Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal display element
The polymer synthesized by specific tetracarboxylic acids and diamines is solved by imidation reactions and diamines to block the closed-loop reaction, which solves the charge accumulation and scintillation problems in liquid crystal display elements and improves the display quality.
Patent Information
- Application Number
- CN202380036389.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-21
- Publication Date
- 2024-12-06
AI Technical Summary
In the high-brightness liquid crystal display element, the accumulated charge caused by the backlight increases, resulting in improved visual confirmation of the afterimage, and the liquid crystal aligning film in the transverse electric field is difficult to reduce the charge accumulation and flicker problems in a short time.
The polymer synthesized with specific tetracarboxylic acid components and diamine components is used as liquid crystal alignment agents to form an imide ring through imidation reaction, reducing charge accumulation, and hindering the closed-loop reaction through the presence of diamines, thereby reducing charge.
The absolute value of accumulated charge is effectively reduced, the charge accumulation and flicker caused by backlight is reduced, and the display quality of the liquid crystal display element is improved.
Smart Images

Figure CN119096187A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a liquid crystal alignment agent, a liquid crystal alignment film and a liquid crystal display element. Background Art
[0002] Liquid crystal display elements are widely used as display parts of personal computers, mobile phones, smart phones, televisions, etc. Liquid crystal display elements, for example, have: a liquid crystal layer, sandwiched between an element substrate and a color filter substrate; pixel electrodes and common electrodes, applying an electric field to the liquid crystal layer; an orientation film, controlling the liquid crystal orientation of liquid crystal molecules in the liquid crystal layer; a thin film transistor (TFT: Thin Film Transistor), switching the electrical signal supplied to the pixel electrode; etc. As a driving method for liquid crystal molecules, longitudinal electric field methods such as TN (Twisted Nematic) method and VA (Vertical Alignment) method are known; transverse electric field methods such as IPS (In-Plane Switching) method and FFS (Frindge Field Switching) method are known. In the transverse electric field method in which electrodes are formed only on one side of the substrate and an electric field is applied in a direction parallel to the substrate, it is known that it has a wide viewing angle characteristic compared to the conventional longitudinal electric field method in which voltage is applied to electrodes formed on the upper and lower substrates to drive the liquid crystal, and a liquid crystal display element that can display a high-quality level.
[0003] In the case of a lateral electric field liquid crystal cell, static electricity is easily accumulated in the liquid crystal cell. Due to the application of positive and negative asymmetric voltages generated by driving, charges are accumulated in the liquid crystal cell. These accumulated charges affect the display in the form of disordered liquid crystal orientation and residual images, significantly reducing the display quality level of the liquid crystal element. In addition, since the backlight is irradiated to the liquid crystal cell just after driving, charges are accumulated, so residual images are generated even if driving for a short time. In addition, flickering (flicker) and other problems occur during driving.
[0004] As a liquid crystal aligning agent for a liquid crystal cell of a transverse electric field system, Patent Document 1 discloses a liquid crystal aligning agent containing a polymer obtained by polycondensing an aromatic diamine having an alkylated terminal amino group and a specific alicyclic tetracarboxylic dianhydride.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-101196 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In recent high-brightness liquid crystal display elements, the brightness of the backlight becomes higher, and the visual confirmation of the residual image generated by the accumulated charge also becomes higher, so it is necessary to reduce the absolute value of the accumulated charge and reduce the generated charge in a short time. In addition, it is more necessary than before to reduce the charge accumulation and flicker caused by the backlight.
[0010] The present inventors have studied and found that, when a polymer obtained by polycondensing an aromatic diamine having an alkylated terminal amino group and an alicyclic tetracarboxylic dianhydride is used for a liquid crystal aligning agent, a liquid crystal aligning agent that fully satisfies the above-mentioned requirements cannot be obtained.
[0011] In view of the above circumstances, an object of the present invention is to provide a liquid crystal alignment agent that can reduce the absolute value of accumulated charges and reduce the generated charges in a short time to obtain a liquid crystal alignment film; and a liquid crystal alignment film that reduces charge accumulation and flickering caused by backlight.
[0012] Solutions for solving problems
[0013] The present inventors have repeatedly conducted various studies to achieve the above-mentioned purpose, and found that the use of a specific tetracarboxylic acid component and a specific diamine component is effective in achieving the above-mentioned purpose. In addition, the present inventors found that a liquid crystal aligning agent based on the following structure is the best for achieving the above-mentioned purpose, thereby completing the present invention.
[0014] Thus, the present invention is based on the above findings and has the following gist.
[0015] A liquid crystal alignment agent, comprising a polymer (P), wherein the polymer (P) is at least one selected from the group consisting of a polyimide precursor obtained by using the following tetracarboxylic acid component and the following diamine component and a polyimide which is an imide product of the polyimide precursor, wherein the tetracarboxylic acid component comprises at least one selected from the group consisting of tetracarboxylic dianhydride represented by the following formula (1) and its derivatives, and the diamine component comprises a diamine represented by the following formula (2).
[0016]
[0017] (X a It represents a tetravalent organic group derived from aromatic tetracarboxylic dianhydride or a derivative thereof. Y2 represents a divalent organic group having 6 to 30 carbon atoms containing one or more aromatic groups. Z2 each independently represents an alkylene group having 1 to 6 carbon atoms. A2 each independently represents an alkyl group having 1 to 6 carbon atoms. Any hydrogen atom of the aromatic group in Y2 is optionally substituted by a monovalent group. ) It should be noted that, in the entire specification, halogen atoms include: fluorine atom, chlorine atom, bromine atom, iodine atom, etc., and * represents a bonding bond.
[0018] Effects of the Invention
[0019] By using the liquid crystal aligning agent of the present invention, it is possible to obtain a liquid crystal aligning film that can reduce the absolute value of the accumulated charge and reduce the generated charge in a short time, and a liquid crystal aligning film that can reduce the charge accumulation and flicker caused by the backlight.
[0020] The mechanism by which the above-mentioned effects of the present invention are obtained is not necessarily clear, but the following is considered to be one of the causes.
[0021] In the firing process of liquid crystal display element production, the polyamic acid as the main component of the liquid crystal aligning agent undergoes thermal imidization reaction. It is a reaction to form an imide ring by heating, and the lower its ratio (imidization rate), the higher the polarity, so it is easy to reduce the charge. It can be considered that in the present invention, due to the presence of A2 of the above-mentioned diamine (2), the ring-closure reaction is hindered, so it is also easy to reduce the charge in normal firing. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic cross-sectional view showing an example of a lateral electric field liquid crystal display element of the present invention.
[0023] Figure 2 This is a schematic cross-sectional view showing another example of the lateral electric field liquid crystal display element of the present invention. DETAILED DESCRIPTION
[0024] <Polymer (P)>
[0025] The liquid crystal aligning agent of the present invention contains a polymer (P), which is at least one selected from the group consisting of a polyimide precursor obtained by using the following tetracarboxylic acid component and the following diamine component and a polyimide as an imide of the polyimide precursor, wherein the tetracarboxylic acid component contains at least one selected from the group consisting of tetracarboxylic dianhydride and its derivatives represented by the above formula (1) (also referred to as a specific aromatic tetracarboxylic acid component (p) in the present invention), and the diamine component contains a diamine represented by the above formula (2) (also referred to as a specific diamine (p) in the present invention). The polymer (P) may be one or more than two.
[0026] Here, the polyimide precursor is a polymer such as polyamic acid and polyamic acid ester which can obtain a polyimide by imidization.
[0027] (Tetracarboxylic acid component)
[0028] The polyamic acid (P′) as the polyimide precursor of the polymer (P) can be obtained, for example, by a polymerization reaction of a diamine component containing the above-mentioned specific diamine (p) and tetracarboxylic dianhydride represented by the above-mentioned formula (1).
[0029] When producing the polymer (P), the tetracarboxylic acid component to be reacted with the diamine component may be not only tetracarboxylic dianhydride but also derivatives of tetracarboxylic dianhydride such as tetracarboxylic acid, tetracarboxylic acid dihalide, tetracarboxylic acid dialkyl ester or tetracarboxylic acid dialkyl ester dihalide.
[0030] In the above formula (1), X a It represents a tetravalent organic group derived from aromatic tetracarboxylic dianhydride or a derivative thereof.
[0031] It should be noted that the aromatic tetracarboxylic dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups including at least one carboxyl group bonded to an aromatic ring, and need not be composed only of an aromatic ring structure, and may have a chain hydrocarbon structure or an alicyclic structure in part.
[0032] In the above formula (1), X a It is preferably a structure selected from the following formulae (Xa-1) and (Xa-2).
[0033]
[0034] (In formula (Xa-1) to (Xa-2), j and k are integers of 0 or 1, and A1 and A2 each independently represent a single bond, -O-, -C(=O)-, -O-C(=O)-, phenylene, -S(=O)2-, or -NR-C(=O)- (R represents a hydrogen atom or a methyl group). Multiple A2s may be the same or different.)
[0035] Preferred specific examples of the above formulae (Xa-1) and (Xa-2) include the following formulae (Xa-3) to (Xa-18).
[0036]
[0037] From the viewpoint of improving the liquid crystal orientation, X a More preferred are the above-mentioned formulas (Xa-3) to (Xa-7), and even more preferred are the above-mentioned formulas (Xa-3) to (Xa-6).
[0038] The usage ratio of the said specific aromatic tetracarboxylic acid component (p) is preferably 10 mol% or more, more preferably 20 mol% or more, and further preferably 50 mol% or more, based on 1 mol of all tetracarboxylic acid components used for polymer (P).
[0039] The tetracarboxylic acid component for producing the polymer (P) may contain tetracarboxylic acid components other than the above-mentioned specific aromatic tetracarboxylic acid component (p) (hereinafter, also referred to as other tetracarboxylic acid components).
[0040] When other tetracarboxylic acid components are used in combination in addition to the above-mentioned specific aromatic tetracarboxylic acid component (p), the usage-amount of the specific aromatic tetracarboxylic acid component (p) is preferably 90 mol% or less, more preferably 80 mol% or less, based on 1 mol of all tetracarboxylic acid components used for the polymer (P).
[0041] As the above-mentioned other tetracarboxylic acid components, non-cyclic aliphatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride or their derivatives can be listed. Here, non-cyclic aliphatic tetracarboxylic dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups bonded to a chain hydrocarbon structure. Among them, it is not necessary to be composed only of a chain hydrocarbon structure, and alicyclic structure or aromatic ring structure may be included in part thereof.
[0042] Alicyclic tetracarboxylic dianhydride is an acid dianhydride obtained by intramolecular dehydration of four carboxyl groups including at least one carboxyl group bonded to an alicyclic structure. Among them, none of these four carboxyl groups is bonded to an aromatic ring. In addition, it is not necessary to be composed only of an alicyclic structure, and a part of it may also have a chain hydrocarbon structure or an aromatic ring structure.
[0043] Among the above-mentioned non-cyclic aliphatic or alicyclic tetracarboxylic dianhydrides or their derivatives, from the viewpoint of improving the liquid crystal orientation, tetracarboxylic dianhydrides or their derivatives having at least one partial structure selected from the group consisting of a cyclobutane ring structure, a cyclopentane ring structure and a cyclohexane ring structure are preferred.
[0044] It is preferable that the said other tetracarboxylic acid component is tetracarboxylic dianhydride represented by following formula (t) or its derivative.
[0045]
[0046] In formula (t), X T It is a structure selected from the following formulae (X1-1) to (X1-23).
[0047]
[0048] In formulas (X1-1) to (X1-4), R1 to R 21 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms containing a fluorine atom, or a phenyl group. 21 Each independently is preferably a hydrogen atom, a halogen atom, a methyl group or an ethyl group, and more preferably a hydrogen atom or a methyl group.
[0049] Specific examples of the formula (X1-1) include the following formulas (1-1) to (1-6). From the viewpoint of improving the liquid crystal orientation, (1-1) to (1-2) are particularly preferred.
[0050]
[0051] From the viewpoint of improving the liquid crystal orientation, the above X T Preferred are the above-mentioned formulas (X1-1) to (X1-10) or (X1-18) to (X1-23), more preferred are the above-mentioned formulas (X1-1), (X1-5), (X1-7) to (X1-10), (X1-21) or (X1-23), and further preferred are the above-mentioned formulas (1-1), (1-2), (X1-5), (X1-7), (X1-8) or (X1-9).
[0052] (Specific diamine (p))
[0053] The specific diamine (p) of the present invention is a diamine represented by the above formula (2). The above specific diamine (p) may be used alone or in combination of two or more.
[0054] The usage-amount of the specific diamine (p) is preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 20 mol% or more, based on 1 mol of the diamine component for producing the polymer (P).
[0055] Y2 in the above formula (2) represents a divalent organic group having 6 to 30 carbon atoms and containing one or more aromatic groups. The above aromatic group refers to an aromatic hydrocarbon group or an aromatic heterocyclic group, including a monocyclic aromatic group, a condensed ring aromatic group, and an aromatic group connected to a monocyclic or condensed ring. Examples of the aromatic ring structure in the above aromatic group include a benzene ring, a naphthalene ring, a biphenyl structure, and the like. Any hydrogen atom of the above aromatic group may be optionally substituted with a monovalent group. Examples of the above monovalent group include a halogen atom, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, a fluoroalkenyl group having 2 to 10 carbon atoms, a fluoroalkoxy group having 1 to 10 carbon atoms, a carboxyl group, a hydroxyl group, an alkoxycarbonyl group having 1 to 10 carbon atoms, a cyano group, a nitro group, and the like.
[0056] Furthermore, Y2 and Z2 are preferably bonded via an atom constituting an aromatic ring, and more preferably bonded via a carbon atom constituting an aromatic ring.
[0057] It is more preferred that the polymer (P) has an aromatic group possessed by Y2 in the main chain direction of the polymer (P). The main chain of the polymer refers to the part consisting of the longest atomic chain in the polymer. Furthermore, "the polymer (P) has an aromatic group possessed by Y2 in the main chain direction of the polymer (P)" means that the aromatic group possessed by Y2 constitutes the main chain of the polymer (P).
[0058] When Y2 contains two or more aromatic groups, the aromatic ring structures in the aromatic groups may be bonded to each other via a linking group. Examples of the linking group include a single bond, -CH2-, -C(CH3)2-, -O-, -C(=O)-, -O-C(=O)-, -NR-C(=O)-, -NR- (R represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a phenyl group, or a tert-butyloxycarbonyl group), an alkylene group having 2 to 18 carbon atoms, or a divalent organic group in which a part of -CH2- of the alkylene group is substituted with -O-, -Si(CH3)2-, -C(=O)-, -O-C(=O)-, -NR-C(=O)-, -NR- (R represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a phenyl group, or a tert-butyloxycarbonyl group).
[0059] From the viewpoint of improving the liquid crystal orientation, Y2 is preferably a structure represented by the following formula (3).
[0060]
[0061] (L is -CH2-, -O-, -C(=O)-, -N(R)- (R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group), a cyclohexylene group or an alkylene group having 2 to 18 carbon atoms. Wherein, any -CH2- of the alkylene group is optionally substituted by -O-, -O-C(=O)-, -C(=O)-, -N(R)- (R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group), -N(R)-C(=O)- (R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group), a cyclohexylene group or a phenylene group. In addition, the hydrogen atoms on the phenylene group are optionally substituted by halogen atoms, or an alkyl group or alkoxy group having 1 to 5 carbon atoms.
[0062] R3 represents a halogen atom, or an alkyl group or alkoxy group having 1 to 5 carbon atoms, any hydrogen atom of the alkyl group or the alkoxy group is optionally substituted by a halogen atom, and any hydrocarbon group is optionally substituted by an amino group protected by a tert-butyloxycarbonyl group.
[0063] Multiple a's are each independently an integer of 0 to 4, b is an integer of 1 to 2, and c is an integer of 0 to 1. When multiple R3 and a's exist, they are optionally the same or different.
[0064] If more preferred specific examples of the above L are listed, they include: -O-, -O-C(=O)-, -C(=O)-, -N(R)- (R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group), -N(R)-C(=O)- (R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group), -N(R)-C(=O)-N(R)- (R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group. Two Rs may be the same or different), -(CH2) p -、-O-(CH2) p -O-, -(CH2) p -O-C(=O)-(CH2) q -, -(CH2) p -N(R)-(CH2) q -(R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group), -(CH2) p -N(R)-C(=O)-N(R)-(CH2) q -(R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group. Two Rs are optionally the same or different), -O-(CH2) p -O-(CH2) q -O-, -(CH2) p’ -O-C(=O)-(CH2) q -C(=O)-O-(CH2) r’ -, -(CH2) p’ -C(=O)-O-(CH2) q -O-C(=O)-(CH2) r’ -, -(CH2) p’ -O-C(=O)-Q-C(=O)-O-(CH2) q’ -(Q represents phenylene or cyclohexylene), -(CH2) p’ -C(=O)-O-Q-O-C(=O)-(CH2) q’ -(Q represents a phenylene group or a cyclohexylene group).
[0065] Here, p is an integer of 1 to 6, preferably an integer of 2 to 6. q is an integer of 1 to 6, more preferably an integer of 2 to 6, and even more preferably an integer of 2 to 4.
[0066] p', q', and r' are integers of 0 to 6. In addition, 0≤p'+q'≤10 and 2≤p'+q+r'≤16 are satisfied.
[0067] Z2 is independently an alkylene group having 1 to 6 carbon atoms. From the viewpoint of improving the liquid crystal orientation, it is preferably a methylene group or an ethylene group. A2 is an alkyl group having 1 to 6 carbon atoms. From the viewpoint of improving the liquid crystal orientation, A2 is preferably a methyl group or an ethyl group.
[0068] As a more preferable specific example of the diamine represented by the above-mentioned formula (2), the diamine represented by any of the following formulae (d2-1) to (d2-3) can be mentioned.
[0069]
[0070] The diamine component used to produce the polymer (P) may contain diamines other than the specific diamine (p) (hereinafter, also referred to as other diamines). When other diamines are used in addition to the specific diamine (p), the amount of the specific diamine (p) used relative to the diamine component is preferably 90 mol% or less, more preferably 80 mol% or less, relative to 1 mol of the diamine component used to produce the polymer (P).
[0071] Examples of other diamines are given below, but are not limited thereto. The above other diamines may be used alone or in combination of two or more.
[0072] p-phenylenediamine, m-phenylenediamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,5-dimethyl-p-phenylenediamine, 2,4-dimethyl-m-phenylenediamine, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diamino biphenyl, 2,2'-difluoro-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 4,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,2'-diaminobiphenyl, 2,3'-diaminobiphenyl, the following formula (d AL -1)~(d AL-9), 1,7-bis(4-aminophenoxy)heptane, 1,7-bis(3-aminophenoxy)heptane, 1,8-bis(4-aminophenoxy)octane, 1,8-bis(3-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,9-bis(3-aminophenoxy)nonane, 1,10-bis(4-aminophenoxy)decane, 1,10-bis(3-aminophenoxy)decane, 1,11-bis(4-aminophenoxy)undecane, 1,11-bis(3-aminophenoxy)undecane, 1,12-bis(4-aminophenoxy)dodecane , 1,12-bis(3-aminophenoxy)dodecane, 1,2-bis(6-amino-2-naphthyl)ethane, 1,2-bis(6-amino-2-naphthyl)ethane, 6-[2-(4-aminophenoxy)ethoxy]-2-naphthylamine, 1,4-phenylenebis(4-aminobenzoate), 1,4-phenylenebis(3-aminobenzoate), 1,3-phenylenebis(4-aminobenzoate), 1,3-phenylenebis(3-aminobenzoate), bis(4-aminophenyl)terephthalate, bis(3-aminophenyl)terephthalate, bis(4-aminophenyl)isophthalate ester, bis(3-aminophenyl)isophthalate, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 4-(2-(methylamino)ethyl)aniline, 4-(2-aminoethyl)aniline, 4,4'-diaminobenzophenone, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene , 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)diphenyl ether, 1,4-bis[4-(4-aminophenoxy)phenoxy]benzene (hereinafter, they are also collectively referred to as the first diamine); diamines having a photo-aligning group such as 4,4'-diaminoazobenzene or diaminodiphenylacetylene; diamines having an amide bond such as 4,4'-diaminobenzanilide; diamines having a urea bond such as 1,3-bis(4-aminophenyl)urea, 1,3-bis(4-aminobenzyl)urea, 1,3-bis(4-aminophenethyl)urea;2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, 1,4-bis-(4-aminophenyl)-piperazine, 3,6-diaminoacridine, N-ethyl-3,6-diaminocarbazole, N-phenyl-3,6-diaminocarbazole, N-(3-(1H-imidazol-1-yl)propyl-3,5-diaminobenzamide, 4-[4-[(4-aminophenoxy)methyl]-4,5-dihydro-4-methyl-2-oxazolyl]-aniline, or a diamine represented by the following formula (z-1) to formula (z-13) or a heterocyclic diamine such as a diamine, or 4,4'-diaminodiphenylamine, 4, A diamine having a diphenylamine structure, such as 4'-diaminodiphenyl-N-methylamine, N,N'-bis(4-aminophenyl)-benzidine, N,N'-bis(4-aminophenyl)-N,N'-dimethylbenzidine or N,N'-bis(4-aminophenyl)-N,N'-dimethyl-1,4-phenylenediamine, and having at least one nitrogen-containing structure selected from the group consisting of a nitrogen-containing heterocyclic ring, a secondary amino group and a tertiary amino group (hereinafter also referred to as a specific nitrogen-containing structure) (wherein the molecule does not have an amino group bonded to a protective group that is detached and substituted with a hydrogen atom by heating. In addition, the above-mentioned specific diamine (p) is not included); 2,4-diaminophenol, 3, 5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol; 4,4'-diamino-3,3'-dihydroxybiphenyl; 2,4-diaminobenzoic acid, 2,5-diaminobenzoic acid, 3,5-diaminobenzoic acid, 4,4'-diaminobiphenyl-3-carboxylic acid, 4,4'-diaminodiphenylmethane-3-carboxylic acid, 1,2-bis(4-aminophenyl)ethane-3-carboxylic acid, 4,4'-diaminobiphenyl-3,3'-dicarboxylic acid, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 3,3'-diaminobiphenyl-4,4'-dicarboxylic acid, 3,3'-diaminobiphenyl-2,4'-dicarboxylic acid, 4 , 4'-diaminodiphenylmethane-3,3'-dicarboxylic acid, 1,2-bis(4-aminophenyl)ethane-3,3'-dicarboxylic acid, 4,4'-diaminodiphenyl ether-3,3'-dicarboxylic acid and the like having a carboxyl group; 4-(2-(methylamino)ethyl)aniline, 4-(2-aminoethyl)aniline, 1-(4-aminophenyl)-1,3,3-trimethyl-1H-indane-5-amine, 1-(4-aminophenyl)-2,3-dihydro-1,3,3-trimethyl-1H-indane-6-amine; diamines having a photopolymerizable group at the end such as 2-(2,4-diaminophenoxy)ethyl methacrylate and 2,4-diamino-N,N-diallylaniline;Diamines having a steroidal skeleton, such as cholesteryloxy-3,5-diaminobenzene, cholesteryloxy-3,5-diaminobenzene, cholesteryloxy-2,4-diaminobenzene, 3,5-diaminobenzoic acid cholesteryl ester, 3,5-diaminobenzoic acid cholesteryl ester, 3,5-diaminobenzoic acid lanosteryl ester, and 3,6-bis(4-aminobenzoyloxy)cholestane; diamines represented by the following formulas (V-1) to (V-2); diamines having a group "-N(D)-" (D represents a group that is released by heating) and the like, A diamine having a siloxane bond such as 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, meta-xylylenediamine, 1,3-propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), or a diamine having two amino groups bonded to a group represented by any of the formulas (Y-1) to (Y-167) described in WO2018 / 117239. ;
[0073]
[0074]
[0075] In the above formula (V-1), m and n are each independently an integer of 0 to 3, and satisfy 1≤m+n≤4. j is an integer of 0 or 1. 1 Indicates - (CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CO-N(CH3)-, -NH-, -O-, -CH2O-, -CH2-OCO-, -COO- or -OCO-. 1 represents a monovalent group such as a fluorine atom, an alkyl group having 1 to 10 carbon atoms and containing a fluorine atom, an alkoxy group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms. 2 represents -O-, -CH2O-, -CH2-OCO-, -COO-, or -OCO-. 1 , R 1 , each independently has the above definition.
[0076]
[0077] (Boc represents tert-butyloxycarbonyl.)
[0078] Examples of the nitrogen-containing heterocyclic ring that the diamine having a structure containing a nitrogen atom may have include pyrrole, imidazole, pyrazole, triazole, pyridine, pyrimidine, pyridazine, pyrazine, indole, benzimidazole, purine, quinoline, isoquinoline, naphthyridine, quinoxaline, phthalazine, triazine, carbazole, acridine, piperidine, piperazine, pyrrolidine, and hexamethyleneimine. Among them, pyridine, pyrimidine, pyrazine, piperidine, piperazine, quinoline, carbazole, or acridine is preferred.
[0079] From the viewpoint of improving the liquid crystal orientation, the above-mentioned other diamine may be a diamine selected from the group consisting of the above-mentioned first diamine, a diamine having an amide bond, a diamine having a urea bond, a diamine having a group "-N(D)-", a diamine having a specific nitrogen atom-containing structure, and a diamine having a carboxyl group.
[0080] (Liquid Crystal Alignment Agent)
[0081] The liquid crystal aligning agent of the present invention is a liquid composition in which the polymer (P) and other components used as needed are preferably dispersed or dissolved in an appropriate solvent.
[0082] The liquid crystal aligning agent of the present invention may also contain other polymers other than the polymer (P). If specific examples of other polymers are listed, in addition to the above-mentioned polymer (P), polymers selected from the group consisting of the following substances can also be listed: at least one polymer selected from the group consisting of a polyimide precursor obtained by using a tetracarboxylic acid component that does not contain the above-mentioned specific aromatic tetracarboxylic acid component (p) and a polyimide that is an imide of the polyimide precursor, at least one polymer selected from the group consisting of a polyimide precursor obtained by using a diamine component that does not have the above-mentioned specific diamine (p) and a polyimide that is an imide of the polyimide precursor (also referred to as polymer (B) in the present invention), polysiloxane, polyester, polyamide, polyurea, polyorganosiloxane, cellulose derivative, polyacetal, polystyrene derivative, poly(styrene-maleic anhydride) copolymer, poly(isobutylene-maleic anhydride) copolymer, poly(vinyl ether-maleic anhydride) copolymer, poly(styrene-phenylmaleimide) derivative, poly(meth)acrylate.
[0083] Specific examples of poly(styrene-maleic anhydride) copolymers include SMA1000, SMA2000, SMA3000 (manufactured by Cray Valley), GSM301 (manufactured by Gifu Shellac Manufacturing), etc. Specific examples of poly(isobutylene-maleic anhydride) copolymers include ISOBAM-600 (manufactured by Kuraray). Specific examples of poly(vinyl ether-maleic anhydride) copolymers include Gantrez AN-139 (methyl vinyl ether maleic anhydride resin, manufactured by Ashland).
[0084] Among them, the polymer (B) is more preferred from the viewpoint of reducing afterimages caused by residual DC.
[0085] The above other polymers may be used alone or in combination of two or more. The content of the other polymers is preferably 90 parts by mass or less, more preferably 10 to 90 parts by mass, and further preferably 20 to 80 parts by mass, relative to 100 parts by mass of the total polymers contained in the liquid crystal aligning agent.
[0086] (Polymer (B))
[0087] Specific examples of the tetracarboxylic acid component used to produce the above-mentioned polymer (B) include compounds similar to those exemplified in the polymer (P), including preferred specific examples. The tetracarboxylic acid component used to produce the polymer (B) more preferably contains tetracarboxylic dianhydride or a derivative thereof having at least one partial structure selected from the group consisting of a benzene ring, a cyclobutane ring, a cyclopentane ring, and a cyclohexane ring (hereinafter, they are also referred to as specific tetracarboxylic acid component (B)).
[0088] Moreover, the usage-amount of the said specific tetracarboxylic acid component (B) is preferably 10 mol% or more, more preferably 20 mol% or more, and further preferably 50 mol% or more, based on 1 mol of all tetracarboxylic acid components for producing the polymer (B).
[0089] As the diamine component for obtaining the polymer (B), for example, the diamines exemplified in the above polymer (P) can be cited. Among them, it is preferred to include at least one diamine selected from the group consisting of the above first diamine, a diamine having a urea bond, a diamine having an amide bond, and a diamine having a group "-N(D)-" (these are also referred to as specific diamine (b) in the present invention). The diamine component may be used alone or in combination of two or more diamines.
[0090] When the above-mentioned specific diamine (b) is used, the usage amount thereof is preferably 10 mol% or more, more preferably 20 mol% or more, of the total diamine components used to produce the polymer (B). When a diamine other than the specific diamine (b) is used, the usage amount of the specific diamine (b) is preferably 90 mol% or less, more preferably 80 mol% or less, relative to 1 mol of the total diamine components used to produce the polymer (B).
[0091] (Manufacture of polyamic acid)
[0092] The manufacture of polyamic acid is carried out by reacting a diamine component with a tetracarboxylic acid component in an organic solvent. As for the use ratio of the tetracarboxylic acid component and the diamine component for the manufacture reaction of polyamic acid, the anhydride group of the tetracarboxylic acid component is preferably 0.5 to 2 equivalents relative to 1 equivalent of the amino group of the diamine component, and more preferably 0.8 to 1.2 equivalents. As in the usual polycondensation reaction, the closer the equivalent of the anhydride group of the tetracarboxylic acid component is to 1 equivalent, the greater the molecular weight of the generated polyamic acid.
[0093] The reaction temperature in the manufacture of polyamic acid is preferably -20 to 150°C, more preferably 0 to 100°C. In addition, the reaction time is preferably 0.1 to 24 hours, more preferably 0.5 to 12 hours. The manufacture of polyamic acid can be carried out at any concentration, but the concentration of polyamic acid is preferably 1 to 50% by mass, more preferably 5 to 30% by mass. It is also possible to carry out the reaction at a high concentration in the initial stage and then add a solvent.
[0094] Specific examples of the organic solvent include cyclohexanone, cyclopentanone, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and 1,3-dimethyl-2-imidazolidinone. In addition, when the polymer has high solvent solubility, solvents such as methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, diethylene glycol monomethyl ether, or diethylene glycol monoethyl ether can be used.
[0095] (Production of polyamic acid ester)
[0096] Polyamic acid ester can be obtained by, for example, a known method such as [I] a method of reacting a polyamic acid obtained by the above method with an esterifying agent, [II] a method of reacting a tetracarboxylic acid diester with a diamine, or [III] a method of reacting a tetracarboxylic acid diester dihalide with a diamine.
[0097] (Manufacture of polyimide)
[0098] As for polyimide, polyimide can be obtained by ring-closing (imidizing) a polyimide precursor such as the above-mentioned polyamic acid or polyamic acid ester. It should be noted that the imidization rate mentioned in this specification refers to the proportion of the imide group in the total amount of the imide group and the carboxyl group (or its derivative) derived from tetracarboxylic dianhydride or its derivative. The imidization rate does not necessarily have to be 100%, and can be arbitrarily adjusted according to the use and purpose.
[0099] Examples of a method for imidating a polyimide precursor include thermal imidization in which a solution of a polyimide precursor is heated while it is maintained, and catalytic imidization in which a catalyst is added to a solution of a polyimide precursor.
[0100] The temperature when thermally imidizing the polyimide precursor in a solution is preferably 100 to 400° C., more preferably 120 to 250° C., and the imidization reaction is preferably performed while removing water generated by the imidization reaction to the outside of the system.
[0101] The catalytic imidization of the polyimide precursor can be carried out as follows: add a basic catalyst and an acid anhydride to a solution of the polyimide precursor, preferably stirring at -20 to 250°C, more preferably at 0 to 180°C. The amount of the basic catalyst is preferably 0.5 to 30 times the molar amount of the amic acid group, more preferably 2 to 20 times, and the amount of the acid anhydride is preferably 1 to 50 times the molar amount of the amic acid group, more preferably 3 to 30 times. As the basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine or trioctylamine can be listed, among which pyridine has a moderate alkalinity for the progress of the reaction, so it is preferred. As the acid anhydride, acetic anhydride, trimellitic anhydride or pyromellitic anhydride can be listed, among which, when acetic anhydride is used, purification after the reaction becomes easy, so it is preferred. The imidization rate based on catalytic imidization can be controlled by adjusting the amount of catalyst, reaction temperature and reaction time.
[0102] In the case of recovering the generated polyimide precursor or polyimide from the reaction solution of the polyimide precursor or polyimide, it is sufficient to put the reaction solution into a solvent to precipitate it. As solvents for precipitation, methanol, ethanol, isopropanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, toluene, benzene, water, etc. can be listed. The polymer precipitated by being put into the solvent can be filtered and recovered, and then dried at room temperature or heated under normal pressure or reduced pressure. In addition, when the recovered polymer is repeatedly dissolved in an organic solvent and reprecipitated and recovered 2 to 10 times, the impurities in the polymer can be reduced. As solvents at this time, for example, alcohols, ketones or hydrocarbons can be listed. When three or more solvents selected from these are used, the efficiency of purification is further improved, so it is preferred.
[0103] When the polyimide precursor and polyimide in the present invention are manufactured, a suitable end-capping agent can be used together with a tetracarboxylic acid component containing tetracarboxylic dianhydride or its derivative and a diamine component containing diamine to manufacture an end-capped polymer. The end-capped polymer has the effect of improving the film hardness of the liquid crystal alignment film obtained from the coating film and improving the adhesion characteristics between the sealant and the liquid crystal alignment film.
[0104] Examples of the terminal of the polyimide precursor or polyimide in the present invention include amino groups, carboxyl groups, acid anhydride groups, or groups derived from the terminal blocking agent described below. The amino groups, carboxyl groups, and acid anhydride groups can be obtained by a common condensation reaction or by blocking with the following terminal blocking agent.
[0105] Examples of the end-capping agent include: anhydrides such as acetic anhydride, maleic anhydride, nadic anhydride, phthalic anhydride, itaconic anhydride, 1,2-cyclohexanedicarboxylic anhydride, 3-hydroxyphthalic anhydride, trimellitic anhydride, 3-(3-trimethoxysilyl)propyl-3,4-dihydrofuran-2,5-dione, 4,5,6,7-tetrafluoroisobenzofuran-1,3-dione, and 4-ethynylphthalic anhydride; dicarbonic acid diester compounds such as di-tert-butyl dicarbonate and diallyl dicarbonate; acryloyl chloride, methyl Chlorocarbonyl compounds such as acryloyl chloride and nicotinoyl chloride; monoamine compounds such as aniline, 2-aminophenol, 3-aminophenol, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, cyclohexylamine, n-butylamine, n-pentylamine, n-hexylamine, n-heptylamine, n-octylamine; isocyanates with unsaturated bonds such as ethyl isocyanate, phenyl isocyanate, naphthyl isocyanate or 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, etc.
[0106] The usage ratio of the terminal blocking agent is preferably 0.01 to 20 parts by mole, more preferably 0.01 to 10 parts by mole, based on 100 parts by mole of the total diamine component used.
[0107] The polyimide precursor and the polyimide preferably have a weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) of 1,000 to 500,000, and more preferably 2,000 to 300,000. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) in terms of polystyrene measured by GPC is preferably 15 or less, and more preferably 10 or less. By being in this molecular weight range, good liquid crystal orientation of the liquid crystal display element can be ensured.
[0108] The organic solvent contained in the liquid crystal aligning agent of the present invention is not particularly limited as long as it uniformly dissolves the polymer (P) and other polymers added as needed. For example, N, N-dimethylformamide, N, N-dimethylacetamide, N, N-dimethyllactamide, N, N-dimethylpropionamide, tetramethylurea, N, N-diethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethyl sulfoxide, γ-butyrolactone, γ-valerolactone, 1, 3-dimethyl-2-imidazolidinone, methyl ethyl ketone, cyclohexanone, cyclopentanone, 3-methoxy-N, N-dimethylpropionamide , 3-butoxy-N, N-dimethylpropionamide, N-n-propyl-2-pyrrolidone, N-isopropyl-2-pyrrolidone, N-n-butyl-2-pyrrolidone, N-tert-butyl-2-pyrrolidone, N-n-pentyl-2-pyrrolidone, N-methoxypropyl-2-pyrrolidone, N-ethoxyethyl-2-pyrrolidone, N-methoxybutyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone (these are also collectively referred to as good solvents), etc. Among them, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 3-methoxy-N, N-dimethylpropionamide, 3-butoxy-N, N-dimethylpropionamide or γ-butyrolactone is preferred. The content of the good solvent is preferably 20 to 99% by mass of the total solvent contained in the liquid crystal aligning agent, more preferably 20 to 90% by mass, and particularly preferably 30 to 80% by mass.
[0109] In addition, the organic solvent contained in the liquid crystal aligning agent is preferably used in addition to the above-mentioned solvent and a mixed solvent of a solvent (also referred to as a poor solvent) that improves the coating property and surface smoothness of the coating film when the liquid crystal aligning agent is applied. Specific examples of poor solvents are described below, but are not limited thereto. The content of the poor solvent is preferably 1 to 80% by mass of the entire solvent contained in the liquid crystal aligning agent, more preferably 10 to 80% by mass, and particularly preferably 20 to 70% by mass. The type and content of the poor solvent are appropriately selected according to the coating device, coating conditions, coating environment, etc. of the liquid crystal aligning agent.
[0110] Examples of the poor solvent include diisopropyl ether, diisobutyl ether, diisobutyl carbinol (2,6-dimethyl-4-heptanol), ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 3-ethoxybutyl acetate, 1-methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, ethylene glycol monoacetate, ethylene glycol diacetate, propylene carbonate, ethylene carbonate, ethylene glycol monobutyl ether, ethylene glycol monoisopentyl ether, ethylene glycol monohexyl ether, propylene glycol monomethyl ether, propylene glycol monobutyl ether, 1-(2-butoxyethoxy)-2-propanol, 2-(2-butoxyethoxy)-1-propanol, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol monopropyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, propylene glycol diacetate, n-butyl acetate, propylene glycol monoethyl acetate, cyclohexyl acetate, 4-methyl-2-pentyl acetate, 3-methoxypropionic acid methyl ester, 3-ethoxypropionic acid ethyl ester, 3-methoxypropionic acid ethyl ester, 3-methoxypropionic acid propyl ester, 3-methoxypropionic acid butyl ester, n-butyl lactate, isopentyl lactate, diethylene glycol monoethyl ether, diisobutyl ketone (2,6-dimethyl-4-heptanone), etc.
[0111] Among them, diisobutylcarbinol, propylene glycol monobutyl ether, propylene glycol diacetate, diethylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate or diisobutyl ketone is preferred.
[0112] Preferred combinations of good solvents and poor solvents include: N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone; N-ethyl-2-pyrrolidone and propylene glycol diacetate; N,N-dimethyl lactamide and diisobutyl ketone; N-methyl-2-pyrrolidone and ethyl 3-ethoxypropionate; N-ethyl-2-pyrrolidone and ethyl 3-ethoxypropionate; N-methyl-2-pyrrolidone, ethyl 3-ethoxypropionate and and dipropylene glycol monomethyl ether; N-ethyl-2-pyrrolidone, ethyl 3-ethoxypropionate and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, ethyl 3-ethoxypropionate and diethylene glycol monopropyl ether; N-ethyl-2-pyrrolidone, ethyl 3-ethoxypropionate and diethylene glycol monopropyl ether; N-methyl-2-pyrrolidone and ethylene glycol monobutyl ether acetate; N-ethyl-2-pyrrolidone and dipropylene glycol dimethyl ether; N,N-dimethyl lactamide and ethylene glycol monobutyl ether; N,N-dimethyl lactamide and propylene glycol diacetate; N-ethyl-2-pyrrolidone and diethylene glycol diethyl ether; N-ethyl-2-pyrrolidone, diethylene glycol monoethyl ether and butyl cellosolve acetate; N-methyl-2-pyrrolidone Ketone, diethylene glycol monomethyl ether and butyl cellosolve acetate; N,N-dimethyl lactamide and diethylene glycol diethyl ether; N-methyl-2-pyrrolidone, gamma-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diethylene glycol diethyl ether; N-ethyl-2-pyrrolidone, N-methyl-2-pyrrolidone and 4-hydroxy-4-methyl-2-pentanone; N-ethyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and diisobutyl ketone; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and dipropylene glycol monomethyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4 N-methyl-2-pentanone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; N-ethyl-2-pyrrolidone, 4-hydroxy-4-methyl-2-pentanone and dipropylene glycol dimethyl ether; γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diisobutyl ketone; γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and propylene glycol diacetate; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisobutyl ketone; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisopropyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisobutyl carbinol;N-methyl-2-pyrrolidone, gamma-butyrolactone and dipropylene glycol dimethyl ether; N-methyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol dimethyl ether; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and dipropylene glycol monomethyl ether; N-ethyl-2-pyrrolidone, diethylene glycol diethyl ether and dipropylene glycol monomethyl ether; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and propylene glycol diacetate; N-ethyl-2-pyrrolidone, propylene glycol monobutyl ether and diisobutyl ketone; N-ethyl-2-pyrrolidone, gamma-butyrolactone and diisobutyl ketone; N-ethyl-2-pyrrolidone, N,N-dimethyl Lactamide and diisobutyl ketone; N-methyl-2-pyrrolidone, ethylene glycol monobutyl ether and ethylene glycol monobutyl ether acetate; γ-butyrolactone, ethylene glycol monobutyl ether acetate and dipropylene glycol dimethyl ether; N-ethyl-2-pyrrolidone, ethylene glycol monobutyl ether acetate and propylene glycol dimethyl ether; N-methyl-2-pyrrolidone, 4-methyl-2-pentyl acetate and ethylene glycol monobutyl ether; N-ethyl-2-pyrrolidone, cyclohexyl acetate and 4-hydroxy-4-methyl-2-pentanone; cyclohexanone and propylene glycol monomethyl ether; cyclopentanone and propylene glycol monomethyl ether; N-methyl-2-pyrrolidone, cyclohexanone and propylene glycol monomethyl ether, etc.;
[0113] (Liquid Crystal Alignment Agent)
[0114] The liquid crystal aligning agent of this invention contains the said polymer (P) and, as needed, the said other polymer and the said organic solvent.
[0115] The total content of the polymers contained in the liquid crystal aligning agent of the present invention can also be appropriately changed according to the setting of the thickness of the coating film to be formed. From the perspective of forming a uniform and defect-free coating film, it is preferably 1% by mass or more, and from the perspective of the storage stability of the solution, it is preferably 10% by mass or less. The total content of the polymers is particularly preferably 2 to 8% by mass.
[0116] The content of the polymer (P) used in the present invention is preferably 1 to 100 mass %, more preferably 10 to 100 mass %, particularly preferably 20 to 100 mass %, based on the total amount of the polymers contained in the liquid crystal aligning agent.
[0117] The liquid crystal alignment agent of the present invention may contain other components (hereinafter referred to as additive components) in addition to the above-mentioned polymer (P), the above-mentioned other polymers and the above-mentioned organic solvent. As the above-mentioned additive components, for example, at least one cross-linking compound selected from the group consisting of a cross-linking compound having the following substituents and a cross-linking compound having a polymerizable unsaturated group; a functional silane compound; a metal chelate compound; a curing accelerator; a surfactant; an antioxidant; a sensitizer; a preservative; a compound for adjusting the dielectric constant and resistance of the obtained liquid crystal alignment film, etc., wherein the substituent is selected from at least one of an oxirane group, an oxetane group, a blocked isocyanate group, an oxazoline group, a cyclocarbonate group, a hydroxyl group and an alkoxy group.
[0118] Preferred specific examples of the crosslinking compound include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, bisphenol A type epoxy resins such as EPIKOTE 828 (manufactured by MITSUBISHI CHEMICAL Co., Ltd.), bisphenol F type epoxy resins such as EPIKOTE 807 (manufactured by MITSUBISHI CHEMICAL Co., Ltd.), hydrogenated bisphenol A type epoxy resins such as YX-8000 (manufactured by MITSUBISHI CHEMICAL Co., Ltd.), YX6954BH30 (manufactured by MITSUBISHI CHEMICAL Co., Ltd.), and bisphenol A type epoxy resins such as EPICOTE 828 (manufactured by MITSUBISHI CHEMICAL Co., Ltd.). Epoxy resins containing biphenyl skeletons, such as EPPN-201 (manufactured by Nippon Kayaku Co., Ltd.), phenol novolac type epoxy resins, such as EOCN-102S (manufactured by Nippon Kayaku Co., Ltd.), (o-, m-, p-) cresol novolac type epoxy resins, such as TEPIC (manufactured by Nissan Chemical Co., Ltd.), alicyclic epoxy resins such as CELLOXIDE2021P (manufactured by Daicel Co., Ltd.), N,N,N',N'-tetraglycidyl tertiary nitrogen atom-containing compounds represented by 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane or N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, compounds having two or more oxirane groups such as tetra(glycidyloxymethyl)methane; compounds having two or more oxetane groups described in paragraphs 0170 to 0175 of WO2011 / 132751; CORONATE AP stable M, CORONATE 2503, 2515, 2507, 2513, 2555, MILLIONATE MS-50 (all manufactured by TOSOH), TAKENATE Compounds having a blocked isocyanate group such as B-830, B-815N, B-820NSU, B-842N, B-846N, B-870N, B-874N, and B-882N (all manufactured by Mitsui Chemicals, Inc.); compounds having an oxazoline group such as 2,2'-bis(2-oxazoline), 2,2'-bis(4-methyl-2-oxazoline), 2,2'-bis(5-methyl-2-oxazoline), 1,2,4-tri(2-oxazolinyl)-benzene, and EPOCROS (manufactured by Nippon Shokubai Co., Ltd.); compounds having a cyclic carbonate group as described in paragraphs 0025 to 0030 and 0032 of WO2011 / 155577;Compounds having hydroxyl groups or alkoxy groups, such as N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide, 2,2-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethoxyphenyl)propane, and 2,2-bis(4-hydroxy-3,5-dihydroxymethylphenyl)-1,1,1,3,3,3-hexafluoropropane; compounds represented by glycerol mono(meth)acrylate, glycerol di(meth)acrylate (1,2-, 1,3-type mixture), glycerol tri(meth)acrylate, glycerol 1,3-diglycerol alcohol di(meth)acrylate, pentaerythritol tri(meth)acrylate, diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, tetraethylene glycol mono(meth)acrylate, pentaethylene glycol mono(meth)acrylate, and hexaethylene glycol mono(meth)acrylate. ;
[0119] As for content of the crosslinking compound, it is preferably 0.1-30 mass parts, more preferably 0.1-20 mass parts with respect to 100 mass parts of the polymer components contained in the liquid crystal aligning agent.
[0120] Examples of the compound for adjusting the dielectric constant and the resistance include monoamines having an aromatic heterocyclic ring containing a nitrogen atom, such as 3-aminomethylpyridine. The content of the monoamine having an aromatic heterocyclic ring containing a nitrogen atom is preferably 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, based on 100 parts by mass of the polymer component contained in the liquid crystal aligning agent.
[0121] Preferred specific examples of the functional silane compound include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldiethoxymethylsilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, tris(3-trimethoxysilylpropyl)isocyanurate, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, etc. The content of the functional silane compound is preferably 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, relative to 100 parts by mass of the polymer component contained in the liquid crystal aligning agent.
[0122] The solid content concentration in the liquid crystal aligning agent (the ratio of the total mass of components other than the solvent of the liquid crystal aligning agent to the total mass of the liquid crystal aligning agent) is appropriately selected in consideration of viscosity, volatility, etc., and is preferably 1 to 10 mass %.
[0123] The range of particularly preferred solid content concentration varies depending on the method used when the liquid crystal alignment agent is applied to the substrate. For example, in the case of using a spin coating method, the solid content concentration is particularly preferably 1.5 to 4.5% by mass. In the case of a printing method, it is particularly preferred to set the solid content concentration to 3 to 9% by mass, thereby setting the solution viscosity to 12 to 50 mPa·s. In the case of an inkjet method, it is particularly preferred to set the solid content concentration to 1 to 5% by mass, thereby setting the solution viscosity to 3 to 15 mPa·s. The temperature when preparing the polymer composition is preferably 10 to 50°C, more preferably 20 to 30°C.
[0124] <Liquid crystal alignment film / liquid crystal display element>
[0125] By using the above-mentioned liquid crystal alignment agent, a liquid crystal alignment film can be manufactured. The liquid crystal display element of the present invention has the above-mentioned liquid crystal alignment film. The operation mode of the liquid crystal display element of the present invention is not particularly limited, for example, it can be applied to various operation modes such as TN type, STN (Super Twisted Nematic) type, vertical alignment type (including VA-MVA (Multi-domain Vertical Alignment: multi-domain vertical alignment) type, VA-PVA (Patterned Vertical Alignment: image vertical alignment) type, etc.), IPS mode, FFS mode, optically compensated bending type (OCB: Optically Compensated Birefringence type). Among them, the liquid crystal alignment film of the present invention is a liquid crystal alignment film suitable for horizontally oriented liquid crystal display elements such as IPS mode or FFS mode.
[0126] The liquid crystal display element of the present invention can be manufactured, for example, by a method comprising the following steps (1) to (4); a method comprising steps (1) to (2) and (4); a method comprising steps (1) to (3), (4) and (5); or a method comprising steps (1) to (3), (4) and (6).
[0127] <Step (1): Step of applying a liquid crystal aligning agent onto a substrate>
[0128] The step (1) is a step of applying the liquid crystal aligning agent of the present invention onto a substrate. Specific examples of the step (1) are as follows.
[0129] For example, by a suitable coating method such as a roller coater method, a spin coating method, a printing method, an inkjet method, etc., the liquid crystal alignment agent of the present invention is applied to one side of a substrate provided with a patterned transparent conductive film. As a substrate here, as long as it is a substrate with high transparency, there is no particular limitation, and a plastic substrate such as an acrylic substrate, a polycarbonate substrate, etc. can also be used together with a glass substrate, a silicon nitride substrate, etc. In addition, in a reflective liquid crystal display element, if it is a substrate on only one side, an opaque object such as a silicon wafer can also be used, and the electrode in this case can also use a material that reflects light such as aluminum. In addition, in the case of manufacturing a liquid crystal display element of an IPS method or an FFS method, a substrate provided with an electrode composed of a transparent conductive film or a metal film patterned into a comb-shaped pattern and an opposing substrate without an electrode are used.
[0130] As a method of applying a liquid crystal aligning agent to a substrate to form a film, screen printing, offset printing, flexographic printing, an inkjet method, a spray method, etc. are mentioned. Among them, the coating and film-forming method using the inkjet method can be preferably used.
[0131] <Step (2): Step of calcining the applied liquid crystal aligning agent>
[0132] The step (2) is a step of baking the liquid crystal aligning agent applied on the substrate to form a film. Specific examples of the step (2) are as follows.
[0133] After the liquid crystal aligning agent is applied to the substrate in step (1), the solvent can be evaporated by a heating unit such as a heating plate, a heat circulation oven or an IR (infrared) oven; or thermal imidization of polyamic acid or polyamic acid ester can be performed. The drying and firing steps after applying the liquid crystal aligning agent of the present invention can be selected at any temperature and time, and can also be performed multiple times. As a temperature for reducing the solvent of the liquid crystal aligning agent, for example, it can be performed at 40 to 180°C. From the perspective of shortening the process, it can be performed at 40 to 150°C. As for the firing time, it is not particularly limited, and 1 to 10 minutes or 1 to 5 minutes can be listed. In the case of thermal imidization of polyamic acid or polyamic acid ester, a firing step can be added after the above step, for example, in the temperature range of 150 to 300°C or 150 to 250°C. As for the firing time, it is not particularly limited, and 5 to 40 minutes or 5 to 30 minutes can be listed.
[0134] If the film thickness of the film-like material after firing is too thin, the reliability of the liquid crystal display element may be reduced, so it is preferably 5 to 300 nm, and more preferably 10 to 200 nm.
[0135] <Step (3): Step of orienting the film obtained in step (2)>
[0136] Step (3) is a step of subjecting the film obtained in step (2) to an orientation treatment, depending on the circumstances. That is, in a horizontally oriented liquid crystal display element such as an IPS mode or an FFS mode, the coating is subjected to an orientation capability imparting treatment. On the other hand, in a vertically oriented liquid crystal display element such as a VA mode or a PSA (Polymer-Sustained Alignment: polymer stabilized alignment) mode, the formed coating can be used as a liquid crystal alignment film while maintaining the state, or the coating can be subjected to an orientation capability imparting treatment. As an orientation treatment method for a liquid crystal alignment film, a rubbing treatment method and a photo-orientation treatment method can be listed. As a photo-orientation treatment method, the following method can be listed: the surface of the above-mentioned film-like object is irradiated with radiation polarized in a certain direction, and a heat treatment is preferably performed at a temperature of 150 to 250° C., depending on the circumstances, to impart liquid crystal orientation (also referred to as liquid crystal orientation capability). As radiation, ultraviolet rays or visible light having a wavelength of 100 to 800 nm can be used. Among them, ultraviolet rays having a wavelength of 100 to 400 nm are preferred, and ultraviolet rays having a wavelength of 200 to 400 nm are more preferred.
[0137] Examples of the rubbing treatment method include a treatment in which the coating film is rubbed in a certain direction using a roller wound with a cloth made of fibers such as nylon, rayon, and cotton.
[0138] In the above-mentioned photo-alignment treatment method, when the radiation is polarized, it can be linear polarization or partial polarization. In addition, when the radiation used is linear polarization or partial polarization, the irradiation can be performed from a direction perpendicular to the substrate surface, or from an oblique direction, or a combination of them. When irradiating non-polarized radiation, the irradiation direction is preferably set to an oblique direction.
[0139] <Step (4): Step of manufacturing a liquid crystal cell>
[0140] As described above, two substrates on which liquid crystal alignment films are formed are prepared, and liquid crystal is arranged between the two substrates arranged to face each other. Specifically, the following two methods can be cited.
[0141] In the first method, two substrates are first arranged oppositely with a gap (cell gap) between the two liquid crystal alignment films. Next, the peripheries of the two substrates are bonded together using a sealant, and a liquid crystal composition is injected into the cell gap defined by the substrate surface and the sealant, and after the liquid crystal composition contacts the film surface, the injection hole is sealed.
[0142] In addition, the second method is a method called ODF (One Drop Fill: liquid crystal dripping) method. For example, a UV-curable sealant is applied to a specified position on one of the two substrates on which a liquid crystal alignment film is formed, and a liquid crystal composition is further dripped into several specified positions on the surface of the liquid crystal alignment film. Then, the substrate of the other side is bonded in a manner that the liquid crystal alignment film is opposite, and the liquid crystal composition is extended to the entire surface of the substrate and contacts the film surface. Then, ultraviolet light is irradiated on the entire surface of the substrate to cure the sealant. Regardless of which method is used, it is ideal that after further heating to a temperature at which the liquid crystal composition used becomes an isotropic phase, it is slowly cooled to room temperature, thereby removing the flow orientation during liquid crystal filling.
[0143] In addition, when the coating film is subjected to the rubbing treatment, the two substrates are disposed to face each other so that the rubbing directions of the coating films form a predetermined angle with each other, for example, are orthogonal or antiparallel.
[0144] As the sealant, for example, an epoxy resin containing a curing agent and alumina balls as spacers can be used.
[0145] As the above-mentioned liquid crystal composition, there is no particular limitation, and various liquid crystal compositions containing at least one liquid crystal compound (liquid crystal molecule) and having a positive or negative dielectric anisotropy can be used. It should be noted that, hereinafter, a liquid crystal composition having a positive dielectric anisotropy is also referred to as a positive liquid crystal, and a liquid crystal composition having a negative dielectric anisotropy is also referred to as a negative liquid crystal.
[0146] The above-mentioned liquid crystal composition may contain liquid crystal compounds having fluorine atoms, hydroxyl groups, amino groups, fluorine-containing groups (such as trifluoromethyl groups), cyano groups, alkyl groups, alkoxy groups, alkenyl groups, isothiocyanate groups, heterocyclic rings, cycloalkanes, cycloolefins, steroid skeletons, benzene rings or naphthalene rings, and may also contain compounds having two or more rigid sites (mesogenic skeletons) that embody liquid crystal properties in the molecule (for example, a bimesogenic compound formed by two rigid biphenyl structures or terphenyl structures linked by an alkylene group).
[0147] The liquid crystal composition may be a liquid crystal composition in a nematic phase, a liquid crystal composition in a smectic phase, or a liquid crystal composition in a cholesteric phase.
[0148] In addition, from the perspective of improving the orientation of the liquid crystal, the liquid crystal composition may further contain additives. Such additives include: photopolymerizable monomers such as compounds having polymerizable groups; optically active compounds (e.g., S-811 manufactured by Merck, Inc.); antioxidants; ultraviolet absorbers; pigments; defoamers; polymerization initiators; or polymerization inhibitors.
[0149] Examples of the positive liquid crystal include ZLI-2293, ZLI-4792, MLC-2003, MLC-2041, and MLC-7081 manufactured by Merck.
[0150] As a negative liquid crystal, MLC-6608, MLC-6609, MLC-6610, or MLC-7026-100 manufactured by Merck is mentioned, for example.
[0151] Moreover, as a liquid crystal containing the compound which has a polymerizable group, MLC-3023 manufactured by Merck can be mentioned.
[0152] The liquid crystal alignment agent of the present invention is also preferably used for a liquid crystal display element (PSA liquid crystal display element) having a liquid crystal layer between a pair of substrates having electrodes, which is manufactured by the following process: a liquid crystal composition containing a polymerizable compound that is polymerized by at least one of active energy rays and heat is arranged between a pair of substrates, a voltage is applied between the electrodes, and the polymerizable compound is polymerized by at least one of irradiation with active energy rays and heating (hereinafter, this process is also referred to as process (5)).
[0153] In addition, the liquid crystal alignment agent of the present invention is also preferably used for a liquid crystal display element (SC-PVA liquid crystal display element) having a liquid crystal layer between a pair of substrates having electrodes, which is manufactured by the following process: a liquid crystal alignment film containing polymerizable groups that are polymerized by at least one of active energy rays and heat is arranged between the above-mentioned pair of substrates, and a voltage is applied between the electrodes (hereinafter, this process is also referred to as process (6)).
[0154] Furthermore, a liquid crystal display element can be obtained by attaching a polarizing plate to the outer surface of a liquid crystal cell as required. Examples of the polarizing plate attached to the outer surface of the liquid crystal cell include a polarizing plate formed by sandwiching a polarizing film called an "H film" between cellulose acetate protective films, or a polarizing plate composed of the H film itself, wherein the H film is formed by absorbing iodine while stretching and aligning polyvinyl alcohol.
[0155] An IPS substrate, which is a comb-teeth electrode substrate used in the IPS method, includes: a substrate; a plurality of linear electrodes formed on the substrate and arranged in a comb-teeth shape; and a liquid crystal alignment film formed on the substrate so as to cover the linear electrodes.
[0156] It should be noted that the FFS substrate, which is a comb-tooth electrode substrate used in the FFS method, comprises: a substrate; a surface electrode formed on the substrate; an insulating film formed on the surface electrode; a plurality of linear electrodes formed on the insulating film and configured in a comb-tooth shape; and a liquid crystal orientation film formed on the insulating film in a manner covering the linear electrodes.
[0157] Figure 1 It is a schematic cross-sectional view showing an example of a lateral electric field liquid crystal display element of the present invention, which is an example of an IPS mode liquid crystal display element.
[0158] exist Figure 1 In the lateral electric field liquid crystal display element 1 shown as an example in FIG, a liquid crystal 3 is sandwiched between a comb-tooth electrode substrate 2 having a liquid crystal alignment film 2c and an opposing substrate 4 having a liquid crystal alignment film 4a. The comb-tooth electrode substrate 2 has: a substrate 2a; a plurality of linear electrodes 2b formed on the substrate 2a and arranged in a comb-tooth shape; and a liquid crystal alignment film 2c formed on the substrate 2a in a manner covering the linear electrodes 2b. The opposing substrate 4 has: a substrate 4b; and a liquid crystal alignment film 4a formed on the substrate 4b. The liquid crystal alignment film 2c is, for example, the liquid crystal alignment film of the present invention. The liquid crystal alignment film 4a is also the liquid crystal alignment film of the present invention.
[0159] In the lateral electric field liquid crystal display element 1 , when a voltage is applied to the linear electrodes 2 b , an electric field is generated between the linear electrodes 2 b as indicated by electric force lines L.
[0160] Figure 2It is a schematic cross-sectional view showing another example of the lateral electric field liquid crystal display element of the present invention, which is an example of an FFS mode liquid crystal display element.
[0161] exist Figure 2 In the lateral electric field liquid crystal display element 1 shown as an example in FIG, a liquid crystal 3 is sandwiched between a comb-tooth electrode substrate 2 having a liquid crystal orientation film 2h and an opposing substrate 4 having a liquid crystal orientation film 4a. The comb-tooth electrode substrate 2 has: a substrate 2d; a surface electrode 2e formed on the substrate 2d; an insulating film 2f formed on the surface electrode 2e; a plurality of linear electrodes 2g formed on the insulating film 2f and arranged in a comb-tooth shape; and a liquid crystal orientation film 2h formed on the insulating film 2f in a manner covering the linear electrodes 2g. The opposing substrate 4 has: a substrate 4b; and a liquid crystal orientation film 4a formed on the substrate 4b. The liquid crystal orientation film 2h is, for example, the liquid crystal orientation film of the present invention. The liquid crystal orientation film 4a is also the liquid crystal orientation film of the present invention.
[0162] In the lateral electric field liquid crystal display element 1, when a voltage is applied to the surface electrode 2e and the linear electrode 2g, an electric field is generated between the surface electrode 2e and the linear electrode 2g as indicated by electric force lines L.
[0163] The liquid crystal alignment film of the present invention can be applied to various uses in addition to the liquid crystal alignment film for the above-mentioned purposes, such as a liquid crystal alignment film for a phase difference film; a liquid crystal alignment film for a scanning antenna, a liquid crystal array antenna, or a liquid crystal alignment film for a liquid crystal dimming element of a transmission scattering type. Furthermore, it can also be used for purposes other than the liquid crystal alignment film, such as a protective film (e.g., a protective film for a color filter), a spacer film, an interlayer insulating film, an anti-reflective film, a wiring coating film, an antistatic film, and a motor insulating film (a gate insulating film for a flexible display).
[0164] The liquid crystal display element of the present invention can be effectively applied to various devices, for example, it can be used in various display devices such as clocks, portable game consoles, word processors, notebook computers, car navigation systems, portable cameras (camcorders), PDAs (Personal Digital Assistants), digital cameras, portable phones, smart phones, various monitors, liquid crystal televisions, information displays, etc.
[0165] Example
[0166] The present invention will be described in further detail below with reference to Examples, but the present invention is not limited to these Examples. The abbreviations of the compounds used and the methods for measuring the properties are as follows.
[0167] (Organic Solvent)
[0168] NMP: N-methyl-2-pyrrolidone.
[0169] GBL: gamma-butyrolactone.
[0170] BCS: Butyl Cellosolve.
[0171] (Tetracarboxylic dianhydride)
[0172] CA-1: a compound represented by the following formula (CA-1).
[0173] In addition, the compound represented by the said formula (CA-1) is a compound included in the range of the said specific aromatic tetracarboxylic acid component (p).
[0174] (Diamine)
[0175] DA-1 to DA-3: compounds represented by the following formulae (DA-1) to (DA-3), respectively.
[0176] The compound represented by the above formula (DA-1) is a compound included in the scope of the above specific diamine (p), and the compounds represented by the above formulas (DA-2) to (DA-3) are compounds included in the scope of other diamines.
[0177] DA-1 was synthesized according to the synthesis method described in WO2015 / 030071.
[0178]
[0179] <Viscosity measurement>
[0180] The measurement was performed at a temperature of 25° C. using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample amount of 1.1 mL and a conical rotor TE-1 (1°34′, R24).
[0181] <Determination of molecular weight>
[0182] The measurement was performed using the following room temperature GPC (gel permeation chromatography) apparatus, and Mn and Mw were calculated as polyethylene glycol and polyethylene oxide equivalent values.
[0183] GPC apparatus: GPC-101 (manufactured by Showa Denko K.K.), chromatographic columns: GPC KD-803 and GPC KD-805 (manufactured by Showa Denko K.K.) connected in series, chromatographic column temperature: 50°C, eluent: N,N-dimethylformamide (as additives, lithium bromide monohydrate (LiBr·H2O) at 30 mmol / L, phosphoric acid·anhydrous crystals (o-phosphoric acid) at 30 mmol / L, tetrahydrofuran (THF) at 10 mL / L), flow rate: 1.0 mL / min.
[0184] Standard samples for preparing the calibration curve: TSK standard polyethylene oxide (molecular weight: about 900,000, 150,000, 100,000 and 30,000) (manufactured by TOSOH) and polyethylene glycol (molecular weight: about 12,000, 4,000 and 1,000) (manufactured by Polymer Laboratories).
[0185] [Synthesis of polymer]
[0186] <Synthesis example 1>
[0187] DA-1 (2.30 g, 14.0 mmol) and NMP (17.0 g) were added to a 50 mL four-necked flask with a stirring device, and stirred at room temperature to dissolve. Then, CA-1 (3.79 g, 12.9 mmol) and NMP (27.8 g) were added, and stirred at room temperature for 24 hours to obtain a polyamic acid solution (PAA1) with a solid content concentration of 12% by mass (viscosity: 70 mPa·s). The Mn of the polyamic acid was 3500 and the Mw was 6300.
[0188] <Synthesis example 2>
[0189] DA-2 (1.50 g, 10.00 mmol) and NMP (11.3 g) were added to a 50 mL four-necked flask with a stirring device, and stirred at room temperature to dissolve. Then, CA-1 (2.93 g, 9.95 mmol) and NMP (20.0 g) were added, and stirred at 50° C. for 24 hours to obtain a polyamic acid solution (PAA2) with a solid content concentration of 12% by mass (viscosity: 302 mPa·s). The Mn of the polyamic acid was 5600 and the Mw was 11900.
[0190] <Synthesis example 3>
[0191] DA-3 (2.04 g, 15.0 mmol) and NMP (15.1 g) were added to a 50 mL four-necked flask with a stirring device, and stirred at room temperature to dissolve. Then, CA-1 (4.06 g, 13.8 mmol) and NMP (29.8 g) were added, and stirred at room temperature for 3 hours to obtain a polyamic acid solution (PAA3) with a solid content concentration of 12% by mass (viscosity: 356 mPa·s). The Mn of the polyamic acid was 5200 and the Mw was 13800.
[0192] <Example 1>
[0193] The polyamic acid solution (PAA1) obtained in Synthesis Example 1 was diluted with NMP, GBL and BCS, and stirred at room temperature for 2 hours to obtain a liquid crystal aligning agent (AL-1) having a mass ratio of polymer solid content to each solvent (polymer solid content: NMP: GBL: BCS) of 4:46:30:20. It was confirmed that the liquid crystal aligning agent was a uniform solution without abnormalities such as turbidity and precipitation.
[0194] <Comparative Examples 1 and 2>
[0195] Liquid crystal aligning agents AL-R1 and AL-R2 were prepared by the same method as in Example 1, except that PAA2 and PAA3 were used instead of PAA1.
[0196] The composition of each liquid crystal aligning agent obtained in the Example and the comparative example is shown in Table 1. In Table 1, the numerical value in the bracket|parenthesis of a composition ratio shows the ratio (mass part) of each structural component with respect to 100 mass parts of structural components of a liquid crystal aligning agent.
[0197] [Table 1]
[0198]
[0199] [Fabrication of FFS-driven liquid crystal cell]
[0200] A liquid crystal cell having a structure of a fringe field switching (FFS) mode liquid crystal display element was produced.
[0201] First, prepare a substrate with electrodes. A glass substrate with a size of 30mm×35mm and a thickness of 0.7mm is used as the substrate. An ITO electrode with a dense pattern constituting a counter electrode is formed on the substrate as the first layer, and a SiN (silicon nitride) film formed by CVD (chemical vapor deposition) is formed on the counter electrode of the first layer as the second layer. A SiN film with a film thickness of 300nm is used as an interlayer insulating film. A comb-shaped pixel electrode formed by patterning the ITO film is arranged on the second layer of the SiN film as the third layer, and two types of pixels, the first pixel and the second pixel, are formed, and the size of each pixel is 10mm long and about 5mm wide. At this time, the counter electrode of the first layer and the pixel electrode of the third layer are electrically insulated due to the action of the SiN film of the second layer.
[0202] The pixel electrode of the third layer has a comb-tooth shape in which multiple electrode elements with a width of 3 μm are arranged in parallel at intervals of 6 μm and the central part is bent at an internal angle of 160°. One pixel has a first area and a second area with a line connecting the bent parts of the multiple electrode elements as the boundary.
[0203] When the first area and the second area of each pixel are compared, the electrode elements constituting the pixel electrodes thereof are formed in different directions. That is, with reference to the line connecting the curved portions of the plurality of electrode elements, the electrode elements of the pixel electrodes in the first area of the pixel are formed at an angle of 80° clockwise, and the electrode elements of the pixel electrodes in the second area of the pixel are formed at an angle of 80° counterclockwise. That is, in the first area and the second area of each pixel, the directions of the rotational movement (in-plane conversion) of the liquid crystal within the substrate surface caused by the application of the voltage between the pixel electrode and the opposing electrode are opposite to each other.
[0204] Next, the liquid crystal alignment agent obtained in the above was filtered with a filter with a pore size of 1.0 μm, and then applied to the surface of the substrate with electrodes (first glass substrate) prepared in the above by spin coating. Then, after drying on a hot plate at 80°C for 2 minutes, it was calcined in a hot air circulation oven at 230°C for 20 minutes to obtain a polyimide film with a thickness of 60 nm. The polyimide film was subjected to a friction orientation treatment with a rayon cloth (HY-5318 manufactured by Hyperflex) (roller diameter: 120 mm, roller speed: 1000 rpm, moving speed: 30 mm / sec, pressing length: 0.4 mm, rubbing direction: 180° to the direction of the bending part of the above-mentioned multiple electrode elements connecting the pixel electrode of the third layer). Then, it was cleaned by ultrasonic irradiation in pure water for 1 minute, and after removing water droplets by blowing, it was dried in an oven at 80°C for 15 minutes to obtain a substrate with a liquid crystal alignment film. In addition, a glass substrate with a columnar spacer of 4 μm in height and an ITO electrode formed on the back as an opposing substrate was treated in the same manner as described above, and a substrate with a liquid crystal orientation film that had been subjected to orientation treatment was obtained. The two substrates with liquid crystal orientation films were grouped together, and a sealant (XN-1500T manufactured by Mitsui Chemicals Co., Ltd.) was printed in the form of a liquid crystal injection port on one substrate, and the other substrate was bonded in a manner in which the liquid crystal orientation film faces each other and the rubbing direction is antiparallel. Then, a heat treatment was performed at 150°C for 60 minutes to cure the sealant and produce an empty box with a cell gap of 4 μm. Negative liquid crystal MLC-7026-100 (manufactured by Merck) was injected into the empty box by a reduced pressure injection method, and the injection port was sealed to obtain a liquid crystal box of the FFS method. Then, the obtained liquid crystal box was heated at 120°C for 1 hour, and left at 23°C overnight for evaluation.
[0205] [Measurement of the absolute value of stored charge]
[0206] The liquid crystal box prepared in the above was placed between two polarizing plates arranged in an orthogonal manner, and the LED backlight was irradiated from below the two polarizing plates while the pixel electrode and the opposing electrode were short-circuited and in an equipotential state, and the angle of the liquid crystal box was adjusted so that the brightness of the LED backlight transmission light measured on the two polarizing plates was minimized. Then, while applying an AC voltage with a frequency of 30 Hz to the liquid crystal box, the V-T curve (voltage-transmittance curve) was measured, and the AC voltage at which the relative transmittance became 23% was calculated as the driving voltage.
[0207] In the absolute value measurement, an AC voltage with a frequency of 30Hz is applied to drive the liquid crystal box. The AC drive is performed every 3 minutes until the transmittance in the box reaches 100%. The V-F (voltage-flicker curve) curve is measured just after lighting, and the offset voltage at which the flicker becomes the minimum is calculated. Then, the change in the minimum offset voltage value is measured every 3 minutes, and the maximum voltage value when it changes from just after lighting to 30 minutes is calculated. At this time, if the change in the maximum offset voltage exceeds 20mV, it is defined as "bad" and evaluated. In addition, if the change in the maximum offset voltage does not exceed 20mV, it is defined as "good" and evaluated.
[0208] [Measurement of relaxation rate of stored charge]
[0209] The angle adjustment of the liquid crystal cell and the AC voltage (hereinafter, also referred to as AC voltage (V B The calculation of )) is performed in the same procedure as the determination of the absolute value of the accumulated charge described above.
[0210] Next, an AC voltage (V B ) to drive the liquid crystal box while applying a DC voltage of 1 V for 30 minutes. Then, the application of the DC voltage was stopped and the liquid crystal box was driven for a further 15 minutes using only the AC voltage.
[0211] The results are shown in Table 2. The results were evaluated as follows: if the relative transmittance relaxed to 25% or less after 10 minutes from the time when the DC voltage application was stopped, it was defined as "good", and if it took more than 10 minutes for the relative transmittance to drop to 25% or less, it was defined as "poor".
[0212] It should be noted that the evaluation of the relaxation rate of the stored charge according to the above method was performed under room temperature conditions.
[0213] [Photoresponse evaluation]
[0214] The liquid crystal cell produced above was placed between two polarizing plates arranged so that their polarization axes were perpendicular to each other.
[0215] In the photoresponse evaluation, the LED backlight was irradiated from below the two polarizing plates at the same time as the measurement started, and the flicker amplitude was tracked when the liquid crystal box was driven for 30 minutes with an AC voltage of 30 Hz at a relative transmittance of 23%. For the flicker amplitude, the transmitted light of the LED backlight that passed through the two polarizing plates and the liquid crystal box between them was read by a data collection / data recorder switch unit 34410A (manufactured by KEYSIGHT) connected via a photodiode and an IV conversion amplifier. The flicker level was calculated by the following formula.
[0216] Flicker level (%) = {flicker amplitude / (2×z)}×100
[0217] In the above formula, z is the value of brightness when driven by an AC voltage of a frequency of 30 Hz at a relative transmittance of 23%, which is read by the data collection / data recorder switch unit 34410A.
[0218] Regarding the evaluation of the photoresponsivity, the case where the change in flicker level was maintained at less than 3% from the time when the LED backlight was turned on and the AC voltage was applied until 30 minutes had passed was defined as "good", and the case where the change in flicker level reached 3% or more was defined as "poor". The results are shown in Table 2.
[0219] It should be noted that the evaluation of photoresponsivity according to the above method was performed at room temperature.
[0220] <Evaluation Results>
[0221] (Example 1 and Comparative Examples 1-2)
[0222] Table 2 shows the results of characteristic evaluation about the liquid crystal display elements obtained using the liquid crystal aligning agents (AL-1) and (AL-R1) to (AL-R2) obtained in Example 1 and Comparative Examples 1 to 2.
[0223] [Table 2]
[0224] Liquid crystal alignment agent Accumulation of charge Easing speed Photoresponse Example 1 AL-1 Good (18.5mV) good Good (1.2%) Comparative Example 1 AL-R1 Bad (89.5mV) good Bad (4.9%) Comparative Example 2 AL-R2 Bad (23.9mV) bad Good (1.3%)
[0225] As shown in Table 2, the liquid crystal display element using the liquid crystal orientation film of Example 1 obtained by the following liquid crystal orientation agent has good both the relaxation rate of accumulated charge and the light responsiveness, wherein the liquid crystal orientation agent uses a tetracarboxylic acid component containing CA-1 as a specific aromatic tetracarboxylic acid component (p) and a diamine component containing DA-1 as a specific diamine (p).
[0226] Description of Reference Numerals
[0227] 1: lateral electric field liquid crystal display element; 2: comb-tooth electrode substrate; 2a: substrate; 2b: linear electrode; 2c: liquid crystal orientation film; 2d: substrate; 2e: surface electrode; 2f: insulating film; 2g: linear electrode; 2h: liquid crystal orientation film; 3: liquid crystal; 4: opposing substrate; 4a: liquid crystal orientation film; 4b: substrate; L: electric line.
[0228] It should be noted that the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2022-073221 filed on Apr. 27, 2022 are incorporated herein by reference in their entirety and are incorporated as a disclosure of the specification of the present invention.
Claims
1. A liquid crystal alignment agent, wherein: The invention contains a polymer P, wherein the polymer P is at least one selected from the group consisting of a polyimide precursor obtained by using a tetracarboxylic acid component and a diamine component, and a polyimide which is an imide product of the polyimide precursor, wherein the tetracarboxylic acid component contains at least one selected from the group consisting of tetracarboxylic dianhydride represented by the following formula (1) and its derivatives, and the diamine component contains a diamine represented by the following formula (2), In the formula, X a represents a tetravalent organic group derived from aromatic tetracarboxylic dianhydride or a derivative thereof; Y2 represents a divalent organic group having 6 to 30 carbon atoms and containing one or more aromatic groups; Z2 each independently represents an alkylene group having 1 to 6 carbon atoms; A2 each independently represents an alkyl group having 1 to 6 carbon atoms; any hydrogen atom of the aromatic group in Y2 is optionally substituted by a monovalent group.
2. The liquid crystal alignment agent according to claim 1, wherein The Y2 is a structure represented by the following formula (3), In the formula, L is -CH2-, -O-, -C(=O)-, -N(R)-, cyclohexylene or alkylene having 2 to 18 carbon atoms, in the -N(R)-, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group; in the alkylene having 2 to 18 carbon atoms, any -CH2- of the alkylene is optionally substituted by -O-, -O-C(=O)-, -C(=O)-, -N(R)-, -N(R)-C(=O)-, cyclohexylene or phenylene, in the -N(R)-, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group, in the -N(R)-C(=O)-, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group, R3 represents a halogen atom, or an alkyl group or alkoxy group having 1 to 5 carbon atoms, any hydrogen atom of the alkyl group or the alkoxy group is optionally substituted by a halogen atom, and any hydrocarbon group is optionally substituted by an amino group protected by a tert-butyloxycarbonyl group, Multiple a's are each independently an integer of 0 to 4, b is an integer of 1 to 2, and c is an integer of 0 to 1; when multiple R3's and a's exist, they are optionally the same or different; * represents a bonding bond.
3. The liquid crystal alignment agent according to claim 2, wherein: The L is selected from any group of the following groups: -O-, -O-C(=O)-, -C(=O)-, -N(R)-, -N(R)-C(=O)-, -N(R)-C(=O)-N(R)-, -(CH2) p -、-O-(CH2) p -O-, -(CH2) p -O-C(=O)-(CH2) q -、 -(CH2) p -N(R)-(CH2) q -、 -(CH2) p -N(R)-C(=O)-N(R)-(CH2) q -、 -O-(CH2) p -O-(CH2) q -O-、 -(CH2) p’ -O-C(=O)-(CH2) q -C(=O)-O-(CH2) r’ -、 -(CH2) p’ -C(=O)-O-(CH2) q -O-C(=O)-(CH2) r’ -、 -(CH2) p’ -O-C(=O)-Q-C(=O)-O-(CH2) q’ -、 or -(CH2) p’ -C(=O)-O-Q-O-C(=O)-(CH2) q’ - In the formula, p is an integer of 1 to 6; q is an integer of 1 to 6; p', q', r' are each independently an integer of 0 to 6; in addition, 0≤p'+q'≤10, 2≤p'+q+r'≤16 are satisfied, in the -N(R)-, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group, in the -N(R)-C(=O)-, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group, in the -N(R)-C(=O)-N(R)-, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group; the two R's are optionally the same or different, the -(CH2) p -N(R)-(CH2) q -, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group, and the -(CH2) p -N(R)-C(=O)-N(R)-(CH2) q -, R represents a hydrogen atom, a methyl group or a tert-butyloxycarbonyl group; two Rs are optionally the same or different, and the -(CH2) p’ -O-C(=O)-Q-C(=O)-O-(CH2) q’ -, Q represents phenylene or cyclohexylene, the -(CH2) p’ -C(=O)-O-Q-O-C(=O)-(CH2) q’ -, Q represents a phenylene group or a cyclohexylene group. 4 . The liquid crystal aligning agent according to claim 1 , wherein The diamine represented by the formula (2) is a diamine represented by any of the following formulas (d2-1) to (d2-3), 5. The liquid crystal aligning agent according to any one of claims 1 to 3, wherein The amount of the diamine represented by the formula (2) used is 5 mol% or more based on 1 mol of the diamine component used to produce the polymer P.
6. The liquid crystal aligning agent according to any one of claims 1 to 5, wherein X in the formula (1) a is any structure selected from the structures of the following formulae (Xa-1) and (Xa-2), In formulas (Xa-1) to (Xa-2), j and k are integers of 0 or 1, A1 and A2 each independently represent a single bond, -O-, -C(=O)-, -O-C(=O)-, phenylene, -S(=O)2- or -NR-C(=O)-, in which -NR-C(=O)-, R represents a hydrogen atom or a methyl group; multiple A2s are optionally the same or different; * represents a bonding bond.
7. The liquid crystal alignment agent according to claim 6, wherein: The formulae (Xa-1) and (Xa-2) are any structures selected from the following formulae (Xa-3) to (Xa-18), In the formula, * represents a bonding bond.
8. The liquid crystal aligning agent according to any one of claims 1 to 7, wherein The amount of the tetracarboxylic dianhydride represented by the formula (1) and its derivatives used is 10 mol% or more based on 1 mol of the tetracarboxylic acid component used to produce the polymer P. 9 . A liquid crystal alignment film obtained from the liquid crystal alignment agent according to claim 1 . 10 . A liquid crystal display element comprising the liquid crystal alignment film according to claim 9 .
11. A method for manufacturing a liquid crystal display element, comprising the following steps 1 to 3: Step 1: a step of applying the liquid crystal alignment agent according to any one of claims 1 to 8 onto a substrate; Step 2: a step of calcining the applied liquid crystal alignment agent to obtain a film; Step 3: a step of subjecting the film obtained in step 2 to an orientation treatment.
Citation Information
Patent Citations
Liquid crystal aligning agent, liquid crystal alignment film and liquid crystal display element
JP2019101196A
Arrangement structure of drive device, fitting method of the same and vehicle organization
JP2022073221A
Liquid-crystal alignment agent, liquid-crystal alignment film, and liquid-crystal display element
WO2011132751A1
Liquid crystal alignment treatment agent, liquid crystal alignment film, and liquid crystal display element
WO2011155577A1
Method for producing ion-exchange membrane and ion-exchange membrane obtained thereby
WO2015030071A1