Prepreg, laminate, printed wiring board, and semiconductor package

By using prepregs with high and low filling area structures in the substrate, using the combination of thermosetting resin and inorganic filling materials, the problem of insufficient dimensional stability of the substrate is solved, and higher dimensional stability and conductor bonding strength are achieved. It is suitable for High frequency electronic equipment.

CN119095707APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380037009.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-28
Filing Date
2023-07-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The problem of the resin composition of the substrate material in the prior art is limited, resulting in insufficient substrate dimensional stability and it is difficult to meet the needs of high-density installation and high-performance electronic equipment.

Method used

Prepregs containing high and low filling area structures containing thermosetting resins and inorganic filling materials are used to prevent heat shrinkage and reduce dielectric constant through high filling areas, thereby improving the dimensional stability of the substrate and conductor bonding strength.

Benefits of technology

It significantly improves the dimensional stability of the substrate and conductor bonding strength, and is suitable for electronic equipment for high-frequency signal processing, enhancing the performance and reliability of electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095707A_ABST
    Figure CN119095707A_ABST
Patent Text Reader

Abstract

Provided is a prepreg capable of exhibiting dimensional stability of a substrate (laminate). Also provided are a laminate, a printed wiring board, and a semiconductor package, each of which is obtained using the prepreg. Specifically, the present invention provides a prepreg or the like having a thermosetting resin composition containing a thermosetting resin (A) and an inorganic filler (B), or a prepreg thereof, and one fiber base material, the prepreg has a high-filling region in which the content of the inorganic filler (B) is 45 vol% or more and a low-filling region in which the content of the inorganic filler (B) is less than 45 vol%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a prepreg, a laminate, a printed wiring board and a semiconductor package. Background Art

[0002] In various electronic devices such as mobile communication devices represented by mobile phones, their base station devices, network infrastructure devices such as servers and routers, and large computers, the speed and capacity of the signals used are being promoted year by year. On the other hand, in recent years, the demand for high performance and miniaturization of electronic devices has gradually increased, and the narrow pitch connection accompanied by the miniaturization of silicon chips has also been promoted. In order to stably install electronic components corresponding to these high-density installations, it has become increasingly important to suppress the dimensional changes of the substrate caused during installation. As a method for improving dimensional stability, etc., there is a known method of using a thermosetting resin composition containing a specific siloxane compound and a maleimide compound as a substrate material (for example, refer to Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-131590 Summary of the invention

[0006] Problems to be solved by the invention

[0007] However, the method described in Patent Document 1 has a problem that the resin component of the substrate material is limited in order to improve dimensional stability, etc. Therefore, there is a demand for the development of other means for improving the dimensional stability of the substrate without limiting the substrate material.

[0008] In view of the above-mentioned situation, an object of the present disclosure is to provide a prepreg capable of exhibiting dimensional stability of a substrate (laminated board), and to provide a laminated board, a printed wiring board, and a semiconductor package obtained by using the prepreg.

[0009] Means for solving problems

[0010] The present inventors have conducted intensive studies and found that the above-mentioned object can be achieved with the resin composition disclosed herein.

[0011] The present disclosure includes the following embodiments [1] to [9].

[0012] [1] A prepreg comprising a thermosetting resin composition containing a thermosetting resin (A) and an inorganic filler (B) or a semi-cured product thereof, and a fiber substrate,

[0013] The prepreg includes a high-filling region in which the content of the inorganic filler (B) is 45% by volume or more, and a low-filling region in which the content of the inorganic filler (B) is less than 45% by volume.

[0014] [2] The prepreg according to [1] above, wherein the content of the inorganic filler (B) in the high filling region is 55% by volume or more.

[0015] [3] The prepreg according to [1] or [2] above, wherein the high filling region and the low filling region are in a layered form.

[0016] [4] The prepreg according to [3] above, which has two or more layers of the highly filled region.

[0017] [5] The prepreg according to any one of [1] to [4], wherein the thermosetting resin (A) comprises at least one selected from epoxy resins, maleimide compounds, phenolic resins, polyimide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins and melamine resins.

[0018] [6] The prepreg according to any one of [1] to [5], wherein the inorganic filler (B) comprises at least one selected from the group consisting of silica, alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, molybdate compounds, talc, aluminum borate and silicon carbide.

[0019] [7] A laminate comprising a cured product of the prepreg according to any one of [1] to [6] above and a metal foil.

[0020] [8] A printed wiring board comprising a cured product of the prepreg according to any one of [1] to [6] above.

[0021] [9] A semiconductor package comprising the printed wiring board described in [8] above and a semiconductor element.

[0022] Effects of the Invention

[0023] The present disclosure can provide a prepreg capable of exhibiting dimensional stability of a substrate (laminated board), and can provide a laminated board, a printed wiring board, and a semiconductor package obtained by using the prepreg. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is a schematic cross-sectional view showing one form of the prepreg according to the present embodiment.

[0025] Figure 2 This is a schematic cross-sectional view showing one form of the prepreg according to the present embodiment.

[0026] Figure 3 This is a schematic cross-sectional view showing one form of the prepreg according to the present embodiment.

[0027] Figure 4 This is a schematic cross-sectional view showing one form of the prepreg according to the present embodiment.

[0028] Figure 5 This is a schematic cross-sectional view showing the state of the prepreg produced in Comparative Example 1. DETAILED DESCRIPTION

[0029] In the numerical range described in this specification, the lower limit or upper limit of the numerical range can be replaced by the value shown in the embodiment. In addition, the lower limit and upper limit of the numerical range can be arbitrarily combined with the lower limit or upper limit of other numerical ranges. In the expression of the numerical range "AA to BB", the numerical values ​​AA and BB at both ends are included in the numerical range as the lower limit and upper limit, respectively.

[0030] In this specification, for example, a description such as "10 or more" means a value of 10 or more, and this shall prevail even if the values ​​are different. In addition, for example, a description such as "10 or less" means a value of 10 or less, and this shall prevail even if the values ​​are different.

[0031] In addition, each component and material exemplified in this specification may be used alone or in combination of two or more unless otherwise specified. In this specification, when there are multiple substances equivalent to each component in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition unless otherwise specified.

[0032] In this specification, the "resin component" refers to all components except inorganic compounds such as inorganic fillers described later, among the solid components constituting the resin composition.

[0033] In this specification, the "solid content" means components other than the organic solvent described later, and components that are liquid at 25°C are also considered to be solid contents.

[0034] The expression "containing XX" described in the present specification includes both meanings of containing in a state where XX is reacted when XX is capable of reacting and simply containing XX.

[0035] A mode in which the matters described in this specification are arbitrarily combined is also included in the present disclosure and the present embodiment.

[0036] [Prepreg]

[0037] The prepreg of the present embodiment is a prepreg comprising a thermosetting resin composition or a semi-cured product thereof containing a thermosetting resin (A) and an inorganic filler (B), and a fiber substrate, wherein the prepreg comprises a high-filling region having a content of the inorganic filler (B) of 45% by volume or more [hereinafter sometimes referred to as a "high-filling region"], and a low-filling region having a content of the inorganic filler (B) of less than 45% by volume [hereinafter sometimes referred to as a "low-filling region"].

[0038] By making the prepreg with a fiber substrate have the above-mentioned high filling area and the above-mentioned low filling area, it is possible to show the high dimensional stability of the substrate (laminated plate). It is speculated that this result can be obtained because, by setting the high filling area, the high filling area will prevent the heat shrinkage that is easy to occur in the low filling area. In addition, by making the prepreg with a fiber substrate have the above-mentioned high filling area and the above-mentioned low filling area, there is a trend to reduce transmission loss. In particular, by making the prepreg not only have the above-mentioned high filling area but also have the above-mentioned low filling area, there is a trend that can suppress the relative dielectric constant (Dk) from increasing.

[0039] From the viewpoint of dimensional stability, the content of the inorganic filler (B) in the high-filling region is preferably 50% by volume or more, more preferably 55% by volume or more.

[0040] Similarly, from the viewpoint of dimensional stability, it is preferred that the content of the inorganic filler (B) in the high-filling region is 45 to 95% by volume, and that in the low-filling region, the content of the inorganic filler (B) is 10% by volume or more and less than 45% by volume. It is preferred that the content of the inorganic filler (B) in the high-filling region is 50 to 80% by volume, and that in the low-filling region, the content of the inorganic filler (B) is 10 to 40% by volume. It is more preferred that the content of the inorganic filler (B) in the high-filling region is 55 to 70% by volume, and that in the low-filling region, the content of the inorganic filler (B) is 15 to 40% by volume. It is further preferred that the content of the inorganic filler (B) in the high-filling region is 55 to 70% by volume, and that in the low-filling region, the content of the inorganic filler (B) is 20 to 35% by volume.

[0041] From the viewpoint of dimensional stability, it is preferred that the above-mentioned high-filled region and the above-mentioned low-filled region are layered. If the above-mentioned high-filled region and the above-mentioned low-filled region are layered, there is a tendency that the high-filled region is easy to prevent the thermal shrinkage effect of the low-filled region. When the above-mentioned high-filled region and the above-mentioned low-filled region are layered, they may also be referred to as a high-filled layer and a low-filled layer, respectively. It should be noted that, from the viewpoint of dimensional stability, the prepreg of this embodiment preferably has more than 2 layers of the above-mentioned high-filled region, more preferably 2 to 6 layers, further preferably 2 to 4 layers, and particularly preferably 2 layers.

[0042] A preferred embodiment of the prepreg of this embodiment is shown in Figure 1 to Figure 4 In each case, the prepreg comprises a thermosetting resin composition containing a thermosetting resin (A) and an inorganic filler (B) or a semi-cured product thereof and a fiber substrate, but the fiber substrate is not shown in the figure.

[0043] Figure 1 This is a prepreg in which low-filling regions (low-filling layers) 2 are sandwiched between high-filling regions (high-filling layers) 1 . Figure 2 This is a prepreg material in which a high-filling region (high-filling layer) 1 is sandwiched between low-filling regions (low-filling layers) 2 . Figure 3 The prepreg is formed in layers in the order of high filling region (high filling layer) 1 - low filling region (low filling layer) 2 - high filling region (high filling layer) 1 - low filling region (low filling layer) 2 - high filling region (high filling layer) 1. Figure 4 The prepreg is formed in layers in the order of low filling region (low filling layer) 2 - high filling region (high filling layer) 1 - low filling region (low filling layer) 2 - high filling region (high filling layer) 1 - low filling region (low filling layer) 2.

[0044] By like Figure 1 to Figure 4 As in the above-mentioned prepreg, the warpage of the prepreg itself tends to be reduced by forming the upper and lower surfaces symmetrically, which is preferable from the viewpoint of improving the ease of handling of the prepreg.

[0045] From the perspective of dimensional stability, whether Figure 1 to Figure 4 Any prepreg is preferred, especially Figure 1 The prepreg shown can also be Figure 3 From the viewpoint of easy manufacturing, it is more preferred Figure 1 The prepreg shown, Figure 2 In addition, if the prepreg Figure 1 and Figure 4 The prepreg having the low filling area 2 near the center of the prepreg as in the example above is preferred because it is easy to fully impregnate the thermosetting resin composition into the fiber base material and there is a tendency to suppress the generation of voids. Figure 2 and Figure 4 Having the low-filling region 2 in the outermost layer as described above tends to improve the bonding strength with the conductor, which is preferred.

[0046] In the prepreg of the present embodiment, the thickness of the high-filled region (high-filled layer) 1 is not particularly limited, but is preferably 5 to 35 μm, more preferably 10 to 30 μm, and further preferably 15 to 25 μm. If the thickness of the high-filled region (high-filled layer) 1 is 5 μm or more, there is a tendency for excellent dimensional stability, and if it is 35 μm or less, there is a tendency for the prepreg of the present embodiment to have sufficient room for containing the low-filled region (low-filled layer) 2.

[0047] In addition, in the prepreg of the present embodiment, the thickness of the low-filled area (low-filled layer) 2 is not particularly limited, but is preferably 5 to 35 μm, more preferably 10 to 30 μm, and further preferably 15 to 25 μm. If the thickness of the low-filled area (low-filled layer) 2 is 5 μm or more, there is a tendency to reduce the relative dielectric constant (Dk), especially when the low-filled area (low-filled layer) 2 is located near the center of the prepreg, it is easy to make the thermosetting resin composition infiltrate the fiber substrate, so there is a tendency to suppress the generation of voids. If it is less than 35 μm, there is a tendency to increase the room for the prepreg of the present embodiment to contain a high-filled area (high-filled layer) 1.

[0048] The thickness of the prepreg of the present embodiment is not particularly limited, but may be 20 to 200 μm, 30 to 150 μm, or 40 to 120 μm.

[0049] (Method for producing prepreg)

[0050] The manufacturing method of the prepreg of the present embodiment is not particularly limited. For example, first, a resin film for a high-filling region and a resin film for a low-filling region are respectively prepared, and they are formed by a thermosetting resin composition containing a thermosetting resin (A) and an inorganic filler (B), and the content of the inorganic filler (B) in the resin film for the high-filling region is 45 volume % or more, and the content of the inorganic filler (B) in the resin film for the low-filling region is less than 45 volume %.

[0051] The resin film can be produced, for example, by applying a thermosetting resin composition containing an organic solvent described later to a support, drying it by heating, and then semi-curing (B-staging) it as needed. Here, in this specification, the so-called B-staging is a state of being made into the B-stage defined in JIS K6900 (1994).

[0052] Examples of the support include plastic films, metal foils, and release papers.

[0053] The drying temperature and drying time in forming the resin film may be appropriately determined according to the amount of the organic solvent used and the boiling point of the organic solvent used. However, the resin film can be suitably formed by drying at 50 to 200° C. for about 1 to 10 minutes.

[0054] The prepreg of the present embodiment can be produced by impregnating the fiber substrate with these resin films while overlapping them in the desired number of sheets and in the desired order. Here, there is no particular limitation on the method of overlapping the resin films in the desired number of sheets and in the desired order. The resin films may be simply overlapped directly up and down, or laminated at 60 to 140° C. using a laminating machine or the like. In addition, there is no particular limitation on the method of impregnating the fiber substrate with the resin film, and a known method such as a method of impregnating the fiber substrate at 80 to 200° C. using a laminating machine may be used.

[0055] As the fiber substrate, a known fiber substrate used in various laminates for electrical insulating materials can be used. As the material of the fiber substrate, inorganic fibers such as E glass, D glass, S glass, and Q glass; organic fibers such as polyimide, polyester, and tetrafluoroethylene; and mixtures thereof can be cited. These fiber substrates have the form of woven fabrics, nonwoven fabrics, rovings, chopped strand mats, or surface mats.

[0056] The above-mentioned fiber base material is preferably a sheet-like fiber base material.

[0057] The thickness of the fiber substrate is not particularly limited, but may be 1 to 100 μm, 3 to 70 μm, 5 to 55 μm, 15 to 55 μm, or 25 to 55 μm.

[0058] Hereinafter, each component contained in the thermosetting resin composition contained in the prepreg of this embodiment or its semi-cured product will be described.

[0059] [Resin composition]

[0060] The thermosetting resin composition or semi-cured product thereof contained in the prepreg of the present embodiment contains a thermosetting resin (A) [hereinafter sometimes referred to as component (A)] and an inorganic filler (B) [hereinafter sometimes referred to as component (B)].

[0061] ((A) Thermosetting resin)

[0062] As (A) component, epoxy resin, maleimide compound, phenolic resin, polyimide resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin, silicone resin, triazine resin, melamine resin etc. can be enumerated.Among them, as (A) component, preferably include at least one selected from epoxy resin, maleimide compound, phenolic resin, polyimide resin, cyanate resin and isocyanate resin, more preferably include at least one selected from epoxy resin and maleimide compound, from the viewpoint of low thermal expansion, further preferably include maleimide compound.Above-mentioned maleimide compound is not particularly limited, but from the viewpoint of reducing relative dielectric constant (Dk) and dielectric loss tangent (Df), preferably include the mode of aromatic bismaleimide containing indane ring. The aromatic bismaleimide containing an indane ring can be obtained by an industrial method.

[0063] (A) As the component, one type may be used alone, or two or more types may be used in combination.

[0064] (Content of component (A))

[0065] The content of the (A) thermosetting resin in the thermosetting resin composition is not particularly limited, but from the viewpoint of heat resistance and moldability, it is preferably 5 to 95 parts by mass, more preferably 10 to 80 parts by mass, further preferably 10 to 70 parts by mass, particularly preferably 15 to 60 parts by mass, and most preferably 15 to 45 parts by mass, relative to 100 parts by mass of the total of the resin components in the resin composition.

[0066] ((B) Inorganic filler)

[0067] As (B) component, there is no particular limitation, but silicon dioxide, aluminum oxide, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (calcined clay, etc.), molybdate compounds such as zinc molybdate, talc, aluminum borate, silicon carbide, etc. can be cited. (B) component can be used alone or in combination of two or more. Among them, from the viewpoint of thermal expansion coefficient, heat resistance and flame retardancy, silicon dioxide, aluminum oxide, mica, talc are preferred, silicon dioxide, aluminum oxide are more preferred, and silicon dioxide is further preferred. As silicon dioxide, crushed silicon dioxide, pyrogenic silica, fused silica (fused spherical silica) and the like can be cited.

[0068] The shape and particle size of the component (B) are not particularly limited, but the particle size is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, further preferably 0.2 to 5 μm, particularly preferably 0.3 to 3 μm, and may also be 0.3 to 1.5 μm, or 0.3 to 1.0 μm. Here, the particle size refers to the average particle size, which is the particle size corresponding to the point of 50% volume when the total volume of the particles is taken as 100% and the cumulative degree distribution curve based on the particle size is obtained. The particle size of the component (B) can be measured using a particle size distribution measuring device using a laser diffraction scattering method, etc.

[0069] (Content of component (B))

[0070] The content of component (B) in the thermosetting resin composition is the same as the content of component (B) in the prepreg. That is, the content of component (B) in the thermosetting resin composition, if it is used for high filling area, can be 45 to 95 volume %, can be 55 to 80 volume %, can be 55 to 70 volume %. In addition, if it is used for low filling area, it can be 10 volume % or more and less than 45 volume %, can be 10 to 40 volume %, can be 15 to 40 volume %, can be 20 to 35 volume %.

[0071] In addition, when using component (B), a coupling agent may be used in combination as required for the purpose of improving the dispersibility of component (B) and the adhesion of component (B) to the organic component in the thermosetting resin composition. The coupling agent is not particularly limited, and for example, a silane coupling agent or a titanate coupling agent may be appropriately selected for use. One coupling agent may be used alone, or two or more coupling agents may be used in combination. In addition, the amount of the coupling agent used is not particularly limited either.

[0072] It should be noted that when a coupling agent is used, the so-called overall blending treatment method in which the coupling agent is added after the (B) component is mixed with the thermosetting resin composition, but it is preferably a method in which the inorganic filler material is surface-treated with a coupling agent in advance in a dry or wet manner. By adopting this method, the advantages of the (B) component can be more effectively demonstrated.

[0073] (Other ingredients)

[0074] The thermosetting resin composition may further include one or more selected from thermoplastic resins, compatibilizers, flame retardants, flame retardant aids, curing accelerators, antioxidants, adhesion improvers, heat stabilizers, antistatic agents, ultraviolet absorbers, pigments, colorants and lubricants as other ingredients. In addition, it may also contain ingredients other than the above.

[0075] (Organic Solvent)

[0076] The thermosetting resin composition of the present embodiment may be a so-called "varnish" containing an organic solvent from the viewpoint of easy handling and easy production of a prepreg or a resin film described later.

[0077] The organic solvent is not particularly limited, but examples thereof include alcohol solvents such as ethanol, propanol, butanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur-containing solvents such as dimethyl sulfoxide; ester solvents such as γ-butyrolactone, etc. From the viewpoint of solubility, ketone solvents are preferred, and methyl ethyl ketone is more preferred. The organic solvent may be used alone or in combination of two or more.

[0078] When the thermosetting resin composition is used as a varnish, the solid content concentration of the varnish is preferably set to 30 to 90% by mass, more preferably 40 to 80% by mass, and further preferably 45 to 60% by mass. If the solid content concentration of the resin composition is within the above range, the operability of the thermosetting resin composition becomes easy, and the coating property when it is made into a resin film becomes good.

[0079] The thermosetting resin composition can be prepared by mixing the components (A) and (B) and the above components which can be used as needed by a known method. At this time, each component can be dissolved or dispersed while stirring in the above organic solvent. The conditions such as the mixing order, temperature, and time are not particularly limited and can be set arbitrarily.

[0080] [Laminated board]

[0081] The laminated plate of the present embodiment is a laminated plate including a cured product of the prepreg of the present embodiment and a metal foil.

[0082] The laminated plate of the present embodiment can be manufactured, for example, by the following operation, that is, metal foil is arranged on one side or both sides of one sheet of prepreg of the present embodiment, or metal foil is arranged on one side or both sides of a laminated product obtained by overlapping two or more sheets (preferably 2 to 30 sheets, more preferably 2 to 20 sheets, and further preferably 4 to 15 sheets) of prepreg of the present embodiment, and then heating and pressing are performed. In the laminated plate obtained by the manufacturing method, the prepreg of the present embodiment is C-staged. The so-called C-stage in this specification is a state of being made into the C-stage defined in JIS K6900 (1994). It should be noted that the laminated plate with metal foil is sometimes also referred to as a metal-clad laminated plate.

[0083] The metal of the metal foil is not particularly limited, but from the viewpoint of conductivity, it can be copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, or an alloy containing one or more of these metal elements, preferably copper and aluminum, more preferably copper.

[0084] The method for performing the heat press molding is not particularly limited, but for example, it can be performed at a temperature of 100 to 300° C., a pressure of 0.2 to 10 MPa, and a time of 0.1 to 5 hours. Alternatively, the heat press molding can be performed by maintaining a vacuum state for 0.5 to 5 hours using a vacuum press or the like.

[0085] [Printed circuit board]

[0086] The printed wiring board of the present embodiment has a cured product of the prepreg of the present embodiment.

[0087] The printed wiring board of this embodiment can be manufactured by using the laminate of this embodiment to perform circuit forming processing based on hole processing, metal plating processing, etching of metal foil, etc. using a known method. In addition, a multilayer printed wiring board can also be manufactured by further performing multilayer bonding processing as needed. In the printed wiring board of this embodiment, the prepreg of this embodiment is C-staged.

[0088] [Semiconductor package]

[0089] The semiconductor package of this embodiment is a semiconductor package having a printed wiring board of this embodiment and a semiconductor element. The semiconductor package of this embodiment can be manufactured by mounting a semiconductor element such as a semiconductor chip or a memory on a given position of the printed wiring board of this embodiment and sealing the semiconductor element with a sealing resin or the like.

[0090] The prepreg, laminate, printed wiring board, and semiconductor package of this embodiment can be suitably used in electronic devices that process high-frequency signals of 10 GHz or higher. In particular, the printed wiring board is useful as a printed wiring board for millimeter wave radar.

[0091] Preferred embodiments have been described above, but they are merely examples for describing the present disclosure and are not intended to limit the scope of the present disclosure to these embodiments. The present disclosure may also include various forms different from the above embodiments without departing from the gist of the present disclosure.

[0092] Example

[0093] Hereinafter, the present embodiment will be described in detail with reference to examples, but the present embodiment is not limited to the following examples.

[0094] In addition, in each example, the number average molecular weight (Mn) was measured by the following method.

[0095] (Method for determining number average molecular weight)

[0096] The number average molecular weight is calculated by gel permeation chromatography (GPC) based on a calibration curve using standard polystyrene. The calibration curve uses standard polystyrene: TSK standard POLYSTYRENE (type: A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by TOSOH Co., Ltd., trade name] and is approximated by a cubic equation. The measurement conditions of GPC are given below.

[0097] (GPC measurement conditions)

[0098] Device: High-speed GPC device HLC-8320GPC

[0099] Detector: UV-8320 ultraviolet absorption detector [manufactured by TOSOH Corporation]

[0100] Column: Guard column: TSK Guardcolumn SuperHZ-L + Column: TSKgelSuperHZM-N + TSKgel SuperHZM-M + TSKgel SuperH-RC (all manufactured by TOSOH Corporation, trade names)

[0101] Column size: 4.6×20mm (guard column), 4.6×150mm (chromatographic column), 6.0×150mm (reference column)

[0102] Eluent: Tetrahydrofuran

[0103] Sample concentration: 10mg / 5mL

[0104] Injection volume: 25 μL

[0105] Flow rate: 1.00mL / min

[0106] Measurement temperature: 40℃

[0107] [Production Example 1] Preparation of Modified Conjugated Diene Polymer 1

[0108] Into a 2 L glass flask container equipped with a thermometer, a reflux condenser and a stirring device capable of heating and cooling, the raw materials and toluene as an organic solvent in the amounts shown in Table 1 were charged. Then, the mixture was reacted under a nitrogen atmosphere at 90 to 100° C. for 5 hours while stirring, thereby obtaining a solution of a modified conjugated diene polymer 1 (solid content concentration: 35% by mass).

[0109] [Table 1]

[0110] Table 1

[0111]

[0112] The amount of each component in the table is based on solid content when a solution or a dispersion is used.

[0113] In addition, the details of each raw material described in Table 1 are as follows.

[0114] ■Polybutadiene: 1,2-polybutadiene homopolymer, number average molecular weight = 1200, vinyl content = 85% or more

[0115] ■Bismaleimide compound: an aromatic bismaleimide compound containing an indane ring (number average molecular weight = 1300)

[0116] ■Organic peroxide: reaction catalyst, α, α'-bis(tert-butylperoxy)diisopropylbenzene

[0117] [Production Examples 2 to 4]

[0118] (Preparation of varnish)

[0119] The components listed in Table 2 were stirred and mixed with toluene at 25° C. or while heated to 50 to 80° C. according to the amounts listed in Table 2, thereby preparing a thermosetting resin composition (varnish) A having an inorganic filler content of 30% by volume, a thermosetting resin composition (varnish) B having an inorganic filler content of 45% by volume, and a thermosetting resin composition (varnish) C having an inorganic filler content of 60% by volume.

[0120] (Production of resin film)

[0121] Each varnish obtained above was applied onto a polyethylene terephthalate (PET) film having a thickness of 50 μm and then dried by heating at 110° C. for 5 minutes to perform B-stage treatment, thereby producing resin films A to C with PET film (thickness: all 20 μm).

[0122] [Table 2]

[0123] Table 2

[0124]

[0125] The amount of each component in the table is based on solid content when a solution or a dispersion is used.

[0126] *1: Amount (parts by mass) relative to 100 parts by mass of the total resin components

[0127] The details of each component described in Table 2 are as follows.

[0128] [(A) Thermosetting resin]

[0129] ■Maleimide compound 1: Aromatic bismaleimide containing an indane ring, number average molecular weight = 1300

[0130] [(B) Inorganic filler]

[0131] Inorganic filler 1: spherical silica, average particle size = 0.5 μm

[0132] [Thermoplastic resin]

[0133] ■Thermoplastic elastomer 1: "Tuftec (registered trademark) H1221" (manufactured by Asahi Kasei Corporation), hydrogenated styrene-based thermoplastic elastomer (SEBS), styrene unit content = 12% by mass, number average molecular weight = 170,000

[0134] [Compatibilizer]

[0135] Modified conjugated diene polymer 1: Modified conjugated diene polymer 1 prepared in Production Example 1

[0136] [Flame retardant]

[0137] ■Flame retardant 1: Aluminum tris(diethylphosphinate)

[0138] [Curing accelerator]

[0139] ■Organic peroxide 1: α, α'-bis(tert-butylperoxy)diisopropylbenzene

[0140] [Example 1]

[0141] (Prepreg production)

[0142] The resin film A with a PET film and the resin film C with a PET film were placed face to face so that the resin films were in contact with each other, thereby obtaining a laminated product having a structure of "PET film-resin film A-resin film C-PET film". Then, the resin film C was laminated on the resin film A by laminating them using a laminator while heating at 100°C. Then, the PET film on the side of the resin film A was peeled off, thereby producing a laminated resin film. The same operation was performed again, thereby producing two identical laminated resin films.

[0143] On both sides of the E glass cloth having a thickness of 40 μm, one sheet of the above-mentioned laminated resin film was arranged in a state where the resin film A and the glass cloth faced each other, and after lamination using a laminator while heating at 150° C., the PET films on both sides were peeled off, thereby producing Figure 1 The prepreg composed of.

[0144] (Production of double-sided copper-clad laminate)

[0145] After arranging electrolytic copper foil with a thickness of 12 μm on the upper and lower sides of a laminate obtained by overlapping 6 prepregs obtained in this way so that the M surface (matt surface) is in contact with the prepreg, heating and pressing are performed under the conditions of a temperature of 230° C. and a pressure of 4 MPa for 120 minutes, thereby producing a double-sided copper-clad laminate 1.

[0146] The dimensional change rate was measured using the obtained double-sided copper-clad laminate 1 according to the following method. The results are shown in Table 3.

[0147] [Example 2]

[0148] (Prepreg production)

[0149] The resin film A with a PET film and the resin film C with a PET film were placed face to face so that the resin films were in contact with each other, thereby obtaining a laminated product having a structure of "PET film-resin film A-resin film C-PET film". Then, the resin film C was laminated on the resin film A by laminating them using a laminator while heating at 100°C. Then, the PET film on the side of the resin film C was peeled off to produce a laminated resin film. The same operation was repeated to produce two identical laminated resin films.

[0150] The laminated resin film was placed on both sides of a 40 μm thick E glass cloth so that the resin film C and the glass cloth faced each other, and after lamination using a laminator while heating at 150° C., the PET films on both sides were peeled off to produce a Figure 2 The prepreg composed of.

[0151] (Production of double-sided copper-clad laminate)

[0152] A double-sided copper-clad laminate 2 was produced by performing the same operation as in Example 1 except that the prepreg was changed to the above-mentioned prepreg.

[0153] The dimensional change rate was measured by the following method using the obtained double-sided copper-clad laminate 2. The results are shown in Table 3.

[0154] [Comparative Example 1]

[0155] (Prepreg production)

[0156] Two sheets of resin film B with PET film are placed face to face so that the resin films are in contact with each other, thereby obtaining a laminated product having a structure of "PET film-resin film B-resin film B-PET film". Then, the two sheets of resin film B are laminated using a laminator while being heated at 100°C, thereby forming a single layer. Then, one PET film is peeled off to produce a laminated resin film. The same operation is performed again to produce two identical laminated resin films.

[0157] The laminated resin film was placed on both sides of a 40 μm thick E glass cloth so that the resin film B and the glass cloth faced each other, and after lamination using a laminator while heating at 150° C., the PET films on both sides were peeled off to produce Figure 5 The prepreg composed of.

[0158] (Production of double-sided copper-clad laminate)

[0159] A double-sided copper-clad laminate 3 was produced by performing the same operation as in Example 1 except that the prepreg was changed to the above-mentioned prepreg.

[0160] The dimensional change rate was measured using the obtained double-sided copper-clad laminate 3 according to the following method. The results are shown in Table 3.

[0161] [Evaluation of double-sided copper-clad laminate]

[0162] (Measurement of dimensional change rate)

[0163] The copper foil on both sides of the double-sided copper-clad laminate obtained in each example was removed by etching to produce a 5 mm square test piece. Using a TMA test device (manufactured by TA Instruments, Q400), the above test piece was subjected to thermomechanical analysis using a compression method. After the test piece was mounted on the above device along the X direction, it was heated from 25°C to 260°C under a load of 0.4N and a heating rate of 45°C / minute. After being kept at 260°C for 1 hour, it was cooled from 260°C to 25°C, and measured using such a temperature curve. The dimensional change rate (%) of the test piece was evaluated based on the dimensional change when kept at 260°C for 1 hour. Specifically, the dimensional change rate of the test piece was calculated using the following formula. The smaller the dimensional change rate, the better the dimensional stability.

[0164] [Mathematical formula 1]

[0165]

[0166] [Table 3]

[0167] Table 3

[0168]

[0169] From the results in Table 3, it can be seen that the dimensional change rate of the copper-clad laminates produced in Examples 1 and 2 when kept at a high temperature of 260° C. for a given time is reduced.

[0170] On the other hand, the copper-clad laminate produced in Comparative Example 1 had a larger dimensional change rate than those of Examples 1 and 2 when kept at a high temperature of 260° C. for a given period of time.

[0171] Description of Reference Numerals

[0172] 100 prepreg, 1 high filling area (high filling layer), 2 low filling areas (low filling layers).

Claims

1. A prepreg comprising: A thermosetting resin composition or a semi-cured product thereof, and A fiber substrate, The thermosetting resin composition or its semi-cured product contains a thermosetting resin (A) and an inorganic filler (B). The prepreg has: A high filling region in which the content of the inorganic filler (B) is 45% by volume or more, and The content of the inorganic filler (B) is in a low filling region of less than 45% by volume.

2. The prepreg according to claim 1, in, In the high filling region, the content of the inorganic filler (B) is 55% by volume or more.

3. The prepreg according to claim 1, in, The high filling area and the low filling area are layered. The prepreg according to claim 3 , comprising two or more layers of the high filling region.

5. The prepreg according to claim 1, in, The (A) thermosetting resin comprises at least one selected from epoxy resins, maleimide compounds, phenolic resins, polyimide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins and melamine resins.

6. The prepreg according to claim 1, in, The inorganic filler (B) comprises at least one selected from the group consisting of silicon dioxide, aluminum oxide, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, molybdate compounds, talc, aluminum borate and silicon carbide. 7 . A laminate comprising a cured product of the prepreg according to claim 1 and a metal foil. 8 . A printed wiring board comprising a cured product of the prepreg according to claim 1 .

9. A semiconductor package comprising the printed wiring board according to claim 8 and a semiconductor element.