Adhesive film

By designing the surface exposure method of rare earth molybdenum-based composite oxides in the paste film, the problem that the application of rare earth molybdenum-based composite oxides in the film in the prior art has been solved, and the film is highly efficient and antibacterial and Antiviral properties and ensure the mechanical properties of the membrane.

CN119095726APending Publication Date: 2024-12-06NITERRA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380014864.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-09
Filing Date
2023-04-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has not studied the functions of the adhesive film using rare earth molybdenum-based composite oxides such as La-Mo composite oxides, especially its application and surface exposure method in the adhesive film.

Method used

A adhesive film is designed, which contains a film layer of rare earth molybdenum-based composite oxide and a substrate, and the surface exposed area of ​​the rare earth molybdenum-based composite oxide is controlled by exposing the rare earth molybdenum-based composite oxide on the opposite side surface of the adhesive layer. The proportion and film layer thickness ensure its antibacterial and antiviral functions in the adhesion film.

Benefits of technology

The effective exposure of rare earth molybdenum-based composite oxides in the adhesive film is achieved, which significantly improves the antibacterial and antiviral properties of the film, meets the functional requirements, and ensures the mechanical properties of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095726A_ABST
    Figure CN119095726A_ABST
Patent Text Reader

Abstract

The adhesive film (1) comprises a film layer (2) containing a rare earth molybdenum composite oxide (4) and a substrate (5), and an adhesive layer (3) disposed on one surface (2a) of the film layer (2), wherein the rare earth molybdenum composite oxide (4) is exposed on a surface (2b) on the opposite side of the one surface (2a).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film. Background Art

[0002] As shown in Patent Document 1, an antibacterial film having antibacterial properties and being pasted on an object for use is known. The antibacterial film comprises a resin substrate, a hard coating layer containing an antibacterial agent formed on one side of the substrate, and an adhesive layer formed on the other side of the substrate. The antibacterial agent is composed of a substance obtained by loading an antibacterial metal such as silver, silver complex, copper, zinc, titanium oxide on a carrier such as calcium phosphate, silica gel, glass, calcium silicate, etc.

[0003] In addition, as shown in Patent Document 2, ceramics composed of composite oxides containing rare earths and molybdenum (Mo) are known as novel inorganic materials having antibacterial and antiviral properties. Examples of such ceramics include La-Mo composite oxides containing lanthanum (La) as a rare earth (e.g., La-Mo-based composite oxides). 2 Mo 2 O 9 ).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-47659

[0007] Patent Document 2: International Publication No. 2020 / 017493

[0008] (Problems to be solved by the invention)

[0009] Conventionally, there has been no research into adhesive films utilizing the functions (antibacterial properties, antiviral properties, etc.) of rare earth molybdenum-based composite oxides such as La-Mo-based composite oxides. Summary of the invention

[0010] An object of the present invention is to provide an adhesive film in which a rare earth molybdenum-based composite oxide is exposed on the other surface opposite to the one surface on which an adhesive layer is disposed so as to exhibit its function.

[0011] (Methods for solving problems)

[0012] The means for solving the above-mentioned problems are as follows.

[0013] <1> An adhesive film comprising: a film layer including a rare earth molybdenum-based composite oxide and a substrate; and an adhesive layer disposed on one surface of the film layer, wherein the rare earth molybdenum-based composite oxide is exposed on a surface opposite to the one surface.

[0014] <2> The adhesive film according to <1>, wherein the film layer has a thickness of 10 μm to 400 μm.

[0015] <3> The adhesive film according to <1> or <2>, wherein the rare earth molybdenum-based composite oxide includes at least one selected from the group consisting of La-Mo-based composite oxides, La-Mo-W-based composite oxides, and Ce-Mo-based composite oxides.

[0016] <4> The adhesive film according to any one of <1> to <4>, wherein the base material is a resin.

[0017] <5> The adhesive film according to any one of <1> to <4>, wherein the film layer has a thickness of more than 10 μm, and the rare earth molybdenum-based composite oxide is present only within a range of 10 μm from the opposite surface.

[0018] <6> The adhesive film according to any one of <1> to <4>, wherein the rare earth molybdenum-based composite oxide is dispersed in the base material.

[0019] <7> The adhesive film according to any one of <1> to <6>, wherein an exposed area ratio of the rare earth molybdenum-based composite oxide on the surface on the opposite side of the film layer is 4% or more.

[0020] (Effects of the Invention)

[0021] According to the present invention, there can be provided a sticking film in which a rare earth molybdenum-based composite oxide is exposed on the other surface opposite to the one surface on which the adhesive layer is arranged so as to exhibit its function. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] [ Figure 1 ] schematically shows a cross-sectional view of the adhesive film involved in embodiment 1.

[0023] [ Figure 2 ] schematically shows a cross-sectional view of the adhesive film involved in embodiment 2.

[0024] [ Figure 3 ](A) SEM image of the surface of the film layer of Example 1 (magnification: 100 times), (B) SEM image of the surface of the film layer of Example 1 (magnification: 500 times).

[0025] [ Figure 4 ](A) SEM image of the surface of the film layer of Example 2 (magnification: 100 times), (B) SEM image of the surface of the film layer of Example 2 (magnification: 500 times).

[0026] [ Figure 5 ](A) SEM image of the surface of the film layer of Example 3 (magnification: 100 times), (B) SEM image of the surface of the film layer of Example 3 (magnification: 500 times).

[0027] [ Figure 6 ](A) SEM image of the surface of the film layer of Example 4 (magnification: 100 times), (B) SEM image of the surface of the film layer of Example 4 (magnification: 500 times).

[0028] [ Figure 7 ] is a graph showing the X-ray diffraction spectrum of the La-Mo based composite oxide obtained from the film layer of Example 1.

[0029] [ Figure 8 ] is a graph showing the X-ray diffraction spectrum of the La-Mo based composite oxide obtained from the film layer of Example 3.

[0030] [ Fig. 9 ] represents the a-TiO obtained from the film layer of Comparative Example 1 2 Figure 1 shows the X-ray diffraction spectrum of . DETAILED DESCRIPTION

[0031] <Implementation method 1>

[0032] Reference Figure 1 The adhesive film 1 according to the first embodiment of the present invention will be described. Figure 1 Schematically shows a cross-sectional view of the adhesive film 1 according to the first embodiment. Figure 1 As shown, the adhesive film 1 of this embodiment mainly includes a film layer 2 and an adhesive layer 3 .

[0033] The film layer 2 is a film-like layer including a La-Mo composite oxide 4 and a substrate 5. An adhesive layer 3 is arranged on one surface 2a of the film layer 2. In addition, a large amount of powdered (particulate) La-Mo composite oxide 4 is exposed on a surface 2b on the opposite side of one surface 2a in the film layer 2 (that is, the other surface 2b, the opposite surface 2b). It should be noted that, in the case of the present embodiment, powdered La-Mo composite oxide 4 is also dispersed inside the film layer 2 (inside the substrate 5). In the film layer 2, for the powdered La-Mo composite oxide 4 dispersed in the substrate 5, in order to expose the La-Mo composite oxide 4 on the surface of the film layer 2 at a predetermined exposure area ratio during the manufacturing process of the film layer 2, a predetermined amount of powdered La-Mo composite oxide 4 is mixed into the raw material of the substrate 5, and as a result, such a film layer 2 can be obtained.

[0034] It should be noted that the La-Mo composite oxide 4 is an example of a rare earth molybdenum composite oxide. The rare earth molybdenum composite oxide is a composite oxide containing a rare earth element and molybdenum (Mo). There is no particular limitation on the rare earth element as long as it does not impair the purpose of the present invention, and examples thereof include lanthanum (La), cerium (Ce), etc.

[0035] Examples of the rare earth molybdenum-based composite oxide include La-Mo-W-based composite oxides, Ce-Mo-based composite oxides, and the like, in addition to the La-Mo-based composite oxide 4.

[0036] As the rare earth molybdenum composite oxide, it is preferably composed of at least one substance selected from the group consisting of La-Mo composite oxides, La-Mo-W composite oxides, and Ce-Mo composite oxides. It should be noted that these composite oxides can be used alone or in combination of two or more as long as they do not impair the purpose of the present invention.

[0037] La-Mo composite oxides are composite oxides containing lanthanum (La) and molybdenum (Mo) (lanthanum-molybdenum composite oxides). 2 Mo 2 O 9 La-Mo composite oxide as the main phase (main crystalline phase). As a La-Mo composite oxide, it can be composed only of La 2 Mo 2 O 9 Composition, may also include La 2 Mo 2 O 9 The lanthanum-molybdenum composite oxide other than the above is used as a sub phase (sub crystalline phase).

[0038] As the La 2 Mo 2 O 9 The lanthanum-molybdenum composite oxide may include a lanthanum-molybdenum composite oxide selected from the group consisting of La 2 Mo 3 O 12 ,La 6 Mo 1 O 12 ,La 7 Mo 7 O 30 ,La 2 Mo 4 O 15 ,La 2 MoO 6 ,La 4 MoO 9 and LaMo 2 O 5Among them, it is particularly preferred to include a 2 Mo 3 O 12 ,La 6 MoO 12 ,La 7 Mo 7 O 30 and LaMo 2 O 5 At least one of the group consisting of.

[0039] La-Mo-W composite oxides are composite oxides containing lanthanum (La), molybdenum (Mo) and tungsten (W) (lanthanum-molybdenum-tungsten composite oxides). Such La-Mo-W composite oxides are not particularly limited as long as they do not impair the purpose of the present invention. For example, the following can be mentioned: La 2 MoWO 9 ,La 2 Mo x W 2-x O 9 (0<x<2), La 2 Mo 1.5 W 0.5 O 9 ,La 2 Mo 0.5 W 1.5 O 9 Etc. These substances can be used alone or in combination of two or more.

[0040] Ce-Mo composite oxides are composite oxides containing cerium (Ce) and molybdenum (Mo) (cerium-molybdenum composite oxides). Such Ce-Mo composite oxides are not particularly limited as long as they do not impair the purpose of the present invention, and examples thereof include: Ce 2 Mo 3 O 13 、Ce(MoO 4 ) 2 、Ce 2 MoO 6 、Ce 2 (MoO 4 ) 3 、Ce 2 Mo 4 O 15 、Ce 5 (MoO 4 ) 8 、Ce 6 (MoO 4 ) 8 (Mo 2 O 7 )、Ce 8Mo 12 O 49 Etc. These substances can be used alone or in combination of two or more.

[0041] Rare earth molybdenum-based composite oxides such as La—Mo-based composite oxides can be identified by analyzing an X-ray diffraction spectrum obtained by powder X-ray diffraction (XRD) (for example, by comparing with known X-ray diffraction spectrum data).

[0042] Rare earth molybdenum composite oxides are used for the film layer in the form of powder (particles). It should be noted that in this specification, "rare earth molybdenum composite oxide powder" or "powdered rare earth molybdenum composite oxide" is sometimes referred to as "rare earth molybdenum composite oxide powder". For example, in this specification, "La-Mo composite oxide powder" or "powdered La-Mo composite oxide" is sometimes referred to as "La-Mo composite oxide powder".

[0043] The center particle size of the rare earth molybdenum composite oxide powder is not particularly limited as long as it does not impair the purpose of the present invention, and is preferably 50 nm or more and 10 μm or less. The center particle size of the rare earth molybdenum composite oxide powder is obtained as the particle size (D50) when the cumulative frequency measured by a laser diffraction particle size distribution analyzer becomes 50%.

[0044] The rare earth molybdenum-based composite oxide powder is produced, for example, through a conditioning step and a first calcination step. Here, the case of producing the La-Mo-based composite oxide powder is exemplified.

[0045] The adjustment step is a step of preparing a mixed powder by mixing a lanthanum compound and a molybdenum compound.

[0046] The lanthanum compound is a compound containing lanthanum (La) required for producing La-Mo composite oxides, and examples thereof include La(OH) 3 ,La 2 O 3 ,La 2 (CO 3 ) 3 As the lanthanum compound, for example, La(OH) 3 ,La 2 O 3 ,La 2 (CO 3 ) 3 It should be noted that, as the lanthanum compound, La(OH) is preferred. 3 .

[0047] The molybdenum compound is a compound containing molybdenum (Mo) required for producing La-Mo composite oxides, and examples thereof include: MoO 3 、MoO 2 、MoO、Mo(OH) 3 、Mo(OH) 5 As the molybdenum compound, for example, a compound selected from the group consisting of MoO 3 、MoO 2 、MoO、Mo(OH) 3 、Mo(OH) 5 It should be noted that as the molybdenum compound, MoO 3 .

[0048] The mixing ratio of the lanthanum compound and the molybdenum compound is not particularly limited unless the object of the present invention is impaired. For example, it is preferably adjusted to a molar ratio of La:Mo=1:1.

[0049] The lanthanum compound and the molybdenum compound are each powdered, and they can be mixed in the state of powders, or a solvent such as a lower alcohol (ethanol) can be added to these powders to perform wet mixing. The mixing of the lanthanum compound and the molybdenum compound can be performed, for example, by wet mixing using alumina balls (alumina ball stone). It should be noted that the mixture (wet mixture) after wet mixing is appropriately dried by hot water bath drying, spray drying, etc.

[0050] Through such a conditioning step, a mixed powder of a lanthanum compound and a molybdenum compound can be obtained.

[0051] The first firing step is a step of firing the mixed powder obtained in the conditioning step in order to react the lanthanum compound and the molybdenum compound in the mixed powder. In the first firing step, the mixed powder is fired for more than 2 hours at a temperature of 500° C. to 700° C., for example. It should be noted that the first firing step does not need to be performed in a special synthetic air atmosphere, but can be performed in a normal atmospheric pressure atmosphere.

[0052] Through the first firing step, the lanthanum compound in the mixed powder reacts with the molybdenum compound to obtain a lanthanum-containing 2 Mo 2 O 9 La-Mo composite oxides such as those described above.

[0053] The obtained La—Mo-based composite oxide is processed into a powder (particle) having a center particle diameter within a predetermined range by a pulverization step as necessary.

[0054] The pulverizing step is a step of obtaining a powdered La-Mo composite oxide having a center particle size within a predetermined range by pulverizing the first fired La-Mo composite oxide using a medium stirring pulverizing device such as a bead mill. Various conditions such as the pulverizing time are appropriately set so that the center particle size of the La-Mo composite oxide is within a predetermined range. La-Mo composite oxide powder is obtained by the above operation.

[0055] It should be noted that the obtained La-Mo composite oxide powder can be granulated as needed. For example, a slurry is prepared by adding a solvent such as ethanol to the La-Mo composite oxide powder and performing wet mixing and crushing using alumina balls, etc., and the dried product of the slurry is passed through a sieve with a predetermined mesh size to obtain a La-Mo composite oxide powder granulated to a predetermined size.

[0056] In addition, as long as the present invention is not impaired, a substance (crushed product) obtained by sintering the La-Mo composite oxide powder and then crushing the obtained sintered body can be used as the "La-Mo composite oxide powder" used in the film layer 2. The sintered body is obtained, for example, by forming the La-Mo composite oxide powder before sintering into a predetermined shape and firing the obtained molded body under predetermined temperature conditions (for example, above 900°C). In this specification, the firing process performed to sinter the La-Mo composite oxide powder is referred to as the "second firing process". The second firing process can be performed in an atmospheric atmosphere.

[0057] The La—Mo-based composite oxide obtained after the second calcination step may be adjusted to a powdery state (particulate state) having a center particle diameter within a predetermined range through a pulverization step as necessary.

[0058] In the case of manufacturing La-Mo-W composite oxide powder, in the conditioning step, a lanthanum compound, a molybdenum compound and a tungsten compound are mixed to prepare a mixed powder. Examples of tungsten compounds include: WO 3 , WO 2 , W 2 O 3 As the tungsten compound, WO is preferred. 3 It should be noted that as the molybdenum compound, the same molybdenum compound as that used in the production of the La—Mo-based composite oxide powder can be used.

[0059] The mixing ratio of the lanthanum compound, the molybdenum compound, and the tungsten compound is not particularly limited unless the object of the present invention is impaired. For example, the mixing ratio may be adjusted to La:Mo:W=2:1.5-0.5:0.5-1.5 in molar ratio.

[0060] When manufacturing Ce-Mo composite oxide powder, in the conditioning step, a cerium compound and a molybdenum compound are mixed to prepare a mixed powder. Examples of the cerium compound include CeO 2 , cerium nitrate, cerium chloride, cerium sulfate, cerium hydroxide, cerium carbonate, cerium acetate, etc. As the cerium compound, CeO 2 It should be noted that as the molybdenum compound, the same molybdenum compound as that used in the production of the La—Mo-based composite oxide powder can be used.

[0061] The mixing ratio of the cerium compound and the molybdenum compound is not particularly limited as long as it does not impair the purpose of the present invention. For example, it can be adjusted so that the molar ratio of Ce:Mo=2:3, it can be adjusted so that the molar ratio of Ce:Mo=1:2, it can be adjusted so that the molar ratio of Ce:Mo=1:1, it can be adjusted so that the molar ratio of Ce:Mo=2:1, it can be adjusted so that the molar ratio of Ce:Mo=3:4, it can also be adjusted so that the molar ratio of Ce:Mo=3:5. It should be noted that as the mixing ratio, it is preferably adjusted so that the molar ratio of Ce:Mo=2:3.

[0062] When producing La—Mo—W composite oxide powder and Ce—Mo composite oxide powder, each step including the first firing step and the pulverizing step is performed in the same manner as when producing the La—Mo composite oxide powder.

[0063] Rare earth molybdenum composite oxides such as La-Mo composite oxides exhibit various functions of antibacterial properties (antibacterial activity) and antiviral properties (antiviral activity) in both the state of powder before sintering and the state of powder after sintering. The evaluation method of the antiviral property of rare earth molybdenum composite oxides will be described later.

[0064] Rare earth molybdenum composite oxides show antibacterial properties against Staphylococcus aureus (Gram-positive bacteria), Escherichia coli (Gram-negative bacteria), etc. In addition, it is speculated that rare earth molybdenum composite oxides show antibacterial properties against Klebsiella pneumoniae, methicillin-resistant Staphylococcus aureus, Staphylococcus epidermidis, Pseudomonas aeruginosa, multidrug-resistant Pseudomonas aeruginosa, etc.

[0065] In addition, rare earth molybdenum composite oxides show antiviral properties against bacteriophage Qβ, bacteriophage φ6, etc. It should be noted that bacteriophage Qβ has no envelope and is known as a substitute virus for norovirus, and bacteriophage φ6 has an envelope and is known as a substitute virus for influenza virus. In addition, it is speculated that rare earth molybdenum composite oxides will show antiviral properties against feline calicivirus (a substitute for human norovirus), human influenza virus, swine fever virus, bovine viral diarrhea virus, border disease virus, giraffe plague virus, coronavirus, avian influenza virus, etc.

[0066] The substrate is a main material constituting the film layer, and the rare earth molybdenum composite oxide is maintained in a manner that the rare earth molybdenum composite oxide is exposed on the surface of the film layer. In the case of this embodiment, during the manufacturing process, the rare earth molybdenum composite oxide is dispersed in the interior of the substrate, so that a part of the rare earth molybdenum composite oxide is exposed on the surface of the film layer (substrate).

[0067] The material used in the substrate can be appropriately selected in consideration of being able to be processed into a film shape, being able to disperse the rare earth molybdenum composite oxide inside in a manner that a portion of the rare earth molybdenum composite oxide is exposed on the surface, etc. Examples of the material used in the substrate include glass and resin.

[0068] As the resin used in the substrate, there is no particular limitation as long as the purpose of the present invention is not impaired, and examples thereof include polyolefin resins such as polysiloxane resins, thermosetting elastomers (polysiloxane rubber, etc.), thermoplastic elastomers, polyethylene (PE), polypropylene (PP), ethylene-propylene copolymers, acrylic resins, polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene resins, acrylonitrile-butadiene-styrene (ABS) resins, modified polyphenylene ethers, polyphenylene sulfides, polyamides, polycarbonates, thermoplastic resins such as polyacetals, phenolic resins, epoxy resins, melamine resins, urea resins, etc. These resins can be used alone or in combination of two or more.

[0069] For example, when the adhesive film is required to be flexible (for example, when the surface shape of the object to which the adhesive film is attached is a curved surface, etc.), the film layer (base material) is required to be flexible. Therefore, as the material of the base material in such a case, resin is preferably used for the reason that it has excellent flexibility when processed into a film shape. It should be noted that when a resin is used as the base material of the film layer, the film layer is not always required to be flexible.

[0070] The rare earth molybdenum composite oxide is adjusted in such a way that it is exposed on the other surface (opposite surface) 2b of the film layer at a predetermined exposure area ratio. The exposure area ratio of the rare earth molybdenum composite oxide is not particularly limited as long as it does not harm the purpose of the present invention, for example, it is preferably 4% or more. It should be noted that the upper limit value of the exposure area ratio of the rare earth molybdenum composite oxide is not particularly limited as long as it does not harm the purpose of the present invention, for example, it can be set to less than 50%, preferably set to less than 40%, and further preferably set to less than 30%. The calculation method of the exposure area ratio of the rare earth molybdenum composite oxide will be described later.

[0071] In this embodiment, the content ratio (%) of the rare earth molybdenum composite oxide in the film layer is appropriately adjusted in such a way that the exposed area ratio of the rare earth molybdenum composite oxide is within a desired range. For example, when the substrate is a resin (e.g., a polysiloxane resin), the content ratio (%) of the rare earth molybdenum composite oxide in the film layer can be set to be greater than 20% and less than 70%.

[0072] The film layer may contain known additives such as antioxidants, colorants (pigments, dyes, etc.), ultraviolet absorbers, antioxidants, softeners, cross-linking agents, curing retarders, curing accelerators, surfactants, fillers, solvents, catalysts, adhesives, natural rubber, synthetic rubber, etc. within the range that does not impair the purpose of the present invention.

[0073] The thickness of the film layer is not particularly limited unless the purpose of the present invention is impaired, and can be set, for example, to 10 μm or more and 400 μm or less.

[0074] The film layer of this embodiment can be manufactured so that a predetermined amount of rare earth molybdenum composite oxide powder is exposed at least on the surface 2b. A specific example of the method for manufacturing such a film layer will be described later.

[0075] The adhesive layer is a layer formed by an adhesive having adhesive force (pressure-sensitive adhesive force). The type of adhesive used in the adhesive layer is not particularly limited, and examples thereof include known adhesives such as acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, polysiloxane adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, fluorine adhesives, and epoxy adhesives. These adhesives can be used alone or in combination of two or more.

[0076] In order to protect one surface (adhesive surface) 3a of the adhesive layer, the adhesive film 1 may have a release liner 6 before use. Such a release liner is not particularly limited and can be appropriately selected from known release liners (for example, release liners made of plastic films).

[0077] The adhesive layer is laminated on the film layer so that the other surface 3b thereof is bonded to the surface 2a of the film layer 2. The thickness of the adhesive layer is not particularly limited unless the purpose of the present invention is impaired, and can be set to, for example, 1 μm or more and 30 μm or less.

[0078] The adhesive film 1 of this embodiment, when adhered to an object using the adhesive surface 3a of the adhesive layer 3, can exert antibacterial and antiviral properties mainly caused by rare earth molybdenum-based composite oxides such as La-Mo-based composite oxides present on the surface 2a of the film layer 2.

[0079] <Implementation method 2>

[0080] Next, refer to Figure 2 A sticking film 1A according to a second embodiment of the present invention will be described. Figure 2 2 is a cross-sectional view schematically showing an adhesive film 1A according to Embodiment 2. Figure 2 As shown, the adhesive film 1A of this embodiment has a film layer 2A and an adhesive layer 3 similarly to the first embodiment described above.

[0081] The film layer 2A is a film-like layer including the La-Mo composite oxide 4 and the substrate 5A, similarly to the first embodiment, and the adhesive layer 3 is disposed on one surface 2Aa of the film layer 2A, similarly to the first embodiment. In addition, in the state before use of the adhesive film 1A, a release liner 6 is attached to the adhesive layer 3, similarly to the first embodiment.

[0082] However, the film layer 2A of the present embodiment is composed of a material in which a large amount of powdered La-Mo composite oxide 4 is fixed on the surface 2Ab of the film-forming substrate 5A. That is, in the film layer 2A, the powdered La-Mo composite oxide 4 is formed on the surface 2Ab of the substrate 5A in a manner of forming one layer or in a manner of not forming one layer but extending in layers as a whole.

[0083] The La-Mo composite oxide 4 is an example of a rare earth molybdenum composite oxide as in Embodiment 1, and the same La-Mo composite oxide as in Embodiment 1 can be used. In addition, as for the substrate 5A, as long as it is a substrate that can fix a rare earth molybdenum composite oxide such as a powdered La-Mo composite oxide 4 on the surface 2Ab, basically the same substrate as in Embodiment 1 can be used.

[0084] In addition, the rare earth molybdenum composite oxide such as La-Mo composite oxide is adjusted in such a way that it is exposed on the other surface 2Ab of the film layer 4A at a predetermined exposure area ratio. The exposure area ratio of the rare earth molybdenum composite oxide is not particularly limited as long as it does not harm the purpose of the present invention, for example, it is preferably 4% or more. It should be noted that the upper limit value of the exposure area ratio of the rare earth molybdenum composite oxide is not particularly limited as long as it does not harm the purpose of the present invention, for example, it can be a state where the surface 2Ab is covered with the rare earth molybdenum composite oxide (that is, the exposure area ratio of the rare earth molybdenum composite oxide is 100% or less). In addition, the upper limit value of the exposure area ratio of the rare earth molybdenum composite oxide can be set to the same value as in the above-mentioned embodiment 1.

[0085] It should be noted that, in the case of the present embodiment, the rare earth molybdenum-based composite oxide such as the powdery La—Mo-based composite oxide 4 is not actively dispersed inside the substrate 5A.

[0086] The film layer 2A may contain various known additives as in the first embodiment within the range not impairing the purpose of the present invention.

[0087] The thickness of the film layer 2A is not particularly limited unless the object of the present invention is impaired, and can be set to, for example, 10 μm or more and 400 μm or less.

[0088] In the present embodiment, for example, the thickness of the film layer 2A can be set to be thicker than 10 μm, and the film layer 2A can be configured so that the La—Mo composite oxide 4 exists only within a range of 10 μm in the thickness direction from the surface 2Ab of the film layer 2A.

[0089] The film layer 2A of this embodiment can be manufactured in such a manner that a predetermined amount of rare earth molybdenum composite oxide powder is fixed on the surface of the substrate 5A and a predetermined amount of rare earth molybdenum composite oxide powder is exposed at least on the surface 2Ab. A specific example of the method for manufacturing such a film layer 2A will be described later.

[0090] The adhesive film 1A of this embodiment, when adhered to an object using the adhesive surface 3a of the adhesive layer 3, can exert antibacterial and antiviral properties mainly caused by rare earth molybdenum-based composite oxides such as La-Mo-based composite oxide 4 present on the surface 2Aa of the film layer 2A.

[0091] As described above, in the adhesive films 1 and 1A according to the first and second embodiments, the rare earth molybdenum composite oxide is exposed on the surfaces 2b and 2Ab at a predetermined ratio, so the functions (antibacterial properties, antiviral properties, etc.) of the rare earth molybdenum composite oxide can be expected. The antibacterial properties and antiviral properties of the rare earth molybdenum composite oxide in the adhesive films 1 and 1A can be estimated by understanding the amount of rare earth molybdenum composite oxide eluted, which will be described later.

[0092] The adhesive films 1 and 1A according to the first and second embodiments can be used by sticking them to an object using the adhesive layer.

[0093] Hereinafter, the present invention will be further described based on examples. It should be noted that the present invention is not limited to these examples.

[0094] [Example 1]

[0095] (Preparation of La-Mo Composite Oxide)

[0096] Preparation of La(OH) 3 As lanthanum compound, prepare MoO 3As a molybdenum compound. Then, the raw material powder of the lanthanum compound and the raw material powder of the molybdenum compound are weighed respectively so that the molar ratio is 1:1 (La:Mo=1:1). The weighed raw material powders are mixed with a predetermined amount of ethanol, and the obtained wet mixture is dried to obtain a mixed powder. It should be noted that the mixed powder is a state in which the lanthanum compound in a solid phase and the molybdenum compound in a solid phase are mixed with each other.

[0097] Next, the mixed powder was fired at 550° C. for 10 hours in an air atmosphere to obtain a fired powder consisting of a reaction product of a lanthanum compound and a molybdenum compound. Then, the following operation was performed to granulate the obtained fired powder.

[0098] The fired powder was placed in a resin pot together with a predetermined amount of ethanol, and the mixture was subjected to wet mixing and pulverization using alumina balls to obtain a slurry.

[0099] Then, the obtained slurry was dried at 80° C. for about 2 hours, and the obtained dried product was passed through a sieve with a mesh size of 250 μm, thereby obtaining La—Mo based composite oxide powder as granulated powder.

[0100] The granulated La-Mo composite oxide powder was subjected to powder compacting using a predetermined pressing machine (compacting pressure: 98 MPa), and then subjected to cold isostatic pressing at a pressure of 150 MPa, thereby obtaining a compact. Then, the compact was fired at a temperature of 900° C. for 10 hours in an atmospheric atmosphere, thereby obtaining a sintered body. The obtained sintered body was coarsely pulverized using a mortar, and then wet pulverized using alumina balls, thereby obtaining a La-Mo composite oxide powder consisting of a pulverized product of the sintered body.

[0101] The particle size of the obtained La-Mo composite oxide powder was obtained as the volume-based central particle size (D50) using the laser diffraction method. Specifically, the central particle size (D50) of the La-Mo composite oxide powder was obtained using a laser diffraction particle size distribution measuring device (model "LA-950", manufactured by Horiba, Ltd.). The result was 0.5 μm.

[0102] (Film production)

[0103] A predetermined amount of La-Mo composite oxide powder is mixed into an uncured thermosetting polysiloxane resin using a mixer, thereby obtaining a paste-like mixed composition. The mixed composition is applied to a release sheet in a thinly spread manner, and then the obtained coating is heated under predetermined temperature conditions, thereby semi-curing the coating. Then, by further heating the semi-cured coating under predetermined temperature conditions, a film layer (the content ratio of La-Mo composite oxide: 66 mass %) using a thermosetting polysiloxane resin as a substrate and dispersing a predetermined amount of La-Mo composite oxide powder in the substrate is obtained.

[0104] [Example 2]

[0105] A film layer was produced in the same manner as in Example 1 except that the content ratio of the La—Mo-based composite oxide in the film layer was changed to 36 mass %.

[0106] [Example 3]

[0107] Prepare the same La-Mo composite oxide powder and uncured thermosetting polysiloxane resin as in Example 1. Then, without adding the La-Mo composite oxide powder, the uncured thermosetting polysiloxane resin is kneaded by a mixer to form a paste. The obtained paste-like uncured thermosetting polysiloxane resin is applied to a peeling sheet in a thinly spread manner, and then the obtained coating is heated under predetermined temperature conditions, thereby semi-curing the coating. Then, La-Mo composite oxide powder is placed in a manner covering the surface of the semi-cured coating. The La-Mo composite oxide powder in such a state is pressed against the surface of the semi-cured coating by a predetermined fixture, thereby pressing and fixing the La-Mo composite oxide powder on the surface. Then, by heating the coating under predetermined temperature conditions, a film layer using a thermosetting polysiloxane resin as a substrate and fixing a predetermined amount of La-Mo composite oxide powder on the surface of the substrate is obtained.

[0108] [Example 4]

[0109] A film layer was produced in the same manner as in Example 1 except that the content ratio of the La—Mo-based composite oxide in the film layer was changed to 23 mass %.

[0110] [Comparative Example 1]

[0111] In addition to using anatase titanium oxide (a-TiO 2 A film layer was produced in the same manner as in Example 3 except that the predetermined amount of La—Mo composite oxide powder was replaced by powder of ).

[0112] [Example 5]

[0113] (Preparation of La-Mo-W Composite Oxide)

[0114] Preparation of La(OH) 3 As lanthanum compound, prepare MoO 3 As the molybdenum compound, prepare WO 3 As a tungsten compound. Then, the raw material powder of the lanthanum compound, the raw material powder of the molybdenum compound, and the raw material powder of the tungsten compound are weighed respectively so that the molar ratio is 2:1:1 (La:Mo:W=2:1:1). The weighed raw material powders are mixed with a predetermined ethanol, and the obtained wet mixture is dried to obtain a mixed powder. It should be noted that the mixed powder is a state in which the lanthanum compound in a solid phase, the molybdenum compound in a solid phase, and the tungsten compound in a solid phase are mixed with each other.

[0115] Next, the mixed powder was fired at 700° C. for 10 hours in an air atmosphere to obtain a fired powder consisting of a reaction product of a lanthanum compound, a molybdenum compound and a tungsten compound. Then, the fired powder was granulated in the same manner as in Example 1.

[0116] The median particle size (D50) of the obtained La—Mo—W based composite oxide powder was 0.81 μm.

[0117] (Film production)

[0118] A film layer was produced in the same manner as in Example 1 except that the La-Mo composite oxide powder was replaced with the La-Mo-W composite oxide powder. Thus, a film layer was obtained in which a predetermined amount of La-Mo-W composite oxide powder was dispersed in a substrate using a thermosetting polysiloxane resin (the content ratio of the La-Mo-W composite oxide: 66 mass %).

[0119] [Example 6]

[0120] A film layer was produced in the same manner as in Example 5 except that the content of the La—Mo—W composite oxide in the film layer was changed to 23 mass %.

[0121] [Example 7]

[0122] Prepare the same La-Mo-W composite oxide powder and uncured thermosetting polysiloxane resin as in Example 5. Then, without adding the La-Mo-W composite oxide powder, the uncured thermosetting polysiloxane resin is kneaded by a mixer to form a paste. The obtained paste-like uncured thermosetting polysiloxane resin is applied to a peeling sheet in a thinly spread manner, and then the obtained coating is heated under predetermined temperature conditions, thereby semi-curing the coating. Then, La-Mo-W composite oxide powder is placed in a manner covering the surface of the semi-cured coating. The La-Mo-W composite oxide powder in such a state is pressed against the surface of the semi-cured coating by a predetermined fixture, thereby pressing and fixing the La-Mo-W composite oxide powder on the surface. Then, by heating the coating under predetermined temperature conditions, a film layer using a thermosetting polysiloxane resin as a substrate and fixing a predetermined amount of La-Mo-W composite oxide powder on the surface of the substrate is obtained.

[0123] [Example 8]

[0124] (Preparation of Ce-Mo Composite Oxide)

[0125] Preparation of CeO 2 As the cerium compound, prepare MnO 3 As a molybdenum compound. Then, the raw material powder of the cerium compound and the raw material powder of the molybdenum compound are weighed respectively so that the molar ratio is 2:3 (Ce:Mo=2:3). The weighed raw material powders are mixed with a predetermined ethanol, and the obtained wet mixture is dried to obtain a mixed powder. It should be noted that the mixed powder is a state in which the cerium compound in a solid phase and the molybdenum compound in a solid phase are mixed with each other.

[0126] Next, the mixed powder was fired at 550° C. for 12 hours in an air atmosphere to obtain a fired powder consisting of a reaction product of a cerium compound and a molybdenum compound. Then, the fired powder was granulated in the same manner as in Example 1.

[0127] The median particle size (D50) of the obtained Ce-Mo based composite oxide powder was 0.94 μm.

[0128] (Film production)

[0129] A film layer was prepared in the same manner as in Example 1 except that the La-Mo composite oxide powder was replaced with the Ce-Mo composite oxide powder. Thus, a film layer was obtained in which a thermosetting polysiloxane resin was used as a base material and a predetermined amount of Ce-Mo composite oxide powder was dispersed in the base material (the content ratio of the Ce-Mo composite oxide: 66 mass %).

[0130] [Example 9]

[0131] A film layer was produced in the same manner as in Example 8 except that the content of the Ce-Mo-based composite oxide in the film layer was changed to 23 mass %.

[0132] [Measurement and evaluation]

[0133] (Thickness of film layer)

[0134] The film thickness of the film layer in Example 1 and the like was the average value of the film thickness measured at 10 points using a contact film thickness meter (product name "Litematic (registered trademark) VL-50A", manufactured by Mitutoyo Co., Ltd.).

[0135] (Exposed area ratio of rare earth molybdenum composite oxide)

[0136] The exposed area ratio of rare earth molybdenum composite oxides such as La-Mo composite oxides in the surface of the film layer of Example 1 etc. is calculated according to the following steps. First, a scanning electron microscope (SEM: Scanning Electron Microscope) is used to photograph the surface of the film layer under the conditions of accelerating voltage: 5kV and magnification: 100 times to obtain a SEM image (reflected electron image) of the surface of the film layer. For the obtained SEM image, a predetermined image analysis software (ImageJ, manufactured by the National Institutes of Health, USA) is used to adjust the brightness threshold so that the area between particles (powder) and particles can be distinguished, and a binarization process is performed at the same time. The threshold is determined using the Yen method. The exposed area ratio (%) of the rare earth molybdenum composite oxides in the surface of the film layer is calculated using the obtained binarized image. The results are shown in Table 1.

[0137] (SEM image)

[0138] The surface of the film layer of Example 1 was photographed using a scanning electron microscope, and the obtained SEM image is shown in Figure 3 to Figure 6 It should be noted that Figure 3 to Figure 6 Each of the photographs (A) shown is a SEM image at a magnification of 100 times, and each of the photographs (B) shown is a SEM image at a magnification of 500 times.

[0139] (Determine the rare earth molybdenum composite oxide under the following conditions)

[0140] Rare earth molybdenum-based composite oxides such as La-Mo-based composite oxides were respectively taken out from the film layers of Example 1, etc., and the structures of the obtained rare earth molybdenum-based composite oxides were determined by X-ray diffraction spectrum. Figure 7 is a diagram showing an X-ray diffraction spectrum of the La-Mo composite oxide obtained from the film layer of Example 1, Figure 8 : is a graph showing the X-ray diffraction spectrum of the La-Mo composite oxide obtained from the film layer of Example 3. The measurement was performed by a powder X-ray diffraction method.

[0141] <Measurement conditions>

[0142] Measurement device: Powder X-ray diffraction device (device name "Smart lab", manufactured by Rigaku Co., Ltd.)

[0143] Detector: D / teX Ultra250.

[0144] Optical system: Centralized optical system Bragg-Brentano type

[0145] X-ray output: 40kV-30mA

[0146] Step width: 0.0200°

[0147] Scan axis: 2θ / θ

[0148] Scanning range: 10.00°~80.00°

[0149] Rotation: Yes

[0150] In addition, the a-TiO obtained from the film layer of Comparative Example 1 2 The X-ray diffraction spectrum is shown in Fig. 9 middle.

[0151] (Dissolution amount)

[0152] As an alternative test for the simple antibacterial and antiviral properties of the film layer of Example 1, the dissolution amount of the metal ions shown below was measured. A square slice with a side of 50 mm was cut from the obtained film layer, and the slice was immersed in 100 ml of ultrapure water placed in a predetermined container. Next, while the slice was immersed in ultrapure water, the ultrapure water in the container was stirred for 1 minute using a glass rod, and then the container in this state was allowed to stand for 24 hours. Then, the supernatant was collected from the container after standing for 24 hours and used as a sample for measurement. The dissolution amount of lanthanum (La), cerium (Ce), Mo (molybdenum), etc. contained in the sample for measurement obtained by this operation was measured by ICP emission spectrometry (Inductively coupled plasma optical emission spectrometry). The results are shown in Table 1. It should be noted that for Examples 5 to 7, the total value (total dissolution amount) of the dissolution amount of molybdenum (Mo) and the dissolution amount of tungsten (W) is shown.

[0153] (Anti-Virus Performance Evaluation)

[0154] For the film layer of Example 3, which is representative of each embodiment, an antiviral performance evaluation test was conducted in accordance with JIS R 1756:2013 "Antiviral test method for fine ceramic visible light responsive photocatalyst materials using bacteriophage Qβ". Specifically, bacteriophage Qβ was used as the test virus, and the antiviral activity value (dark place) VD after 6 hours was calculated. The antiviral activity value (dark place) VD was calculated for the action time (6 hours) by VD=Log(UD)-Log(TD). Log(UD) is the logarithmic value (average value) of the number of bacteriophages for the action time (6 hours) of the unprocessed test product, and Log(TD) is the logarithmic value (average value) of the number of bacteriophages for the action time (6 hours) of the processed test product. The number of samples of each test product is 3.

[0155] It should be noted that the concentration of the inoculated phage solution was set to 2.6×10 7 cfu / ml, and the infection value (pfu / sample) was counted when the inoculum volume of the phage solution was set to 0.1 ml per sample.

[0156] In addition, the lower limit of detection (definition) in the evaluation of antiviral performance is as follows. 0 , if the infection value after t hours is N, then N / N 0 The common logarithm of 0). Time t is the action time. Although the antiviral activity value VD is 3.0 or more (i.e., VD ≥ 3.0), in Log(N t / N 0 )-Log(N t+1 / N 0 )≤0.5, Log(N t / N 0 ) and Log(N t+1 / N 0 ) was taken as the lower limit of detection.

[0157] The results of the antiviral performance evaluation of Example 3 (antiviral activity value VD) are shown in Table 1. In addition, the film layer of Comparative Example 1 was also evaluated for antiviral performance in the same manner.

[0158] [Table 1]

[0159]

[0160] In Examples 1 to 9, Examples 1, 2, 4 to 6, 8, and 9 correspond to the above-mentioned Embodiment 1, and Examples 3 and 7 correspond to Embodiment 2. In Table 1, the manufacturing method of the film layer corresponding to Embodiment 1 is indicated as "mixing", and the manufacturing method of the film layer corresponding to Embodiment 2 is indicated as "surface fixing".

[0161] The film layer of Example 1 is a film layer obtained by dispersing La-Mo composite oxide powder in a thermosetting polysiloxane resin as a base material at a ratio of 66 mass %. The thickness of the film layer is 350 μm, and the exposed area ratio of La-Mo composite oxide on the surface of the film layer is 20%. It should be noted that Figure 3 As shown in the SEM image of Example 1, a large amount of La-Mo composite oxide powder was confirmed to be dispersed on the surface of the film layer of Example 1. Then, when the La-Mo composite oxide powder present on the surface of the film layer was analyzed by XRD, it was found that Figure 7 The X-ray diffraction spectrum shown in the figure shows that the La-Mo composite oxide contains La 2 MoO 6 In addition, the elution amount of lanthanum and molybdenum in the film layer of Example 1 was 0.89 ppm and 1.1 ppm, respectively. Therefore, it is fully expected that the film layer of Example 1 has antibacterial and antiviral properties due to the La-Mo composite oxide present on the surface.

[0162] The film layer of Example 2 is a film layer obtained by dispersing La-Mo composite oxide powder at a ratio of 36 mass % in a thermosetting polysiloxane resin as a base material. The thickness of the film layer is 350 μm, and the exposed area ratio of La-Mo composite oxide on the surface of the film layer is 10%. Figure 4 As shown in the SEM image, it is confirmed that a large amount of La-Mo composite oxide powder is still scattered on the surface of the film layer of Example 2, although it is less than that of Example 1. It should be noted that the X-ray diffraction spectrum obtained from the La-Mo composite oxide present on the surface of the film layer of Example 2 is roughly the same as that of Example 1, and its detailed description is omitted. In addition, for the dissolution amount of the film layer of Example 2, lanthanum is 0.29ppm and molybdenum is 0.59ppm. Therefore, it is fully expected that the film layer of Example 2 has antibacterial and antiviral properties generated by the La-Mo composite oxide present on the surface, etc.

[0163] The film layer of Example 3 is a film layer obtained by fixing La-Mo composite oxide powder on the surface of a film-like thermosetting polysiloxane resin as a substrate. The thickness of the film layer is 350 μm, and the exposed area ratio of the La-Mo composite oxide on the surface of the film layer is 100%. That is, in Example 3, the La-Mo composite oxide powder is formed in a thin layer on one surface of the film-like substrate in the form of covering the surface (refer to Figure 5 SEM image of the film layer). It should be noted that the thickness of the film layer of Example 3 is 350 μm (i.e., thicker than 10 μm), and the La-Mo composite oxide powder is present only within a range of 10 μm from the surface of the side where the La-Mo composite oxide powder is formed. Then, when the La-Mo composite oxide powder present on the surface of the film layer is analyzed by XRD, it is found that Figure 8 The X-ray diffraction spectrum shown in the figure confirms that the La-Mo composite oxide contains La 2 MoO 6 . In addition, the elution amount of the film layer of Example 3 was 5.8 ppm for lanthanum and 4.3 ppm for molybdenum. Therefore, it is fully expected that the film layer of Example 3 has antibacterial and antiviral properties generated by the La-Mo composite oxide present on the surface, etc. In addition, as shown in Table 1, the antiviral activity value of the film layer of Example 3 is 5.5, which is confirmed to be superior to that of Comparative Example 1.

[0164] The film layer of Example 4 is a film layer obtained by dispersing La-Mo composite oxide powder at a ratio of 23 mass % in a thermosetting polysiloxane resin as a base material. The thickness of the film layer is 350 μm, and the exposed area ratio of La-Mo composite oxide on the surface of the film layer is 4.1%. Figure 6As shown in the SEM image, it is confirmed that a large amount of La-Mo composite oxide powder is still scattered on the surface of the film layer of Example 4, although it is less than that of Examples 1 and 2. It should be noted that the X-ray diffraction spectrum obtained from the La-Mo composite oxide present on the surface of the film layer of Example 4 is roughly the same as that of Example 1, and its detailed description is omitted. In addition, for the dissolution amount of the film layer of Example 4, lanthanum is 0.03ppm and molybdenum is 0.26ppm. Therefore, it is fully expected that the film layer of Example 4 has antibacterial and antiviral properties generated by the La-Mo composite oxide present on the surface, etc.

[0165] The film layer of Comparative Example 1 is anatase-type titanium oxide (a-TiO 2 ) was fixed on the surface of a film-like thermosetting polysiloxane resin as a substrate. The thickness of the film layer was 350 μm, and the exposed area ratio of the anatase type titanium oxide on the surface of the film layer was 100%. That is, in Comparative Example 1, the anatase type titanium oxide powder was formed in a thin layer on one surface of the film-like substrate in the form of covering the surface. Then, when the oxide powder present on the surface of the film layer was analyzed by XRD, it was found that Fig. 9 The X-ray diffraction spectrum shown confirms that the oxide contains a-TiO 2 Therefore, although the film layer of Comparative Example 1 is expected to have antibacterial and antiviral properties due to the La-Mo composite oxide present on the surface, the antiviral activity value is 0.6 as shown in Table 1. This is because the evaluation of antiviral activity was performed in the dark, so the a-TiO 2 Cannot function.

[0166] The film layer of Example 5 is a film layer obtained by dispersing La-Mo-W composite oxide powder at a ratio of 66 mass % in a thermosetting polysiloxane resin as a base material. The thickness of the film layer is 350 μm, and the exposed area ratio of La-Mo-W composite oxide on the surface of the film layer is 24%. Then, when the La-Mo-W composite oxide powder existing on the surface of the film layer is analyzed by XRD, it can be seen from the X-ray diffraction spectrum that the La-Mo-W composite oxide contains La 2 MoWO 9 In addition, the elution amount of lanthanum in the film layer of Example 5 was 0.44 ppm, and the total elution amount of molybdenum and tungsten was 0.56 ppm. It is fully expected that the film layer of Example 5 has antibacterial and antiviral properties caused by the La-Mo-W composite oxide powder present on the surface.

[0167] The film layer of Example 6 is a film layer obtained by dispersing La-Mo-W composite oxide powder in a thermosetting polysiloxane resin as a substrate at a ratio of 23 mass %. The thickness of the film layer is 350 μm, and the exposed area ratio of the La-Mo-W composite oxide on the surface of the film layer is 7.3%. It was confirmed that a large amount of La-Mo-W composite oxide powder was still scattered on the surface of the film layer of Example 6, although it was less than that of Example 5. It should be noted that the X-ray diffraction spectrum obtained from the La-Mo-W composite oxide present on the surface of the film layer of Example 6 is roughly the same as that of Example 5, and its detailed description is omitted. In addition, for the dissolution amount of the film layer of Example 6, lanthanum is 0.04 ppm and molybdenum is 0.15 ppm. Therefore, it is fully expected that the film layer of Example 6 has antibacterial and antiviral properties produced by the La-Mo-W composite oxide present on the surface, etc.

[0168] The film layer of Example 7 is a film layer obtained by fixing La-Mo-W composite oxide powder on the surface of a film-like thermosetting polysiloxane resin as a substrate. The thickness of the film layer is 350 μm, and the exposed area ratio of the La-Mo-W composite oxide on the surface of the film layer is 100%. That is, in Example 7, the La-Mo-W composite oxide powder is formed on one surface of the film-like substrate in the form of a thin layer covering the surface. It should be noted that the thickness of the film layer of Example 7 is 350 μm (that is, thicker than 10 μm), resulting in a state in which the La-Mo-W composite oxide powder only exists within a range of 10 μm from the surface on one side where the La-Mo-W composite oxide powder is formed. Then, when the La-Mo-W composite oxide powder existing on the surface of the film layer is analyzed by XRD, it is confirmed from the X-ray diffraction spectrum that the La-Mo-W composite oxide contains La 2 MoWO 9 In addition, the elution amount of the film layer of Example 7 was 2.5 ppm of lanthanum, and the total amount of molybdenum and tungsten was 4.1 ppm. Therefore, it is fully expected that the film layer of Example 7 has antibacterial and antiviral properties due to the La-Mo-W composite oxide present on the surface, etc.

[0169] The film layer of Example 8 is a film layer obtained by dispersing Ce-Mo composite oxide powder at a ratio of 66 mass % in a thermosetting polysiloxane resin as a base material. The thickness of the film layer is 350 μm, and the exposed area ratio of Ce-Mo composite oxide on the surface of the film layer is 14%. Then, when the Ce-Mo composite oxide powder existing on the surface of the film layer is analyzed by XRD, it can be seen from the X-ray diffraction spectrum that the Ce-Mo composite oxide contains Ce. 2 Mo 3 O13 In addition, the elution amount of the film layer of Example 8 was 0.09 ppm for cerium and 1 ppm for molybdenum. Such a film layer of Example 8 is expected to have antibacterial and antiviral properties due to the Ce-Mo composite oxide powder present on the surface.

[0170] The film layer of Example 9 is a film layer obtained by dispersing Ce-Mo composite oxide powder at a ratio of 23 mass % in a thermosetting polysiloxane resin as a substrate. The thickness of the film layer is 350 μm, and the exposed area ratio of Ce-Mo composite oxide on the surface of the film layer is 9%. Then, it was confirmed that a large amount of Ce-Mo composite oxide powder was still scattered on the surface of the film layer of Example 9, although it was less than that of Example 8. It should be noted that the X-ray diffraction spectrum obtained from the Ce-Mo composite oxide present on the surface of the film layer of Example 9 is roughly the same as that of Example 8, and its detailed description is omitted. In addition, for the dissolution amount of the film layer of Example 9, the cerium is 0.04 ppm and the molybdenum is 0.57 ppm. It is fully expected that such a film layer of Example 9 has antibacterial and antiviral properties generated by the Ce-Mo composite oxide powder present on the surface, etc.

[0171] (Production of adhesive film)

[0172] Adhesive films were obtained by laminating an adhesive layer (silicone resin or acrylic resin, thickness: 10 μm) formed on a release liner on the film layers of Examples 1 to 9.

[0173] Explanation of symbols

[0174] 1, 1A...adhesive film, 2, 2A...film layer, 2a, 2Aa...one surface, 2b, 2Ab...the other surface (opposite surface), 3...adhesive layer, 4...La-Mo composite oxide (rare earth molybdenum composite oxide), 5...substrate, 6...peeling liner.

Claims

1. An adhesive film, comprising: A film layer comprising a rare earth molybdenum composite oxide and a substrate, and An adhesive layer is disposed on one surface of the film layer, wherein The rare earth molybdenum-based composite oxide is exposed on a surface opposite to the one surface.

2. The adhesive film according to claim 1, wherein The thickness of the film layer is greater than or equal to 10 μm and less than or equal to 400 μm.

3. The adhesive film according to claim 1 or claim 2, wherein: The rare earth molybdenum-based composite oxide includes at least one selected from the group consisting of La-Mo-based composite oxides, La-Mo-W-based composite oxides, and Ce-Mo-based composite oxides.

4. The adhesive film according to any one of claims 1 to 3, wherein The substrate is resin.

5. The adhesive film according to any one of claims 1 to 4, wherein The thickness of the film layer is thicker than 10 μm, The rare earth molybdenum-based composite oxide exists only within a range of 10 μm from the opposite surface.

6. The adhesive film according to any one of claims 1 to 4, wherein The rare earth molybdenum-based composite oxide is dispersed in the substrate.

7. The adhesive film according to any one of claims 1 to 6, wherein The exposed area ratio of the rare earth molybdenum-based composite oxide on the surface on the opposite side of the film layer is 4% or more.

Citation Information

Patent Citations

  • Complex oxide ceramic, method for producing same, and article

    CN112533885A

  • Complex oxide ceramic, method for producing same, and article

    US20210261432A1

  • Antiviral film, packaging bag, and seal

    WO2022050390A1