Coated paper
By using starch-based polymer compounds and dextrin as adhesives in coated paper and optimizing the structure of the coating layer, the problems of taking into account both surface strength and white paper gloss are solved, and efficient printing quality and environmental protection performance are achieved .
Patent Information
- Application Number
- CN202380036246.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-26
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to take into account both the surface strength and the gloss of the coated paper without the synthetic adhesive, especially in coated papers that require a high gloss.
Adhesives mainly composed of starch polymer compounds, by using dextrin as the adhesive in the pigment coating layer of coated paper, and adjusting the adhesive amount in the upper and lower layers to ensure 90% of the total adhesive More than % is a starch-based polymer compound, and the structure of the coating layer is optimized by combining the characteristics of white dextrin and the particle size distribution of calcium carbonate.
It is achieved without using synthetic adhesives, and the surface strength and gloss of the coated paper are improved, cost-effective, and easy dissociation and low environmental load during recycling.
Smart Images

Figure BDA0005100632340000171 
Figure BDA0005100632340000181
Abstract
Description
Technical Field
[0001] The present invention relates to coated paper. Background Art
[0002] As a printing method for coated paper, offset printing is often used. Among the qualities of coated paper for offset printing, important qualities include printing surface strength, printing glossiness, anti-bubbling, etc. In particular, printing glossiness is basically easily affected by the glossiness of white paper before printing.
[0003] To date, in order to improve the white paper glossiness of coated paper, studies have been conducted on controlling the amount, particle size, and particle size distribution of calcium carbonate, kaolin, etc. contained in the coating layer (for example, Patent Documents 1 to 4), and using a synthetic adhesive with a specific glass transition temperature (Patent Document 5). In addition, in order to improve the printed surface strength, studies have been conducted on optimizing the synthetic adhesive (Patent Document 6) and adding a styrene-acrylic polymer to a coating containing a natural adhesive and a synthetic adhesive (Patent Document 7). Furthermore, Patent Document 8 proposes to achieve white paper glossiness and printed surface strength by using an adhesive other than a synthetic adhesive.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 4542188
[0007] Patent Document 2: Japanese Patent No. 3755597
[0008] Patent Document 3: Japanese Patent Application Publication No. 2007-46189
[0009] Patent Document 4: Japanese Patent Application Laid-Open No. 2006-132024
[0010] Patent Document 5: Japanese Patent Application Publication No. 2006-188783
[0011] Patent Document 6: Japanese Patent No. 5288544
[0012] Patent Document 7: Japanese Patent No. 4486861
[0013] Patent Document 8: Japanese Patent No. 6435034 Summary of the invention
[0014] However, for cost reduction and environmental considerations, what has attracted much attention is not petroleum-based synthetic materials, but cheap and highly biodegradable materials. Among them, adhesives made from starch-based materials have attracted much attention. In particular, although coated paper requiring high gloss has two pigment coating layers, it is difficult to achieve both white paper gloss and surface strength in such coated paper without containing synthetic adhesives. In view of the above situation, the subject of the present invention is to provide a coated paper that achieves both surface strength and white paper gloss when using an adhesive with a starch-based polymer compound as the main component.
[0015] The above-mentioned problems are solved by the following present invention.
[0016] Method 1
[0017] A coated paper has two pigment coating layers containing pigment and adhesive on at least one side of a base paper.
[0018] More than 90% by weight of the total adhesive in each layer of the pigment coating layer is a starch-based polymer compound.
[0019] At least one of the two layers contains dextrin as a binder.
[0020] Method 1A
[0021] The coated paper according to aspect 1, wherein, when the amount of the adhesive in the lower layer of the two layers is L and the amount of the adhesive in the upper layer is U, L>U.
[0022] Method 2
[0023] A coated paper has two pigment coating layers containing pigment and adhesive on at least one side of a base paper.
[0024] More than 90% by weight of the total adhesive in each layer of the pigment coating layer is a starch-based polymer compound.
[0025] When the amount of the adhesive in the lower layer of the two layers is L and the amount of the adhesive in the upper layer is U, L>U.
[0026] Method 3
[0027] The coated paper according to aspect 1, 1A or 2, wherein the white paper glossiness is 40 to 80%.
[0028] Method 4
[0029] The coated paper according to any one of aspects 1 to 3 (including aspect 1A), wherein the content of the adhesive in the upper layer is 20 parts by weight or less based on 100 parts by weight of the pigment in the layer,
[0030] The content of the binder in the lower layer is 55 parts by weight or less based on 100 parts by weight of the pigment in the layer.
[0031] Method 5
[0032] The coated paper according to any one of aspects 1 to 4 (including aspect 1A), wherein the dextrin is white dextrin and has the following two characteristics:
[0033] 1) The weight average molecular weight is 100,000 to 500,000.
[0034] 2) After steaming at a concentration of 35 wt% for 16 minutes, the RVA viscosity at 50°C is 1000 mPa·s or less.
[0035] Method 6
[0036] The coated paper according to any one of aspects 1 to 5 (including aspect 1A), wherein any one or two of the following characteristics are satisfied:
[0037] i) When 1 mg of the coated paper is measured by instantaneous thermal decomposition method, the styrene content is 0.5 μg or less.
[0038] ii) Distilled water was dropped onto the coated paper and the contact angle was 75° or less 0.1 seconds later.
[0039] Method 7
[0040] The coated paper according to any one of aspects 1 to 6 (including aspect 1A), wherein the pigment in the pigment coating layer is composed of calcium carbonate.
[0041] According to the present invention, it is possible to provide a coated paper which achieves both surface strength and white paper glossiness by using an adhesive containing a starch-based polymer compound as a main component. DETAILED DESCRIPTION
[0042] Hereinafter, the present invention will be described in detail. In the present invention, "X to Y" include the endpoint values, that is, X and Y are included.
[0043] 1. Coated paper
[0044] The coated paper of this embodiment (hereinafter also referred to as "coated paper") has two pigment coating layers containing pigment and adhesive on at least one side, i.e., one side or both sides, of the base paper. The coated paper may be a printing coated paper for offset printing, gravure printing, relief printing, etc., or may be a white board paper having a pigment coating layer on a board base paper. The coated paper may also have two or more pigment coating layers.
[0045] (1) Pigment coating layer
[0046] The coated paper has at least two pigment coating layers, and the adhesive in the layers is mainly composed of starch-based polymer compounds. That is, more than 90% by weight of the total adhesive in each layer is composed of starch-based polymer compounds. In the first embodiment, at least one of the two layers contains dextrin as an adhesive. In this embodiment, only the upper layer may contain dextrin. When there are more than two pigment coating layers, the layer in which dextrin exists is preferably only the uppermost layer. In this embodiment, the glossiness of white paper can be particularly improved.
[0047] In addition, in the second embodiment, the coated paper has at least two pigment coating layers, more than 90 weight % of the total adhesive in each layer is composed of a starch-based polymer compound, and when the amount of the adhesive in the lower layer of the two layers is set to L and the amount of the adhesive in the upper layer is set to U, L>U. The lower layer refers to a layer close to the base paper. When there are more than two pigment coating layers, the "upper layer" is the uppermost layer, and the "lower layer" is a layer adjacent to the uppermost layer and close to the base paper. L / U is not limited, and is preferably 0.5 to 10, and more preferably 1 to 9. In the second embodiment, it is preferred that at least one of the two layers contains dextrin as an adhesive.
[0048] [Adhesive]
[0049] The pigment coating layer is formed by applying a pigment coating liquid mainly comprising a pigment, an adhesive (binder), and water. The adhesive preferably does not contain a styrene copolymer. Furthermore, even if the pigment coating layer is for purposes other than an adhesive, it is preferably free of styrene. Styrene copolymers refer to synthetic adhesives such as copolymers containing styrene as a monomer, such as styrene-butadiene copolymers and styrene-acrylic copolymers.
[0050] In addition, the adhesive preferably does not include a synthetic adhesive that does not contain styrene. Synthetic adhesives are a general term for hydrophobic and chemically synthesized synthetic adhesives. As synthetic adhesives, specifically, copolymers such as styrene-butadiene, styrene-acrylic acid, ethylene-vinyl acetate, butadiene-methyl methacrylate, vinyl acetate-butyl acrylate, polyvinyl alcohol, maleic anhydride copolymers, and acrylic acid-methyl methacrylate copolymers can be cited. By not using synthetic adhesives, it is possible to prevent the support roller from being fouled, improve anti-bubbling properties, and further reduce costs due to the reduction in the use of expensive synthetic adhesives, and improve the dissociation properties when used as waste paper.
[0051] As described above, of the total adhesive of each layer, more than 90% by weight is composed of starch-based polymer compounds. The lower limit of this content is preferably more than 95% by weight, more preferably more than 98% by weight, and further preferably more than 99% by weight. The upper limit is not limited, and is preferably less than 100% by weight or less than 99% by weight. The starch-based polymer compound used as an adhesive is not particularly limited, and the modification method, the variety of raw materials, etc. are also not limited. As starch-based polymer compounds, starch, various processed starches, dextrins obtained by hydrolyzing starch, etc. are suitable. Starch refers to a mixture composed of straight-chain starch and amylopectin, and generally speaking, the mixing ratio varies depending on the plant used as the raw material of the starch.
[0052] As for the modification, modification, processing, etc. of starch, for example, oxidized starch, hydroxy ester starch (HES), phosphate starch, esterified starch, crosslinking agent modified starch, dextrin, etc. can be cited. Among them, dextrin is preferred because it makes the fluidity further better (low viscosity) when combined with the coating. In addition, as the preferred raw materials of the starch-based polymer compound, corn, potato, cassava, etc. can be cited, and glutinous varieties of corn (glutinous corn) and cassava are particularly preferred.
[0053] From the viewpoint of low viscosity and high viscosity stability, dextrin, especially roasted dextrin, is preferably used as an adhesive. In each layer, the amount of dextrin is preferably 40% by weight or more in the total adhesive, and more preferably 50% by weight or more. The upper limit is not limited, and is preferably 100% by weight or less, and more preferably 90% by weight or less. Dextrin refers to the general term for starch-based polymers obtained by hydrolyzing starch. α-Glucose is polymerized through glycosidic bonds and is also called dextrin. The molecular weight of ordinary starch is large, but dextrin is an intermediate product produced in the hydrolysis process of starch, and it can be considered to have a molecular weight of about oligomers (substances with several to 20 glucoses bonded). Roasted dextrin is a dextrin generated by adding acid and baking with dry heat. There are white dextrin, yellow dextrin, English gum and other types. In the present invention, white dextrin is particularly preferably used. If white dextrin is further hydrolyzed, it becomes so-called yellow dextrin, but yellow dextrin has low stability and may color the pigment coating layer, so it is preferred to use white dextrin.
[0054] In addition, white dextrin can also be used in combination with other starch-based adhesives. Examples of starch-based adhesives that can be used in combination include oxidized starch, hydroxyesterified starch (HES), phosphate starch, esterified starch, crosslinker-modified starch, etc., preferably acid-treated starch. By using acid-treated starch in combination, coated paper with excellent surface strength and white paper glossiness can be obtained.
[0055] The molecular weight of white dextrin can be about 100,000 to 500,000 in terms of weight average molecular weight. The higher the molecular weight, the higher the viscosity of the paste, and the viscosity of the coating when mixed also increases, so the weight average molecular weight is preferably 150,000 to 220,000. White dextrin preferably contains many branches in dextrin. If there are many branches, it is easy to show strength. It is believed that the degree of branching is related to the radius of inertia. If it is the same molecular weight, there are many branches when the radius of inertia is small, and when the radius of inertia is large, there are few branches and it is considered to be a straight chain. Therefore, white dextrin preferably has a small radius of inertia.
[0056] Since the viscosity of the white dextrin slurry after cooking is low, the slurry can be highly concentrated. In addition, the viscosity of the slurry of cold water soluble starch represented by α-starch is also low, but since these cold water soluble starches are treated to dissolve in cold water, the surface strength of dextrin is high and advantageous. Therefore, as white dextrin, it is preferred that the solubility in water at 20°C is less than 20% by weight. The behavior of such starch-based polymers can be measured using a rapid viscosity analyzer (RapidVisco Analyzer: RVA, model RVA-4, manufactured by New Port Scientific). In a preferred embodiment, when a starch-based polymer slurry with a concentration of 35% by weight is cooked under the following conditions, a dextrin having a viscosity of 1000 mPa·s or less at 50°C and 160rpm 16 minutes after the start of cooking (hereinafter referred to as "viscosity after cooking") is used. The white dextrin slurry exhibits excellent adhesion after cooking.
[0057] The paddle was rotated under the following conditions using RVA, the torque of the paddle during stirring was measured, and the viscosity of the dextrin after cooking was calculated.
[0058] (Stirring conditions)
[0059] 10 seconds after the start of measurement: 960 rpm
[0060] Afterwards: 160rpm
[0061] (Cooking conditions)
[0062] 0-5 minutes: Heat to 98°C in 5 minutes
[0063] 5-9 minutes: Maintain at 98°C
[0064] 9-12 minutes: Cool down to 50°C in 3 minutes
[0065] 12-16 minutes: Maintain at 50°C
[0066] The viscosity after the above cooking is preferably 1000mPa·s or less, more preferably 850mPa·s or less. Since the viscosity of white dextrin after a certain period of time after cooking is particularly low, even if it is combined with a pigment coating liquid, its viscosity will not increase significantly, and the fluidity of the coating liquid can be improved. Therefore, the concentration of the pigment coating liquid can be increased, thereby improving the printing quality of the coated paper. That is, since the penetration of the coating into the base paper can be suppressed and the effective coating layer can be increased, various qualities of the coated paper such as gloss expression, whiteness, and surface strength can be improved. The lower limit of the above viscosity is not limited, for example, it can be above 100Pa·s.
[0067] The amount of the above-mentioned adhesive in the upper layer, which is preferably a starch-based polymer compound (including dextrin, the same below), is preferably 20 parts by weight or less, 15 parts by weight or less, or 10 parts by weight or less relative to 100 parts by weight of the pigment of the layer. Its lower limit can be 0.01 parts by weight or more, preferably 3 parts by weight or more, or 5 parts by weight or more relative to 100 parts by weight of the above-mentioned pigment. The amount of the above-mentioned adhesive in the lower layer, which is preferably the amount of the above-mentioned starch-based polymer compound, is preferably 55 parts by weight or less, 50 parts by weight or less, or 30 parts by weight or less relative to 100 parts by weight of the pigment of the layer. Its lower limit is preferably 10 parts by weight or more, or 15 parts by weight or more relative to 100 parts by weight of the above-mentioned pigment.
[0068] It is also possible to use starch-based polymers together with adhesives that have been used for coated paper. In this case, the total adhesive content of the upper and lower layers is appropriately adjusted so that the amount of starch-based polymers in the total adhesive of each layer is 90% by weight or more. Examples of adhesives other than starch-based polymers include natural adhesives. As natural adhesives, proteins such as casein, soy protein, and synthetic protein can be cited; or cellulose derivatives such as carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxymethyl cellulose can be cited. In addition, synthetic adhesives can also be used. As synthetic adhesives, various copolymers such as ethylene-vinyl acetate, butadiene-methyl methacrylate, and vinyl acetate-butyl acrylate, polyvinyl alcohol, maleic anhydride copolymers, and acrylic acid-methyl methacrylate copolymers are included, which are common adhesives for coated paper. Among them, from the perspective of environmental load, it is preferred not to use synthetic adhesives as much as possible.
[0069] The pigment coating layer of the coated paper contains a water-soluble starch-based polymer compound as a hydrophobic and chemically synthesized synthetic adhesive, preferably without a styrene-based copolymer. Therefore, when recycled, the pigment coating layer also has the characteristics of being easily soluble in water and easy to dissociate. In recent years, due to the transition to a recycling-oriented society, recycling waste paper to make recycled paper has become popular, and the demand for easily dissociated waste paper is very high. The so-called easy dissociation of waste paper means that the power consumption of the pulper during dissociation can be suppressed or the use of dissociation chemicals can be suppressed, thereby saving resources. In addition, since the coated paper does not contain a styrene-based copolymer as a synthetic adhesive, the wastewater after dissociation does not contain chemical substances, and the environmental load is also low.
[0070] [pigment]
[0071] In the present invention, unless otherwise specified, "pigment" means "white pigment". There is no particular limitation on the pigment, and pigments that have been used for coated paper can be used. As examples thereof, inorganic pigments such as kaolin, clay, engineered kaolin, coated clay, calcium carbonate (e.g., heavy calcium carbonate, light calcium carbonate), talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, satin white, and organic pigments of dense type, hollow type, or core-shell type, and combinations thereof can be cited. However, if environmental load is considered, it is preferred not to use organic pigments as much as possible. In addition, as the type of pigment, heavy calcium carbonate and light calcium carbonate are preferred from the viewpoint of requiring a small amount of adhesive and being able to use a small amount of adhesive to improve surface strength and high whiteness. Furthermore, from the viewpoint of also improving transparency, light calcium carbonate with consistent particle size and shape can also be used. The fluffy coating layer structure is to scatter light efficiently.
[0072] When calcium carbonate is added to the coating liquid, the content of light calcium carbonate or heavy calcium carbonate or the combination of the two is preferably 50 parts by weight or more per 100 parts by weight of pigment, more preferably 70 parts by weight or more, further preferably 80 parts by weight or more, and particularly preferably 100 parts by weight. In addition, from the viewpoint of uniformly forming a coating layer on the base paper, the average particle size is preferably 0.2 to 5 μm, more preferably 0.2 to 3 μm. The average particle size is measured using a laser diffraction particle size distribution measuring device such as Mastersizer S manufactured by Malvern, and is defined as D50. In addition, when the pigment coating layer is two layers, the average particle size of the calcium carbonate contained in each layer preferably satisfies the relationship of (particle size of calcium carbonate contained in the upper layer) < (particle size of calcium carbonate contained in the lower layer). By reducing the particle size of the calcium carbonate contained in the upper layer, a coated paper with high white paper gloss can be obtained, and by increasing the particle size of the calcium carbonate contained in the lower layer, a coated paper with high surface strength can be obtained. The particle size of calcium carbonate is preferably 0.5 to 1.0 μm in the upper layer and preferably 1.0 to 2.0 μm in the lower layer.
[0073] As pigment, plate-like inorganic filler materials such as kaolin can be included. Since the pigment is plate-like, the light is reflected specularly and the glossiness of white paper is improved. Relative to 100 parts by weight of the pigment in the coating layer, it is preferably more than 1 part by weight. Its upper limit is not limited, and it is preferably less than 60 parts by weight. In addition, when there are more than two layers of pigment coating layers, the upper layer with a large impact on the glossiness of white paper preferably contains a plate-like inorganic filler. However, the adhesive requirement of the plate-like inorganic filler is very high, and when it is too much, the surface strength of the coated paper may be reduced. From such a viewpoint, the content of the plate-like inorganic filler is preferably less than 15 parts by weight, and more preferably less than 5 parts by weight, relative to 100 parts by weight of the pigment in the upper layer.
[0074] [Other ingredients]
[0075] In the present invention, various auxiliary agents usually blended in pigments for coated paper, such as a dispersant, a thickener, a water-retaining agent, a defoaming agent, a water-proofing agent, and a coloring agent, can be appropriately used as necessary.
[0076] (2) Base paper
[0077] Coated paper has at least a base paper layer. Base paper can be manufactured by a known method, for example, the papermaking raw material (paper stock) can be made into paper in a mesh section, and then supplied to a press section and a pre-drying section to manufacture base paper. The base paper can be a single-layer papermaking or a multi-layer papermaking, but in the case of manufacturing white paper, a multi-layer papermaking base paper is preferably used. The method for making base paper is not particularly limited, and known raw materials can be used by known methods. The base paper used in the present invention is not particularly limited, and generally used high-grade paper, medium-grade paper, groundwood paper, machine-coated paper, coated paper, cast-coated paper, synthetic paper, resin printing paper, plastic film, etc. can be used without exception.
[0078] The weight per unit area of the base paper is not particularly limited and can be appropriately selected according to the application, for example, it can be 35 to 580 g / m 2 When used as a coated paper for printing, for example, it can also be 40 to 100 g / m 2 .
[0079] [Raw material pulp]
[0080] As the pulp raw material used in base paper, chemical pulp can be used. In addition to chemical pulp, various pulps can be used according to the purpose, such as deinked pulp (DIP), groundwood pulp (GP), refiner groundwood pulp (RGP), thermomechanical pulp (TMP), thermomechanical pulp (CTMP), chemical grinding pulp (CGP), semi-chemical pulp (SCP), etc. As deinked pulp, deinked pulp made of classified waste paper such as high-grade paper, medium-grade paper, low-grade paper, newspapers, leaflets, magazines, and unclassified waste paper mixed with these can be used.
[0081] [filler]
[0082] As fillers for base paper, known fillers can be used arbitrarily, for example, heavy calcium carbonate, light calcium carbonate, clay, silicon dioxide, light calcium carbonate-silicon dioxide composite, kaolin, calcined kaolin, coated kaolin, white carbon, talc, magnesium carbonate, barium carbonate, barium sulfate, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, zinc oxide, titanium oxide, inorganic fillers such as amorphous silica produced by neutralization of minerals based on sodium silicate, urea-formalin resin, melamine resin, polystyrene resin, phenolic resin, etc. organic fillers. Among them, heavy calcium carbonate and light calcium carbonate, which are representative fillers in neutral papermaking and alkaline papermaking, are also preferably used to improve opacity. The filler rate in paper is not particularly limited, preferably 1 to 40% by weight of solid content, and more preferably 10 to 35% by weight of solid content.
[0083] [Handling of base paper]
[0084] In order to make the coating layer uniform after coating, it is preferred to pre-calender the base paper before coating using an online soft calender, online cold calender, etc., and smooth the base paper in advance. In this case, the treatment line pressure is preferably 30 to 100 kN / m, more preferably 50 to 100 kN / m. In addition, the moisture content of the base paper during the pre-calendering treatment is also important, and the moisture content is preferably 3 to 5%.
[0085] [additive]
[0086] Known papermaking additives can be used in the base paper. For example, aluminum sulfate, various anionic, cationic, nonionic or amphoteric yield improvers, filterability improvers, various paper strength enhancers, internal sizing agents and other papermaking internal additives can be used as needed. As dry paper strength enhancers, polyacrylamide and cationic starch can be mentioned, and as wet paper strength enhancers, polyamide epichlorohydrin and the like can be mentioned. These chemical reagents are added within the range that does not affect the texture, operability, etc. As neutral sizing agents, alkyl ketene dimers, alkenyl succinic anhydrides, neutral rosin sizing agents, etc. can be mentioned. Furthermore, dyes, fluorescent whitening agents, pH adjusters, defoamers, resin control agents, slime control agents, etc. can be added as needed.
[0087] [Papermaking]
[0088] The papermaking method of the base paper is not particularly limited, and can be carried out using a fourdrinier papermaking machine including a top wire, an on top former, a net former, a cylinder papermaking machine, a paperboard papermaking machine using a fourdrinier papermaking machine and a cylinder papermaking machine, a Yankee dryer papermaking machine, etc. The pH during papermaking can be any of acidic, neutral, and alkaline, preferably neutral or alkaline. The papermaking speed is not particularly limited.
[0089] (3) Transparent coating layer, etc.
[0090] A coating liquid without pigment can be applied to one or both sides of the base paper to form a clear coating layer. By applying a clear coating on the base paper, the surface strength and smoothness of the base paper can be improved, and the coating property of the pigment can be improved. The clear coating layer can also contain a polymer compound derived from the above-mentioned starch as a binder. The amount of the clear coating is preferably 0.1 to 4.0 g / m per single side in terms of solid content. 2 , more preferably 0.5 to 2.5 g / m 2 .
[0091] Transparent coating refers to coating (size pressing) a coating liquid (surface treatment liquid) mainly composed of various starches such as starch, oxidized starch, polyacrylamide, polyvinyl alcohol and other water-soluble polymers on the base paper using a coating machine (coating machine) such as a size press, a gate roll coater, a pre-metered size press, a curtain coater, a sprayer, etc.
[0092] 2. Characteristics of coated paper, etc.
[0093] [Styrene content]
[0094] As described above, the above-mentioned two pigment coating layers in the coated paper preferably do not contain styrene copolymers, and in a more preferred embodiment do not contain synthetic adhesives. The content of styrene contained in 1 mg of coated paper is preferably 0.5 μg or less. The content of styrene is an indicator of the content of styrene copolymers, and further an indicator of synthetic adhesives. The styrene content in this range means that the pigment coating layer does not contain styrene copolymers as adhesives. Originally, the styrene content is preferably 0g. However, considering the possibility of unintentional mixing of styrene from waste paper or other papermaking chemicals used as raw material pulp, it is preferred that the above-mentioned styrene content is 0.5 μg or less. Styrene copolymers refer to copolymers having styrene polymerization units. As an example thereof, styrene butadiene latex of copolymers of monomers copolymerizable with styrene can be cited. This latex is a representative adhesive for papermaking. In addition, in one embodiment, the styrene copolymer contains a styrene homopolymer.
[0095] The content of styrene contained in 1 mg of coated paper can be measured as follows.
[0096] 0.5 to 1 mg of coated paper was cut out and the amount of styrene was measured by instantaneous thermal decomposition using GC-MS to determine the content of styrene contained in 1 mg of coated paper. At this time, polystyrene (LX303A manufactured by Zeon Co., Ltd., Japan) was used as a standard sample. An example of the device used is shown below.
[0097] Device used:
[0098] Thermal decomposition furnace: PY-2020iD manufactured by Frontier Labs
[0099] GC: 6890N manufactured by Agilent Technologies
[0100] Column used: DV-1 (30m×0.25mm, film thickness 1μm)
[0101] MASS: JEOL JMS-AX505HA
[0102] GC usage conditions:
[0103] Thermal decomposition furnace
[0104] The sample was thermally decomposed at 550℃
[0105] GC injection temperature 280℃
[0106] GC
[0107] 40℃ for 5 minutes
[0108] Heat up to 90°C at 5°C / min
[0109] Heat up to 240℃ at 20℃ / min
[0110] Raise the temperature to 280°C at 5°C / min
[0111] Hold for 5 minutes
[0112] Mass Interface 260℃
[0113] Device used:
[0114] Pyrolysis furnace: Frontier Lab PY-3030D
[0115] GC: 7890A manufactured by Agilent Technologies
[0116] Column used: DB-1 manufactured by Agilent Technologies, 30 m × 0.25 mm, film thickness 1 μm
[0117] MS: 5975C manufactured by Agilent Technologies
[0118] [Contact angle]
[0119] The contact angle of coated paper is measured 0.1 seconds after distilled water is dropped onto the surface of the coated paper. The drop amount is preferably 5 μL. The contact angle can be measured using a contact angle measuring device (DAT1100 manufactured by FIBRO System AB) using coated paper pretreated under the standard conditions specified in JIS-P8111 as a test object. The value of the contact angle is preferably 75° or less. The lower limit is set to 10° or more. If in contact with a liquid, the paper absorbs the liquid. The contact angle of paper relative to a liquid is an indicator of the degree of penetration of the liquid into the paper. In the present invention, in the case of double-sided coating, the contact angles of one surface and the other surface of the coated paper are measured separately, and the contact angle is defined as the average value thereof.
[0120] For coated paper, since the pigment coating layer does not contain styrene copolymer as a synthetic binder, the wet strength of the coated paper is reduced, and it is easy to cause accumulation during printing. Therefore, in order to suppress water absorption, the contact angle of the coated paper is adjusted. By controlling the contact angle of the coated paper, the surface strength can be adjusted to an appropriate state to prevent accumulation.
[0121] As a method for adjusting the contact angle, for example, adjusting the surface roughness of the coated paper to suppress water absorption, coating the base paper with a material that delays or prevents water absorption or penetration into the paper, etc. Among them, it is preferred to add the above-mentioned agent. The agent is preferably added to the outermost pigment coating layer.
[0122] Examples of the above-mentioned agents include various sizing agents, paper strengthening agents such as polyacrylamide and modified polyacrylamide, zirconium carbonate, etc. Among them, alkyl ketene dimer, wax, polyamine / amide resin, and polyacrylamide polymer are preferred.
[0123] Alkyl ketene dimer is used as a neutral sizing agent in the papermaking industry and is produced by dimerization of alkyl ketene with a hydrophobic long-chain alkyl group attached to the ketene. Alkyl ketene dimer can be in wax or emulsion form.
[0124] Examples of wax include paraffin wax. Paraffin wax is obtained by fractionation of petroleum and is mainly a mixture of normal alkanes with carbon atoms of 20 or more. Since it is insoluble in water, it has excellent moisture resistance, isotropic properties, and water repellency.
[0125] Polyamine / amide resin refers to polyamine resin, polyamide resin or both. Specifically, polyamine resin, polyamide resin, modified polyamine resin, modified polyamide resin, polyamide urea resin, polyalkylene polyamine resin, polyalkylene polyamide resin, polyamine polyurea resin, modified polyamine resin, modified polyamide resin, polyalkylene polyamine urea formalin resin, polyalkylene polyamine polyamide polyurea resin, etc. can be cited.
[0126] The polyacrylamide-based polymer refers to a polymer obtained by polymerizing acrylamide, or a copolymer obtained by polymerizing acrylamide and other monomers polymerizable with acrylamide, such as acrylic acid.
[0127] These agents are preferably added to the pigment coating layer. It is particularly preferred to add them to the outermost pigment coating layer. The amount added to the coating layer is 0.05 to 1.0 parts by weight, preferably 0.1 to 0.5 parts by weight, relative to 100 parts by weight of the pigment. If the amount added is more than 1.0 parts by weight, the contact angle is large, that is, water absorption does not occur and the ink is emulsified, and in multi-color printing, the ink adhesion of the rear part deteriorates. In addition, the viscosity of the coating becomes significantly thicker, and the coating operability becomes worse. On the other hand, if the amount added is less than 0.05 parts by weight, the contact angle is very small, that is, the effect of fully suppressing water absorption cannot be obtained, the wet strength of the coated paper decreases, and accumulation is likely to occur during printing.
[0128] [Ash content in paper]
[0129] The ash content of the coated paper is preferably 10% by weight or more, more preferably 30% by weight or more. In particular, when the coated paper is used as a coated printing paper, it is preferred to increase the ash content to increase the opacity.
[0130] [Surface treatment]
[0131] The coated paper can be surface treated as needed. Conventional smoothing treatment devices such as super calender, gloss calender, soft calender, hot calender, suction cup calender, etc. can be used for the smoothing treatment. The smoothing treatment device can be used on or off the machine as appropriate, and the shape of the pressurizing device, the number of pressurizing zones, heating, etc. can also be appropriately adjusted. In a preferred embodiment, the coated paper can be surface treated with a calender such as a super calender, a high-temperature soft zone calender, etc. The surface treatment can improve the smoothness and glossiness of the coated paper. In the present invention, soft zone calendering treatment is preferred. By performing soft zone calendering treatment, whiteness and opacity can be improved at the same time. In the soft zone calendering treatment, the surface temperature of the metal roller is 20°C to 60°C, and the linear pressure is 30 to 60 kN / m, more preferably 40 to 60 kN / m. In addition, if the surface temperature of the metal roll is 40°C to 250°C, the linear pressure is 60 to 400 kN / m, preferably 150 to 300 kN / m, and more preferably 100 to 350 kN / m. If the temperature is increased, the gloss and smoothness of the surface of the coated paper will increase.
[0132] [Taking into account both surface strength and white paper gloss]
[0133] If the amount of synthetic adhesive in the pigment coating layer is reduced, the quality of the coated paper may be reduced, such as the surface strength of the coated paper. In particular, since coated paper and light coated paper have high quality requirements, it is not easy to reduce the amount of synthetic adhesive. In addition, if synthetic adhesives are not used, in addition to the above problems, there is also a tendency to easily produce blanket piling during offset printing. Felt piling refers to the accumulation and bulging of paper powder and ink around the drawing line on the felt. As a countermeasure to these, it is considered to replace synthetic adhesives with natural adhesives in high proportions, but if natural materials are used in high proportions, the viscosity of the coating will increase significantly, and the operability and coating adaptability will deteriorate. Therefore, it is also considered to dilute the coating to achieve low viscosity, but due to the increase in water content, the load of the drying process after coating becomes large, resulting in adverse effects on productivity such as reduced coating speed. In addition, even if the coating speed is reduced for manufacturing, the water retention of the coating decreases due to the low coating concentration, and the coating penetrates into the base paper more, which cannot avoid the quality reduction such as the reduction of white paper gloss and surface strength. Therefore, the adhesive has a great influence on the operability, coating adaptability, and coated paper quality. In the quality of coated paper, the surface strength and the white paper gloss are greatly affected by the adhesive, and further, the two show opposite behaviors in terms of the increase or decrease of the adhesive. That is, if the adhesive is increased, the surface strength increases, and on the other hand, the white paper gloss decreases. Conversely, if the adhesive is reduced, the white paper gloss increases, and on the other hand, the surface strength decreases. Therefore, in coated paper requiring high surface strength and white paper gloss, and in coated paper with two layers of pigment coating layers on each single side on the coated base paper, it is difficult to achieve both. However, in the present invention, as described above, by using a specific adhesive and setting the amount of adhesive in each layer to a specific range, it is achieved to achieve both excellent surface strength and white paper gloss. The glossiness of white paper is preferably 40 to 80%, more preferably 45 to 70%, and even more preferably 45 to 55%.
[0134] 4. Manufacturing method
[0135] Coated paper can be manufactured by any method within the scope of not impairing the effect of the invention. Coated paper can be manufactured by a manufacturing method having the following steps, for example, 1) a step of preparing base paper; 2) a step of setting a pigment coating layer (lower layer) on one side or both sides of the base paper; 3) a step of setting a pigment coating layer (upper layer) on the above-mentioned lower layer. The steps 2) and 3) can also be implemented at one time using a multi-layer pigment coating liquid. In addition, as mentioned above, the above-mentioned manufacturing method can also include a step of setting a transparent coating layer and a surface treatment step. Each step can be implemented as a known method. The pigment coating step is described below.
[0136] In the pigment coating process, a commonly used coating machine can be used. As such a coating machine, an on-machine coating machine and an off-machine coating machine can be cited. As the on-machine coating machine, a coating machine such as a size press coater, a gate roll coater, a roller coater such as a bar metering size press coater, a bill blade coater, a blade metering size press coater, a short-stay blade coater, a melt-spraying blade coater, etc. can be used. The coating speed is not particularly limited, but in the current technology, the blade coater is preferably 500 to 1800 m / min, and the size press coater is preferably 500 to 2000 m / min.
[0137] The method for drying the wet coating layer is not limited, and various methods such as a steam superheated drum, a heated hot air dryer, a gas heater dryer, an electric heater dryer, and an infrared heater dryer may be used alone or in combination.
[0138] The coating amount of the coating liquid can be appropriately selected according to the application. Generally, the coating amount is 5 to 20 g / m2 in terms of solid content per single side. 2 The solid content concentration of the pigment coating liquid is not particularly limited, but is preferably about 50 to 75% by weight in consideration of printing quality. In addition, the viscosity of the pigment coating liquid is preferably about 2000 mPa·s to 3000 mPa·s in consideration of operability and the like.
[0139] Example
[0140] [Example 1]
[0141] Light calcium carbonate as a filler was added to a pulp slurry consisting of 50 parts by weight of waste paper pulp, 20 parts by weight of NBKP, and 30 parts by weight of LBKP so that the ash content in the paper was 15% by weight, and 3 parts by weight of cationic starch as an internal paper strength agent was added to prepare paper stock. Intermediate base paper was manufactured from the paper stock according to a general method.
[0142] Calcium carbonate as shown in Table 1 as a pigment, white dextrin (RVA viscosity 200-1000 mPa·s, weight average molecular weight 150,000-200,000) as a binder, and water were mixed to prepare an upper layer pigment coating liquid and a lower layer pigment coating liquid having a solid content concentration of 60% by weight. The mixing amount of white dextrin was 15.5 parts by weight in the upper layer pigment coating liquid and 16.2 parts by weight in the lower layer pigment coating liquid relative to 100 parts by weight of calcium carbonate.
[0143] This coating liquid was used so that the single-side coating amount was 20.0 g / m2 for the lower layer. 2 , Upper layer 17.8g / m 2 The coating was carried out by a melt spraying knife coater and dried. The coating speed was 900 m / min.
[0144] Next, in the processing step, the coated paper was surface treated using a two-roller, four-pile soft calender having an elastic roll with a Shore hardness of D90°. The conditions were as follows.
[0145] Each metal roller: 100°C
[0146] Linear pressure of each pressing area: 100kN / m
[0147] Calendering speed: 300m / min
[0148] [Example 2]
[0149] A coated paper was produced in the same manner as in Example 1 except that the white dextrin was blended as a binder in an amount of 12.2 parts by weight of the upper coating layer and 16.2 parts by weight of the lower coating layer.
[0150] [Example 3]
[0151] A coated paper was produced in the same manner as in Example 1 except that the white dextrin was blended as a binder in an amount of 8.9 parts by weight for the upper coating layer and 16.2 parts by weight for the lower coating layer.
[0152] [Comparative Example 1]
[0153] A coated paper was produced in the same manner as in Example 1 except that the adhesive to be blended in the coating layer was changed as follows.
[0154] Upper layer: 6.6 parts by weight of styrene-butadiene copolymer latex and 2.3 parts by weight of acetylated tapioca starch were blended.
[0155] Lower layer: 2.0 parts by weight of styrene-butadiene copolymer latex and 10.2 parts by weight of acetylated tapioca starch were blended.
[0156] These results are shown in Table 1. As can be seen from this table, the coated papers obtained in Examples have excellent balance in printing surface strength and printing glossiness.
[0157] [Example 4]
[0158] Calcium carbonate as a pigment shown in Table 2, white dextrin (RVA viscosity 200-1000 mPa·s, weight average molecular weight 150,000-200,000) as a binder, and acid-treated starch were mixed with water to prepare an upper layer pigment coating liquid having a solid content concentration of 68% by weight and a lower layer pigment coating liquid having a solid content concentration of 50% by weight. The mixing amounts of white dextrin and acid-treated starch were 2.5 parts by weight and 2.5 parts by weight in the upper layer pigment coating liquid and 22.5 parts by weight and 22.5 parts by weight in the lower layer pigment coating liquid, respectively, based on 100 parts by weight of calcium carbonate.
[0159] The same base paper as that used in Example 1 was prepared, and the base paper was coated on both sides with the coating liquid using a gate roll coater (circumferential speed ratio 60%) for the lower layer and a knife coater using a melt-blowing method for the upper layer, and then dried. The coating amount in the lower layer was 3.3 g / m 2 , in the upper layer is 8.1g / m 2 The coating speed was 900 m / min. Next, the obtained paper was surface treated in the same manner as in Example 1 to obtain coated paper for printing.
[0160] [Example 5]
[0161] A coated paper was produced in the same manner as in Example 4 except that the amount of white dextrin in the upper layer was 2.75 parts by weight and the amount of starch was 2.75 parts by weight.
[0162] [Example 6]
[0163] A coated paper was produced in the same manner as in Example 4 except that the amount of white dextrin in the upper layer was 3 parts by weight and the amount of starch was 3 parts by weight.
[0164] [Example 7]
[0165] The coated paper was manufactured in the same manner as in Example 4 except that the amount of white dextrin in the upper layer was set to 5 parts by weight, the amount of starch was set to 0 parts by weight, and the amount of white dextrin in the lower layer was set to 0 parts by weight, the amount of starch was set to 45 parts by weight.
[0166] [Comparative Example 2]
[0167] A coated paper was produced in the same manner as in Example 4 except that the adhesive to be blended in the coating layer was changed as follows.
[0168] Upper layer: 3.3 parts by weight of styrene-butadiene copolymer latex and 3.9 parts by weight of acid-treated starch were blended.
[0169] Lower layer: 2.8 parts by weight of styrene-butadiene copolymer latex and 22.0 parts by weight of acid-treated starch were blended.
[0170] These results are shown in the table. As can be seen from the table, the coated paper obtained in the examples has excellent balance in printing surface strength and printing glossiness.
[0171] [Table 1]
[0172]
[0173]
[0174] The evaluation method and the like are shown below.
[0175] 1) Weight per unit area, paper thickness, density: JIS P8124
[0176] 2) Ash content: JIS P 8251: 2003
[0177] 3) White paper glossiness: JIS P8142
[0178] 4) Wangyan smoothness: JIS P8115
[0179] 5) PPS roughness: PPS surface roughness measured according to ISO8791.
[0180] 6) Air permeability resistance: JIS P8117: 2009
[0181] 7) Anti-bubble property: Cut the paper into 9 cm in the flow direction and 8 cm in the width direction and adjust the humidity. Add silicone oil to the jacket heater (manufactured by Shin-Etsu Chemical Co., Ltd.), set the temperature appropriately and put the paper in. Pull out the paper 3 seconds after putting it in and check the bubbling. Lower the temperature gradually to 5-10°C and repeat the operation until no bubbling occurs. The higher the value, the better the anti-bubble property.
[0182] 8) ISO bending stiffness: ISO 2493
[0183] 9) Printing glossiness
[0184] Using an offset sheet-processing printing press (4 colors) manufactured by Roland Co., Ltd., using offset sheet-processing ink (NEX-M manufactured by Toyo Ink Co., Ltd.), printing was performed in the order of cyan, magenta, yellow, and black (CMYK) at a printing speed of 8000 sheets / hr, with the ink concentration of the single-color portion being 1.60 for cyan, 1.50 for magenta, 1.10 for yellow, and 1.80 for black. The glossiness of the blue (C) single-color printed portion of the obtained printed product was measured in accordance with JIS P-8142.
[0185] 10) Ink concentration
[0186] Using an offset sheet-processing printing press (4 colors) manufactured by Roland, using an offset sheet-processing ink (NEX-M manufactured by Toyo Ink Co., Ltd.), printing was performed in the order of cyan, red, yellow, and black (CMYK) at a printing speed of 8000 sheets / hr, and the ink concentration of the single-color portion was 1.60 for cyan, 1.50 for red, 1.10 for yellow, and 1.80 for black. The ink concentration of the blue (C) single-color printed portion of the obtained print was measured using a spectrophotometer (SpectroEye, manufactured by X-rite).
[0187] 11) Paper picking evaluation (marked as picking up 10 sheets in the table)
[0188] A single-sheet offset printing press manufactured by Roland was used, and Leo Echo-Y blue manufactured by Toyo Ink Co., Ltd. was used as the ink to print a blue single color at a speed of 8000 sph. Evaluation was performed based on the occurrence of paper peeling (peeling) on the F side and the W side during printing of 10 sheets. Specifically, evaluation was performed based on the total number of paper peeling (peeling) in 10 samples. Therefore, the smaller the value, the better the resistance to paper peeling.
Claims
1. A coated paper having two pigment coating layers containing a pigment and an adhesive on at least one side of a base paper, More than 90% by weight of the total adhesive in each layer of the pigment coating layer is a starch-based polymer compound. At least one of the two layers contains dextrin as a binder.
2. A coated paper having two pigment coating layers containing a pigment and an adhesive on at least one side of a base paper, More than 90% by weight of the total adhesive in each layer of the pigment coating layer is a starch-based polymer compound. When the amount of the adhesive in the lower layer of the two layers is L and the amount of the adhesive in the upper layer is U, L>U.
3. The coated paper according to claim 1 or 2, wherein: The glossiness of white paper is 40-80%.
4. The coated paper according to claim 1 or 2, wherein: The content of the adhesive in the upper layer is 20 parts by weight or less relative to 100 parts by weight of the pigment in the layer. The content of the binder in the lower layer is 55 parts by weight or less based on 100 parts by weight of the pigment in the layer.
5. The coated paper according to claim 1 or 2, wherein: The dextrin is white dextrin and has the following two characteristics: 1) The weight average molecular weight is 100,000 to 500,000, 2) After steaming at a concentration of 35 wt% for 16 minutes, the RVA viscosity at 50°C is 1000 mPa·s or less.
6. The coated paper according to claim 1 or 2, wherein: Satisfy any one or both of the following characteristics: i) when 1 mg of the coated paper is measured by instantaneous thermal decomposition method, the content of styrene is less than 0.5 μg, ii) After distilled water is dropped onto the coated paper and 0.1 seconds have passed, the contact angle is 75° or less.
7. The coated paper according to claim 1 or 2, wherein: The pigment in the pigment coating layer is composed of calcium carbonate.
Citation Information
Patent Citations
Coated paper for printing
JP2006132024A
Coated paper for printing
JP2006188783A
Multilayer-coated bulky coated paper
JP2009270211A
Coated paper and its manufacturing method
JP2014080715A