Continuous casting slab and method for producing same
By controlling the original austenite particle size and microstructure structure, combined with the three-stage cooling process, the problem of seasonal cracks in high-strength steel slabs is solved, and the high toughness and yield of slabs are improved.
Patent Information
- Application Number
- CN202380035302.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-09
- Filing Date
- 2023-03-29
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively suppress seasonal cracking during cooling in highly alloyed high-strength steel slabs, resulting in breaking or surface defects during cooling or hot rolling, affecting the yield rate.
By controlling the average original austenite particle size of the continuous cast slab within the range of 0.5 mm to 2.0 mm, and ensuring that the total area ratio of bainite and ferrite reaches more than 90% and the ferrite area ratio is achieved in the microstructure. It is 0% or more, and a three-stage cooling process is adopted: the first stage is 1200℃~1450℃, the second stage is 700℃~850℃, the second stage is 25℃/hr~50℃/hr, and the third stage is 500 The average cooling rate of ℃ to 700°C is 15°C/hr or above.
It effectively inhibits the occurrence of seasonal cracks of the slab, improves the toughness and yield of the slab, and avoids fractures and surface defects during cooling and hot rolling.
Smart Images

Figure CN119095995A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a continuous casting slab that prevents cracks during cooling and a method for manufacturing the same. More specifically, the present invention relates to a continuous casting slab for high-strength steel (high-tensile steel) that effectively prevents season cracks and a method for manufacturing the same. Background Art
[0002] In recent years, in the automotive field, in order to achieve both further thinning of the vehicle body and ensuring collision safety, the strength of high-strength steel has been further increased and high alloying has been carried out for this purpose. However, high alloying leads to a significant decrease in the toughness of the slab.
[0003] As the toughness of the slab decreases due to high alloying, cracks during cooling of the slab, so-called "seasonal cracks", become more frequent. If seasonal cracks occur, there is a possibility that the slab breaks during the slab transportation and the slab cannot be supplied to hot rolling. In addition, even if the slab does not break, there is a possibility that cracks open during the hot rolling of the slab and cause the hot-rolled steel sheet to break. Or, even if the cracks in the slab are fine, they appear as surface defects such as scars and strip scratches on the steel sheet after hot rolling, cold rolling, annealing or plating. Usually, cracks on the surface of the slab are removed by a grinder. However, due to the high alloying, the toughness of the slab is reduced, so the cracks in the slab expand due to the stress of the grinder, and sometimes the cracks in the slab cannot be completely removed. On the other hand, when the cracks in the slab are fine, they are sometimes ignored, and appear as surface defects on the steel sheet after hot rolling, cold rolling, annealing or plating. In view of these circumstances, it is necessary to suppress seasonal cracks in the slab.
[0004] Figure 1 This is an enlarged photograph of the cross section of a cracked portion of a high-strength steel slab that broke due to seasonal cracking, taken using a scanning electron microscope (SEM). Figure 1 It can also be seen that the cross section of the cracked part of the slab presents the appearance of a grain boundary cross section along the original austenite grain boundary. Figure 2 The cross section of the slab crack is shown in the microstructure photograph. The depth of the slab crack is mainly about 20 mm from the surface of the slab. The slab crack extends near the original austenite grain boundary, and grain boundary ferrite exists at the front end of the slab crack. In addition, pearlite or pearlite and bainite are observed in the original austenite grains.
[0005] Grain boundary fracture occurs when the original austenite grains are coarse and the grain boundaries are embrittled. Precipitates and ferrite are more likely to form at the grain boundaries than in the grains. Precipitates at the grain boundaries become an important factor in reducing the grain boundary strength and the toughness of the slab. If the original austenite grains are coarse, the proportion of the grain boundaries decreases and the density of the precipitates increases, so the grain boundaries become further embrittled. In addition, when grain boundary ferrite is generated, due to the strength difference between the pearlite and bainite in the grains, stress concentration occurs in the grain boundary ferrite part with low strength, and even under lower stress, it will develop into cracks in the slab. Here, if the original austenite grains are coarse, the grain boundary ferrite extending thinly along a straight line will precipitate, so it is impossible to prevent the extension of the slab cracks, and the damage caused by the cracks in the slab will expand. On the other hand, if the slab is cooled, stress caused by the difference in thermal contraction and phase change expansion between the surface and the inside of the slab is generated. If this stress is large, cracks in the slab will occur when the slab is cooled to room temperature. In recent high-alloy high-strength steels, since the toughness of the slab is low, it is difficult to remove such deep cracks in the slab by trimming with a grinder or the like, which has caused a problem of significantly reducing the yield of the slab.
[0006] From this point of view, a method for suppressing the occurrence of season cracks in high-tensile steel slabs has been proposed. For example, Patent Document 1 proposes a method for suppressing the bainite / martensite phase transformation by slowly cooling the temperature region of austenite to ferrite phase transformation, i.e., 700 to 500°C, thereby reducing the stress generated by the phase transformation expansion. That is, Patent Document 1 discloses a method for suppressing the occurrence of season cracks even in steel types that are prone to seasonal cracks in high-tensile steel. Specifically, the method for cooling the high-tensile steel slab disclosed in Patent Document 1 is based on the understanding that the internal stress of high-tensile steel depends on its cooling rate, and is a method for suppressing the occurrence of season cracks by controlling the cooling rate of the slab according to the length of the internal cracks generated in the high-tensile steel.
[0007] In addition, Patent Document 2 proposes a method of reducing the temperature difference and stress during phase transformation by starting slow cooling immediately after casting the slab, cooling the slab at a temperature above 700°C for more than 10 hours, and then further slowly cooling the temperature from 700°C to 500°C. That is, Patent Document 2 discloses a method for cooling a slab for high-strength steel plates, which does not produce slab cracks when the slab is cooled even if the slab contains Si, and does not produce quality defects such as scars during hot rolling. Specifically, in the method for cooling a slab for high-strength steel plates disclosed in Patent Document 2, the average cooling rate of a continuously cast slab of a high-strength hot-rolled steel plate with limited chemical component contents such as C, Si, and Mn at 500 to 700°C is set to less than 20°C / hr.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2020-139209
[0011] Patent Document 2: Japanese Patent Application Publication No. 2019-167560 Summary of the invention
[0012] However, the prior art has the following problems. The method of cooling a high-tensile steel slab after casting described in Patent Document 1 only focuses on the temperature range from 700°C to 500°C when the slab is cooled after casting, and controls the internal stress generated in the slab to be reduced. However, in recent years, the toughness of highly alloyed high-strength steel slabs is low, so the state of the original austenite grain boundaries where seasonal cracks propagate also becomes very important. In the method described in Patent Document 1, since the original austenite grain size and grain boundary ferrite are not controlled, even if the method for cooling a high-tensile steel slab described in Patent Document 1 is used to manufacture a slab with an increased carbon content, the occurrence of seasonal cracks in the slab cannot be fully suppressed.
[0013] Furthermore, the cooling method for a high-strength steel plate described in Patent Document 2 is based on the understanding that the cause of the slab fracture is the thermal stress caused by the addition of Si to the steel and the temperature unevenness in the slab, and focuses on reducing the thermal stress to suppress the fracture of the slab. However, in the cooling method for a high-strength steel plate described in Patent Document 2, the microstructure of the slab is not limited in any form. Therefore, even if the slab is manufactured using the cooling method for a high-strength steel plate described in Patent Document 2, the occurrence of seasonal cracks in the slab cannot be fully suppressed.
[0014] In addition, the inventors of the present invention conducted intensive research and found that the toughness of slabs containing a large amount of C, Si, and Mn according to the prior art is quite low, and it is impossible to completely suppress seasonal cracking if only slow cooling is performed with the intention of reducing thermal stress.
[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a continuously cast slab and a method for producing the same in which seasonal cracks of the slab do not occur during cooling of the slab even if the slab has low toughness.
[0016] In order to achieve the above-mentioned purpose, the inventors have repeatedly conducted in-depth research. As a result, the fracture morphology of the slab cracks was analyzed, and it was found that there was at least one of the grain boundary sections along the original austenite grain boundaries and the intragranular sections (cleavage fracture surfaces) crossing the original austenite grain boundaries on the cross section. In addition, the inventors have repeatedly conducted detailed research and found that the seasonal cracking of the slab cannot be suppressed only by controlling the cooling rate and reducing the stress reduction caused by temperature unevenness, and the morphology of the microstructure greatly affects the seasonal cracking of the slab. Specifically, it was found that by controlling the average original austenite grain size and microstructure of the continuously cast slab to improve its toughness, it is possible to suppress the seasonal cracking of the slab during the cooling process of the continuously cast slab, thereby obtaining the present invention.
[0017] That is, the continuous casting slab of the present invention which advantageously solves the above-mentioned problems is a continuous casting slab for high-strength steel, characterized in that the average original austenite grain size at a position 10 mm away from the surface of the continuous casting slab is 0.5 mm to 2.0 mm, and the area ratio of bainite and the area ratio of ferrite in the microstructure are greater than 90% in total, and the area ratio of the above-mentioned ferrite is 0% or greater than 3%.
[0018] It should be noted that the continuous cast slab of the present invention may be a more preferable solution if it contains (a) 0.10% to 0.40% C, 0.10% to 2.50% Si, 1.00% to 5.00% Mn, etc. in terms of mass %.
[0019] Furthermore, the method for manufacturing a continuously cast slab of the present invention is a method for manufacturing a continuously cast slab for high-strength steel in which seasonal cracking of the slab caused by cooling is suppressed, and is characterized in that it comprises a first cooling step, a second cooling step, and a third cooling step of cooling the continuously cast slab having the component composition described in (a),
[0020] The first cooling step is to cool the continuously cast slab at a position 10 mm from the surface of the continuous cast slab and at a center of the width direction of the continuous cast slab at a temperature of 1200°C to 1450°C, and to cool the continuously cast slab for a residence time of less than 130 seconds.
[0021] The second cooling step is performed by cooling the continuous cast slab under the cooling conditions that the surface temperature in the center of the width direction is 700°C to 850°C and the average cooling rate is 25°C / hr to 40°C / hr or 50°C / hr or more;
[0022] The third cooling step is performed under cooling conditions in which the surface temperature of the center of the continuous cast slab in the width direction is 500° C. to 700° C. and the average cooling rate is 15° C. / hr or more.
[0023] According to the present invention, it is possible to provide a continuously cast slab in which season cracking does not occur during cooling even in a component system of a continuously cast slab for high-strength steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The following is a photograph of a cross section of a cracked portion of a high-strength steel continuous cast slab that was fractured due to seasonal cracking, taken using a scanning electron microscope (SEM).
[0025] Figure 2 This is a cross-sectional microstructure photograph of the above-mentioned crack.
[0026] Figure 3 This is an enlarged photograph of a continuously cast slab produced in the invention example (test No. D-2) of the continuously cast slab according to the embodiment of the present invention observed with an optical microscope. DETAILED DESCRIPTION
[0027] The following is a detailed description of the embodiments of the present invention. It should be noted that each of the drawings is a schematic diagram and may differ from the actual situation. In addition, the following embodiments are devices and methods for implementing the technical ideas of the present invention, and the configuration is not limited to the following contents. That is, the technical ideas of the present invention can be variously modified within the scope of the technology described in the scope of the claims.
[0028] [First embodiment]
[0029] The continuous casting slab of the first embodiment is described. The continuous casting slab of the present embodiment is a continuous casting slab for high-strength steel, characterized in that (i) the average original austenite grain size at a position 10 mm away from the surface of the continuous casting slab is 0.5 mm to 2.0 mm, (ii) the total area ratio of bainite and the area ratio of ferrite in the microstructure is 90% or more, and (iii) the area ratio of the above-mentioned ferrite is 0% or 3% or more. That is, according to the invention of the present embodiment, by having at least the above-mentioned characteristics (i) to (iii), even in the continuous casting slab for high-strength steel in recent years where the toughness of the continuous casting slab is very low, seasonal cracking of the slab does not occur during the cooling process, thereby providing a continuous casting slab for high-strength steel with good yield.
[0030] First, the appropriate range of the microstructure of the continuously cast slab and the reasons for the limitation are described. It should be noted that in the following description, "%" indicating the composition ratio of the microstructure refers to "area %" unless otherwise specified. In addition, the observation of the microstructure of the continuously cast slab is carried out at room temperature.
[0031] As described above, by observing the damage morphology of the cross-section of the cracked part of the high-strength steel continuous casting slab that broke due to seasonal cracking, it was found that most of the fractures had extended to about 20 mm below the surface of the slab and the cracks progressed to "grain boundary fracture" at the original austenite grain boundaries. That is, in the high-strength steel continuous casting slab, the main reason for the seasonal cracking due to grain boundary fracture is the coarse original austenite grain size and the presence of grain boundary ferrite structure that becomes a factor of embrittled grain boundaries. Therefore, as a necessary condition for the high-strength steel continuous casting slab that does not produce seasonal cracks in the slab during the cooling process, the present embodiment focuses on the two phenomena of (i) the average original austenite grain size from the surface of the continuous casting slab to the specified position and (ii) to (iii) the microstructure of the above-mentioned continuous casting slab.
[0032] <(i) Average prior austenite grain size>
[0033] The high-strength steel continuous casting slab of the present embodiment is a high-strength steel continuous casting slab that suppresses seasonal cracking caused by cooling, and is characterized in that (i) the average original austenite grain size at a position 10 mm away from the surface of the continuous casting slab is 0.5 mm to 2.0 mm. Here, the average original austenite grain size is a factor that determines the unit of fracture of the slab. That is, the larger the average original austenite grain size, the lower the toughness of the continuous casting slab. Here, the average original austenite grain size is the value obtained by averaging the values of multiple original austenite grain sizes calculated from the original austenite grain sizes measured in multiple fields of view.
[0034] In the existing continuous casting slab, the average original austenite grain size is very large if it is a size of several mm. Therefore, the toughness of the continuous casting slab is greatly reduced. In the past low alloy steel, because the toughness of the original continuous casting slab is also high, the average original austenite grain size does not become a problem, but in high alloy high strength steel, the average original austenite grain size may become a very significant problem. Therefore, in the continuous casting slab of the present embodiment, the average original austenite grain size at a position 10mm away from the surface of the continuous casting slab is set to less than 2.0mm. If the average original austenite grain size is less than 2.0mm, the toughness of the continuous casting slab will not be reduced, so it is preferred.
[0035] On the other hand, the lower limit of the average original austenite grain size is not strictly limited, and in order to make the average original austenite grain size smaller than 0.5mm, for example, strong cooling is required in the early stage of solidification. In this case, there is a danger of leakage of uneven solidification. Therefore, the lower limit of the average original austenite grain size is preferably 0.5mm. It should be noted that the lower limit of the average original austenite grain size is more preferably 0.8mm, and further preferably 1.0mm.
[0036] The average original austenite grain size is defined as the grain size of the crystal grains constituting the original austenite structure at a position 10 mm away from the surface of the continuous casting slab. Here, when setting the average original austenite grain size, the reason for setting the position 10 mm away from the surface of the continuous casting slab is that the seasonal cracks of most slabs progress to about 20 mm below the surface of the slab, so the position 10 mm away from the surface of the continuous casting slab is a necessary position to suppress the seasonal cracks of the slab.
[0037] On the other hand, the area less than 5 mm from the surface of the continuous casting slab is directly quenched by the mold or the water sprayer directly below the mold. Therefore, the γ grain size of the continuous casting slab is a tiny structure, the toughness of the slab is high, and it is difficult to generate the starting point of the season crack from this area. Therefore, the area less than 5 mm from the surface of the continuous casting slab can be excluded from the position required to control the slab structure. Therefore, the position where the microstructure of the continuous casting slab needs to be controlled is a position 10 mm deep in the thickness direction of the slab. For example, the position 10 mm from the surface of the continuous casting slab can be used as a reference, and the depth from the surface of the continuous casting slab is 5 to 20 mm.
[0038] In the continuous casting slab of the present embodiment, the factor determining the average original austenite grain size is the temperature when the continuous casting slab is cooled. The temperature of cooling the continuous casting slab is particularly in the range of 1450°C to 1200°C and is affected by its residence time. Moreover, the longer the residence time of the continuous casting slab in this temperature range, the coarser the average original austenite grain size. That is, in order to satisfy the condition that the average original austenite grain size at a position 10mm away from the surface of the continuous casting slab is 0.5mm to 2.0mm, it is important to control the residence time of the continuous casting slab at 1450°C to 1200°C. Specifically, if the residence time of the continuous casting slab at 1450°C to 1200°C at a position 10mm from the surface of the continuous casting slab in the thickness direction is less than 130s, the average original austenite grain size can be made less than 2.0mm, and the seasonal cracking of the slab can be suppressed by controlling the average original austenite grain size to be small, so it is preferred.
[0039] Furthermore, from such a viewpoint, the residence time of the continuously cast slab is preferably 120 s or less, more preferably 110 s or less, and still more preferably 100 s or less.
[0040] It should be noted that the lower limit of the residence time of the continuously cast slab is not particularly limited, but if the residence time is too short, the risk of steel leakage during continuous casting due to uneven solidification increases, so it is set to 40 seconds or more.
[0041] That is, if the residence time of the continuously cast slab at 1450°C to 1200°C is 40 seconds or more, the risk of steel leakage can be reduced, the average prior austenite grain size can be made 2.0 mm or less, and the seasonal cracking of the slab can be suppressed, which is preferred. It should be noted that the residence time of the continuously cast slab is more preferably 60 seconds or more, and even more preferably 70 seconds or more.
[0042] The residence time of the continuously cast slab can be controlled by adjusting the cooling conditions in the initial stage of slab casting. For example, in the continuous casting of steel, the molten steel with adjusted composition is first injected into a water-cooled copper mold to form an initial solidified shell. Then drawing begins, and cooling is implemented by a water sprayer after leaving the water-cooled copper mold. The surface temperature of the slab in the above range is greatly affected by the cooling in the mold and directly below the mold. Therefore, for example, it can be controlled by increasing the thermal conductivity of the crystallizer powder used for lubrication in the mold, or by increasing the flow rate of the water sprayer directly below the mold.
[0043] By controlling their cooling conditions, the average original austenite grain size at a position 10 mm from the surface of the continuous casting slab can be controlled. It is actually difficult to measure the cooling temperature of the continuous casting slab. Therefore, by heat transfer analysis, the temperature history at a position 10 mm into the thickness direction is calculated from the surface of the continuous casting slab, for example, from the depth of 5 mm to the position of 20 mm into the thickness direction of the slab as a representative, so that the cooling temperature of the continuous casting slab can be inferred. In the interior of the continuous casting slab, in order to make the residence time of the above-mentioned temperature zone the longest, the position of the heat transfer analysis can be set to the center of the width of the above-mentioned continuous casting slab.
[0044] <Regarding the microstructure of (ii) to (iii) continuous casting slabs>
[0045] The continuous casting slab of the present embodiment is characterized in that (ii) the area ratio of bainite and the area ratio of ferrite in the microstructure are 90% or more in total, and (iii) the area ratio of ferrite is 0% or 3% or more. That is, it is known that in addition to the average original austenite grain size of 2.0 mm or less at a position 10 mm away from the surface of the continuous casting slab, the ratio of the internal structure of bainite and ferrite is also a factor that determines the unit of fracture, and the toughness of the slab can be improved by an appropriate ratio. Here, the inventors have found that the toughness of the slab can be improved by controlling the cooling rate, the total area ratio of bainite and ferrite in the microstructure is 90% or more, and the area ratio of ferrite is 0% or 3% or more. It should be noted that the area ratio of bainite and the area ratio of ferrite can be calculated based on the observation results of the microstructure of the continuous casting slab using an optical microscope or other observation means. Moreover, using an optical microscope or other observation means, bainite and ferrite contained in the microstructure of the continuous casting slab can be identified.
[0046] According to the identification results of the microstructure of the continuous casting slab, the area S of the microstructure of the continuous casting slab is calculated. total , the area of bainite S bainite , the area of ferrite S ferrite , the area of bainite S bainite and the area S of ferrite ferrite Total area S (bainite+ferrite) Next, the area S of bainite bainite Relative to the area S of the microstructure of the continuous casting slab total The ratio of ferrite area S ferrite Relative to the area S of the microstructure of the continuous casting slab total The ratio of the bainite area S bainite and the area S of ferrite ferrite Total area S (bainite+ferrite) Relative to the area S of the microstructure of the continuous casting slab total The ratios are defined and calculated as the area ratio of bainite, the area ratio of ferrite, and the total area ratio (%) of bainite and ferrite.
[0047] The continuous casting slab of the present embodiment is characterized in that (ii) the total area ratio of bainite and ferrite in the microstructure is 90% or more. That is, in the continuous casting slab of the present embodiment, (ii) if the area ratio of bainite S bainite and the area S of ferrite ferrite Total area S (bainite+ferrite) Relative to the area S of the microstructure of the continuous casting slab total If the area ratio (%) of the ratio is 90% or more, it is preferred because the toughness of the continuously cast slab can be improved. On the other hand, if the above area ratio is less than 90%, it is not preferred because the toughness of the continuously cast slab decreases.
[0048] Furthermore, the continuous casting slab of the present embodiment is characterized in that (iii) the area ratio of ferrite is 0% or 3% or more. That is, in the microstructure of the continuous casting slab of the present embodiment, the area ratio of ferrite is 0% or 3% or more. ferrite Relative to the area S of the microstructure of the continuous casting slab totalThe ferrite area ratio of the ratio is 0% or 3% or more. If the ferrite area ratio is 0%, it is preferred because cracks caused by stress concentration of the soft ferrite mentioned above will not occur. If the ferrite area ratio is 3% or more, the proportion of the ferrite part is fully guaranteed, and the fracture caused by stress concentration in the ferrite part will not extend, so it is preferred. On the other hand, when the ferrite area ratio is greater than 0% and less than 3%, there is a state of thin ferrite at the grain boundary, and stress concentrates on a trace amount of ferrite. It is not preferred because the fracture extends.
[0049] Here, grain boundary ferrite is a factor that determines the grain boundary strength. If grain boundary ferrite is generated, the toughness of the continuous casting slab is reduced. In addition, since ferrite is lower in strength than austenite, pearlite, and bainite, when stress is generated, there is a problem that stress is easily concentrated in the grain boundary ferrite. Based on this viewpoint, the inventors of the present invention have found, after repeated investigations, that the microstructure of the continuous casting slab of the present embodiment can significantly improve the toughness of the continuous casting slab by suppressing the generation of grain boundary ferrite or by fully ensuring the thickness of ferrite even in the structure of the bainite main body.
[0050] It should be noted that ferrite contains a maximum of 0.02 mass% carbon, which is a structure close to pure iron. Ferrite is a ferromagnetic body in the range of room temperature to 780°C, and is the softest and most ductile of steel structures. Pearlite is a structure obtained by slowly cooling austenite. Pearlite is composed of ferrite layers and cementite layers, and is formed by alternating these layers.
[0051] The cooling rate in the ferrite transformation domain greatly affects the precipitation of grain boundary ferrite. When the cooling rate is slower than the critical rate, ferrite precipitation will occur. Therefore, the cooling rates of 850°C to 700°C and 700°C to 500°C are controlled above a certain level to suppress the precipitation of grain boundary ferrite and pearlite in their respective temperature regions. Specifically, by increasing the cooling rate in the ferrite-pearlite transformation region, thereby suppressing their precipitation, the microstructure of the continuously cast slab can be made bainite-based, thereby improving the toughness of the slab.
[0052] Bainite is a phase transformation structure generated from austenite of carbon steel or alloy steel. It has excellent ductility and impact resistance compared to the structure obtained by ordinary quenching and tempering, and is a tough and durable structure. Bainite is a black needle-shaped crystal located between martensite and micro-pearlite and has mechanical properties. In addition, martensite is a hard and brittle structure generated when austenite is quenched.
[0053] It should be noted that the cooling of the continuous casting slab after leaving the continuous casting machine can be controlled by changing the slab temperature at the outlet side of the continuous casting machine, the time required to stack a plurality of slabs, the number of stacked slabs, the conditions of water toughening, etc. The cooling rate can be measured using a thermocouple. For example, after the slab leaves the continuous casting machine, the measurement can be performed by setting a thermocouple at the center of the upper surface of the wide side (long side) of the slab.
[0054] The toughness of the continuously cast slab containing a large amount of C, Si, and Mn is extremely low. Therefore, in such a control that only (i) the average original austenite grain size at a position 10 mm away from the surface of the continuously cast slab is 0.5 mm to 2.0 mm or less, or only (ii) the area ratio of bainite and ferrite in the microstructure is 90% or more in total, or only (iii) the area ratio of ferrite is 0% or 3% or more, it is impossible to ensure sufficient toughness to prevent the occurrence of seasonal cracks in the slab, so seasonal cracks in the slab occur. Therefore, it is important for the continuous cast slab for high-strength steel of the present embodiment to simultaneously meet the conditions of (i) the average original austenite grain size and (ii) to (iii) the microstructure.
[0055] As described above, according to the invention of the first embodiment, even in recent high-strength steel slabs whose toughness is very low, high-strength steel continuously cast slabs with good yield and no seasonal cracking of the slabs during the cooling process can be obtained.
[0056] [Second Embodiment]
[0057] The continuously cast slab of the second embodiment is described below. The continuously cast slab of this embodiment is the continuous cast slab of the above embodiment, and contains, by mass%, 0.10% to 0.40% C, 0.10% to 2.50% Si, and 1.00% to 5.00% Mn.
[0058] In the following description, "%" representing the content of component elements in steel means "mass %" unless otherwise specified.
[0059] <C: 0.10% to 0.40%>
[0060] In the continuous casting slab of the present embodiment, the reason for limiting the composition of each chemical component contained in the continuous casting slab is explained. It should be noted that the content of each chemical component contained in the continuous casting slab is mass %. The reason for making the C content contained in the continuous casting slab 0.10% to 0.40% is as follows. The C contained in the continuous casting slab for high-strength steel is an element required to improve the strength of the high-strength steel plate using the continuous casting slab as a raw material. If the C content is less than 0.10%, the strength required for the high-strength steel plate cannot be obtained, so the lower limit of the C content is 0.10%. On the other hand, if the C content is greater than 0.40%, the microstructure in which bainite and ferrite are the main body as described above cannot be obtained within the range of the cooling rate of the continuous casting slab, so it is not preferred.
[0061] Therefore, from such a viewpoint, in the continuously cast slab of the present embodiment, the C content contained in the continuously cast slab is preferably 0.10% to 0.40%, more preferably 0.12% to 0.35%, and further preferably 0.15% to 0.30%.
[0062] <Si: 0.10% to 2.50%>
[0063] Secondly, the reason for setting the Si content in the continuous casting slab for high-strength steel to 0.10% to 2.50% is as follows. The Si contained in the continuous casting slab is an element required to ensure that austenite remains on the high-strength steel plate in the annealing process of the high-strength steel plate using the continuous casting slab as the raw material. In addition, the Si contained in the continuous casting slab is also an indispensable additive element for improving the strength of the high-strength steel plate through solid solution strengthening. If the Si content is less than 0.10%, the strength required for the high-strength steel plate cannot be obtained, so the lower limit of the Si content is 0.10%.
[0064] On the other hand, if the Si content exceeds 2.50%, the effect of obtaining the strength required for the high-strength steel sheet is saturated, and a strong scale is generated on the hot-rolled sheet before being processed into the high-strength steel sheet. As a result, the appearance and pickling properties of the high-strength steel sheet are deteriorated, so the upper limit of the Si content is 2.50%.
[0065] Therefore, from such a viewpoint, in the continuously cast slab of the present embodiment, the Si content contained in the continuously cast slab is preferably 0.10% to 2.50%, more preferably 0.50% to 2.00%, and further preferably 1.00% to 1.80%.
[0066] <Mn: 1.00% to 5.00%>
[0067] Furthermore, the reason for making the content of Mn contained in the continuous casting slab 1.00% to 5.00% is as follows. The Mn contained in the continuous casting slab is an element required to further improve the strength of the high-strength steel plate. Specifically, Mn is an element added in the hot rolling process of the continuous casting slab in order to control the strength of the high-strength steel plate by phase change control. If the content of Mn is less than 1.00%, the high-strength steel plate cannot be fully strengthened, so the lower limit of the content of Mn is 1.00%. On the other hand, if the content of Mn is greater than 5.00%, the degree to which the high-strength steel plate is fully strengthened is saturated, and the manufacturing cost of the high-strength steel plate increases, which is not preferred from an economic point of view.
[0068] Therefore, from such a viewpoint, in the continuously cast slab of the present embodiment, the Mn content contained in the continuously cast slab is preferably 1.00% to 5.00%, more preferably 1.50% to 4.50%, and further preferably 1.80% to 4.00%.
[0069] The continuous casting slab of the present embodiment has the above-mentioned composition, and the remainder is composed of Fe and inevitable impurities, and has an average original austenite grain size and microstructure of appropriate composition. In this range, considering other characteristics, P can be contained to be less than 0.100%, S to be less than 0.0200%, N to be less than 0.0100%, Al to be less than 0.100%, and O to be less than 0.0100%. Here, as inevitable impurities, Zn, Pb and As can be cited. It is allowed to contain a total of less than 0.100% of these inevitable impurities.
[0070] P segregates at the original austenite grain boundary and makes the grain boundary embrittled, so it sometimes causes seasonal cracks in the slab. Therefore, it is preferred that the P content be 0.100% or less. It should be noted that the lower limit of the P content is not particularly specified, but P is a solid solution strengthening element that can improve the strength of the steel plate, so it is preferably 0.001% or more. Therefore, it is preferred that the P content be 0.100% or less. It is preferably 0.001% or more. It is further preferred that it be 0.070% or less.
[0071] S, which exists as sulfide, is an element that causes slab embrittlement. Therefore, it is preferred that the S content be 0.0200% or less. It should be noted that the lower limit of the S content is not particularly specified, but from the perspective of production technology constraints, it is preferred that the S content be 0.0001% or more. Therefore, it is preferred that the S content be 0.0200% or less. It is preferred to make it 0.0001% or more. It is further preferred to make it 0.0050% or less.
[0072] Al inhibits the formation of carbides during slab cooling and promotes the formation of retained austenite, so it is an element that affects the fraction of retained austenite in the slab. In addition, it is preferably added in an amount of 0.005% or more for deoxidation. If the Al content is greater than 0.100%, there is a concern that the slab will become brittle. Therefore, it is preferred that the Al content be 0.100% or less. It is more preferred that it be 0.010% or more. It is further preferred that it be 0.080% or less.
[0073] N present as nitride is an element that causes slab embrittlement. Therefore, it is preferred that the N content is 0.0100% or less. It should be noted that the lower limit of the N content is not particularly specified, but from the perspective of production technology constraints, it is preferred that the N content is 0.0001% or more. Therefore, it is preferred that the N content is 0.0100% or less. It is preferred to make it 0.0001% or more. It is further preferred to make it 0.0050% or less.
[0074] O present as an oxide is an element that causes embrittlement of the slab. Therefore, it is preferred that the content of O is 0.0100% or less. It should be noted that the lower limit of the content of O is not particularly specified, but from the perspective of production technology constraints, it is preferred that the content of O is 0.0001% or more. Therefore, it is preferred that the content of O is 0.0100% or less. It is preferred to make it 0.0001% or more. It is further preferred to make it 0.0050% or less.
[0075] The continuous cast slab of the present embodiment is a continuous cast slab used for high-strength steel plates. In addition to the above-mentioned component composition, at least one element selected from less than 0.200% Ti, less than 0.200% Nb, less than 0.200% V, less than 0.10% Ta, less than 0.10% W, less than 2.00% Cr, less than 2.00% Mo, less than 2.00% Ni, less than 2.00% Cu, and less than 0.0100% B may be contained alone or in combination of two or more elements.
[0076] If the contents of Ti, Nb and V are respectively less than 0.200%, coarse precipitates and inclusions cannot be generated in large quantities, thereby not reducing the toughness of the slab. Therefore, it is preferred that the contents of Ti, Nb and V are respectively less than 0.200%. It should be noted that the lower limits of the contents of Ti, Nb and V are not specifically specified, but during hot rolling or continuous annealing of the continuously cast slab, the strength of the steel sheet is improved by forming tiny carbides, nitrides or carbonitrides, so it is preferred that the contents of Ti, Nb and V are respectively more than 0.001%. Therefore, when Ti, Nb and V are contained, their contents are respectively less than 0.200%. It is more preferred that they are respectively more than 0.001%. It is further preferred that they are respectively less than 0.100%.
[0077] If the contents of Ta and W are respectively less than 0.10%, coarse precipitates and inclusions cannot be generated in large quantities, thereby not reducing the toughness of the slab. Therefore, it is preferred that the contents of Ta and W are respectively less than 0.10%. It should be noted that the lower limits of the contents of Ta and W are not specifically specified, but during hot rolling or continuous annealing of the continuously cast slab, the strength of the steel sheet is improved by forming tiny carbides, nitrides or carbonitrides, so it is preferred that the contents of Ta and W are respectively more than 0.01%. Therefore, when Ta and W are included, their contents are respectively 0.10%. It is more preferred that they are respectively more than 0.01%. It is further preferred that they are respectively less than 0.08%.
[0078] Without prejudice to the purpose of the present invention, the continuous casting slab of the present embodiment may contain at least one selected from Cr, Mo, Ni and Cu as needed. Cr, Mo, Ni and Cu achieve the effect of improving the strength of the steel plate by controlling the structure of the hot rolling of the continuous casting slab. This effect becomes significant by adding 0.01% or more of Cr, Mo, Ni and Cu, respectively, so it is preferred to add 0.01% or more. If the amount of each element exceeds the upper limit of each element, the weldability, hot workability, etc. of the steel plate are degraded, so the upper limit of the amount of each element of Cr, Mo, Ni and Cu is set to 1.00%. Therefore, when the continuous casting slab contains Cr, Mo, Ni and Cu, the content of each element is set to less than 1.00%. It is preferably set to more than 0.01%. It is further preferred to set it to less than 0.80%.
[0079] B controls the microstructure transformation during hot rolling and annealing of the continuous casting slab, so it can be added from the perspective of affecting the strength through microstructure strengthening. If B is less than 0.0100%, the toughness of the slab is not affected. Therefore, it is preferred that the B content is less than 0.0100%. It should be noted that the lower limit of the B content is not particularly specified, but B is an element that segregates at the austenite grain boundary during hot rolling and annealing of the continuous casting slab to improve the hardenability, so it is preferred that the B content is more than 0.0003%. Therefore, when B is included, its content is less than 0.0100%. It is more preferred to make it more than 0.0003%. It is further preferred to make it less than 0.0080%.
[0080] If Co is 1.00% or less, coarse precipitates and inclusions cannot be increased, and the toughness of the slab cannot be reduced. Therefore, it is preferable that the content of Co is 1.00% or less. It should be noted that the lower limit of the content of Co is not particularly specified, but Co is an element that improves hardenability, so it is more preferable that the content of Co is 0.001% or more. Therefore, when Co is included, its content is 1.00% or less. It is more preferable to make it 0.001% or more. It is further preferable to make it 0.80% or less.
[0081] If Cu is less than 1.00%, coarse precipitates and inclusions cannot be increased, and the toughness of the slab cannot be reduced. Therefore, it is preferred that the Cu content is less than 1.00%. It should be noted that the lower limit of the Cu content is not particularly specified, but Cu is an element that improves hardenability, so it is preferred that the Cu content is more than 0.01%. Therefore, when Cu is included, its content is less than 1.00%. It is more preferred to make it more than 0.01%. It is further preferred to make it less than 0.80%.
[0082] If Sn is 0.200% or less, the toughness of the slab is not affected. Therefore, it is preferred that the content of Sn is 0.200% or less. It should be noted that the lower limit of the content of Sn is not particularly specified, but Sn is an element that improves hardenability, so it is more preferred that the content of Sn is 0.001% or more. Therefore, when Sn is included, the content is 0.200% or less. It is more preferred to make it 0.001% or more. It is further preferred to make it 0.100% or less.
[0083] If Sb is 0.200% or less, coarse precipitates and inclusions cannot be increased, and the toughness of the slab cannot be reduced. Therefore, it is preferred that the Sb content is 0.200% or less. It should be noted that the lower limit of the Sb content is not particularly specified, but Sb is an element that suppresses decarburization and can adjust the strength of the steel sheet, so it is more preferred that the Sb content is 0.001% or more. Therefore, when Sb is included, its content is 0.200% or less. It is more preferred to make it 0.001% or more. It is further preferred to make it 0.100% or less.
[0084] If Ca, Mg and REM are 0.0100% or less, coarse precipitates and inclusions will not increase, and the toughness of the slab will not be reduced. Therefore, it is preferred that the contents of Ca, Mg and REM are 0.0100% or less. It should be noted that the lower limits of the contents of Ca, Mg and REM are not particularly specified, but Ca, Mg and REM are elements that make the shapes of nitrides and sulfides spherical and thus improve the toughness of the slab, so it is more preferred that the contents of Ca, Mg and REM are 0.0005% or more, respectively. Therefore, when Ca, Mg and REM are included, their contents are 0.0100% or less, respectively. It is more preferred that they are 0.0005% or more, respectively. It is further preferred that they are 0.0050% or less, respectively.
[0085] If Zr and Te are respectively less than 0.100%, coarse precipitates and inclusions cannot be increased, and the toughness of the slab cannot be reduced. Therefore, it is preferred that the content of each Zr and Te is less than 0.100%. It should be noted that the lower limit of each content of Zr and Te is not particularly specified, but Zr and Te are elements that make the shape of nitrides and sulfides spherical and thus improve the toughness of the slab, so it is more preferred that the content of Zr and Te is more than 0.001%. Therefore, when Zr and Te are included, their contents are each less than 0.100%. It is more preferred to make it more than 0.001%. It is further preferred to make it less than 0.080%.
[0086] If Hf is less than 0.10%, coarse precipitates and inclusions cannot be increased, and the toughness of the slab cannot be reduced. Therefore, it is preferred that the Hf content be less than 0.10%. It should be noted that the lower limit of the Hf content is not particularly specified, but Hf is an element that makes the shape of nitrides and sulfides spherical and thus improves the ultimate deformation capacity of the steel sheet, so it is more preferred that the Hf content be 0.01% or more. Therefore, when Hf is included, its content is less than 0.10%. It is more preferred to make it more than 0.01%. It is further preferred to make it less than 0.08%.
[0087] If Bi is less than 0.200%, coarse precipitates and inclusions cannot be increased, and the toughness of the slab cannot be reduced. Therefore, it is preferred that the Bi content be less than 0.200%. It should be noted that the lower limit of the Bi content is not particularly specified, but Bi is an element that reduces segregation, so it is more preferred that the Bi content be 0.001% or more. Therefore, when Bi is included, the content is less than 0.200%. It is more preferred to make it more than 0.001%. It is further preferred to make it less than 0.100%.
[0088] It should be noted that the above-mentioned Ti, Nb, V, Ta, W, B, Cr, Mo, Ni, Co, Cu, Sn, Sb, Ca, Mg, REM, Zr, Te, Hf and Bi are contained as unavoidable impurities because the effects of the present invention are not hindered when the contents thereof are less than the preferred lower limits.
[0089] As described above, according to the invention of the second embodiment, it is possible to obtain the strength required for a high-strength steel sheet and to obtain a continuously cast slab excellent in weldability, workability, and appearance of a high-strength steel sheet.
[0090] [Third Embodiment]
[0091] The method for manufacturing a continuous casting slab of the third embodiment is described. The method for manufacturing a continuous casting slab of the present embodiment is a method for manufacturing a continuous casting slab for high-strength steel that suppresses the seasonal cracking of the slab caused by cooling, and includes a first cooling step, a second cooling step, and a third cooling step for cooling the continuous casting slab having the composition of the continuous casting slab described in the above embodiment. Among them, the first cooling step is to cool the continuous casting slab at the center of the width direction of the continuous casting slab and at a position 10mm away from the surface of the continuous casting slab at a cooling temperature of 1200℃ to 1450℃, and the residence time of the continuous casting slab is 130s or less; the second cooling step is to cool the continuous casting slab at a surface temperature of 700℃ to 850℃ in the center of the width direction of the continuous casting slab, and an average cooling rate of 25℃ / hr to 40℃ / hr or 50℃ / hr or more; the third cooling step is to cool the continuous casting slab at a surface temperature of 500℃ to 700℃ in the center of the width direction of the continuous casting slab at an average cooling rate of 15℃ / hr or more.
[0092] Here, the upper limit of the average cooling rate of the second cooling process and the third cooling process is not particularly specified, but the average cooling rates of 700℃~850℃ and 500℃~700℃ when a slab is cooled in air are 120℃ / hr and 70℃ / hr at maximum, respectively. In the second cooling process and the third cooling process, cooling according to an average cooling rate faster than the above average cooling rate requires, for example, water spraying and air injection on the slab, which is not preferred from the economic point of view because equipment is required. Therefore, the upper limit of the average cooling rate of 700℃~850℃ in the second cooling process is 120℃ / hr, and the upper limit of the average cooling rate of 500℃~700℃ in the third cooling process is 70℃ / hr.
[0093] It should be noted that the method for manufacturing slabs for high-strength steel plates of the present embodiment may be subject to a transfer depending on the conditions of its manufacturing process. In the event of a transfer, the cooling rate of the slab may temporarily exceed the predetermined cooling rate. However, if the time required for the phase change is more than 10 hours, it is very slow, so if the processing time is a transfer degree (the longest is 1 to 2 hours), seasonal cracking will not occur. Therefore, the present invention does not specify a maximum cooling rate but an average cooling rate. Below, each process included in the method for manufacturing a continuous casting slab of the present embodiment is described.
[0094] (First Cooling Step)
[0095] The method for manufacturing a continuously cast slab of the present embodiment is a method for manufacturing a continuously cast slab for high-strength steel that suppresses seasonal cracking of the slab caused by cooling, and includes a first cooling step of cooling the continuously cast slab having the component composition of the continuously cast slab described in the above embodiment.
[0096] Among them, the first cooling process is to cool the continuous casting slab under cooling conditions such that the cooling temperature of the continuous casting slab at the center of the width direction of the continuous casting slab and at a position 10 mm away from the surface of the continuous casting slab is 1200℃~1450℃ and the residence time of the continuous casting slab is less than 130s.
[0097] The first cooling step is a step for controlling the average original austenite grain size contained in the continuous casting slab of the above embodiment to be less than 2.0 mm in a predetermined position. In the method for manufacturing the continuous casting slab of the present embodiment, the factor that determines the average original austenite grain size is the temperature when the slab is cooled. In the first cooling step, the temperature for cooling the continuous casting slab is in the range of 1450°C to 1200°C. As such, the method for manufacturing the continuous casting slab of the present embodiment focuses on the cooling temperature of the continuous casting slab in the range of 1450°C to 1200°C, which is the factor that determines the average original austenite grain size, and controls the temperature.
[0098] Furthermore, in the first cooling step, the residence time of the continuously cast slab in the above temperature range of the cooling continuously cast slab is 130 seconds or less. If the residence time of the continuously cast slab at the above temperature is 130 seconds or less, the average original austenite grain size can be made less than 2.0 mm, and the seasonal cracking of the slab can be suppressed, so it is preferred. It should be noted that the lower limit of the residence time of the continuously cast slab at 1200°C to 1450°C is not particularly specified, but if the residence time is too short, the risk of steel leakage in continuous casting due to uneven solidification becomes high, so it is preferably 40 seconds or more, more preferably 60 seconds or more, and even more preferably 70 seconds or more.
[0099] (Second Cooling Step)
[0100] Next, the method for manufacturing the continuous casting slab of the present embodiment includes a second cooling step of cooling the continuous casting slab under cooling conditions such that the surface temperature in the center of the width direction of the continuous casting slab is 700°C to 850°C and the average cooling rate is 25°C / hr to 40°C / hr or 50°C / hr or more. The second cooling step is a step for controlling the precipitation of ferrite included in the microstructure of the continuous casting slab of the above embodiment, so that the above microstructure becomes a bainite-based structure.
[0101] In the second cooling step, the temperature at which the continuously cast slab is further cooled is 700° C. to 850° C. As described above, the method for producing a continuously cast slab according to the present embodiment focuses on the cooling rate in the temperature range of the ferrite transformation region where ferrite precipitation can be controlled, and controls the temperature.
[0102] In the second cooling step, in the above-mentioned temperature range for cooling the continuously cast slab, the average cooling rate of the continuously cast slab is 25°C / hr to 40°C / hr or 50°C / hr or more. When the average cooling rate of the continuously cast slab is less than 25°C / hr, after ferrite is generated, solutes such as carbon exceeding the solid solubility of the ferrite generate concentrated residual austenite, and then pearlite precipitates in large quantities from the residual austenite, so it is not preferred. In addition, when the average cooling rate of the continuously cast slab is greater than 40°C / hr and less than 50°C / hr, ferrite precipitates thinly only on the original austenite grain boundaries due to the steel components and the average original austenite grain size, making the grain boundaries embrittled, so it is not preferred.
[0103] From this point of view, if the average cooling rate of the continuously cast slab is 25°C / hr to 40°C / hr or 50°C / hr or above, the amount of ferrite precipitation is reasonable and the precipitation of pearlite and seasonal cracking of the slab can be suppressed, which is preferred.
[0104] It should be noted that the upper limit of the average cooling rate is not particularly specified. When a continuous cast slab is cooled in air at 700°C to 850°C, the maximum average cooling rate is 120°C / hr. Cooling at an average cooling rate faster than this requires, for example, water spraying and air injection on the continuous cast slab, which requires equipment and is not preferred from an economic point of view. Therefore, the upper limit of the average cooling rate of 700°C to 850°C is 120°C / hr.
[0105] (Third Cooling Step)
[0106] Furthermore, the method for producing a continuously cast slab of the present embodiment includes a third cooling step of cooling the continuously cast slab under cooling conditions in which the surface temperature at the center in the width direction is 500°C to 700°C and the average cooling rate is 15°C / hr or more.
[0107] The third cooling step is a step for further suppressing the precipitation of pearlite included in the microstructure of the continuous casting slab of the above embodiment, so that the above microstructure becomes a bainite-based structure. Specifically, the third cooling step is a step for reducing the area S of bainite to bainite and the area S of ferrite ferrite Total area S (bainite+ferrite) Relative to the area S of the microstructure of the continuous casting slab totalThe process is to set the area ratio (%) of the ratio to 90% or more.
[0108] In the third cooling step, the temperature of the continuously cast slab is further cooled to 500° C. to 700° C. As described above, the method for producing a continuously cast slab according to the present embodiment focuses on the cooling rate in the temperature range of the pearlite transformation region where the precipitation of pearlite can be suppressed, and controls the temperature.
[0109] In the third cooling step, in the above temperature range for cooling the continuously cast slab, the average cooling rate of the continuously cast slab is 15°C / hr or more. When the average cooling rate of the continuously cast slab is less than 15°C / hr, pearlite precipitates relative to the main body of bainite. Pearlite has a higher phase transition temperature than bainite, and phase transition stress is generated in the first precipitated pearlite portion. Pearlite alone has a lower strength than bainite, so the dislocation caused by the strength difference between pearlite and bainite is concentrated in pearlite, which becomes an important factor in promoting fracture.
[0110] From such a viewpoint, if the average cooling rate of the continuously cast slab is 15° C. / hr or more, a large amount of precipitation of pearlite can be avoided and seasonal cracking of the slab can be suppressed, which is preferred.
[0111] It should be noted that the upper limit of the average cooling rate is not particularly specified. When a continuously cast slab is cooled in air at 500°C to 700°C, the maximum average cooling rate is 70°C / hr. Cooling at an average cooling rate faster than this, for example, requires water spraying and air injection on the continuously cast slab, which is not preferred from the economic point of view because it requires equipment. Therefore, the upper limit of the average cooling rate of 500°C to 700°C can be set to 70°C / hr.
[0112] Thus, in the manufacturing method of the continuous casting slab of the present embodiment, as the cooling process of the continuous casting slab, a cooling process based on three stages is adopted to control the average original austenite grain size and the microstructure of the continuous casting slab, thereby providing a continuous casting slab for high-strength steel that suppresses the seasonal cracking of the slab caused by cooling.
[0113] As described above, according to the manufacturing method of the continuous casting slab of the third embodiment, even if the composition system of the slab is for high-strength steel, by dividing the cooling process into three stages and strictly controlling each cooling process, it is possible to provide a continuous casting slab for high-strength steel that does not produce seasonal cracks during the cooling process.
[0114] [Other embodiments]
[0115] The above is an explanation of the present invention with reference to the embodiments, but the present invention is not limited to the above embodiments. The composition and details of the present invention can be subject to various changes that can be understood by those skilled in the art within the technical scope of the present invention. In addition, the system or device of how to combine other features respectively included in each embodiment is also included in the technical scope of the present invention.
[0116] Hereinafter, the effects of the present invention will be specifically described based on the examples, but the present invention is not limited to these examples. That is, in order to confirm the effects of the present invention, the inventors of the present invention used various steel types as raw materials to produce continuous casting slabs in comparative examples (test No. A-1 to A-4, test No. B-1 to B-8, test No. C-1 to C-3) and inventive examples (test No. D-1 to D-20). Table 1 shows the steel types A to F of the raw materials of the continuous casting slabs used in comparative examples (test No. A-1 to A-4, test No. B-1 to B-8, test No. C-1 to C-3) and inventive examples (test No. D-1 to D-20).
[0117] [Table 1]
[0118]
[0119] Among them, the cooling conditions of the continuously cast slab adopt a three-stage cooling process consisting of (I) a residence time (s) of 1200℃~1450℃, (II) an average cooling rate (℃ / hr) of 700℃~850℃ and (III) an average cooling rate (℃ / hr) of 500℃~700℃, and cooling is performed by appropriately changing the conditions of each stage.
[0120] Tables 2 to 4 show the cooling conditions (I) to (III) of the continuously cast slabs, the microstructures of the obtained continuously cast slabs, and the evaluation of the slab seasonal cracks. In Tables 2 to 4, F, P, and B in the column of microstructure represent ferrite, pearlite, and bainite, respectively.
[0121] The measurement of the average prior austenite grain size and the calculation of the area ratios of bainite, pearlite, and ferrite of the continuously cast slabs produced in the comparative examples and the inventive examples, and the evaluation of the season cracking of the continuously cast slabs were performed as follows.
[0122] <Measurement of average prior austenite grain size>
[0123] Among them, the method for determining the average original austenite grain size is as follows. A sample is cut out from the center of the width of the cooled slab, and a thick section of the slab parallel to the width direction of the slab is used as the observation surface. Next, the observation surface is mirror-polished using diamond paste, and then final polishing is performed using colloidal silica, and etching is performed using a 3 vol.% nitric acid alcohol solution to make the observation surface show the structure. Using an optical microscope, 5 fields of view are observed at a magnification of 10 times at a distance of 10 mm from the surface of the slab to obtain a microstructure image of the continuously cast slab. The obtained microstructure image is used to obtain the original austenite grain sizes obtained by observing the 5 fields of view respectively by the cutting method in accordance with JIS G 0551:2020, and the average value of these is calculated as the average original austenite grain size.
[0124] <Method for measuring ferrite area ratio>
[0125] In the method for determining the ferrite area ratio, the observation surface of the slab is prepared in the same manner as the method for determining the average prior austenite grain size described above. Next, the observation surface is mirror-polished using diamond paste, and then final polishing is performed using colloidal silica, and etching is performed using a 3 vol.% nitric acid alcohol solution to make the observation surface show the structure. Using a SEM (Scanning Electron Microscope) at an accelerating voltage of 15 kV, 10 fields of view are observed at a magnification of 50 times at a position 10 mm away from the surface of the slab, and the microstructure image of the continuously cast slab obtained is calculated using Adobe's PHOTOSHOP (registered trademark) to calculate the area ratio of ferrite in 10 fields of view, and these values are averaged and obtained as the area ratio of ferrite. It should be noted that ferrite has a larger grain size than other structures (pearlite, bainite, tempered martensite, quenched martensite, and retained austenite), and has a darker contrast on a smooth surface, so it is easy to distinguish at a magnification of 50 times.
[0126] <Method for measuring the area ratio of pearlite and bainite>
[0127] In the method for measuring the area ratio of the pearlite and bainite structures, the structures are displayed on the observation surface of the slab in the same manner as the above-mentioned method for measuring ferrite. Using SEM under the condition of an accelerating voltage of 15 kV, ferrite is avoided from the field of view at a position 10 mm away from the surface of the slab, and 10 fields of view are observed at a magnification of 10,000 times. The obtained structure image is calculated using Adobe's PHOTOSHOP (registered trademark) for the area ratio of pearlite and bainite in 10 fields of view, and these values are averaged and combined with the area ratio of ferrite measured by the above-mentioned method to make the total 100% to calculate and obtain the area ratio of each structure. Bainite is a structure in the concave part, and pearlite is a structure in the concave part that contains thin-plate carbides.
[0128] A comprehensive evaluation of the microstructure was performed. The evaluation criteria are as follows.
[0129] · Microstructure evaluation: 0···S (bainite+ferrite) Relative to S total The ratio of bainite and ferrite, that is, the total area ratio (%) is 90% or more, and S (ferrite) Relative to S total The ratio of ferrite, that is, the area ratio (%) of ferrite is 0% or more than 3%.
[0130] ·Evaluation of microstructure: ×···S (bainite+ferrite) Relative to S total The ratio of bainite to ferrite, i.e. the total area ratio (%), is less than 90%, or S (ferrite) Relative to S total The ratio of ferrite, that is, the area ratio (%) of ferrite is 0 or more and less than 3%
[0131] <Seasonal crack evaluation of slab>
[0132] The evaluation method for slab quarter cracks is based on the penetrant flaw detection test specified in JIS Z 2343: 2017, and the presence or absence of cracks on the wide and narrow surfaces of the slab is evaluated. After applying the developer, the appearance of the penetrant is visually observed, and the quarter cracks and defects of the slab occurring on the surface are visually inspected.
[0133] In addition, since cracks and defects in the slab with a length of 10 mm or less do not cause openings, openings, and fractures during heating in the hot rolling process, the evaluation criteria for seasonal cracks in the slab are as follows.
[0134] ·Seasonal cracks of slab: 0···No cracks or defects with a length of 10 mm or more are visually observed on the slab surface
[0135] ·Seasonal cracks of slab: ×···Cracks or defects with a length of 10 mm or more can be visually observed on the slab surface
[0136]
[0137]
[0138]
[0139] <Comparative Examples (Test Nos. A-1 to A-5)>
[0140] The microstructure of the slab that the continuously cast slabs produced in Test No. A-1 to A-5 satisfy is called Condition A. Condition A is a condition in which the average prior austenite grain size at a position 10 mm away from the surface of the slab in the thickness direction becomes larger than 2.0 mm. In these cases, since the density of precipitates at the prior austenite grain boundaries increases and the toughness of the prior austenite grain boundaries decreases, even if various changes are made to the conditions for slow cooling of the slab after leaving the slab continuous casting machine, the seasonal cracking of the slab cannot be suppressed.
[0141] <Comparative Examples (Test Nos. B-1 to B-8)>
[0142] The microstructure of the slabs satisfied by the continuously cast slabs manufactured in Test No. B-1 to B-8 is referred to as Condition B. Condition B is a condition in which the average prior austenite grain size at a position 10 mm from the surface of the slab is 2.0 mm or less, but pearlite precipitates more than 10%, and thus the seasonal cracking of the slab cannot be suppressed.
[0143] <Comparative Examples (Test Nos. C-1 to C-3)>
[0144] The microstructure of the slabs satisfied by the continuously cast slabs manufactured in Test No. C-1 to C-3 is called Condition C. Condition C is a condition in which the average prior austenite grain size at a position 10 mm from the surface of the slab is 2.0 mm or less and the area ratio of bainite and ferrite is 90% or more, but the area ratio of ferrite is 1% or 2%, so that a thin layer of ferrite is precipitated on the grain boundary. Condition C is an example of a condition that cannot suppress the seasonal cracking of the slab.
[0145] <Examples (Test Nos. D-1 to D-20)>
[0146] The microstructure of the slabs satisfied by the continuously cast slabs manufactured in Test No. D-1 to D-20 is called Condition D. Condition D is the condition of the present invention example. In the continuously cast slabs manufactured in the present invention example, the average original austenite grain size 10 mm away from the surface of the slab is 0.5 mm to 2.0 mm, and the microstructure of the continuously cast slab is a bainite single phase or a bainite + ferrite structure. That is, from the perspective of the refinement of the original austenite grain size and the optimization of the microstructure, the toughness of the slab is improved, so that the slab does not produce seasonal cracks after the slab is cooled.
[0147] According to Tables 2 to 4, it can be seen that by making the average original austenite grain size at a position 10 mm away from the surface of the slab in the thickness direction of the slab less than 2.0 mm, and the area ratio of bainite and the area ratio of ferrite in the microstructure of the continuous casting slab total more than 90%, and making the area ratio of ferrite 0% or more than 3%, it is possible to suppress the seasonal cracking of the slab during cooling of the slab.
[0148] Figure 3 This is an enlarged photograph of a continuously cast slab produced in the invention example (Test No. D-2) by optical microscope observation. Figure 3 The enlarged photo of the continuous casting slab observed under an optical microscope is shown, and the metal structure contained in the continuous casting slab is identified, and the area S of bainite is bainite and the area S of ferrite ferrite The total area S (bainite+ferrite) Relative to the area S of the microstructure of the continuous casting slab total The ratio is calculated as the area ratio (%). As a result, the average original austenite grain size of the continuous casting slab of the present invention example at a position 10 mm away from the surface of the slab in the thickness direction of the slab is 0.5 mm to 2.0 mm, and the area ratio of bainite and ferrite in the microstructure is more than 90% in total, and the area ratio of ferrite is 0% or more than 3%.
[0149] Thus, the continuous cast slab of the present invention has an average original austenite grain size of 0.5 mm to 2.0 mm at a position 10 mm from the slab surface, and a microstructure in which the area ratio of bainite and ferrite is 90% or more, and the area ratio of ferrite is 0% or 3% or more, so that a high-alloy high-strength steel slab without slab seasonal cracking after casting can be provided, and hole opening accidents during rolling can be prevented. That is, according to the inventive examples and comparative examples, it can be seen that by making the average original austenite grain size of 0.5 mm to 2.0 mm at a position 10 mm from the slab surface in the slab thickness direction, and making the microstructure in which the area ratio of bainite and ferrite is 90% or more, and the area ratio of ferrite is 0% or 3% or more, the slab seasonal cracking during slab cooling can be suppressed.
[0150] In order to obtain such a microstructure of a slab for high-strength steel plate, for example, it is preferred to adopt three-stage cooling, for example, cooling the slab surface at a retention time of 130 seconds or less at a temperature of 1450°C to 1200°C, then cooling the slab width center surface at a temperature of 850°C to 700°C at a cooling rate of 25°C / hr to 40°C / hr or 50°C / hr or more, and cooling the slab width center surface at a temperature of 700°C to 500°C at an average cooling rate of 15°C / hr or more. It should be noted that the method for manufacturing a continuously cast slab having a microstructure of a slab for high-strength steel plate is not limited thereto.
[0151] The continuous casting slab of the present invention has an average original austenite grain size of 0.5 mm to 2.0 mm at a position 10 mm away from the surface of the slab, and the total area ratio of bainite and ferrite in the microstructure is more than 90%, and the area ratio of ferrite is 0% or more than 3%. Therefore, it is possible to provide a high-strength steel slab without slab seasonal cracking after casting, and can also prevent hole opening accidents during rolling, so it is useful in industry.
Claims
1. A continuous casting slab, It is characterized in that It is a continuous casting slab for high-strength steel. The average prior austenite grain size at a position 10 mm from the surface of the continuously cast slab is 0.5 mm to 2.0 mm. Furthermore, the total area ratio of bainite and ferrite in the microstructure is 90% or more, and the area ratio of ferrite is 0% or 3% or more.
2. The continuously cast slab according to claim 1, It is characterized in that The continuously cast slab comprises, by mass %, 0.10%~0.40% C, 0.10% to 2.50% Si, 1.00% to 5.00% Mn.
3. A method for manufacturing a continuous casting slab, It is characterized in that A method for producing a high-strength steel continuous casting slab in which seasonal cracking of the slab due to cooling is suppressed. The method comprises cooling the continuously cast slab of the composition according to claim 2 in a first cooling step, a second cooling step and a third cooling step; The first cooling step is to cool the continuously cast slab at a cooling temperature of 1200° C. to 1450° C. at a position 10 mm away from the surface of the continuously cast slab in the center of the width direction of the continuously cast slab and 130 seconds or less; The second cooling step is to cool the continuously cast slab under the cooling condition that the surface temperature in the center of the width direction of the continuously cast slab is 700°C to 850°C and the average cooling rate is 25°C / hr to 40°C / hr or 50°C / hr or more; The third cooling step is performed by cooling under cooling conditions in which the surface temperature of the center in the width direction of the continuous cast slab is 500° C. to 700° C. and the average cooling rate is 15° C. / hr or more.