential adsorption characteristics of the third biochar material for cobalt, and performs a three-stage adsorption treatment on the acid hydrolysis liquid of the nickel-cobalt-manganese ternary positive electrode material waste, so that the recovery rates of nickel, cobalt and manganese are all greater than 85%.
[0109] 2. The nickel, cobalt and manganese recovery method of the present application has a simple recovery process, low cost, good environmental protection, high efficiency, and stronger industrial operability. At the same time, it can also specifically obtain nickel, cobalt and manganese metal salts that can be directly used in industry.
[0110] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0111] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention is described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. Anything not described in detail in the present invention is a well-known technology to those skilled in the art.
Claims
1. A method for recycling nickel-cobalt-manganese ternary positive electrode materials. It is characterized in that The steps include: S1. Preparation of acid solution The nickel-cobalt-manganese ternary positive electrode material is crushed, immersed in an inorganic acid to dissolve to obtain a solution, the solution is filtered, and the filtrate is taken to obtain an acid solution; S2. Adsorption treatment of acid solution Using a first biochar material as an adsorption medium, the acid hydrolyzed liquid is subjected to a first-stage adsorption treatment to obtain a first support body and a first filtrate loaded with nickel; then using a second biochar material as an adsorption medium, the first filtrate is subjected to a second-stage adsorption treatment to obtain a second support body and a second filtrate loaded with manganese; and then using a third biochar material as an adsorption medium, the second filtrate is subjected to a third-stage adsorption treatment to obtain a third support body and a third filtrate loaded with cobalt; The first biochar material, the second biochar material, and the third biochar material are respectively obtained by modifying the biochar obtained by anaerobic pyrolysis of the first carbon-containing organic matter, the second carbon-containing organic matter, and the third carbon-containing organic matter at 400-900° C. S3, elution The first support body, the second support body and the third support body are subjected to elution treatment respectively, and a first eluent containing nickel, a second eluent containing manganese and a third eluent containing cobalt are obtained accordingly; S4. Precipitation adjusting the pH of the first eluent to obtain a nickel-containing precipitate; adding sulfate to the second eluent to obtain a manganese dioxide precipitate; The pH of the third eluate is adjusted to obtain a cobalt-containing precipitate.
2. The recycling method according to claim 1, It is characterized in that The first carbon-containing organic matter is selected from at least one of peanut shells and reed straws, and the biochar obtained by anaerobic pyrolysis of at least one of the peanut shells and reed straws is acid-washed and modified to obtain the first biochar material; The second carbon-containing organic matter is selected from at least one of mangosteen shells and buckwheat shells, and the biochar obtained by anaerobic pyrolysis of at least one of mangosteen shells and buckwheat shells is acid-washed and modified to obtain a second biochar material; The third carbon-containing organic matter is selected from at least one of rice straw and grapefruit peel. The biochar obtained by anaerobic pyrolysis of at least one of rice straw and grapefruit peel is modified by acid washing to obtain the third biochar material.
3. The recovery method according to claim 2, It is characterized in that The acid used for the pickling modification includes an inorganic acid or an organic acid. The inorganic acid is selected from any one of sulfuric acid, hydrochloric acid, and nitric acid. The organic acid is selected from any one of citric acid, oxalic acid, and formic acid.
4. The recovery method according to claim 3, It is characterized in that The concentration of the organic acid or inorganic acid is 0.5-1 mol / L.
5. The recycling method according to claim 1, It is characterized in that The specific surface area of the first biochar material, the second biochar material and the third biochar material is 200-400m 2 / g.
6. The recycling method according to claim 1, It is characterized in that In the first stage adsorption treatment, the liquid-solid ratio of the acid hydrolyzate to the first biochar material is 1000 ml: (1-50) g, and the adsorption time is 10-60 min; In the second stage adsorption treatment, the liquid-to-solid ratio of the first filtrate to the second biochar material is 1000 ml:(1-50) g, and the adsorption time is 10-60 min; In the third stage adsorption treatment, the liquid-to-solid ratio of the second filtrate to the third biochar material is 1000 ml: (1-50) g, and the adsorption time is 10-60 min.
7. The recycling method according to claim 1, It is characterized in that In S2, the temperature of the acid hydrolysis solution is 25°C to 50°C, and the pH value is 5.5 to 7.
0.
8. The recycling method according to claim 1, It is characterized in that The step S1 further includes adding alkaline solution to the acid hydrolysis solution to adjust the pH value of the acid hydrolysis solution to 4.0-4.5 to remove impurity ions and hydroxide ions.
9. The recycling method according to claim 1, It is characterized in that In S3, an acidic solution or an alkaline solution is selected for elution treatment.
10. The recycling method according to claim 1, It is characterized in that The general chemical formula of the nickel-cobalt-manganese ternary positive electrode material is LiNi x Co y Mn 1-x-y O 2 , where x+y≤1; The recovery method further comprises adding sodium carbonate to the third filtrate to obtain a lithium carbonate precipitate.
Citation Information
Patent Citations
Preparation method of biochar-based adsorbent for manganese pollution treatment
CN108671891A
Grading recovery method for waste ternary lithium battery
CN109182732A
Biomass adsorbent
CN110075800A
Modified biochar and preparation method thereof and application thereof in nickel-containing waste water
CN110152605A
Method for recovering metal from waste ternary lithium battery positive electrode material
CN114525406A
Cited By
Activated carbon and method for adsorbing and removing volatile organic compounds and mercury in flue gas