Method for producing structured protein product
By using nozzles and forming element equipment to process protein-containing materials under high pressure conditions, forming structured protein products with aligned protein fibers, the problem of difficult to simulate the complex structure and sensory characteristics of animal muscle tissue in the prior art is solved, and the problem of non-existential arts is achieved Efficient production of animal-based foods.
Patent Information
- Application Number
- CN202380031128.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-29
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively simulate structured protein products of animal muscle tissue, especially in providing non-animal-based foods with directional fibers, and it is difficult to reproduce the complex structural and sensory properties of animal muscles.
Using a device including nozzle elements and forming elements, the protein-containing material is pumped into the cavity of the forming element through the nozzle elements, forming a structured protein product with aligned proteins under high pressure and specific conditions to ensure the maintenance and enhancement of fiber length. .
A structured protein product without animal source components is achieved, whose protein fibers are aligned in a manner similar to animal source products, maintaining and enhancing fiber properties, suitable for processing and consumption as a meat alternative.
Smart Images

Figure BDA0005063545270000191 
Figure HDA0005063545280000011 
Figure HDA0005063545280000012
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a structured protein product. In particular, the method provides a product that does not contain animal-derived components but still has similar or identical features and / or properties to the animal-derived product that it is intended to replace. In particular, the method provides a product having protein fibres that are aligned in a manner similar to the muscle fibre structure of the animal-derived product that it is intended to replace. Background Art
[0002] Meat is considered the highest quality source of protein, not only due to its nutritional profile, but also due to its popular taste. Meat is nutritious, as meat protein contains all the essential amino acids for the human body. In addition, meat contains essential vitamins, such as vitamin B12, and is rich in minerals. Meat also contains muscle tissue, which contributes greatly to food acceptability by imparting specific characteristics, such as appearance, texture, and taste. Muscle tissue also contributes to the properties of meat when it is prepared and cooked, for example, in the way it shrinks, undergoes color changes during cooking, and relaxes after cooking.
[0003] However, the demand for meat substitutes has increased due to animal diseases such as mad cow disease, global shortage of animal protein, growing consumer requirements for religious (halal or kosher) food, and for economic reasons.
[0004] Meat analogs are prepared so that they resemble meat as closely as possible in appearance, taste and texture. Meat analogs are typically made from proteinaceous fibres of non-animal origin. Protein fibres, such as textured vegetable proteins, are characterised by having a recognizable structure and structural integrity so that each unit will withstand hydration, cooking, and other manipulations used to prepare the fibre for consumption.
[0005] The present invention seeks to help consumers switch from animal-based diets to meat analogs. It is widely believed that this change in consumption is beneficial in many ways. The meat industry is harmful to the environment and is very inefficient compared to crops used to produce plant-based diets. In addition, animal-derived adipose tissue is known to contain components such as cholesterol and saturated fat, which are significant health risk factors, while non-animal-derived foods are healthier and can also be produced more efficiently and in a sustainable and environmentally acceptable manner.
[0006] While many consumers are motivated to voluntarily switch to a plant-based diet, other consumers face significant challenges in giving up animal-based foods. The main challenge in providing acceptable non-animal-based foods (also referred to herein as meat analogs) is to ensure that they mimic the animal-based foods they replace as closely as possible. However, as should be understood, meat comes from animals, and providing non-animal alternatives is not an easy task. Meat products are made from animal muscle tissue, so the complex structure of the protein-based portion of this tissue (i.e., connective muscle fibers) is critical to the properties of meat, which needs to be replicated in non-animal alternatives.
[0007] The muscle structure is organized in layers and consists of a complex architecture. The structured network in the muscle is responsible for the typical structure of meat. The solid material of the muscle contains about 70% protein. The complex mixture of proteins in the muscle consists overwhelmingly of fibrous proteins, which give meat its typical structure. The muscle fibers are covered by a coarser connective tissue membrane (perimysium) and surrounded by connective tissue containing collagen and elastin. The muscle fibers consist of myofibrils, which consist of myofilaments. These myofilaments form sarcomeres, which consist of myosin and actin. Myosin forms thick filaments, while actin forms thin filaments. The sensory and quality attributes of meat are mainly related to these structural elements.
[0008] The object of the present invention is to provide a structured protein product derived from non-animal components that closely mimics the tissue and muscle structure of animal origin in terms of its characteristics and properties. In addition, the product must also be suitable as a meat analog or for use in the manufacture of meat analogs, e.g., it must be processable under the same conditions as any other components of the meat analog and must adhere and / or bond with those other components during manufacture, storage, transport, cooking, and consumption.
[0009] Providing structured protein products that closely mimic animal tissue is particularly challenging because animal muscle tissue is an extremely complex organic growth tissue that contains connective tissue within a fibrillar network of protein. It is this complex structure that provides the properties that consumers expect from meat foods, and which are difficult to reproduce in non-animal based products. In providing acceptable structured protein products, it is particularly important to provide aligned fibers, especially egg white fibers, that mimic as closely as possible the organoleptic properties of protein fibers in animal muscle tissue.
[0010] The prior art provides examples of previous attempts to provide structured protein products having oriented fibers.
[0011] US2007269567 discloses a method for producing a restructured meat composition, the method comprising: extruding a vegetable protein material through a die assembly under conditions of elevated temperature and pressure to form a structured vegetable protein product having substantially aligned protein fibers. US2008254199 discloses a method for producing a colored structured protein product having substantially aligned protein fibers, the method comprising: a. combining a protein material with at least one colorant to form a blended protein mixture; and b. extruding the blended protein mixture through a die assembly under conditions of elevated temperature and pressure to form a colored structured protein product comprising substantially aligned protein fibers. US2009208633 discloses a granular composition comprising: (A) a hydrated vegetable protein material and (B) a hydrated structured protein material having substantially aligned protein fibers; wherein the weight ratio of (A) to (B) is from about 1.5 to about 5 to about 1, to produce a granular composition having a particle size of from about 2 mm to about 10 mm. US2010074989 discloses a method for preparing a layered fibrous food structure comprising subjecting an edible protein suspension to simple shear flow and enzymatic cross-linking during shearing. These disclosures utilize a die assembly.
[0012] US2012207904 claims a method for producing a structured protein product, the method comprising: extruding at least one gluten-free protein material and a binder through a die assembly to form a structured protein product having substantially aligned protein fibers. US2021100263 claims a high-throughput continuous extrusion method for making a fibrous textured high-moisture protein food having an organoleptic quality comparable to that of cooked meat, the method comprising the following steps: preparing a blend of dry protein material and / or wet protein material streams; then feeding the blend together with water to the feed port of an extrusion cooker at a ratio of 18%-53% dry protein material to 6%-70% water, wherein the combination has a protein content greater than 15% and a fat content less than 10%; wherein the extrusion cooker is preferably a heating barrel and a container suitable for receiving the blend. The invention relates to a twin screw co-rotating type having a feed port for protein material and water; and wherein the feed port of the extrusion cooker is configured so that at least part of the protein material and water enter the extrusion cooker at the same position relative to the length of the extruder barrel, and so that the protein material and water enter the extrusion cooker at a position offset from the centerline so as to be immediately moved downstream of the water by the flights of the screws; the output of the extrusion cooker is then continuously transferred to a cooling die suitable for cooling the extrudate so that the fibers forming the protein in the extrudate are internally aligned; the cooled extrudate is then transferred to a mechanical comminution device suitable for tenderizing the extrudate and chopping it into pieces of uniform size distribution. Both of these disclosures utilize extrusion.
[0013] WO21095034 discloses a method for producing a meat substitute, the method comprising: introducing a protein-containing material into a print head of a digital printer; and operating the digital printer to dispense a single curled protein-containing filament or a plurality of separate protein-containing filaments onto a printer bed, the single filament being folded, or a plurality of said filaments being arranged so that the segments between the folds of the single filament or the plurality of filaments are substantially parallel along their longitudinal axes; wherein the protein-containing filament comprises texturized protein; and wherein at least a portion of the texturized protein comprises elongated fibers having a length exceeding 5 mm.
[0014] US11241024 discloses a method for producing a fibrous meat analog, which comprises: subjecting an ingestible polysaccharide hydrogel to directional freezing to induce the formation of aligned elongated ice crystals to form a directional frozen polysaccharide hydrogel having aligned channels, wherein the aligned elongated ice crystals are located in the aligned channels; thawing the directional frozen polysaccharide hydrogel having aligned channels by immersing the frozen ingestible polysaccharide hydrogel in a solution containing at least one ingestible soluble thermogelling protein, thereby melting at a temperature below the gelling temperature of the soluble thermogelling protein and replacing the aligned elongated ice crystals with the at least one ingestible soluble thermogelling protein to produce a protein-infused polysaccharide hydrogel, wherein the protein loading varies based on the immersion time; and heating the protein-infused ingestible polysaccharide hydrogel at a temperature above the gelling temperature of the at least one ingestible soluble thermogelling protein to produce protein fibers, thereby forming a fibrous meat analog food.
[0015] Despite the above, there remains a need for an improved method of producing structured protein products. The present inventors have now discovered, through extensive research, a new method for producing structured protein products which provides products with excellent fiber orientation. Furthermore, not only is the method capable of providing products with oriented fibers, but it has been found that the properties of these fibers are maintained and even enhanced during processing. SUMMARY OF THE INVENTION
[0017] Thus, in a first aspect, the present invention provides a method for producing a structured protein product. As used herein, the term structured protein product means that the protein fibers are aligned as described below. The resulting product may be free of animal-derived components, but still have similar or identical features and / or characteristics to the animal-derived product it is intended to replace. The method actually provides a product having protein fibers that are aligned in a manner similar to the myofiber structure of the animal-derived product it is intended to replace. The method also provides for the maintenance of protein fiber length and may even provide for an increase in protein fiber length.
[0018] The method of the first aspect uses an apparatus comprising a nozzle element and a forming element, wherein:
[0019] i) the nozzle element comprises an opening (1);
[0020] ii) the shaped element comprises one or more cavities (4) that are recessed relative to the shaped element surface (5); and
[0021] iii) the nozzle element and the shaping element are movable relative to each other so that
[0022] - in the closed configuration, the opening (1) is blocked by the surface (5), and
[0023] - in an open configuration, the opening (1) is at least partially aligned with the cavity (4),
[0024] The method comprises the following steps:
[0025] a) moving the nozzle element and the forming element relative to each other so that the opening (1) is at least partially aligned with the one or more cavities (4), thereby configuring the opening (1) into an open structure;
[0026] b) pumping a protein-containing material (6) into the cavity (4) through the opening (1), thereby forming a structured protein product (8) in the cavity (4);
[0027] c) moving the nozzle element and the forming element relative to each other so that the opening (1) is aligned with the surface (5) of the forming element, thereby configuring the opening (1) into a closed configuration; and then
[0028] d) removing the structured protein product (8) from the cavity (4).
[0029] Preferably, the opening has an aspect ratio of 1:100 to 100:1.
[0030] Preferably, the width of the opening (1) is at least 100% of the widest part of the cavity (4) of the shaped element.
[0031] Preferably, the nozzle element comprises a sealing element (2).
[0032] Preferably, the shaped element is in the form of a cylinder with a horizontal axis of rotation, the cylinder having a plurality of cavities located on the outer surface of the cylinder.
[0033] Preferably, the protein-containing material comprises 1 to 65 wt% protein.
[0034] Preferably, the protein-containing material does not contain animal protein.
[0035] Preferably, the protein-containing material comprises 1 to 20 wt% of a binder.
[0036] Preferably, the protein-containing material comprises 0.5 to 15% by weight fat or oil.
[0037] Preferably, the protein fibers forming the structured protein product abut each other at an angle of less than 45°.
[0038] Preferably, at least 25% of the protein fibers are adjacent to each other.
[0039] In a second aspect, the present invention provides a structured protein product directly obtainable by the method of the first aspect.
[0040] In a third aspect, the present invention provides use of the product of the second aspect for the manufacture of a meat substitute product.
[0041] In a third aspect, the present invention provides a meat substitute product comprising the product of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] FIG. 1 shows a view of a nozzle element used in the present invention.
[0043] FIG. 2 shows a view of a forming element used in the present invention.
[0044] Figure 3 shows the device configured for mass production.
[0045] Figure 4 shows the equipment configured for serial production.
[0046] FIG5 illustrates the method of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0048] The present invention provides a new and improved method for producing a structured protein product. The resulting product need not contain animal-derived components, but still has similar or identical features and / or characteristics to the animal-derived product it is intended to replace. The method actually provides a product having protein fibers that are aligned in a manner similar to the muscle fiber structure of the animal-derived product it is intended to replace. The method also provides for the maintenance of protein fiber length and can even provide for an increase in protein fiber length.
[0049] equipment
[0050] The method of the present invention uses an apparatus comprising a nozzle element and a forming element.
[0051] Nozzle components
[0052] Figure 1 shows views of a nozzle element for use in the present invention, A) in perspective from above, B) in perspective from below, and C) in cross section. The nozzle element comprises an opening (1). The nozzle element may further comprise a sealing element (2) and a conduit (3), such as a pipe, tube, or the like, through which the protein-containing material can be delivered to the opening (1).
[0053] Opening
[0054] The opening (1) may be of any suitable size and / or shape. For example, the opening (1) may be circular, oval, or rectangular. It may preferably have an aspect ratio of 1:100 to 100:1, more preferably 1:75 to 75:1, still more preferably 1:50 to 50:1, even more preferably 1:25 to 25:1, still more preferably 1:10 to 10:1, even still more preferably 1:5 to 5:1, still still more preferably 1:2.5 to 2.5:1, preferably about 1:1.
[0055] The width of the opening (1) is measured as the widest point perpendicular to the direction of movement of the nozzle element relative to the forming element. The opening (1) may be sized so that it has the same width, or approximately the same width, or is wider than the widest part of the cavity of the forming element (the widest part of the cavity is measured as the widest point perpendicular to the direction of movement of the nozzle element relative to the forming element).
[0056] Preferably, the width of the opening is at least 100%, more preferably at least 125%, even more preferably at least 150%, even more preferably still at least 200% of the widest part of the cavity of the shaped element.
[0057] Alternatively, the width of the opening is less than 100%, preferably less than 75%, more preferably less than 50%, even more preferably less than 25% of the widest part of the cavity of the shaped element.
[0058] The size and shape of the opening (1) may correspond to the opening of the cavity. For example, if the cavity is shaped to form a round hamburger product, the opening (1) may have a round shape to correspond to the round shape of the opening of the cavity. Alternatively, if the cavity is shaped to form a chicken fillet product, the opening (1) may have a chicken fillet shape corresponding to the cross-sectional chicken fillet shape of the cavity.
[0059] However, an advantage of this approach is that the opening (1) does not need to be of any particular shape, and may simply be an opening large enough to allow the protein-containing material to be pumped into the cavity.
[0060] Sealing elements
[0061] The nozzle element may optionally comprise a sealing element (2), as shown in Figure 1. Such a sealing element (2) is able to seal the cavity of the shaped element.
[0062] The sealing element (2) may be of any suitable size and / or shape. However, it will be appreciated that such a sealing element (2) is preferably of such size and shape that it covers the cavity until the opening (1) of the nozzle is no longer in the open configuration.
[0063] The nozzle element may be any suitable material, such as stainless steel, plastic, or other such material. Preferably, it is constructed of a flexible but resilient material such as polypropylene.
[0064] Forming elements
[0065] Figure 2 shows views of a shaped element for use in the invention, A) in perspective from above, and B) in cross section.The shaped element comprises one or more cavities (4) recessed into the shaped element relative to its surface (5).
[0066] The shaped element may be of any suitable material, such as stainless steel, plastic, or other such material. The cavity may be of a different material than the rest of the shaped element. The shaped element and hence the cavity (4) may be temperature controlled in order to heat or cool the protein-containing material pumped into the cavity (4).
[0067] Cavity
[0068] The shaped element comprises one or more cavities (4), preferably the shaped element comprises a plurality of cavities (4).
[0069] The cavity (4) may be of any suitable shape. Preferably, the cavity (4) corresponds to the shape of the structured protein product to be produced in the process. For example, if the process is to provide an animal-free alternative to whole meat cuts, the cavity (4) will correspond to the shape of a steak, or a chicken fillet, or a pork fillet, or the like. Alternatively, if the process is to provide an animal-free alternative to formed processed meat products (such as those made from ground meat, such as sausages or burgers), the cavity will be shaped accordingly.
[0070] The cavity may also be textured to provide surface features to the formed product, such as striations corresponding to muscle fibers in a whole meat cut.
[0071] If multiple cavities (4) are used, their shapes and sizes may be similar but different to produce a more heterogeneous product shape that is more realistic to the consumer. The cavity may be coated with a release agent. The release agent may be temporary, such as an oil spray, preferably a vegetable oil. The release agent may be more permanent, such as a Teflon coating applied to the cavity.
[0072] surface
[0073] The cavities (4) are recessed in the surface (5) of the forming element. The cavities may be positioned relative to each other so that they are sufficiently spaced apart from each other to allow a surface (5) area sufficient for the sealing element to interface, that is, the gap between the cavities should be greater than the length of the cavity as measured in the direction of movement of the nozzle element relative to the forming element.
[0074] Interaction of forming elements and nozzle elements
[0075] The nozzle element and the shaping element are movable relative to each other.
[0076] The nozzle element may be movable over the surface (5) and the cavity (4) on which the forming element is fixed; or the forming element may be movable while the nozzle element is stationary; or both the nozzle element and the forming element may be movable.
[0077] Crucially, the nozzle element and the forming element are movable relative to each other so that the opening (1) of the nozzle element can be registered with one or more cavities (4) of the forming element. That is, the nozzle element can be moved to a position such that the opening (1) is in an open configuration so that it can fill the cavity (4).
[0078] The equipment can be configured in a variety of different ways. Figure 3 shows the equipment configured for mass production. Figure 3A ), the forming element is in the form of a plate having a plurality of cavities. The nozzle and the forming element are laterally movable relative to each other so that the opening (1) is aligned with the cavity (4). Figure 3B ) the apparatus is in the form of a carousel having a shaped element in the form of a circle having a plurality of cavities. The nozzle and the shaped element are movable relative to each other so that the opening (1) is aligned with the cavity (4), but in this arrangement it is simpler to rotate the shaped element to bring the cavity (4) into position below the nozzle element. Figure 3C ) shows the Figure 3B) in which the forming element is in the form of a disc having a greater number of cavities arranged in a plurality of concentric circles and with a plurality of nozzle elements, one for each concentric circle. Alternatively, a nozzle element having a plurality of openings may be used, or a nozzle element having a single opening capable of being aligned with all of the cavities may be used. As with the previous configurations, the nozzle element and the forming element may be moved relative to each other, but again, it is simpler to rotate the forming element to bring the cavity (4) to a position below the nozzle element. In these batch configurations, once all of the cavities are filled, the forming element needs to be separated from the nozzle element and then manipulated so that the structured protein product can be removed from the cavity (4). For example, a human operator may manually remove the product from the cavity, or the forming element may be inverted to allow the product to be released from the cavity under the action of gravity.
[0079] Figure 4 shows the equipment configured for continuous production. Figure 4A ), the forming element is in the form of a conveyor belt having a plurality of cavities. The apparatus is shown in perspective and in cross-section. The forming element (i.e., the conveyor belt) can be operated so that the cavities are moved into registration with the openings of the nozzle element. Typically, in this arrangement, there is no need to move the nozzle element. The filled cavities will travel along the conveyor belt until they reach the end, at which point the conveyor belt moves the cavities to an inverted position and the structured protein product can be easily removed from the cavities simply by the action of gravity. In Figure 4B ) in which the forming element is in the form of a cylinder with a horizontal axis of rotation, the cylinder having a plurality of cavities located on the outer surface of the cylinder. The forming element (i.e., the cylinder) is rotated so that the cavities move into alignment with the openings of the nozzle element. Typically, in this arrangement, the nozzle element is positioned at the top of the device and does not need to be moved. The filled cavities are then moved past the nozzle element until they become inverted, at which point the structured protein product can be easily removed from the cavities simply by the action of gravity. The nozzle element may include a sealing element for sealing the cavities until they reach a position where the structured protein product is to be removed. In Figure 4C), the forming element includes a pair of intersecting cylinders, both of which have a horizontal rotation axis and have a plurality of cavities on the outer surface of the cylinder. The cavity of the forming element is designed to correspond to the cavity of another forming element. The forming element (i.e., the cylinder) rotates in the opposite direction so that the cavity moves to align with the opening of the nozzle element. Usually, in this arrangement, the nozzle element is positioned at the top of the device and does not need to move. Then, the filling cavity of each forming element moves through the nozzle element until they meet the corresponding cavity on the other cylinder at the point where the outer surface of the cylinder intersects. In this way, a full three-dimensional product can be formed, whereby the two halves of the structured protein product are provided by each of the two cavities and then joined together at the intersection. The nozzle element can include sealing elements, which are used to seal the cavity until they reach the intersection. When the cavity moves through the intersection, the structured protein product can be easily removed from the cavity simply by gravity.
[0080] Product Remover
[0081] The structured protein product may be removed from the cavity of the apparatus simply by inverting the cavity and allowing gravity to act on the product. Additionally or alternatively, the cavity may include a removal means, such as a mechanical pusher, such as a piston or an actuated plate, which forces the product out of the cavity. Alternatively, the removal means may include a means for injecting a fluid, preferably a gas, into the cavity, thereby forcing the product out of the cavity. Alternatively, the cavity may be formed of a deformable material, such as a flexible plastic, whereby a force, such as air pressure, may be applied to the non-surface side of the cavity, thereby deforming the cavity outwardly toward the surface of the forming element, and even beyond the surface of the forming element, thereby causing the product to fall out of the cavity.
[0082] After the product is removed from the cavity, it can then be transported using suitable means (such as a conveyor belt) to any subsequent processing steps that may be required, such as cooling, freezing, cooking, etc.
[0083] Protein-containing materials
[0084] The method of the present invention comprises the step of pumping a protein-containing material into a cavity (4) through an opening (1), thereby forming a structured protein product within the cavity (4).
[0085] protein
[0086] The protein-containing material preferably comprises 1 to 65 wt. %, more preferably 2 to 50 wt. %, even more preferably 5 to 25 wt. %, still more preferably 10 to 20 wt. %, most preferably about 15 wt. % protein.
[0087] The protein is from a non-animal source, preferably the protein is of plant origin. The plant source protein can be selected from legumes, soybeans, sunflowers, rapeseed, sesame, cottonseed, safflower, peas, lupines, peanuts, chickpeas, dry beans, lentils, dry peas (garden peas), broad beans (fava beans), pigeon peas, cowpeas, wheat, corn, rice, barley, rye, oats, sorghum, quinoa, rapeseed, potatoes, cassava, sweet potatoes, cassava, wild amaranth, beets, aquatic plants, grape seeds, tomato seeds, papaya kernels. Preferably, the vegetable protein is isolated from soybeans or corn, more preferably soybeans. Suitable soy source protein is a texturized vegetable protein, such as Fibertex (supplier: Gushen).
[0088] Preferably, the protein has fibers having a length of 0.1 to 15 cm, more preferably 0.2 to 10 cm, even more preferably 0.3 to 5 cm, most preferably 0.5 to 3 cm.
[0089] Preferably, the protein has fibers having a width of 0.01 to 2 mm, more preferably 0.05 to 1.5 mm, even more preferably 0.075 to 1 mm, most preferably about 0.1 to 0.5 mm.
[0090] water
[0091] In order to prepare the protein-containing material, the protein is hydrated. Thus, the protein-containing material preferably comprises 3 to 95 wt. %, more preferably 5 to 75 wt. %, even more preferably 10 to 50 wt. %, still more preferably 15 to 40 wt. %, most preferably about 25 wt. % water.
[0092] Protein:Water Ratio
[0093] Preferably, the ratio of water to protein is from 1:5 to 10:1, more preferably from 1:2.5 to 7.5:1, still more preferably from 1:1 to 5:1, most preferably about 2:1.
[0094] Binder
[0095] The protein-containing material may include a binder to bind the protein fibers.
[0096] Preferably, the protein-containing material comprises 1 to 20 wt%, more preferably 2 to 15 wt%, still more preferably 3 to 10 wt%, most preferably about 5 wt% of binder.
[0097] Preferably, the binder is methylcellulose, soy protein isolate, or a combination thereof.
[0098] Oil / Fat
[0099] The protein-containing material may contain fat or oil, which may further enhance juiciness. Preferably, the protein-containing material contains 0.5 to 15 wt %, more preferably 1 to 10 wt %, still more preferably 2.5 to 7.5 wt %, most preferably about 5 wt % fat or oil.
[0100] As used herein, the term "fat" refers to a glyceride selected from triglycerides, diglycerides, monoglycerides, phosphoglycerides, and combinations thereof. The term "fat" encompasses fats that are liquid at ambient temperature (referred to herein as "oils"), as well as fats that are solid or semisolid at ambient temperature. The melting point of a fat can be determined according to ISO 6321 (2021).
[0101] The fat or oil can be selected from safflower oil, shea butter, allan blackia butter, linseed oil, castor oil, sunflower oil, soybean oil, rapeseed oil, olive oil, tung oil, cottonseed oil, peanut oil, palm kernel oil, coconut oil, cocoa butter, and palm oil. The fat can also be a mixture thereof.
[0102] Preferably, the fat or oil is linseed oil, castor oil, sunflower oil, soybean oil, rapeseed oil, olive oil, tung oil, cottonseed oil, peanut oil, or a mixture thereof.
[0103] More preferably, the fat or oil is linseed oil, castor oil, sunflower oil, soybean oil, rapeseed oil, olive oil, or a mixture thereof.
[0104] Most preferably, the fat or oil is sunflower oil.
[0105] Flavouring
[0106] The protein-containing material may include one or more additional flavours.
[0107] Additional flavoring agents may include flavoring agents and / or flavor enhancers.
[0108] Flavoring agents can be natural or artificial. Flavoring agents can simulate or replace ingredients present in meat tissue, such as serum protein, muscle protein, hydrolyzed animal protein, beef tallow, fatty acids, etc. Flavoring agents can provide animal meat flavor, barbecue flavor, rare beef flavor, etc. Flavoring agents can be animal meat oil, oleoresins or aquaresins of spice extracts, spice oils, natural liquid smoke, natural smoke extracts, yeast extracts, or mushroom extracts. Additional flavoring agents can include onion flavor, garlic flavor, or vanilla flavor.
[0109] The protein-containing material may also contain a flavor enhancer. Examples of flavor enhancers that may be used include salt (sodium chloride), glutamate (eg, monosodium glutamate), glycinate, guanylate, inosinate, 5'-ribonucleotide salts, hydrolyzed animal protein, and hydrolyzed vegetable protein.
[0110] Preferably, the protein-containing material comprises additional flavouring agents in an amount of 1 to 10 wt%, more preferably 2 to 8 wt%, still more preferably 4 to 6 wt%, most preferably about 5 wt%.
[0111] fiber
[0112] The protein-containing material may also include non-protein fibers. Suitable fibers include cellulose, non-cellulose polysaccharides such as hemicellulose, and non-carbohydrate components such as lignin. Cellulosic fibers are derived from vegetables, beets, and various brans. Hemicellulose can be obtained from cereals. Lignin can be derived from woody plants. Examples include insoluble fibers derived from potatoes, oats, peas, and citrus, apples, psyllium, fenugreek, carrots, and inulin. Preferably, the fiber is oat fiber. It is believed that the fiber serves to retain the aforementioned flavoring agents when used.
[0113] Preferably, the protein-containing material comprises non-protein fibers in an amount of 0.2 to 5 wt%, more preferably 0.5 to 4 wt%, still more preferably 1 to 3 wt%, most preferably about 2 wt%.
[0114] A protein-containing material may also be referred to as a composition comprising protein.
[0115] In one embodiment of the present invention, the protein-containing material (protein-containing composition) comprises one or more ingredients selected from the group consisting of protein, water, a binder, oil / fat, flavoring and fiber.
[0116] In one embodiment of the present invention, the protein-containing material (protein-containing composition) comprises protein, water, a binder, oil / fat, flavoring and fiber.
[0117] In one embodiment of the invention, the protein-containing material (composition comprising protein) comprises:
[0118] a. 1 to 65% by weight of protein,
[0119] b. 3% to 95% by weight of water,
[0120] c. 1 to 20% by weight of a binder,
[0121] d. 0.5 to 15% by weight of fat,
[0122] e. 1 to 10% by weight of flavoring agents,
[0123] f. 0.2 to 5% by weight of fibers.
[0124] The protein-containing material (composition comprising protein) comprises ingredients selected from the group consisting of protein, water, binder, oil / fat, flavoring, fiber and mixtures thereof.
[0125] Processing of protein-containing materials
[0126] The protein-containing material may be formed into any suitable form for use in the method of the present invention. Typically, it will be formed into a pumpable form, such as a fiber dough. Any form of processing known to those skilled in the art may be used to provide the protein-containing material.
[0127] It is preferred that the components of the protein-containing material are processed in a manner such that the protein fibers therein are not adversely affected. For example, in order to maintain the length of the protein fibers, the components of the protein-containing material are combined under low shear and / or low energy input.
[0128] Protein hydration
[0129] The protein, preferably texturized vegetable protein, can be gently hydrated in the presence of water. For example, gentle hydration can be achieved by placing the protein and hydration water in the bowl of a bowl chopper having a very blunt paddle constructed of a metal plate with square edges and no sharp parts. Such processing results in hydrated protein, which can comprise only the protein-containing material and is therefore used in the method of the present invention. However, as mentioned above, it may be desirable to include additional ingredients in the protein-containing material.
[0130] Binders and Oils / Fats
[0131] If used, the binder and oil / fat are mixed in a blender at very high energy whereby they combine to form a pre-emulsion. Protein is not included in this step as doing so would break up the protein fibers, resulting in a paste rather than the desired fibrous dough.
[0132] Non-protein fiber and flavoring
[0133] If used, the dry ingredients other than protein fiber and flavoring can be premixed, added to the aforementioned pre-emulsion, and combined with the pre-emulsion under very high energy conditions. This results in a flavoring emulsion, which can then be gently combined with the hydrated protein to form the protein-containing material for use in the process of the present invention. It has been found that the use of such high energy processing results in a firmer structured protein product due to the formation of a fine pre-emulsion during the preparation of the protein-containing material.
[0134] Alternatively, the pre-emulsion, premixed dry ingredients of non-protein fibers and flavoring, and the hydrated protein may be gently combined using, for example, a chopper as described above for the hydrated protein. It has been found that this lower energy process results in a softer protein-containing material being used in the process of the present invention, and without being bound by theory, it is believed that this type of low viscosity material is a preferred matrix in which the protein fibers can move and align.
[0135] It will be appreciated that the protein-containing material thus formed may be in the form of a dough, preferably a fibrous dough.The protein-containing material is pumpable.
[0136] Process for producing structured protein products
[0137] In the method of the present invention, the nozzle element and the forming element are moved relative to each other so that the opening (1) is at least partially aligned with the cavity (4). Thus, the opening (1) is moved from a closed configuration, in which it is obscured by the surface (5), to an open configuration. Then, the protein-containing material is pumped into the cavity (4) via the opening (1), thereby forming a structured protein product in the cavity (4). It has been surprisingly found that when the protein-containing material enters the cavity through the opening, excellent fiber alignment is achieved in the cavity.
[0138] The method of the invention is illustrated in Figure 5. In Figure 5, the nozzle element moves relative to the forming element in the direction of the arrow.
[0139] - Figure 5A ) shows the nozzle element positioned upstream of the forming element, and the cavity (4) is uncovered. Although the protein-containing material (6) is pumped towards the opening (1), the opening (1) is still in contact with the forming element surface (5) and is therefore in a closed configuration, so that the protein-containing material (6) is retained in the nozzle element.
[0140] -like Figure 5B ) shows that as the nozzle element moves towards the cavity, the sealing element (3) begins to cover the cavity, but the opening (1) remains in a closed structure.
[0141] -exist Figure 5C ), the cavity is completely sealed by the sealing element (3), but the opening (1) is still in a closed structure.
[0142] -exist Figure 5D ), the opening (1) has moved away from the surface (5) of the forming element and is partially aligned with the cavity (4). The opening (1) is thus in an open configuration. The protein-containing material (6) can no longer be retained in the nozzle element and can flow under pressure into the cavity (4). At this stage, it has surprisingly been found that the protein fibers (7) in the protein-containing material (6) are aligned.
[0143] -like Figure 5E ) shows that the cavity is quickly filled with protein-containing material (6), and the fibers are aligned, thereby forming a structured protein product (8) in the cavity (4). At this point, the pressure in the cavity is equal to the pumping pressure, and the protein-containing material (6) stops flowing into the cavity. However, the pressure serves to keep the protein fibers (7) aligned, thereby further ensuring the quality of the structured protein product (8).
[0144] - Fig. 5F ) shows that the nozzle element has further passed through the cavity (4) so that the opening is in a closed configuration, but the cavity is still sealed by the sealing element (3) and the structured protein product (8) is still retained therein.
[0145] -like Figure 5G ) once the nozzle element has completely passed through the cavity (4), the structured protein product (8) can be removed from the cavity (4).
[0146] Pumping of protein-containing materials
[0147] As detailed above, the protein-containing material is pumped into the cavity via an opening in the nozzle element. Any suitable device can be used for this purpose, provided that it is capable of moving the protein-containing material from an upstream location (such as a mixer or storage tank) via a suitable conduit to the opening so that it reaches the opening under pressure. Various pumps can be used, but positive-displacement pumps are preferred. The pump can be: a rotary positive displacement pump (such as an internal or external gear pump, a screw pump, a cam pump, a shuttle pump (shuttle block), an elastic scraper pump (flexible vane) or a sliding vane pump (sliding vane), a circumferential piston pump (circumferential piston), a flexible impeller pump (flexible impeller), a helical twisted root pump (helical twisted roots) or a liquid ring pump); a reciprocating positive displacement pump (such as a piston pump, a plunger pump or a diaphragm pump); or a linear positive displacement pump (such as a rope pump (rope pumps) and a chain pump (chain pumps)). An extruder, such as a single screw or twin screw extruder, may also be used to move the protein-containing material to the opening.
[0148] The temperature of the protein-containing material may be controlled to ensure that the material has the desired consistency and / or viscosity so as to be liquid enough for pumpability, yet compact enough to retain its shape and maintain fiber alignment when metered into the cavity.
[0149] Properties of structured protein products
[0150] As detailed above, the process of the present invention is uniquely capable of providing a structured protein product having oriented fibers.
[0151] Fiber alignment
[0152] In the context of the present invention, oriented fibers means that the protein fibers forming the structured protein product adjoin each other at an angle of less than 45°, preferably less than 40°, more preferably less than 30°, still more preferably less than 20°, even more preferably less than 10° and most preferably less than 5° when viewed on a plane.
[0153] Preferably at least 25%, more preferably at least 50%, still more preferably at least 60%, even more preferably at least 70%, still more preferably at least 80%, even still more preferably at least 90%, most preferably at least 95% of the protein fibers are adjacent to each other.
[0154] Methods for determining the degree of alignment of protein fibers are known to those skilled in the art and include quantitative determinations based on visual or automated analysis of images of the relevant structure or product. The structured protein product formed by the method of the present invention generally has the texture and consistency of animal meat. In contrast, conventional extrudates with misaligned protein fibers (i.e., randomly oriented) generally have an unacceptable texture. For example, it may lack the expected firmness, not produce the same mouthfeel when chewed, and not behave in a desired manner during cooking.
[0155] Shear Strength
[0156] In addition to having aligned protein fibers, the structured protein products formed by the methods of the present invention also have shear strength similar to whole meat muscles. As used herein, the term shear strength provides a method of quantifying the ability of the methods of the present invention to provide a structured protein product with a whole meat-like texture and appearance.
[0157] As used herein, shear strength means the maximum force required to shear through a given sample. The shear strength of a sample is measured in grams and can be determined in the following manner: weigh a sample of a structured protein product; place the sample in a heat-sealable pouch; add water about three times the weight of the sample; evacuate the pouch to a pressure of about 0.01 bar and seal the pouch; allow the sample to hydrate for about 12 to 24 hours; remove the hydrated sample and place it on a texture analyzer floor, which is oriented so that the cutter of the texture analyzer cuts the sample along the diameter (the sample is oriented so that the cutter is perpendicular to the long axis of the textured sheet for cutting). A suitable cutter is a TA-45 toothed blade manufactured by Texture Technologies (USA). A suitable texture analyzer is a TA, TXT2 type equipped with a load of 25, 50 or 100 kilograms manufactured by Stable Micro Systems Ltd. (England). Therefore, shear strength is quantified as the maximum force (in grams) required to shear through a sample.
[0158] The structured protein product produced by the process of the present invention preferably has an average shear strength of at least 250 g, more preferably at least 500 g, still more preferably at least 750 g, even more preferably at least 1000 g, still more preferably at least 1250 g, even still more preferably at least 1500 g, most preferably at least 2000 g.
[0159] Fiber size
[0160] The protein fibers formed in the structured protein product can be determined using a fragmentation characterization test that is capable of determining the percentage of large pieces formed in the structured protein product. The fragmentation characterization percentage can also be used as a proxy measure to quantify the degree of alignment of the protein fibers in the structured protein product—as the percentage of large pieces increases, the degree of alignment of the protein fibers within the structured protein product also increases. Conversely, as the percentage of large pieces decreases, the degree of alignment of the protein fibers within the structured protein product also decreases.
[0161] The method for determining the characteristics of the fragments is as follows: place 150 g of the sample in a heat-sealable plastic bag, add 450 g of 25°C water, vacuum seal the bag at about 150 mm Hg, and allow the contents to hydrate for about 1 hour; place the hydrated sample in the bowl of a mixer (e.g., a Kitchen Aid mixer model KM14G0 equipped with a single-blade paddle) and mix the contents at 130 rpm for two minutes; scrape the paddle and bowl, and pour the scrapings back into the bottom of the bowl; repeat the stirring and scraping twice, and remove 200 g of the mixture from the bowl; separate all fibers or filaments longer than 2.5 cm from the chopped mixture; weigh the separated fibers and divide the weight by the starting weight (200 g) to determine the % of large pieces in the sample.
[0162] The structured protein product achieved by the process of the present invention preferably has an average shred characterisation of at least 10% by weight large pieces, more preferably at least 12%, still more preferably at least 14%, even more preferably at least 16%, still more preferably at least 18%, even still more preferably at least 20%, most preferably at least 25%.
[0163] Fiber length maintenance parameters
[0164] As previously described, the method of the present invention can produce a structured protein product with oriented fibers and characteristics similar to animal muscle tissue. In addition, the method can ensure that the protein fibers in the protein material will not be affected by the negative effects of processing. This is in contrast to other methods, as confirmed by the following examples, which cause protein fibers to be damaged, and protein fibers are broken and shortened, and therefore are less likely to provide characteristics similar to animal muscle tissue. The damage to protein fibers can be calculated by utilizing methods known to those skilled in the art (such as those described above), to measure the length of protein fibers before processing and in the final product. This calculation is referred to as fiber length maintenance parameter (Fiber Length Maintenance Parameter, FLMP) in this article and is calculated in the following manner:
[0165] -Measure the average protein fiber length of the protein-containing material [before filling the cavity] - referred to as "A";
[0166] - measuring the average protein fiber length of the structured protein product, referred to as "B"; and wherein
[0167] -FLMP=B / A.
[0168] Preferably the FLMP is at least 0.5, more preferably at least 0.6, still more preferably at least 0.7, even more preferably at least 0.8, still more preferably at least 0.9, even still more preferably at least 0.95, most preferably at least 0.99.
[0169] Fiber length increase parameters
[0170] As predicted above, method of the present invention can actually increase the length of protein fiber.Not bound by theory, it is assumed that method of the present invention separates or gently depolymerizes the inhomogeneous macromolecular structure or the complex in protein fiber uniquely, thus actually increases the length of protein fiber.The increase of protein fiber length can be calculated by utilizing methods well known to those skilled in the art (such as those described above), to measure the length of protein fiber before processing and in the final product.In this case, this calculation is referred to as fiber length increase parameter (Fiber Length Increase Parameter, FLIP) in this article and is calculated in a manner similar to above-mentioned FLMP in the following manner:
[0171] -Measure the average protein fiber length of the protein-containing material [before filling the cavity] - referred to as "C";
[0172] - measuring the average protein fiber length of the structured protein product, referred to as "D"; and wherein
[0173] -FLIP=D / C.
[0174] Preferably FLIP is at least 1, more preferably at least 1.1, still more preferably at least 1.2, even more preferably at least 1.3, still more preferably at least 1.4, most preferably at least 1.5.
[0175] Subsequent processing steps
[0176] Once the structured protein product is removed from the cavity, it can be subjected to further processing steps. Ideally, the product is processed in a manner that fixes or stabilizes the unique aligned protein structure achieved in the inventive method. The product can be frozen. The product can also or additionally be cooked, where any form of appropriate heating (e.g., boiling, frying, roasting, grilling, oven, microwave oven, etc.) can be used. The product thus formed can then be packaged and shipped to the consumer. The consumer can then cook or reheat the product again, slice it to form cold cuts, use it as cooked meat in salads, deep-fry it, chop the product into soups or stews, or any such use that the consumer may desire for such a meat substitute product.
[0177] Products of the method of the present invention
[0178] As will be appreciated, the process of the present invention provides a unique structured product having distinct physical and organoleptic properties resulting from the process.Thus, the present invention also provides a structured protein product directly obtained by the process of the present invention.
[0179] Use of the product of the method of the present invention for manufacturing meat substitute products
[0180] The structured protein product obtained directly from the process of the present invention can be used together with other product components such as fat components, coatings, further structured protein products, etc., thereby producing additional and distinct meat substitute products. Therefore, the present invention also provides such use, and provides the meat substitute product comprising the structured protein product obtained directly from the process.
[0181] As used herein, the term "comprising / including" encompasses the terms "consisting essentially of" and "consisting of...." When the term "comprising / including" is used, the listed steps or options need not be exhaustive.
[0182] Unless otherwise indicated, numerical ranges expressed in the format "from x to y" are understood to include x and y. In specifying any range of values or amounts, any particular upper value or amount can be correlated to any particular lower value or amount.
[0183] Except in the Examples and Comparative Experiments, or where otherwise expressly indicated, all numbers are understood to be modified by the word "about".
[0184] All percentages and ratios contained herein are calculated by weight unless otherwise specified.
[0185] As used herein, unless otherwise indicated, the indefinite article "a" or "an" and the corresponding definite article "the" mean at least one, or one or more.
[0186] The various features of the invention mentioned in the above sections are appropriately applicable to other sections after making necessary modifications. Therefore, the features specified in one section can be appropriately combined with the features specified in other sections. The addition of any section heading is merely for convenience and is not intended to limit the present disclosure in any way.
[0187] The present invention will be further illustrated in the following examples. The examples are intended to illustrate the present invention and are not intended to limit the present invention to those examples themselves. Example
[0188] Exemplary protein-containing materials were prepared and subjected to various processing methods as described below.
[0189] formula
[0190] The following table provides the formulation of the protein containing material.
[0191]
[0192] Processing of protein-containing materials
[0193] The textured vegetable protein is gently mixed in a blender with a very blunt blade constructed of a metal plate with square edges and no sharp parts in the presence of water (to hydrate the protein). A hydrated protein component is obtained.
[0194] Binder, oil and additional water (crushed ice and 4°C) were blended to form the pre-emulsion component.
[0195] The non-protein fiber and flavoring agent are premixed and then blended with the pre-emulsion components to form the flavored emulsion.
[0196] The hydrated protein and flavored emulsion components are gently mixed in a blender, thereby forming a protein-containing material.
[0197] Production of products
[0198] The resulting protein-containing material is used or intended to be used to produce a variety of structured protein products, including:
[0199] Sample A:
[0200] The protein-containing material is pumped through sausage stuffing tubes with diameters of 25 mm or 20 mm using a Handtmann vane pump. It has been found that these tubes act to align the protein fibers, and the protein-containing material leaving the tubes is fibrous and has an acceptable structure. However, the extruded material must be handled manually with extreme caution to ensure that the aligned structure resulting from the method can be maintained. Despite this caution, it is not possible to use the extruded material to prepare a finished product.
[0201] Sample B:
[0202] The protein-containing material was processed using a Netzsch pump comprising a screw feeder pump followed by a positive displacement pump. However, although protein fibers were visible in the obtained product, they were not aligned.
[0203] Sample C:
[0204] A Netzsch pump comprising a screw feeder pump followed by a positive displacement pump was also used, but a breaker plate was added to create a laminar flow in order to align the protein fibers. However, it was found that the protein fibers were broken by this additional component and no structured protein product could be formed.
[0205] Sample 1:
[0206] Sample 1 is according to the invention. An apparatus comprising a forming element in the form of a rotating cylinder having four rows of chicken breast-shaped cavities and a nozzle element having an opening spanning all four rows was used. Protein-containing material was pumped into a conduit leading to an opening, which, once partially aligned with the cavity, allowed the cavity to fill.
[0207] The resulting structured protein products showed excellent alignment of protein fibers and retained their shape well after removal from the cavity.
[0208] Fiber length analysis
[0209] A 6 g sample was obtained from the following recipe:
[0210] - Hydrated TVP (as above)
[0211] -Protein-containing material (from sample 1)
[0212] -Cooked Structured Protein Product (from Sample 1)
[0213] Fibers were removed from the sample by repeated (×3) washing with water and ethanol, vacuum was applied twice, and the fibers were subjected to stirring in a beaker with water for approximately one hour to allow separation of the fibers. Each fiber was then removed, placed on black paper, and photographed with a DigiEye. The resulting images were analyzed using ImageJ to determine fiber length.
[0214] It was found that the hydrated TVP and the cooked structured protein product had almost identical average protein fiber lengths (3.97 mm and 3.92 mm, respectively). The protein-containing material actually had an average fiber length of 5.2 mm.
Claims
1. A method for producing a structured protein product using an apparatus, The apparatus comprises a nozzle element and a forming element, wherein: i) the nozzle element comprises an opening (1); ii) the shaped element comprises one or more cavities (4) recessed relative to the shaped element surface (5); and iii) the nozzle element and the shaping element are movable relative to each other so that - in the closed configuration, the opening (1) is obscured by the surface (5), and - in the open configuration, the opening (1) is at least partially aligned with the cavity (4), The method comprises the following steps: a) moving the nozzle element and the forming element relative to each other so that the opening (1) is at least partially aligned with the one or more cavities (4), thereby configuring the opening (1) into the open structure; b) pumping a protein-containing (6) material into the cavity (4) through the opening (1), thereby forming the structured protein product (8) within the cavity (4); c) moving the nozzle element and the forming element relative to each other so that the opening (1) is aligned with the surface (5) of the forming element, thereby configuring the opening (1) into the closed configuration; and then d) removing the structured protein product (8) from the cavity (4). 2 . The method of claim 1 , wherein the opening has an aspect ratio of 1:100 to 100:
1.
3. A method according to claim 1 or claim 2, wherein the width of the opening (1) is at least 100% of the widest part of the cavity (4) of the shaped element.
4. Method according to any one of claims 1 to 3, wherein the nozzle element comprises a sealing element (2).
5. A method according to any one of claims 1 to 4, wherein the shaped element is in the form of a cylinder with a horizontal axis of rotation, the cylinder having a plurality of cavities located on the outer surface of the cylinder.
6. The method according to any one of claims 1 to 5, wherein the protein-containing material comprises 1 to 65 wt% protein.
7. The method according to any one of claims 1 to 6, wherein the protein-containing material does not contain animal protein.
8. The method according to any one of claims 1 to 7, wherein the protein-containing material comprises 1 to 20 wt% of a binder.
9. The method according to any one of claims 1 to 8, wherein the protein-containing material comprises 0.5 to 15 wt% fat or oil.
10. The method of any one of claims 1 to 9, wherein the protein fibers forming the structured protein product abut one another at angles of less than about 45°.
11. The method of claim 10, wherein at least 25% of the protein fibers are adjacent to each other.
12. A structured protein product directly obtained by the process according to any one of claims 1 to 11.
13. Use of the product according to claim 12 for the manufacture of a meat substitute product.
14. A meat substitute product comprising the product according to claim 12.
Citation Information
Patent Citations
Process for producing cookable, fibrous meat analogues with directional freezing
US11241024B1
Protein Composition and Its Use in Restructured Meat
US20070269567A1
Colored Structured Protein Products
US20080254199A1
Protein Composition for Meat Products or Meat Analog Products
US20090208633A1
Fibrous food material
US20100074989A1