Preparation method of metal grid and preparation method of antenna
Patent Information
- Application Number
- CN202380008495.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-29
AI Technical Summary
The existing technology is difficult to prepare metal meshes with narrow line widths, which affects the performance of thin film displays and radio frequency devices. In particular, the demand for higher cutoff frequencies in transparent antennas and radio frequency devices cannot be met.
Inductively coupled plasma equipment is used for dry etching to form grid-shaped grooves, and a metal film is grown in the grooves through electroplating technology to form a metal grid with a narrow line width, taking advantage of the anisotropy of inductively coupled plasma equipment. Reduce etching radius loss.
The preparation of a metal mesh with a line width less than 1.5 μm is achieved, which improves the light transmittance and radio frequency performance of the antenna and meets the demand for a higher cut-off frequency.
Smart Images

Figure CN119096336A_ABST
Abstract
Description
Method for preparing metal grid and method for preparing antenna Technical Field
[0001] The present disclosure belongs to the technical field of electronic devices, and particularly relates to a method for preparing a metal grid and a method for preparing an antenna. Background Art
[0002] Currently, the linewidths commonly used in micro-nanofabrication processes in the glass-based semiconductor industry are around 2-3μm. However, certain thin-film display and sensor devices, such as transparent antennas and RF devices, place even higher demands on micro-nanofabrication linewidths. The former primarily uses narrow-linewidth metal meshes as signal transmitters and receivers, while the latter employs narrower channel lengths in RF devices to achieve higher cutoff frequencies.
[0003] Summary of the Invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art and provides a method for preparing a metal grid and a method for preparing an antenna.
[0005] In a first aspect, an embodiment of the present disclosure provides a method for preparing a metal mesh, comprising:
[0006] providing a substrate;
[0007] A dielectric layer is formed on the substrate, and the dielectric layer is dry-etched using an inductively coupled plasma device to form grid-shaped grooves.
[0008] The dielectric layer includes a first dielectric layer and a second dielectric layer stacked together; the step of forming the dielectric layer on the substrate and dry-etching the dielectric layer using an inductively coupled plasma device to form a grid-shaped groove includes:
[0009] forming the first dielectric layer on the base substrate;
[0010] forming the second dielectric layer on a side of the first dielectric layer facing away from the base substrate;
[0011] forming a first photoresist layer on a side of the second dielectric layer facing away from the first dielectric layer, and exposing and developing the first photoresist layer to form a first grid pattern;
[0012] dry-etching the second dielectric layer using an inductively coupled plasma device to remove exposed second dielectric layer material, thereby forming a second grid pattern; using the second grid pattern as a mask, dry-etching the first dielectric layer using an inductively coupled plasma device to remove exposed first dielectric layer material, thereby forming a third grid pattern; the second grid pattern and the third grid pattern are stacked to form the grid-shaped grooves;
[0013] The remaining first photoresist layer is removed.
[0014] The first dielectric layer includes an organic material, and the etching gas used to etch the first dielectric layer is oxygen.
[0015] The organic material includes any one of polyimide, epoxy resin, acrylic, polyester, photoresist, polyacrylate, polyamide, and siloxane.
[0016] Wherein, the thickness of the first dielectric layer is 2 μm-5 μm.
[0017] The second dielectric layer includes an inorganic material; and the etching gas used to etch the second dielectric layer is tetrafluoromethane.
[0018] Wherein, the inorganic material includes any one of silicon nitride, silicon oxide, and silicon oxynitride.
[0019] Wherein, the thickness of the second dielectric layer is 50nm-400nm.
[0020] The step of forming the first dielectric layer on the base substrate includes:
[0021] A first dielectric material is formed on the base substrate through a coating process, and then cured at high temperature to form a first dielectric layer.
[0022] The step of forming the second dielectric layer on the side of the first dielectric layer facing away from the base substrate includes:
[0023] The second dielectric layer is formed on a side of the first dielectric layer facing away from the substrate by using plasma chemical vapor deposition equipment.
[0024] The method for preparing the metal grid further includes: before forming the dielectric layer on the substrate, the method further includes:
[0025] forming a first metal film on the base substrate and using the first metal film as a seed layer;
[0026] After forming the grid-shaped grooves, the method further includes: removing the second grid pattern;
[0027] electroplating the seed layer to enable growth of a first metal film within the groove;
[0028] The dielectric layer and the first metal film on a side of the dielectric layer close to the substrate are removed to form a metal grid.
[0029] Wherein, the material of the first metal film includes copper or silver.
[0030] The method for preparing the metal grid further comprises: after forming the grid-shaped grooves, the method further comprises:
[0031] removing the second grid pattern;
[0032] forming a first metal film on a side of the grid-shaped groove facing away from the base substrate, and using the first metal film as a seed layer;
[0033] The seed layer is electroplated to grow a first metal film, and the grown first metal film outside the grid-shaped groove is removed to form a metal grid.
[0034] Wherein, the material of the first metal film includes copper or silver.
[0035] Wherein, the width of the grid-shaped groove portion is no greater than 1.5 μm.
[0036] In a second aspect, an embodiment of the present disclosure provides a method for manufacturing an antenna, comprising:
[0037] Providing a first dielectric substrate, the first dielectric substrate comprising a first surface and a second surface disposed opposite to each other along a thickness direction thereof;
[0038] forming a reference electrode layer on the first surface of the first dielectric substrate;
[0039] A radiation portion is formed on the second surface of the first dielectric substrate; wherein,
[0040] At least one of the reference electrode layer and the radiation portion includes a metal grid, and the metal grid is prepared by any of the above-mentioned preparation methods.
[0041] The reference electrode layer and the radiating portion are metal grids, and the orthographic projections of the reference electrode layer and the hollow portion of the radiating portion on the first dielectric substrate overlap.
[0042] The first dielectric substrate includes a first sub-dielectric layer, a first bonding layer, and a second sub-dielectric layer that are stacked. The reference electrode layer is formed on a side of the first sub-dielectric layer facing away from the first bonding layer. The radiation portion is provided on a side of the second sub-dielectric layer facing away from the first bonding layer.
[0043] Wherein, the material of the first sub-dielectric layer and / or the second sub-dielectric layer includes polyimide or polyethylene terephthalate.
[0044] The first dielectric substrate is a single-layer structure, and its material includes polyimide or polyethylene terephthalate. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] FIG1 is a schematic diagram of the structure of an exemplary thin film sensor.
[0046] FIG2 is a schematic diagram of a cross-sectional structure of the thin film sensor shown in FIG1 along the AA′ direction.
[0047] FIG3 is a top view of the grid-shaped grooves according to an embodiment of the present disclosure.
[0048] FIG4 is a schematic diagram of the cross-sectional structure of the grid-shaped groove in the BB′ direction shown in FIG3 .
[0049] FIG5 is a flowchart of a first example of forming grid-shaped grooves in a method for preparing a metal grid according to an embodiment of the present disclosure.
[0050] FIG6 is a test diagram of a first example of forming grid-shaped grooves in the method for preparing a metal grid according to an embodiment of the present disclosure.
[0051] FIG. 7 is a test diagram of a second example of forming grid-shaped grooves in the method for preparing the metal grid according to an embodiment of the present disclosure.
[0052] FIG8 is a test diagram of a third example of forming grid-shaped grooves in the method for preparing the metal grid according to an embodiment of the present disclosure.
[0053] FIG. 9 is a top view of a metal grid according to an embodiment of the present disclosure.
[0054] FIG10 is a schematic diagram of the cross-sectional structure of the metal grid shown in FIG9 in the CC′ direction.
[0055] FIG11 is a preparation flow chart of a first example of a method for preparing a metal grid according to an embodiment of the present disclosure.
[0056] FIG. 12 is a test diagram of a fourth example of forming grid-shaped grooves in the method for preparing the metal grid according to an embodiment of the present disclosure.
[0057] FIG. 13 is a test diagram of a fifth example of forming grid-shaped grooves in the method for preparing a metal grid according to an embodiment of the present disclosure.
[0058] FIG. 14 is a test diagram of a sixth example of forming grid-shaped grooves in the method for preparing a metal grid according to an embodiment of the present disclosure.
[0059] FIG15 is a cross-sectional view of the antenna according to an embodiment of the present disclosure.
[0060] FIG16 is another cross-sectional view of the antenna according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0061] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings and specific implementation methods.
[0062] Unless otherwise defined, the technical or scientific terms used in this disclosure should have the usual meanings understood by people with ordinary skills in the field to which this disclosure belongs. The words "first", "second" and similar words used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one", "an" or "the" do not indicate a quantity limitation, but rather indicate the existence of at least one. Words such as "include" or "comprise" mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Words such as "connect" or "connected" are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0063] Figure 1 is a schematic diagram of the structure of an exemplary thin film sensor; Figure 2 is a schematic diagram of the cross-sectional structure of the thin film sensor shown in Figure 1 along the AA' direction. As shown in Figures 1 and 2, the thin film sensor includes: a base substrate 100 having a first surface and a second surface (i.e., an upper surface and a lower surface) disposed opposite each other; a first conductive layer 101 and a second conductive layer 102 located on the first and second surfaces of the base substrate 100, respectively. For example, in the case of a thin film sensor being a transparent antenna, the first conductive layer 101 can be a radiating layer, and the second conductive layer 102 can be a grounding layer. The radiating layer can serve as either the receiving element or the transmitting element of the antenna structure.
[0064] In order to ensure that the first conductive layer 101 and the second conductive layer 102 have good light transmittance, the first conductive layer 101 and the second conductive layer 102 need to be patterned. For example, the first conductive layer 101 can be composed of grid lines made of metal materials, and the second conductive layer 102 can also be composed of grid lines made of metal materials. It is understandable that the first conductive layer 101 and the second conductive layer 102 can also be composed of structures with other patterns, such as block electrodes with patterns such as diamonds and triangles, which are not listed one by one here. As can be seen from Figure 1, the first conductive layer 101 and the second conductive layer 102, that is, grid lines, are not provided on the entire surface of the two surfaces of the base substrate 100. Any grid line is composed of an electrically connected metal grid. Due to the material and formation process of the metal grid, the line width of the metal grid is relatively wide, which seriously affects the light transmittance of the thin film sensor, thereby affecting the user experience.
[0065] In some examples, in order to form a metal grid 501 with a narrow line width, a first dielectric layer 200 and a second dielectric layer 300 can be formed in sequence on the base substrate 100, wherein the first dielectric layer 200 serves as a buffer layer (Buffer) and the second dielectric layer 300 serves as a hard mask layer (Hard Mask), and then wet etching is performed to form a grid-shaped groove 201, and then a metal material is formed in the groove, that is, a metal grid 501 is formed. However, due to the different material types and thicknesses of the buffer layer and the hard mask layer, after the etching process, the vertices of the diamond blocks in the grid-shaped groove 201 will be "passivated" to varying degrees to form rounded corners, and the radius thereof is the etching loss radius. The line width at the intersection of the grid-shaped grooves will increase to varying degrees, thereby affecting the gain of the antenna.
[0066] It should also be noted that the metal grid 501 is not limited to being used in antenna structures, but can also be used in touch panels as touch electrodes. Of course, the metal grid 501 can also be used in various metal wires, which are not listed here one by one.
[0067] First, to address the aforementioned issues, embodiments of the present disclosure provide a method for fabricating a metal grid, comprising: providing a substrate; forming a dielectric layer on the substrate; and dry-etching the dielectric layer using an inductively coupled plasma (ICP) apparatus to form a grid of grooves. The grid-shaped grooves are used for subsequent formation of the metal grid.
[0068] In the embodiment of the present disclosure, an inductively coupled plasma device is used to dry etch the dielectric layer. Compared with the above-mentioned wet etching, it has better anisotropy and less impact on the etching radius loss, which helps to subsequently form a metal grid with a narrower line width, thereby reducing the impact on the antenna gain.
[0069] In some examples, the base substrate in the embodiments of the present disclosure may be glass-based or a flexible film. The flexible film material may be at least one of COP film, polyimide (PI), or polyethylene terephthalate (PET). In the embodiments of the present disclosure, only the glass-based base substrate is used as an example for description.
[0070] In some examples, the dielectric layer may include a first dielectric layer and a second dielectric layer. Specifically, the first dielectric layer 200 may be a buffer layer, and the second dielectric layer may be a hard mask layer. Furthermore, the buffer layer includes, but is not limited to, organic materials, such as polyimide, epoxy resin, acrylic, polyester, photoresist, polyacrylate, polyamide, siloxane and other resin materials. The hard mask layer includes, but is not limited to, inorganic materials, metal oxides, metal materials, etc. Inorganic materials such as silicon nitride (SiNx), silicon oxide (SiO2), silicon oxynitride (SiON), etc.; metal materials such as copper (Cu), aluminum (Al), molybdenum (Mo), silver (Ag); metal oxides such as indium tin oxide (ITO), etc. In the embodiment of the present disclosure, the material of the hard mask layer is an inorganic material as an example.
[0071] The following specifically describes the steps of forming the grid-shaped grooves 201 when the buffer layer and the hard mask layer are made of different materials and have different thicknesses.
[0072] Figure 3 is a top view of the grid-shaped groove of the embodiment of the present disclosure; Figure 4 is a schematic diagram of the cross-sectional structure of the grid-shaped groove in the BB' direction shown in Figure 3; Figure 5 is a preparation flow chart of the first example of forming grid-shaped grooves in the preparation method of the metal grid of the embodiment of the present disclosure; as shown in Figures 3-5, the first example: S11, coating a 4μm thick epoxy resin on the base substrate 100 as a buffer layer, and high-temperature curing the buffer layer.
[0073] S12 . On the side of the buffer layer facing away from the base substrate 100 , a plasma enhanced chemical vapor deposition (PECVD) device is used to deposit silicon nitride with a thickness of about 200 nm at a high temperature as a hard mask layer.
[0074] S13 , coating a first photoresist layer 400 ( BFP100 ) on a side of the hard mask layer away from the buffer layer, and performing exposure and development to form a first grid pattern 401 .
[0075] S14. Use inductively coupled plasma equipment to dry-etch the hard mask layer to remove the exposed hard mask layer material and form a second grid pattern; use the second grid pattern as a mask and use inductively coupled plasma equipment to dry-etch the buffer layer to remove the exposed buffer layer material to form a third grid pattern 2011, and remove the remaining first photoresist layer 400. The second grid pattern and the third grid pattern 2011 are stacked to form a grid-shaped groove 201.
[0076] Among them, the etching gas used for dry etching of the hard mask layer in the inductively coupled plasma equipment is tetrafluoromethane (CF4) gas, which etches the exposed material of the hard mask layer while also slightly etching the first photoresist layer 400. Next, the etching gas used for etching the buffer layer is oxygen (O2), which etches the first photoresist layer 400 while etching the buffer layer. Since dry etching using inductively coupled plasma equipment has better anisotropy than wet etching, it has less effect on the loss of etching radius. Figure 6 is a test diagram of the first example of forming a grid-shaped groove in the method for preparing the metal grid of the embodiment of the present disclosure; as shown in Figure 6, after testing, the etching loss radius finally formed by the first example is about 0.77μm, which meets the process requirement of less than 1.5μm.
[0077] Example 2: The process is the same as Example 1, except for the thickness of the buffer layer and the material of the hard mask layer. The specific steps of Example 2 are as follows:
[0078] S21 , coating a 3.3 μm thick epoxy resin on the base substrate 100 as a buffer layer, and curing the buffer layer at a high temperature.
[0079] S22 . On the side of the buffer layer facing away from the base substrate 100 , a plasma enhanced chemical vapor deposition (PECVD) device is used to deposit silicon oxide with a thickness of about 300 nm at a high temperature as a hard mask layer.
[0080] S23 , coating a first photoresist layer 400 ( BFP100 ) on a side of the hard mask layer away from the buffer layer, and performing exposure and development to form a first grid pattern 401 .
[0081] S24. Use inductively coupled plasma equipment to dry-etch the hard mask layer to remove the exposed hard mask layer material and form a second grid pattern; use the second grid pattern as a mask and use inductively coupled plasma equipment to dry-etch the buffer layer to remove the exposed buffer layer material to form a third grid pattern 2011, and remove the remaining first photoresist layer 400. The second grid pattern and the third grid pattern 2011 are stacked to form a grid-shaped groove 201.
[0082] Among them, the etching gas used for dry etching of the hard mask layer in the inductively coupled plasma equipment is tetrafluoromethane (CF4) gas, which etches the exposed hard mask layer material while also slightly etching the first photoresist layer 400. Next, the etching gas used for etching the buffer layer is oxygen (O2), which etches the first photoresist layer 400 while etching the buffer layer. Since dry etching using inductively coupled plasma equipment has better anisotropy than wet etching, it has less effect on the loss of etching radius. Figure 7 is a test diagram of the second example of forming a grid-shaped groove in the method for preparing the metal grid of the embodiment of the present disclosure; as shown in Figure 7, after testing, the etching loss radius finally formed by the second example is about 1.18μm, which meets the process requirement of less than 1.5μm.
[0083] Example 3: The process is the same as Example 1, except for the thickness of the buffer layer and the material of the hard mask layer. The specific steps of Example 3 are as follows:
[0084] S31 , coating a 5.5 μm thick epoxy resin on the base substrate 100 as a buffer layer, and curing the buffer layer at a high temperature.
[0085] S32 , on the side of the buffer layer facing away from the base substrate 100 , using plasma enhanced chemical vapor deposition (PECVD) equipment to deposit silicon oxynitride (a mixture of silicon oxide and silicon nitride) with a thickness of about 200 nm as a hard mask layer at high temperature.
[0086] S33 , coating a first photoresist layer 400 ( BFP100 ) on a side of the hard mask layer away from the buffer layer, and performing exposure and development to form a first grid pattern 401 .
[0087] S34. Use inductively coupled plasma equipment to dry-etch the hard mask layer to remove the exposed hard mask layer material and form a second grid pattern; use the second grid pattern as a mask and use inductively coupled plasma equipment to dry-etch the buffer layer to remove the exposed buffer layer material to form a third grid pattern 2011, and remove the remaining first photoresist layer 400. The second grid pattern and the third grid pattern 2011 are stacked to form a grid-shaped groove 201.
[0088] Among them, the etching gas used for dry etching of the hard mask layer in the inductively coupled plasma equipment is tetrafluoromethane (CF4) gas, which etches the exposed material of the hard mask layer while also slightly etching the first photoresist layer 400. Next, the etching gas used for etching the buffer layer is oxygen (O2), which etches the first photoresist layer 400 while etching the buffer layer. Since dry etching using inductively coupled plasma equipment has better anisotropy than wet etching, it has less effect on the loss of etching radius. Figure 8 is a test diagram of the third example of forming a grid-shaped groove in the method for preparing the metal grid of the embodiment of the present disclosure; as shown in Figure 8, after testing, the etching loss radius finally formed by the third example is about 0.76μm, which meets the process requirement of less than 1.5μm.
[0089] In some examples, the method for fabricating a thin film sensor according to embodiments of the present disclosure includes not only the step of forming a grid-shaped groove 201 on the base substrate 100, but also the step of forming a metal grid 501. The material of the metal grid 501 includes, but is not limited to, copper, silver, etc. This will be described below with reference to specific examples.
[0090] Fourth Example: Figure 9 is a top view of the metal mesh of the embodiment of the present disclosure. Figure 10 is a schematic diagram of the cross-sectional structure of the metal mesh shown in Figure 9 in the CC' direction. Figure 11 is a preparation flow chart of the first example of the preparation method of the metal mesh of the embodiment of the present disclosure; as shown in Figures 9-11, the preparation method of the fourth example includes: S41, forming a first metal film 500 on the base substrate 100, and the process for forming the first metal film 500 includes but is not limited to magnetron sputtering. The material of the first metal film 500 is copper, and the thickness is 300nm.
[0091] S42 , coating a 4.9 μm thick epoxy resin as a buffer layer on a side of the first metal film layer away from the base substrate 100 , and curing the buffer layer at a high temperature.
[0092] S43 , on the side of the buffer layer facing away from the base substrate 100 , using plasma enhanced chemical vapor deposition (PECVD) equipment to deposit silicon nitride with a thickness of about 300 nm as a hard mask layer at high temperature.
[0093] S44 , coating a first photoresist layer 400 ( BFP100 ) on a side of the hard mask layer away from the buffer layer, and performing exposure and development to form a first grid pattern 401 .
[0094] S45. Use inductively coupled plasma equipment to dry-etch the hard mask layer to remove the exposed hard mask layer material to form a second grid pattern; use the second grid pattern as a mask and use inductively coupled plasma equipment to dry-etch the buffer layer to remove the exposed buffer layer material to form a third grid pattern 2011, and remove the remaining first photoresist layer 400. The second grid pattern and the third grid pattern 2011 are stacked to form a grid-shaped groove 201.
[0095] Among them, the etching gas used for dry etching of the hard mask layer in the inductively coupled plasma equipment is tetrafluoromethane (CF4) gas, which etches the exposed hard mask layer material while also slightly etching the first photoresist layer 400. Next, the etching gas used for etching the buffer layer is oxygen (O2), which etches the first photoresist layer 400 while etching the buffer layer. Since dry etching using an inductively coupled plasma equipment has better anisotropy than wet etching, it has less impact on the loss of etching radius. Figure 12 is a test diagram of the fourth example of forming a grid-shaped groove in the preparation method of the metal grid of the embodiment of the present disclosure; as shown in Figure 12, after testing, the final etching loss radius formed by the fourth example is about 0.82μm, which meets the process requirement of less than 1.5μm. However, it should be noted that when etching the buffer layer with oxygen, the time should not be too long, as this will not only cause loss of etching radius, but also cause oxidation of the seed layer.
[0096] S46, removing the second grid pattern.
[0097] S47: Use the first metal film layer as a seed layer and electroplate the seed layer.
[0098] In some examples, step S47 specifically includes placing one side of the base substrate 100 with the grid-shaped groove 201 on the electroplating machine carrier, pressing the power pad, placing it in a hole-filling electroplating tank (using a dedicated hole-filling electrolyte in the tank), applying current, and maintaining a continuous and rapid flow of the electroplating solution on the surface of the base substrate 100. On the sidewalls of the groove, the cations in the electroplating solution gain electrons and become atoms that are deposited on the sidewalls. Through the specially formulated dedicated hole-filling electrolyte, it is possible to achieve high-speed deposition of metallic copper (deposition rate 0.5-3 μm / min) mainly in the groove. Over time, the metallic copper on the sidewalls of the groove gradually grows thicker, and can even completely fill the groove. Finally, the base substrate 100 is removed and rinsed with deionized water.
[0099] S48 , removing the material of the first metal film layer on the base substrate 100 except the metal material in the groove to form a metal grid 501 .
[0100] Example 5: The process is the same as that of Example 4, except that the thickness of the buffer layer and the material of the hard mask layer are different from those of Example 1. The specific steps of Example 3 are as follows:
[0101] S51, forming a first metal film 500 on the base substrate 100. The process of forming the first metal film 500 includes but is not limited to magnetron sputtering. The material of the first metal film 500 is copper, and the thickness is 300 nm.
[0102] S52 , coating a 3.3 μm thick epoxy resin as a buffer layer on a side of the first metal film layer away from the base substrate 100 , and curing the buffer layer at a high temperature.
[0103] S53 , on the side of the buffer layer facing away from the base substrate 100 , using plasma enhanced chemical vapor deposition (PECVD) equipment to deposit silicon oxynitride (a mixture of silicon nitride and silicon oxide) with a thickness of about 100 nm as a hard mask layer at high temperature.
[0104] S54 , coating a first photoresist layer 400 ( BFP100 ) on a side of the hard mask layer away from the buffer layer, and performing exposure and development to form a first grid pattern 401 .
[0105] S55. Use inductively coupled plasma equipment to dry-etch the hard mask layer to remove the exposed hard mask layer material and form a second grid pattern; use the second grid pattern as a mask and use inductively coupled plasma equipment to dry-etch the buffer layer to remove the exposed buffer layer material to form a third grid pattern 2011, and remove the remaining first photoresist layer 400. The second grid pattern and the third grid pattern 2011 are stacked to form a grid-shaped groove 201.
[0106] Among them, the etching gas used for dry etching of the hard mask layer in the inductively coupled plasma equipment is tetrafluoromethane (CF4) gas, which etches the exposed hard mask layer material while also slightly etching the first photoresist layer 400. Next, the etching gas used for etching the buffer layer is oxygen (O2), which etches the first photoresist layer 400 while etching the buffer layer. Since dry etching using an inductively coupled plasma equipment has better anisotropy than wet etching, it has less effect on the loss of etching radius. Figure 13 is a test diagram of the fifth example of forming a grid-shaped groove in the preparation method of the metal grid of the embodiment of the present disclosure; as shown in Figure 13, after testing, the etching loss radius finally formed by the fifth example is about 0.60μm, which meets the process requirement of less than 1.5μm. However, it should be noted that when etching the buffer layer with oxygen, the time should not be too long, as this will not only cause loss of etching radius, but also cause oxidation of the seed layer.
[0107] S56: Remove the second grid pattern.
[0108] S57: Use the first metal film layer as a seed layer and electroplate the seed layer.
[0109] In some examples, step S57 specifically includes placing one side of the base substrate 100 with the grid-shaped grooves 201 on an electroplating machine carrier, pressing a power pad, and placing it in a hole-filling electroplating tank (using a dedicated hole-filling electrolyte in the tank). Current is applied, and the electroplating solution is maintained to flow rapidly on the surface of the base substrate 100. On the sidewalls of the grooves, cations in the electroplating solution gain electrons, becoming atoms and depositing on the sidewalls. Through the specially formulated dedicated hole-filling electrolyte, it is possible to achieve high-speed deposition of metallic copper (deposition rate 0.5-3 μm / min) primarily in the grooves. Over time, the metallic copper on the sidewalls of the grooves gradually grows thicker, and can even completely fill the grooves. Finally, the base substrate 100 is removed and rinsed with deionized water.
[0110] S58 , removing the material of the first metal film layer on the base substrate 100 except the metal material in the groove to form a metal grid 501 .
[0111] Example 6: The process is the same as that of Example 4, except that the thickness of the buffer layer and the material of the hard mask layer are different from those of Example 1. The specific steps of Example 3 are as follows:
[0112] S61: Form a first metal film 500 on the base substrate 100. The process of forming the first metal film 500 includes but is not limited to magnetron sputtering. The material of the first metal film 500 is silver, and the thickness is 300 nm.
[0113] S62 , coating a 3.3 μm thick epoxy resin as a buffer layer on a side of the first metal film layer away from the base substrate 100 , and curing the buffer layer at a high temperature.
[0114] S63 , on the side of the buffer layer facing away from the base substrate 100 , using plasma enhanced chemical vapor deposition (PECVD) equipment to deposit silicon oxynitride (a mixture of silicon nitride and silicon oxide) with a thickness of about 100 nm as a hard mask layer at high temperature.
[0115] S64 , coating a first photoresist layer 400 ( BFP100 ) on a side of the hard mask layer away from the buffer layer, and performing exposure and development to form a first grid pattern 401 .
[0116] S65. Use inductively coupled plasma equipment to dry-etch the hard mask layer to remove the exposed hard mask layer material and form a second grid pattern; use the second grid pattern as a mask and use inductively coupled plasma equipment to dry-etch the buffer layer to remove the exposed buffer layer material to form a third grid pattern 2011, and remove the remaining first photoresist layer 400. The second grid pattern and the third grid pattern 2011 are stacked to form a grid-shaped groove 201.
[0117] During dry etching of the hard mask layer in an inductively coupled plasma (ICP) device, the etching gas used is tetrafluoromethane (CF4). While etching the exposed hard mask layer material, the first photoresist layer 400 is also slightly etched. Subsequently, the etching gas used to etch the buffer layer is oxygen (O2). This etching also etches the first photoresist layer 400. Because dry etching using an ICP device exhibits greater anisotropy than wet etching, it has less impact on etch radius loss. Figure 14 shows a test image of the sixth example of the grid-shaped grooves of the thin film sensor according to an embodiment of the present disclosure. As shown in Figure 14, the final etch radius loss of the sixth example is approximately 0.68 μm, meeting the process requirement of less than 1.5 μm. However, it should be noted that when etching the buffer layer with oxygen, the etching time should not be too long, as this will not only result in etch radius loss but also oxidation of the seed layer.
[0118] S66: Remove the second grid pattern.
[0119] S67: Use the first metal film layer as a seed layer and electroplate the seed layer.
[0120] In some examples, step S66 specifically includes placing one side of the base substrate 100 with the grid-shaped grooves 201 on an electroplating machine carrier, pressing a power pad, and placing it in a via-filling plating tank (using a dedicated via-filling electrolyte in the tank). Current is applied, and the plating solution is maintained to flow rapidly over the surface of the base substrate 100. On the sidewalls of the grooves, cations in the plating solution gain electrons, becoming atoms that are deposited on the sidewalls. Through the specially formulated dedicated via-filling electrolyte, it is possible to achieve high-speed copper deposition (deposition rate of 0.5-3 μm / min) primarily in the grooves. Over time, the copper on the sidewalls of the grooves gradually grows thicker, and can even completely fill the grooves. Finally, the base substrate 100 is removed and rinsed with deionized water.
[0121] S68 , removing the material of the first metal film layer on the base substrate 100 except the metal material in the groove to form a metal grid 501 .
[0122] Of course, in some examples, after forming the grid-shaped groove 201, a first metal film 500 can be formed as a seed layer, and then electroplating is performed to grow the metal material in the groove, and finally the remaining first metal film 500 outside the metal material in the groove is removed to form a metal grid 501.
[0123] In a second aspect, Figure 15 is a cross-sectional view of an antenna according to an embodiment of the present disclosure. As shown in Figure 15 , an embodiment of the present disclosure provides a method for fabricating an antenna, comprising providing a first dielectric substrate comprising a first surface and a second surface disposed opposite each other along its thickness; forming a reference electrode layer on the first surface of the first dielectric substrate; and forming a radiating portion on the second surface of the first dielectric substrate. At least one of the reference electrode layer and the radiating portion is a metal mesh, which can be fabricated using any of the aforementioned fabrication methods.
[0124] If the reference electrode layer and the radiating portion both adopt a metal grid structure, the antenna formed at this time is a transparent antenna. Transparent antennas can be used in glass window systems including but not limited to cars, trains (including high-speed trains), airplanes, buildings, etc. The transparent antenna can be fixed on the inner side of the glass window (the side close to the interior). Since the optical transmittance of the transparent antenna is relatively high, it does not have a significant impact on the transmittance of the glass window while realizing the communication function, and this type of transparent antenna will also become a trend of beautifying antennas. Among them, the glass windows in the embodiments of the present disclosure include but are not limited to double-layer glass, and the types of glass windows can also be single-layer glass, laminated glass, thin glass, thick glass, etc.
[0125] In the disclosed embodiment, both the reference electrode layer and the radiating portion utilize metal meshes, and the orthographic projections of the hollowed-out portions of the metal meshes overlap on the first dielectric substrate to improve light transmittance. The first and second metal wires of the metal mesh may extend perpendicularly to each other, in which case a perpendicular or rectangular hollowed-out portion is formed. Of course, the first and second metal wires of the metal mesh may extend in non-perpendicular directions, for example, at a 45° angle between the first and second metal wires, forming a diamond-shaped hollowed-out portion.
[0126] In some examples, the first dielectric substrate may be the above-mentioned base substrate, or may be a separately provided dielectric substrate. The first dielectric substrate in the embodiment of the present disclosure may be a single-layer structure, and its material may be polyimide or polyethylene terephthalate. Figure 16 is another cross-sectional view of the antenna of the embodiment of the present disclosure; as shown in Figure 16, the first dielectric substrate in the embodiment of the present disclosure comprises a first sub-dielectric layer, a first bonding layer, a second sub-dielectric layer, a second bonding layer, and a third sub-dielectric layer stacked in sequence; wherein the reference electrode layer is arranged on the side of the first sub-dielectric layer close to the first bonding layer; and the radiating portion is arranged on the side of the second sub-dielectric layer close to the second bonding layer. The material of the first sub-dielectric layer may be polyimide or polyethylene terephthalate, and the material of the second sub-dielectric layer may also be polyimide or polyethylene terephthalate. The material of the first bonding layer may be transparent optical adhesive.
[0127] Of course, the method for preparing the antenna according to the embodiment of the present disclosure may further include steps of forming a feeding network and other structures, which are not listed here one by one.
[0128] It will be understood that the above embodiments are merely exemplary embodiments for illustrating the principles of the present invention, and the present invention is not limited thereto. Those skilled in the art will appreciate that various modifications and improvements can be made without departing from the spirit and substance of the present invention, and such modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a metal grid, wherein include: providing a substrate base plate; A dielectric layer is formed on the substrate, and the dielectric layer is dry-etched by using an inductively coupled plasma device to form grid-shaped grooves.
2. The method for preparing the metal mesh according to claim 1, in, The dielectric layer comprises a first dielectric layer and a second dielectric layer which are stacked; The step of forming a dielectric layer on the substrate and dry-etching the dielectric layer using an inductively coupled plasma device to form grid-shaped grooves includes: forming the first dielectric layer on the base substrate; forming the second dielectric layer on a side of the first dielectric layer away from the substrate; forming a first photoresist layer on a side of the second dielectric layer facing away from the first dielectric layer, and exposing and developing the first photoresist layer to form a first grid pattern; The second dielectric layer is dry-etched by using an inductively coupled plasma device to remove the exposed second dielectric layer material to form a second grid pattern; the first dielectric layer is dry-etched by using an inductively coupled plasma device using the second grid pattern as a mask to remove the exposed first dielectric layer material to form a third grid pattern, wherein the second grid pattern and the third grid pattern are stacked to form the grid-shaped groove; The remaining first photoresist layer is removed.
3. The method for preparing the metal mesh according to claim 2, in, The first dielectric layer includes an organic material, and the etching gas used to etch the first dielectric layer is oxygen.
4. The method for preparing the metal mesh according to claim 3, in, The organic material includes any one of polyimide, epoxy resin, acrylic, polyester, photoresist, polyacrylate, polyamide, and siloxane.
5. The method for preparing the metal grid according to claim 2, in, The thickness of the first dielectric layer is 2 μm-5 μm.
6. The method for preparing the metal mesh according to claim 2, in, The second dielectric layer includes an inorganic material; and the etching gas used to etch the second dielectric layer is tetrafluoromethane.
7. The method for preparing the metal mesh according to claim 6, in, The inorganic material includes any one of silicon nitride, silicon oxide, and silicon oxynitride.
8. The method for preparing the metal grid according to claim 2, in, The thickness of the second dielectric layer is 50nm-400nm.
9. The method for preparing a metal mesh according to claim 2, in, The step of forming the first dielectric layer on the substrate comprises: A first dielectric material is formed on the base substrate by a coating process, and then cured at high temperature to form a first dielectric layer.
10. The method for preparing a metal mesh according to claim 2, in, The step of forming the second dielectric layer on a side of the first dielectric layer away from the substrate includes: The second dielectric layer is formed on a side of the first dielectric layer away from the substrate by using a plasma chemical vapor deposition device.
11. A method for preparing a metal mesh according to any one of claims 2 to 10, in, Also includes: Before forming the dielectric layer on the substrate, the method further includes: forming a first metal film on the base substrate, and using the first metal film as a seed layer; After forming the grid-shaped grooves, the method further includes: removing the second grid pattern; Electroplating the seed layer to grow the first metal film in the groove; The dielectric layer and the first metal film on the dielectric layer near the substrate are removed to form a metal grid.
12. The method for preparing a metal mesh according to claim 11, in, The material of the first metal film includes copper or silver.
13. A method for preparing a metal mesh according to any one of claims 2 to 10, in, The method further comprises: after forming the grid-shaped grooves, the method further comprises: removing the second grid pattern; forming a first metal film on a side of the grid-shaped groove away from the substrate, and using the first metal film as a seed layer; The seed layer is electroplated to grow a first metal film, and the grown first metal film outside the grid-shaped groove is removed to form a metal grid.
14. The method for preparing a metal mesh according to claim 11, in, The material of the first metal film includes copper or silver.
15. A method for preparing a metal mesh according to any one of claims 1 to 10, in, The width of the grid-shaped grooves is no greater than 1.5 μm.
16. A method for preparing an antenna, wherein include: Providing a first dielectric substrate, the first dielectric substrate comprising a first surface and a second surface arranged opposite to each other along a thickness direction thereof; forming a reference electrode layer on the first surface of the first dielectric substrate; A radiation portion is formed on the second surface of the first dielectric substrate; wherein, At least one of the reference electrode layer and the radiation portion comprises a metal mesh, and the metal mesh is prepared by the preparation method according to any one of claims 1 to 15.
17. The preparation method according to claim 16, in, The reference electrode layer and the radiation portion are metal grids, and the reference electrode layer and the hollow portions of the radiation portion have overlapping orthographic projections on the first dielectric substrate.
18. The preparation method according to claim 16, in, The first dielectric substrate includes a first sub-dielectric layer, a first bonding layer, and a second sub-dielectric layer which are stacked. The reference electrode layer is formed on a side of the first sub-dielectric layer away from the first bonding layer. The radiation portion is arranged on a side of the second sub-dielectric layer away from the first bonding layer.
19. The preparation method according to claim 18, in, The material of the first sub-medium layer and / or the second sub-medium layer includes polyimide or polyethylene terephthalate.
20. The preparation method according to claim 18, in, The first dielectric substrate is a single-layer structure, and its material includes polyimide or polyethylene terephthalate.
Citation Information
Patent Citations
Semiconductor device and its making method
CN101238570A
Method of forming pattern for plating and method of forming fine circuit pattern using the same
CN105530760A
Method for etching polyimide sacrificial layer and application
CN115458392A
Pre-patterned lithography templates, processes based on radiation patterning using the templates and processes to form the templates
US20170261850A1
Hydrofluorocarbons containing –NH2 functional group for 3D NAND and dram applications
US20190131140A1