Expansion control structure for direct bonding and method of forming same

By using activation and termination technology of non-conductive materials at the bonding interface of semiconductor components, combined with conductive feature expansion control during annealing, the problem of reliable and direct bonding between semiconductor components is solved, and high-density and high-strength electrical connection is achieved .

CN119096348APending Publication Date: 2024-12-06ADEIA SEMICONDUCTOR BONDING TECHNOLOGIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035781.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to achieve reliable and direct bonding between semiconductor elements without adhesive, especially during the formation of conductive pads, resulting in uneven bonding strength and poor electrical connection.

Method used

By using activation and termination techniques of non-conductive materials on the bonding interface of semiconductor components, a smooth bonding interface is formed and the expansion of conductive features is controlled during the annealing process to achieve direct bonding of metal to metal, reducing pad gaps and Improve bond strength.

Benefits of technology

High-density direct bonding between semiconductor components is achieved, reducing pad gaps, improving bonding strength and reliability, and avoiding defects caused by the use of adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096348A_ABST
    Figure CN119096348A_ABST
Patent Text Reader

Abstract

An element, a bonded structure including the element, and methods of forming the element and the bonded structure are disclosed. The element may include a non-conductive region having a cavity. The element may include a conductive feature formed in the cavity. The conductive feature includes a central portion and an edge portion having a first coefficient of thermal expansion and a second coefficient of thermal expansion, respectively. The central portion and the edge portion are recessed with respect to a contact surface of the non-conductive region by a first depth and a second depth, respectively. The first coefficient of thermal expansion may be at least 5% greater than the second coefficient of thermal expansion. The bonding structure may include an element and a second element having a second non-conductive region and a second conductive feature. A conductive interface between the first conductive feature and the second conductive feature has a central region and an edge region. In a side cross-section of the bonding structure, there are more voids at or near the edge region than at or near the center region.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 334,580, filed on April 25, 2022, the entire contents of which are incorporated herein by reference in their entirety and for all purposes. Technical Field

[0003] The field relates to components prepared for direct bonding, the components including conductive features having controlled expansion. Background Art

[0004] Semiconductor elements (such as integrated device dies or chips) can be mounted or stacked on other elements. For example, semiconductor elements can be mounted to a carrier (such as a package substrate, an interposer, a reconstituted wafer or element, etc.). As another example, a semiconductor element can be stacked on top of another semiconductor element, for example, a first integrated device die can be stacked on a second integrated device die. Each semiconductor element in the semiconductor element can have a conductive pad for mechanically and electrically bonding the semiconductor elements to each other. There is a continuous need for improved methods for forming conductive pads for reliable bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 1A is a schematic cross-sectional side view of the two elements prior to being combined.

[0006] Figure 1B After the combination Figure 1A Schematic cross-sectional side view of the two elements shown.

[0007] Figure 2A A top-down electron backscatter diffraction (EBSD) image of a copper pad formed in the silicon substrate of a component.

[0008] Figure 2B The annealed Figure 2A Simplified illustration of the protrusion height of a cross section of a portion of the element shown.

[0009] Figure 3A is a schematic cross-sectional side view of at least a portion of an element according to an embodiment.

[0010] Figure 3B yes Figure 3A Schematic top view of the elements.

[0011] Figure 4A is a schematic cross-sectional side view of an element according to an embodiment.

[0012] Figure 4B yes Figure 4A A close-up view of a portion of the components shown.

[0013] Figure 4C is a schematic cross-sectional side view of an element according to an embodiment.

[0014] Figure 5A is a schematic cross-sectional side view of an element according to an embodiment.

[0015] Figure 5B is a schematic cross-sectional side view of an element according to an embodiment.

[0016] Figure 5C is a schematic cross-sectional side view of an element according to an embodiment.

[0017] Figure 5D is a schematic cross-sectional side view of an element according to an embodiment.

[0018] FIG. 6A to FIG. 6E Shows the manufacturing Figure 4A The components shown are the various steps in the process.

[0019] Fig. 7A A cross-sectional side view of at least a portion of a joined structure including a first element and a second element is shown.

[0020] Figure 7B yes Fig. 7A A close-up view of a portion of the bonded structure is shown.

[0021] Fig. 8A is a cross-sectional side view of a conductive feature before annealing.

[0022] FIG. 8B to FIG. 8E After annealing Fig. 8A A cross-sectional side view of a conductive feature is shown.

[0023] Fig. 9A is a cross-sectional side view of a conductive feature before annealing.

[0024] FIG. 9B to FIG. 9E After annealing Fig. 9A A cross-sectional side view of a conductive feature is shown. DETAILED DESCRIPTION

[0025] Various embodiments disclosed herein relate to direct-bonded structures in which two or more elements may be directly bonded to one another without an intervening adhesive. Figure 1A and Figure 1B Schematically illustrates a process for forming a direct bond structure without an intervening adhesive according to some embodiments. Figure 1A and Figure 1BIn the embodiment, the combined structure 100 includes two elements 102 and 104, which can be directly combined with each other without the need for intervening adhesives. Two or more semiconductor elements (such as integrated device dies, wafers, etc.) 102 and 104 can be stacked on each other or combined with each other to form a combined structure 100. The conductive feature 106a of the first element 102 (such as a contact pad, an exposed end of a via (such as a TSV) or a through-substrate electrode) can be electrically connected to the corresponding conductive feature 106b of the second element 104. Any suitable number of elements can be stacked in the combined structure 100. For example, a third element (not shown) can be stacked on the second element 104, a fourth element (not shown) can be stacked on the third element, and so on. Additionally or alternatively, one or more additional elements (not shown) can be stacked laterally adjacent to each other along the first element 102. In some embodiments, the laterally stacked additional elements can be smaller than the second element. In some embodiments, the laterally stacked additional elements can be twice smaller than the second element.

[0026] In some embodiments, elements 102 and 104 are directly bonded to each other without an adhesive. In various embodiments, a non-conductive field region comprising a non-conductive material or a dielectric material can be used as a first bonding layer 108a of the first element 102, which can be directly bonded to a corresponding non-conductive field region without an adhesive, and the corresponding non-conductive field region includes a non-conductive material or a dielectric material used as a second bonding layer 108b of the second element 104. Non-conductive bonding layers 108a and 108b can be disposed on respective front sides 114a and 114b of device portions 110a and 110b (such as semiconductor (e.g., silicon) portions of elements 102, 103). Active devices and / or circuit devices can be patterned and / or otherwise disposed in or on device portions 110a and 110b. Active devices and / or circuit devices may be disposed at or near the front sides 114a and 114b of the device portions 110a and 110b, and / or disposed at or near the opposite rear sides 116a and 116b of the device portions 110a and 110b. The non-conductive material may be referred to as a non-conductive bonding region or bonding layer 108a of the first element 102. In some embodiments, the non-conductive bonding layer 108a of the first element 102 may be directly bonded to the corresponding non-conductive bonding layer 108b of the second element 104 using a dielectric-to-dielectric bonding technique. For example, the non-conductive bond or dielectric-to-dielectric bond may be formed without an adhesive using direct bonding techniques disclosed in at least U.S. Patent Nos. 9,564,414; 9,391,143; and 10,434,749, each of which is incorporated herein by reference in its entirety and for all purposes. It should be appreciated that in various embodiments, bonding layers 108a and / or 108b may include non-conductive materials, such as dielectric materials (such as silicon oxide) or undoped semiconductor materials (such as undoped silicon). Suitable dielectric bonding surfaces or materials for direct bonding include, but are not limited to, inorganic dielectrics (such as silicon oxide, silicon nitride, or silicon oxynitride), or may include carbon (such as silicon carbide, silicon carbonitride, low-K dielectric materials, SICOH dielectrics, silicon carbonitride, or diamond-like carbon or materials including diamond surfaces). Such carbon-containing ceramic materials may be considered inorganic despite including carbon.

[0027] In various embodiments, direct hybrid bonding can be formed without intervening adhesives. For example, non-conductive bonding surfaces 112a and 112b can be polished to a high degree of smoothness. Bonding surfaces 112a and 112b can be cleaned and exposed to plasma and / or etchants to activate surfaces 112a and 112b. In some embodiments, surfaces 112a and 112b can be terminated with substances after activation or during activation (e.g., during plasma and / or etching processes). Without being limited by theory, in some embodiments, an activation process can be performed to destroy chemical bonds at bonding surfaces 112a and 112b, and a termination process can provide additional chemicals at bonding surfaces 112a and 112b, thereby improving the binding energy during direct bonding. In some embodiments, activation and termination are provided in the same step, such as plasma for activating and terminating surfaces 112a and 112b. In other embodiments, bonding surfaces 112a and 112b can be terminated in separate processes to provide additional substances for direct bonding. In various embodiments, the termination substance can include nitrogen. For example, in some embodiments, (multiple) bonding surfaces 112a, 112b can be exposed to nitrogen-containing plasma. Further, in some embodiments, bonding surfaces 112a and 112b can be exposed to fluorine. For example, there can be one or more regions with increased fluorine concentration at or near the bonding interface 118 between the first element 102 and the second element 104. Therefore, in the direct bonding structure 100, the bonding interface 118 between the two non-conductive materials (e.g., bonding layers 108a and 108b) can include a very smooth interface, wherein the nitrogen and / or fluorine content at the bonding interface 118 is higher than the nitrogen and / or fluorine content in the bonding layer 108a or 108b. In some embodiments, the bonding layers 108a and 108b can include nitrogen atoms, and after the activation and termination process, an oxygen peak can be set at or near the bonding interface 118 between the first element 102 and the second element 104. Additional examples of activation and / or termination processes may be found in US Pat. Nos. 9,564,414; 9,391,143; and 10,434,749, each of which is hereby incorporated by reference in its entirety and for all purposes.

[0028] In various embodiments, the conductive feature 106a of the first element 102 may also be directly bonded to the corresponding conductive feature 106b of the second element 104. For example, a hybrid bonding technique may be used to provide a conductor-to-conductor direct bond along a bonding interface 118 comprising a covalently directly bonded non-conductive to non-conductive (e.g., dielectric to dielectric) surface prepared as described above. In various embodiments, conductor-to-conductor (e.g., conductive feature 106a to conductive feature 106b) direct bond and dielectric to dielectric hybrid bond may be formed using direct bonding techniques disclosed in at least U.S. Patent Nos. 9,716,033 and 9,852,988, the entire contents of each of which are incorporated herein by reference in their entirety and for all purposes.

[0029] For example, non-conductive (e.g., dielectric) bonding surfaces 112a, 112b (e.g., inorganic dielectric surfaces) can be prepared and directly bonded to each other without the intervening adhesive explained above. Conductive contact features (e.g., conductive features 106a and 106b, which can be at least partially surrounded by non-conductive dielectric field regions within bonding layers 108a, 108b) can also be directly bonded to each other without an intervening adhesive. In various embodiments, conductive features 106a, 106b can include discrete pads at least partially embedded in the non-conductive field regions. In some embodiments, the conductive contact features can include exposed contact surfaces of through-substrate vias (TSVs). In some embodiments, the respective conductive features 106a and 106b may be recessed below the dielectric field region or the outer (e.g., upper) surface (non-conductive bonding surfaces 112a and 112b) of the non-conductive bonding layers 108a and 108b, for example, by less than 30nm, less than 20nm, less than 15nm, or less than 10nm, for example, within a range of 2nm to 20nm or within a range of 4nm to 10nm. In various embodiments, the size of the recesses in the opposing elements prior to direct bonding may be such that the total gap between the opposing contact pads is less than 15nm or less than 10nm. In some embodiments, the non-conductive bonding layers 108a and 108b may be directly bonded to each other at room temperature without an adhesive, and the bonded structure 100 may then be annealed. Upon annealing, the conductive features 106a and 106b may expand in a direction orthogonal to the bonding surfaces 112a, 112b and contact each other to form a metal-to-metal direct bond. Advantageously, direct bonding interconnects or Technology can enable high density of conductive features 106a and 106b to be connected across direct bonding interface 118 (e.g., small pitch or fine pitch of conventional array). In some embodiments, the spacing of conductive features 106a and 106b (such as conductive traces embedded in the bonding surface of one of the bonding elements) can be less than 40 microns or less than 10 microns or even less than 2 microns. For some applications, the ratio of the spacing of conductive features 106a and 106b to one of the dimensions of the bonding pad (e.g., diameter) is less than 5 or less than 3, and sometimes desirably less than 2. In other applications, the width of the conductive trace embedded in the bonding surface of one of the bonding elements in the bonding element can be in the range of between 0.3 and 20 microns (e.g., in the range of 0.3 to 3 microns). In various embodiments, conductive features 106a and 106b and / or traces can include copper, although other metals may be suitable.

[0030] Thus, in a direct bonding process, the first component 102 can be directly bonded to the second component 104 without an intervening adhesive. In some arrangements, the first component 102 can include a singulated component, such as a singulated integrated device die. In other arrangements, such as Figures 1A to 1B As shown, the first component 102 may include a carrier or substrate (e.g., a wafer) including a plurality (e.g., tens, hundreds, or more) of device regions that, when singulated, form a plurality of integrated device dies. Similarly, the second component 104 may include a singulated component (e.g., a singulated integrated device die), such as Figure 1A and 1B As shown. In other arrangements, the second element 104 may include a carrier or substrate (e.g., a wafer). The embodiments disclosed herein may be applied to wafer-to-wafer, die-to-die, or die-to-wafer bonding processes accordingly. In a wafer-to-wafer (W2W) process, two or more wafers may be directly bonded to each other (e.g., direct hybrid bonding) and singulated using a suitable singulation process. After singulation, the side edges of the singulated structure (e.g., the side edges of the two bonded elements) may be substantially flush and may include markings indicating the singulation process (e.g., saw marks if a saw singulation process is used).

[0031] As explained herein, the first element 102 and the second element 104 can be directly bonded to each other without adhesive, which is different from the deposition process. In one application, the width of the first element 102 in the bonding structure is similar to the width of the second element 104. In some other embodiments, the width of the first element 102 in the bonding structure 100 is different from the width of the second element 104. Similarly, the width or area of ​​the larger element in the bonding structure can be at least 10% larger than the width or area of ​​the smaller element. The first element 102 and the second element 104 can include non-deposition elements accordingly. Further, different from the deposition layer, the direct bonding structure 100 can include a defective area along the bonding interface 118, wherein there is a nanometer-level void (nano void). Due to the activation (e.g., exposure to plasma) of the bonding surface 112a and 112b, the nano void can be formed. As explained above, the bonding interface 118 can include the concentration of materials from activation and / or the last chemical treatment process. For example, in an embodiment activated by nitrogen plasma, a nitrogen peak can be formed at the bonding interface 118. The nitrogen peak can be detected using secondary ion mass spectrometry (SIMS) technology. In various embodiments, for example, a nitrogen termination treatment (e.g., exposing the bonding surface to a nitrogen-containing plasma) can replace OH groups of the hydrolyzed (OH-terminated) surface with NH2 molecules, resulting in a nitrogen-terminated surface. In embodiments where activation is performed using an oxygen plasma, an oxygen peak can be formed at the bonding interface 118. In some embodiments, the bonding interface 118 can include silicon oxynitride, silicon carbonitride, or silicon carbonitride. As explained herein, direct bonding can include covalent bonds that are stronger than van der Waals bonds. The bonding layers 108a and 108b can also include polished surfaces that are flattened to a high degree of smoothness.

[0032] In various embodiments, the metal-to-metal bond between the contact pads 106a and 106b can be bonded so that the copper grains grow into each other across the bonding interface 118. In some embodiments, the copper can have grains oriented along the 111 crystal plane to improve copper diffusion across the bonding interface 118. The bonding interface 118 can extend substantially completely to at least a portion of the bonding conductive features 106a and 106b so that there is substantially no gap between the non-conductive bonding layers 108a and 108b at or near the bonding conductive features 106a and 106b. In some embodiments, a barrier layer can be provided below the conductive features 106a and 106b (e.g., which can include copper). However, in other embodiments, there may be no barrier layer below the conductive features 106a and 106b described, for example, in U.S. Patent No. 11,195,748, which is incorporated herein by reference in its entirety and for all purposes.

[0033] Advantageously, very fine pitches between adjacent contact pads 106a and 106b and / or small pad sizes may be achieved using the hybrid bonding techniques described herein. For example, in various embodiments, the pitch p (i.e., the distance from edge to edge or from center to center) between adjacent conductive features 106a (or 106b) may be as small as 1 / 2. Figure 1A The major lateral dimension (e.g., pad diameter) may be in the range of 0.5 micron to 50 micron, in the range of 0.75 micron to 25 micron, in the range of 1 micron to 25 micron, in the range of 1 micron to 10 micron, or in the range of 1 micron to 5 micron. Further, the major lateral dimension (e.g., pad diameter) may also be small, such as in the range of 0.25 micron to 30 micron, in the range of 0.25 micron to 5 micron, or in the range of 0.5 micron to 5 micron.

[0034] The contact pad may have a central portion having higher oriented grains, which are generally oriented vertically along the 111 crystal orientation, and an edge portion, which is close to or along the sidewall of the cavity having lower oriented grains, which are more randomly oriented (e.g., a mixture of 111, 110, 311, 511, and 100 orientations) without a dominant orientation. The difference in crystal orientation may be due to the process of forming the contact pad in the cavity (e.g., an electroplating process). In such a contact pad, the edge portion may protrude a greater distance above the contact surface than the central portion before, during, and / or after the annealing process. For example, the edge portion may protrude a greater distance due to the expansion of the contact pad during the annealing process. The uneven protrusion height on different portions of the contact surface of the conductive structure may cause uneven stress, resulting in uneven bonding strength. When the contact pad is bonded to another contact pad, a gap may be formed above the central portion due to the uneven protrusion of the central portion and the edge portion. When a contact pad of a component is bonded to another contact pad of another component while there is a mismatch (e.g., lateral offset) between the two contact pads, the edge portion may protrude to push against the other component, which may cause debonding and / or poor electrical connection of the two components. Therefore, when annealing, a contact pad having a center portion and an edge portion protruding more than the center portion may hinder the reliability of bonding between the contact pad and the other pad.

[0035] Figure 2A 1 is a top-down electron backscatter diffraction (EBSD) image of a copper pad 10 formed in a silicon substrate 12 of a component 13. The copper pad 10 includes a central portion 14 and an edge portion 16 surrounding the central portion 14. Figure 2A, the boundary region 18 between the center portion 14 and the edge portion 16 is shown with a dashed line. The center portion 14 can have grains that are generally vertically oriented along a 111 crystal orientation (e.g., approximately normal to the surface of the conductive feature), and the edge portion has grains that are more randomly oriented (e.g., a mixture of 111, 110, 311, 511, and 100 orientations) without a dominant orientation. In some embodiments, at least 50% of the grains at the center portion 14 exhibit twinning or highly oriented twins. Twinning is a grain structure in which two or more regions or domains of the crystal lattice are oriented in mirror-image positions relative to each other, separated by twin boundaries. For example, the center portion 14 has microstructural grains that are primarily vertically oriented along a 111 crystal orientation, and the edge portion 16 has nanostructural (e.g., fine grain structure) grains that are oriented without a dominant orientation. As Figure 2A As shown, edge portion 16 may have grains oriented in various crystal orientations. The difference in crystal orientation between center portion 14 and edge portion 16 may be due to a process (e.g., electroplating process) of forming a conductive feature (e.g., copper pad 10) in a cavity formed in silicon substrate 12.

[0036] Figure 2B The annealed Figure 2A A diagram of the protrusion height of a cross section of a portion of the element 13 is shown. Figure 2B In the graph of FIG. 1 , the heights at different locations of the cross section are measured relative to the surface of the silicon substrate 12 before annealing at a temperature between 200° C. and 450° C. Figure 2B As shown in the graph of FIG. 1 , the average protrusion height of the center portion 14 is about 1 μm, and the average protrusion height of the edge portion 16 is about 1.4 μm. The height difference between the protrusion of the center portion 14 and the edge portion 16 may cause excessive stress. When the copper pad 10 is bonded to another contact pad, a gap may be formed above the center portion 14 due to the uneven protrusion between the center portion 14 and the edge portion 16. When the component 13 is bonded to another component, such excessive stress and gap may hinder the reliability of bonding between the components.

[0037] Various embodiments disclosed herein relate to controlling the protrusion height above different positions of a conductive feature in an element formed by an annealing process. The element may include a non-conductive region having a cavity, and a conductive feature at least partially disposed in the cavity. The conductive feature may have a central portion and an edge portion. In some embodiments, the edge portion may be at least partially disposed between the central portion and the sidewall of the cavity. For example, the edge portion may be disposed between the central portion and the sidewall of the cavity so as to surround the side surface of the central portion by the edge portion. In some embodiments, the portion of the central portion and the portion of the edge portion may be exposed on the surface of the conductive feature. For example, the surface of the conductive feature and the surface of the non-conductive region may at least partially define the contact surface of the element.

[0038] In some embodiments, the height of the center portion and the edge portion can be controlled to provide a conductive structure having a substantially uniform protrusion height on the surface of the conductive feature after annealing. For example, the surface of the conductive feature can be recessed relative to the surface of the non-conductive region. The portion of the center portion exposed on the surface of the conductive feature can be recessed to a first depth relative to the surface of the non-conductive region, and the portion of the edge portion exposed on the surface of the conductive feature can be recessed to a second depth different from the first depth relative to the surface of the non-conductive region. For another example, the center portion and the edge portion of the conductive feature can include the same material or different materials with different properties (e.g., different coefficients of thermal expansion (CTE), different grain sizes, or different grain orientations), mechanical properties. For example, in some embodiments, the center portion can have a material with a first CTE, and the edge portion can include a second CTE that is less than the first CTE.

[0039] Various embodiments disclosed herein relate to a combined structure comprising an element (first element) and another element (second element), the first element comprising a conductive feature having a controlled center and edge portion. The second element may have the same, similar or different structure as the first element.

[0040] Figure 3A is a schematic cross-sectional side view of at least a portion of element 20 according to an embodiment. Figure 3B yes Figure 3A2 is a schematic top view of an element 20. The element may include a region such as a non-conductive (e.g., semiconductor or inorganic dielectric) region 22 and a conductive feature 24 such as a contact pad, an exposed end of a via (e.g., TSV), or a through-substrate electrode. In some embodiments, the element 20 may include a barrier layer 26 between the conductive feature 24 and the non-conductive region. For example, the barrier layer 26 may include a diffusion barrier layer that prevents or reduces the diffusion of the material of the conductive feature 24 into the non-conductive region 22. In some embodiments, the barrier layer 26 may include tantalum, titanium, cobalt, nickel, tungsten, or any suitable compound or combination thereof. In some embodiments, the barrier layer 26 may include a multilayer structure.

[0041] The non-conductive region 22 may include a dielectric layer. In some embodiments, the non-conductive region 22 may include multiple layers of different dielectric materials. For example, the non-conductive region 22 may include silicon oxide, silicon nitride, or any other suitable non-conductive bonding material. Figure 3A As shown, cavity 28 can be formed in non-conductive region 22. Cavity 28 can extend at least partially through the thickness of non-conductive region 22. For example, cavity 28 can extend completely through the thickness of non-conductive region 22. In some embodiments, a dielectric material (not shown) can be disposed between barrier layer 26 and non-conductive region 22.

[0042] The non-conductive region 22 has a contact surface 22a that can at least partially define a bonding surface of the element 20. As explained herein, the contact surface 22a of the non-conductive region 22 can be prepared for direct bonding. In some embodiments, the contact surface 22a can be polished, for example, by chemical mechanical polishing (CMP), to have a thickness less than 100 nm. Less than or less than surface roughness.

[0043] The conductive feature 24 may include a first portion (e.g., a center portion 30) and a second portion (e.g., an edge portion 32). A portion of the center portion 30 (e.g., an upper surface 30a) and a portion of the edge portion 32 (e.g., an upper surface 32a) may at least partially define a bonding surface of the element 20. The upper surface 30a of the center portion 30 and the upper surface 32a of the edge portion 32 may be recessed to a first depth relative to the contact surface 22a of the non-conductive region 22. For example, the upper surface 30a of the center portion 30 and the upper surface 32a of the edge portion 32 may be recessed by less than 30nm, less than 20nm, less than 15nm, or less than 10nm, such as in the range of 2nm to 20nm or in the range of 4nm to 10nm.

[0044] In some embodiments, the center portion 30 and the edge portion 32 of the conductive feature 24 may have different material properties. For example, the center portion 30 and the edge portion 32 of the conductive feature 24 may have the same substrate or different materials with different material properties or alloys. In some embodiments, the center portion 30 has a first coefficient of thermal expansion (CTE) and the edge portion 32 has a second CTE different from the first CTE. For example, the first CTE may be greater than the second CTE. In some embodiments, the first CTE may be at least 5% greater than the second CTE. For example, the first CTE may be 5% to 50%, 10% to 50%, 20% to 50%, 5% to 40%, 5% to 30%, or 10% to 40% greater than the second CTE. In some embodiments, the center portion 30 and / or the edge portion 32 may include nickel vanadium (NiV) or nickel boride (NiB). In some embodiments, the NiV or NiB may be formed by electroplating or sputtering. The center portion 30 and / or the edge portion 32 may include copper zirconium (CuZr), copper indium (CuIn), copper tin (CuSn), copper molybdenum (CuMo) or copper vanadium (CuV), for example, an alloy of less than 50%. The center portion 30 and / or the edge portion 32 may include an alloy of copper (Cu) with nickel (Ni), cobalt (Co), vanadium (V), tungsten (W), zirconium (Zr) or molybdenum (Mo). The center portion 30 and / or the edge portion 32 may include an alloy of Co with Ni, V, W, Zr or Mo. For example, the Cu or Co alloy may include less than 5% Ni, Co, V, W, Zr or Mo. The center portion 30 and / or the edge portion 32 may include a nanotwin metal (e.g., nanotwin copper) or a fine grain metal (e.g., fine grain copper). In some applications, it may be advantageous to use a nanotwin metal having a 111 crystal orientation because the 111 nanotwin metal may have a relatively low CTE, a relatively high hardness, and a relatively high resistance to electromigration. Fine grained metals may be defined as metals having an average grain width of less than 20 nm, less than 50 nm, less than 100 nm, less than 300 nm, or less than 500 nm. For example, the maximum width of grains in fine grained metals may be in the range of 10 nm to 500 nm, 10 nm to 300 nm, 20 nm to 500 nm, 20 nm to 300 nm, 20 nm to 100 nm, 20 nm to 50 nm, 50 nm to 500 nm, 50 nm to 300 nm, or 100 nm to 300 nm. The center portion 30 and / or edge portion 32 may include metals having grains that are generally vertically oriented (e.g., approximately normal to the surface of the conductive feature) along a 111 crystal orientation.

[0045] In some embodiments, the materials of the center portion 30 and the edge portion 32 can be selected so that the protrusion height of the center portion 30 after annealing is the same, substantially similar, or greater than the protrusion height of the edge portion 32, so that a substantially uniform bonding interface can be formed after annealing and bonding. The center portion 30 and the edge portion 32 can be annealed at a temperature between 100°C and 400°C, 100°C and 300°C, 100°C and 250°C, 150°C to 400°C, 150°C to 300°C, or 180°C to 300°C for any suitable duration (e.g., a duration in a range between 60 and 180 minutes). In some embodiments, the annealing temperature can vary at least in part based on the size of the conductive feature 24. For example, a conductive feature 24 having a smaller size (e.g., diameter) can be annealed at a higher temperature than a conductive feature 24 having a larger size (e.g., diameter). For example, at the same annealing temperature, a conductive feature 24 having a larger diameter can protrude more than a conductive feature 24 having a smaller diameter. The conductive features 24 of the embodiments described herein, such as contact pads, exposed ends of vias (e.g., TSVs), or through-substrate electrodes, can have a maximum dimension (e.g., a maximum lateral dimension or diameter) in a range between about 0.01 μm and 15 μm, between about 0.1 μm and 10 μm, between about 0.5 μm and 8 μm, between about 2 μm and 5 μm, between about 1 μm and 3 μm, or between about 0.01 μm and 1 μm. The difference between the average height of the center portion 30 and the average height of the edge portion 32 after annealing can be less than 0.2 μm, less than 0.1 μm, or less than 0.05 μm. In some embodiments, the center portion 30 and the edge portion 32 can be selected so that the first CTE of the center portion 30 is equal to or greater than the second CTE of the edge portion 32.

[0046] Central portion 30 and edge portion 32 having materials and / or dimensions selected as disclosed herein may enable conductive feature 24 to be reliably bonded to another conductive feature of another component with sufficient bond strength and minimal resulting stress and / or voids. 4A to 5D Components according to various embodiments are illustrated, which may implement any one or more suitable principles and / or advantages disclosed herein, such as with respect to FIG. 3A to FIG. 3B Those principles and / or advantages described.

[0047] Figure 4A is a schematic cross-sectional side view of an element 40 according to an embodiment. Figure 4B yes Figure 4A A close-up view of a portion of the element 40 is shown. Unless otherwise noted, Figure 4A and Figure 4B The components of can be similar to those disclosed herein (such as FIG. 3A to FIG. 3B Component 40 is generally similar to FIG. 3A to FIG. 3B The element 20 is shown, except that in the element 40, the upper surface 32a of the edge portion 32 is recessed below the upper surface 30a of the center portion 30. The upper surface 30a of the center portion 30 may be recessed by a first depth d1 relative to the contact surface 22a of the non-conductive region 22, and the upper surface 32a of the edge portion 32 may be recessed by a second depth d2 greater than the first depth d1 relative to the contact surface 22a of the non-conductive region 22. Although the barrier layer 26 and the contact surface 22a of the non-conductive region 22 are shown as being flush without any recess, in some embodiments, the barrier layer 26 may be recessed relative to the contact surface 22a.

[0048] The first depth d1 of the center portion 30 and the second depth d2 of the edge portion 32 may be selected based on various factors so that the center portion 30 and the edge portion 32 have a desired protrusion height after annealing. For example, the first depth d1 of the center portion 30 and the second depth d2 of the edge portion 32 may be selected based at least in part on the material of the center portion 30 and the edge portion 32, the width w1 of the center portion 30, the width w2 of the edge portion, the annealing temperature, and / or the CTE difference between the conductive feature 24 and the non-conductive region 22. In some embodiments, the edge portion 32 may include a material with a higher CTE than the material of the center portion 30, and the larger second depth d2 relative to the first depth d1 may compensate for the CTE difference, thereby preventing or mitigating excessive protrusion of the edge portion 32 compared to the center portion 30 after annealing.

[0049] In some embodiments, for deep cavities (e.g., cavities 28 having a depth of 10 μm to 100 μm), such as in some TSV or other through-substrate electrode structures, the difference between the first depth d1 and the second depth d2 may be in a range between 0.01 μm and 0.5 μm, 0.1 μm and 0.5 μm, 0.1 μm and 0.4 μm, 0.2 μm and 0.5 μm, or 0.2 μm and 0.4 μm. In some embodiments, the upper surface 30a of the central portion 30 may be recessed relative to the contact surface 22a of the non-conductive region 22, for example, by less than 100 nm, less than 50 nm, less than 20 nm, or less than 10 nm, for example, in a range between 2 nm and 20 nm, or in a range between 4 nm and 10 nm.

[0050] Figure 4C is a schematic cross-sectional side view of an element 42 according to an embodiment. Unless otherwise noted, Figure 4C The components of can be similar to those disclosed herein (such as FIG. 3A to FIG. 4B Component 42 is generally similar to FIG. 3A to FIG. 4BThe elements 20, 40 are shown with the difference that in the element 42, the upper surface 30a of the central portion 30 is recessed below the upper surface 32a of the edge portion 32. In other words, the first depth d1 may be greater than the depth d2.

[0051] The first depth d1 of the center portion 30 and the second depth d2 of the edge portion 32 may be selected based on various factors so that the center portion 30 and the edge portion 32 have a desired protrusion height after annealing, thereby generating sufficient force for bonding without damaging or debonding the components. For example, the first depth d1 of the center portion 30 and the second depth d2 of the edge portion 32 may be selected based at least in part on the materials of the center portion 30 and the edge portion 32, the width w1 of the center portion 30, the width w2 of the edge portion, the annealing temperature, and / or the CTE difference between the conductive feature 24 and the non-conductive region 22. In some embodiments, the edge portion 32 may include a material with a lower CTE than the material of the center portion 30, and the greater first depth d1 relative to the second depth d2 may compensate for the CTE difference, thereby preventing or mitigating excessive protrusion of the center portion 30 compared to the edge portion 32 after annealing.

[0052] Figure 5A is a schematic cross-sectional side view of an element 44 according to an embodiment. Unless otherwise noted, Figure 5A The components of can be similar to those disclosed herein (such as FIG. 3A to FIG. 4C Component 44 is generally similar to FIG. 4A to FIG. 4C Elements 40, 42 are shown. In element 44, center portion 30 includes bottom region 46 and upper region 48 above bottom region 46. Edge portion 32 may be positioned such that edge portion 32 is disposed between upper region 48 of center portion 30 and sidewalls of cavity 28.

[0053] Figure 5B is a schematic cross-sectional side view of an element 50 according to an embodiment. Unless otherwise noted, Figure 5B The components of can be similar to those disclosed herein (such as Figures 3A to 4C Component 50 is generally similar to FIG. 4A to FIG. 5A Components 40, 42, 44 are shown. In component 50, conductive feature 24 may include a center portion 30, an edge portion 32, and a bottom portion 52. Bottom portion 52 may include the same material as center portion 30 and / or edge portion 32, but may have different material properties, or may include a different material than the material(s) of center portion 30 and / or edge portion 32.

[0054] Figure 5Cis a schematic cross-sectional side view of an element 54 according to an embodiment. Unless otherwise noted, Figure 5C The components of can be similar to those disclosed herein (such as FIG. 3A to FIG. 5B Component 54 is generally similar to FIG. 4A to FIG. 4B Element 40 is shown. In some embodiments, edge portion 32 of element 54 may be a portion of conductive material 56 disposed in cavity 28 that is different from center portion 30.

[0055] Figure 5D is a schematic cross-sectional side view of an element 58 according to an embodiment. Unless otherwise noted, Figure 5D The components of can be similar to those disclosed herein (such as FIG. 3A to FIG. 5C Component 58 is generally similar to FIG. 4A to FIG. 4B Element 40 is shown. In some embodiments, edge portion 32 may be at least partially buried in center portion 30.

[0056] Any suitable combination of features disclosed herein may be implemented to form an element. For example, various features of conductive features 24 may be implemented to form an element that may provide a secure bond when combined with another embodiment.

[0057] FIG. 6A to FIG. 6E Shows the manufacturing Figure 4A The various steps in the process of the element 40 shown can be achieved with FIG. 6A to FIG. 6E The elements disclosed herein are formed by a process similar to that of the process of FIG. 6A to FIG. 6E The components of can be similar to those disclosed herein (such as Figure 4A and Figure 4B components are the same or substantially similar to those shown.

[0058] Fig. 6A 2 is a cross-sectional view showing a non-conductive region 22 and a cavity 28 formed in the non-conductive region 22. The cavity 28 may extend at least partially through the thickness of the non-conductive region 22. In some embodiments, the cavity 28 may extend completely through the thickness of the non-conductive region 22. A barrier layer 26 may be provided in the cavity 28. The barrier layer 26 may have a thickness or width in the nanometer range. For example, the thickness of the barrier layer 26 may be in the range of 10 nm to 50 nm, 20 nm to 50 nm, 10 nm to 40 nm, or 20 nm to 40 nm. In some embodiments, a dielectric layer (not shown) may be disposed between the barrier layer 26 and the non-conductive region 22.

[0059] Figure 6B2 is a cross-sectional view showing the non-conductive region 22, the barrier layer 26, and the conductive material 60 disposed in the cavity 28. In some embodiments, when the conductive material 60 is provided, there may be an excess portion of the conductive material 60 above the non-conductive region 22. Such excess portion may be removed by a removal process such as a chemical mechanical polishing (CMP) process.

[0060] exist Figure 6C , removing at least a portion of conductive material 60. In some embodiments, a portion of conductive material 60 that contacts barrier layer 26 may be removed to define void 62 and center portion 30. For example, a portion of conductive material 60 may be removed by etching (eg, a selective etching process).

[0061] exist Fig.6D In the embodiment of the present invention, an edge portion 32 may be provided in the void 62. The void 62 may be at least partially or completely filled with the material of the edge portion 32. The material of the edge portion 32 may be the same or different from the conductive material 60 of the center portion 30. The edge portion 32 may have a thickness or width in the micrometer range. The thickness of the edge portion 32 may vary based at least in part on the size of the conductive feature 24. For example, the thickness of the edge portion may be in the range of 1 μm to 5 μm, 2 μm to 5 μm, 1 μm to 4 μm, or 2 μm to 4 μm. In some embodiments, the filling material may be formed by an electroless atomic layer deposition method (ALD) or other known methods. After the filling step of forming the edge portion 32, the excess portion may be removed by a mechanical planarization method. The edge portion void may be formed as needed.

[0062] exist Fig. 6E In the embodiment, the element 40 is prepared for direct bonding. For example, at least the contact surface 22a of the non-conductive region 22 may be polished by, for example, CMP to have a surface area less than 100 nm. Less than or less than During the polishing process, recessing may occur so that the surface 30a of the center portion 30 and the surface 32a of the edge portion 32 are recessed below the contact surface 22a. In some embodiments, according to the embodiments disclosed herein, the surface 30a of the center portion 30 and the surface 32a of the edge portion 32 may be intentionally recessed. For example, the surface 32a may be recessed so that the surface 32a is located below the surface 30a.

[0063] An element (first element) according to various embodiments disclosed herein may be bonded to another element (second element) to form a bonded structure. Fig. 7A A cross-sectional side view of at least a portion of a bonded structure 66 including a first element 66a and a second element 66b is shown. Figure 7B yes Fig. 7A 6a and 66b. In some embodiments, the first element 66a and the second element 66b can be directly bonded to each other along the bonding interface 68 without the need for an intervening adhesive. For example, the non-conductive region 22 of the first element 66a and the non-conductive region 72 of the second element 66b can be directly bonded to each other at room temperature, and the conductive features 24 of the first element 66a and the conductive features 74 of the second element 66b can be directly bonded to each other after the non-conductive regions 22 of the first element 66a and the non-conductive regions 72 of the second element 66b are bonded. Bonding the conductive features 24 of the first element 66a and the conductive features 74 of the second element 66b can include an annealing process. The conductive features 24 can include a central portion 30 and an edge portion 32, and the conductive features 74 can include a central portion 80 and an edge portion 82. The portion of the bonding interface 68 between the central portion 30 and the central portion 80 can be referred to as the central region 68a of the bonding interface 68. The portion of the bonding interface 68 between the edge portion 32 and the edge portion 82 can be referred to as the edge region 68b of the bonding interface 68.

[0064] In some embodiments, bonding structure 66 may include a signature indicating the use of conductive features of embodiments disclosed herein. In some embodiments, bonding structure 66 may include voids 76 (e.g., microvoids) that indicate conductive features according to embodiments disclosed herein. Microvoids may be defined as voids having an average dimension (e.g., a linear lateral dimension or width) equal to or less than 300 nm, 100 nm, or 80 nm, such as voids having an average dimension in the range of 10 nm to 300 nm, 10 nm to 100 nm, or 10 nm to 80 nm. In terms of lateral area observed in a cross section, the average area of ​​the microvoids may be between 70 nm and 80 nm. 2 To 70000nm 2 , 100nm 2 To 7000nm 2 or 100nm 2 To 700nm 2range. For example, the voids 76 or void concentration per unit area at or near the edge region 68b of the bonding interface 68 may be greater than at or near the center region 68a. For example, the voids 76 at or near the edge region 68b of the bonding interface 68 may be greater than at or near the center region 68a. Portions of the bonding edge portion 32, 82 may be near the edge region 68b, which is within approximately 500nm of the thickness of the bonding edge portion 32, 82 from the edge region 68b of the bonding interface 68, and portions of the bonding center portion 30, 80 may be near the center region 68b, which is within approximately 500nm of the thickness of the bonding center portion 30, 80 from the center region 68a of the bonding interface 68. During the annealing process, the voids may move in these portions that are within 500nm of the bonding interface 68. By taking Fig. 7A The side cross-section of the bonding structure 66 shown and examining the side cross-section can detect the difference in the number of voids at or near the central region 68a and the number of voids at or near the edge region 68b. In some embodiments, the voids at or near the edge region 68b of the bonding interface 68 can be smaller than the voids at or near the central region 68a.

[0065] Despite Fig. 7A In the bonding structure 66 illustrated in FIG. 1 , two elements (first element 66a and second element 66b) are precisely aligned, but the first element 66a and the second element 66 may be misaligned. Due to the misalignment of the first element 66a and the second element 66b, at least a portion of the edge portion 32 may be aligned with a portion of the center portion 80. In such a bonding structure with misaligned elements, the above characterized structure in which the voids 76 or the void concentration per unit area at or near the edge region 68b of the bonding interface 68 is greater than that in the center region 68a may be maintained.

[0066] In some embodiments, Figure 7B As shown, the combined center portion 30, 80 may expand or bulge into the portion (e.g., gap 76) between the edge portion 32 and the edge portion 82 in the edge region 68b, resulting in a mixture of materials of the center portion 30, 80 and the edge portion 32, 82. The mixture of materials may indicate that there is a depression of the edge portion 32, 82 relative to the contact surface of the elements 66a, 66b that is deeper than the depression of the center portion 30, 80 relative to the contact surface of the elements 66a, 66b. The mixture of materials may indicate that the CTE of the center portion 30, 80 is greater than the CTE of the edge portion 32, 82 and / or that the edge portion 32, 82 is depressed below the center portion 30, 80 prior to annealing.

[0067] although Fig. 7A and Figure 7BA bonded structure 66 including two identical or substantially similar elements 66a, 66b is shown, but the bonded structure may include two or more different elements. For example, the bonded structure may include an element according to one embodiment and another element according to another embodiment. Based at least in part on the materials, size and shape of the conductive structures, annealing temperature, and / or annealing duration, the bonded conductive features may have different structures.

[0068] Fig. 8A 24, 90 before annealing. The conductive features 24, 90 can be along the corresponding non-conductive region ( Fig. 8A 2 and 3. The conductive features 24 may include a central portion 30 and an edge portion 32. In some embodiments, the conductive features 24 may be at least partially disposed between portions of the barrier layer 26. The conductive features 90 may be at least partially disposed between portions of the barrier layer 92. The edge portion 32 is recessed by a depth d2 relative to the bonding interface 68 between the corresponding non-conductive regions.

[0069] Figure 8B is a cross-sectional side view of conductive features 24, 90 after annealing at a first temperature for a first duration. The central portion 30 of conductive feature 24 and conductive feature 90 may expand and bond together. The edge portion 32 may expand, and the depth d3 between the edge portion 32 and the bonding interface 68 may be less than Fig. 8A The depth d2 before bonding is shown. The temperature and / or duration of the annealing may affect the expansion of the central portion 30 , the edge portion 32 , and / or the conductive features 90 .

[0070] Figure 8C 2 is a cross-sectional side view of the conductive feature 24, 90 after annealing at a second temperature for a second duration. The second temperature and / or the second duration may be greater than the first temperature and / or the first duration. The edge portion 32 may expand, and the depth d4 between the edge portion 32 and the bonding interface 68 may be less than Figure 8B The depth d3.

[0071] Fig.8D 2 is a cross-sectional side view of the conductive feature 24, 90 after annealing at a third temperature for a third duration. The third temperature and / or the third duration may be greater than the second temperature and / or the second duration. The edge portion 32 may expand, and the depth d5 ​​between the edge portion 32 and the bonding interface 68 may be less than Figure 8C Depending on the temperature and duration, edge portion 32 may contact and bond with conductive feature 90 .

[0072] Fig. 8Eis a cross-sectional side view of conductive features 24, 90 after annealing at a fourth temperature for a fourth duration. In some embodiments, the interface between edge portion 32 and conductive feature 90 may include voids 94 (e.g., microvoids or nanovoids). For example, edge portion 32 may expand to form a filament or comb shape whose height varies at least in part depending on the material of edge portion 32, the fourth temperature, and / or the fourth duration.

[0073] Fig. 9A is a cross-sectional side view of conductive features 24, 24' before annealing. Conductive features 24, 24' can be portions of an element that are directly bonded along a bonding interface 68 between corresponding non-conductive regions. Conductive features 24, 24' can have the same or substantially similar structures. Conductive feature 24 can include a central portion 30 and an edge portion 32. Conductive feature 24' can include a central portion 30' and an edge portion 32'. In some embodiments, conductive features 24, 24' can be at least partially disposed between barrier layers 26, 26'. Edge portion 32 is recessed by a depth d2 relative to bonding interface 68 between corresponding non-conductive regions.

[0074] Fig. 9B 2 is a cross-sectional side view of conductive features 24, 24' after annealing at a first temperature for a first duration. The central portion 30 of conductive feature 24 and the central portion 30' of conductive feature 24' can expand and bond together. The edge portion 32 can expand, and the depth d6 between the edge portion 32 and the bonding interface 68 can be less than Fig. 9A The depth d2 before bonding is shown. The temperature and / or duration of the annealing may affect the expansion of the central portion 30, 30' and / or the edge portion 32, 32'.

[0075] Fig. 9C 24 ′ after annealing at a second temperature for a second duration. The second temperature and / or the second duration may be greater than the first temperature and / or the first duration. The edge portion 32 may expand, and the depth d7 between the edge portion 32 and the bonding interface 68 may be less than Figure 8B The central portion 30, 30' may expand and at least partially fill the gap between the edge portions 32, 32'.

[0076] Fig.9D 2 is a cross-sectional side view of conductive features 24, 24' after annealing at a third temperature for a third duration. The third temperature and / or the third duration may be greater than the second temperature and / or the second duration. Edge portion 32 may expand, and a depth d8 between edge portion 32 and bonding interface 68 may be less than Fig. 9CThe center portion 30, 30' may expand and at least partially fill the gap between the edge portions 32, 32'. In some other embodiments, depending on the temperature and duration, the edge portion 32 may contact and bond with the edge portion 32'.

[0077] Fig.9E is a cross-sectional side view of conductive features 24, 24' after annealing at a fourth temperature for a fourth duration. In some embodiments, the interface between edge portion 32 and edge portion 24' may include voids 94 (e.g., microvoids or nanovoids). For example, edge portion(s) 32, 32' may expand to form filaments or combs whose height varies at least in part depending on the material of edge portions 32, 32', the fourth temperature, and / or the fourth duration.

[0078] In one aspect, a bonding structure is disclosed. The bonding structure may include: a first element having a first non-conductive region and a first conductive feature; and a second element having a second non-conductive region and a second conductive feature. The second element is bonded to the first element along a bonding interface so that the second non-conductive region is directly bonded to the first non-conductive region along the non-conductive interface, and the second conductive feature is directly bonded to the first conductive feature along the conductive interface. The conductive interface between the first conductive feature and the second conductive feature has a central region and an edge region, the edge region being laterally located between the central region and the non-conductive interface, the non-conductive interface being between the first non-conductive region and the second non-conductive region. In a side cross-section of the bonding structure, there are more voids at or near the edge region than at or near the central region.

[0079] In one embodiment, the first non-conductive region has a cavity extending at least partially through the thickness of the first non-conductive region. The first conductive feature may be formed in the cavity. The first conductive feature may include a center portion and an edge portion, the edge portion being disposed between the sidewall of the cavity and the center portion. The center portion may have a first coefficient of thermal expansion. The edge portion may have a second coefficient of thermal expansion different from the first coefficient of thermal expansion. The center portion and the edge portion may include the same material with different crystal orientations. The center portion and the edge portion may include different materials. The edge region may include filaments of the material of the edge portion of the first conductive feature. The center portion may be partially disposed between the edge portion of the first conductive feature and the edge portion of the second conductive feature. The second non-conductive region may have a second cavity extending at least partially through the thickness of the second non-conductive region, and the second conductive feature may be formed in the second cavity. The second conductive feature may include a second center portion and a second edge portion, the second edge portion being disposed between the second sidewall of the second cavity and the second center portion.

[0080] In one embodiment, the voids at or near the central region have an average void size that is greater than the average void size of the voids at or near the edge region.

[0081] In one aspect, a component having a bonding surface is disclosed. The component may include: a non-conductive region, a cavity having a thickness extending at least partially through the non-conductive region from a contact surface of the non-conductive region. The contact surface at least partially defines the bonding surface of the component. The component may include a conductive feature formed in the cavity. The conductive feature includes a center portion and an edge portion, the edge portion being disposed between a sidewall of the cavity and the center portion. The center portion has a first coefficient of thermal expansion. The edge portion has a second coefficient of thermal expansion different from the first coefficient of thermal expansion. The center portion is recessed to a first depth relative to the contact surface of the non-conductive region. The edge portion is recessed to a second depth different from the first depth relative to the contact surface of the non-conductive region.

[0082] In one embodiment, the contact surface has a surface structure prepared for direct bonding.

[0083] In one embodiment, the first coefficient of thermal expansion is greater than the second coefficient of thermal expansion.The center portion and the edge portion may include the same material with different crystal orientations.The center portion and the edge portion may include different materials.

[0084] In one embodiment, the second depth is greater than the first depth.

[0085] In one embodiment, the component further comprises a barrier layer disposed between the edge portion and the sidewalls of the cavity. The barrier layer may be configured to prevent or reduce diffusion of the conductive features into the non-conductive region.

[0086] In one aspect, a component having a bonding surface is disclosed. The component may include a non-conductive region having a cavity extending at least partially from a contact surface of the non-conductive region through a thickness of the non-conductive region. The contact surface at least partially defines the bonding surface of the component. The component may include a conductive feature formed in the cavity. The conductive feature includes a center portion and an edge portion, the edge portion being disposed between a sidewall of the cavity and the center portion. The center portion has a first coefficient of thermal expansion. The edge portion has a second coefficient of thermal expansion different from the first coefficient of thermal expansion. The center portion is recessed a first depth relative to the contact surface of the non-conductive region. The edge portion is recessed a second depth relative to the contact surface of the non-conductive region. The first coefficient of thermal expansion is at least 5% greater than the second coefficient of thermal expansion.

[0087] In one embodiment, the contact surface has a surface structure prepared for direct bonding.

[0088] In one embodiment, the center portion and the edge portions comprise the same material having different crystal orientations.

[0089] In one embodiment, the central portion and the edge portions comprise different materials.

[0090] In one embodiment, the second depth is greater than the first depth.

[0091] In one embodiment, the element further comprises a barrier layer disposed between the edge portion and the sidewalls of the cavity.

[0092] In one aspect, a method of forming a conductive feature in a cavity in a non-conductive region of a component is disclosed. The cavity extends at least partially through a thickness of the non-conductive region from a contact surface of the non-conductive region. The method may include providing a first conductive material in the cavity, removing at least a portion of the first conductive material from the cavity, providing a second conductive material in the removed portion of the first conductive material, and recessing the first conductive material and the second conductive material relative to the contact surface of the non-conductive region.

[0093] In one embodiment, the first conductive material is recessed to a first depth relative to the contact surface of the non-conductive region, and the second conductive material is recessed to a second depth different from the first depth relative to the contact surface of the non-conductive region. The second conductive material may be positioned between the first conductive material and the sidewall of the cavity. The first conductive material may include copper or a cobalt alloy. The second depth may be greater than the first depth.

[0094] In one embodiment, the first material has a first coefficient of thermal expansion and the second material has a second coefficient of thermal expansion. The first coefficient of thermal expansion may be greater than the second coefficient of thermal expansion.

[0095] In one embodiment, recessing the contacting surface of the first conductive material and the second conductive material relative to the non-conductive region includes polishing the non-conductive region and the conductive features.

[0096] In one embodiment, the method further comprises: providing a barrier layer on the inner surface of the cavity.

[0097] In one aspect, a method of forming a bonding structure is disclosed. The method may include providing a first element and directly bonding a bonding surface of a second element to a bonding surface of the first element. The first element includes a non-conductive region having a cavity extending at least partially through a thickness of the non-conductive region from a contact surface of the non-conductive region. The contact surface at least partially defines the bonding surface of the first element. The first element includes a conductive feature formed in the cavity and at least partially defining the bonding surface of the first element. The conductive feature includes a center portion and an edge portion, the edge portion being disposed between a sidewall of the cavity and the center portion. The center portion has a first coefficient of thermal expansion. The edge portion has a second coefficient of thermal expansion different from the first coefficient of thermal expansion. The center portion is recessed to a first depth relative to the contact surface of the non-conductive region. The edge portion is recessed to a second depth different from the first depth relative to the contact surface of the non-conductive region.

[0098] In one embodiment, directly bonding the bonding surfaces of the first and second components includes directly bonding a non-conductive region of the second component to a non-conductive region of the first component without an intervening adhesive, and directly bonding a conductive feature of the second component to a conductive feature of the first component without an intervening adhesive.

[0099] In one embodiment, directly bonding the conductive feature of the second component to the conductive feature of the first component includes annealing the conductive feature.

[0100] In one embodiment, the first coefficient of thermal expansion is greater than the second coefficient of thermal expansion.The center portion and the edge portion may include the same material with different crystal orientations.The center portion and the edge portion may include different materials.

[0101] In one embodiment, the second depth is greater than the first depth.

[0102] In one embodiment, the conductive feature of the second element includes a center portion and an edge portion. The center portion of the second element may have a third coefficient of thermal expansion. The edge portion of the second element may have a fourth coefficient of thermal expansion. The third coefficient of thermal expansion may be greater than the fourth coefficient of thermal expansion.

[0103] Unless the context clearly requires otherwise, throughout the description and claims, the words "comprise", "comprising", "include", "including", etc. should be interpreted in an inclusive sense, rather than an exclusive or exhaustive sense; that is, in the sense of "including but not limited to". The word "coupled" as generally used herein refers to two or more elements that can be directly connected or connected through one or more intermediate elements. Similarly, the word "connected" as generally used herein refers to two or more elements that can be directly connected or connected through one or more intermediate elements. Additionally, when used in this application, the words "herein", "above", "below" and words of similar meaning should refer to the entire application, rather than any particular part of the application. In addition, as used herein, when a first element is described as being "on" or "above" a second element, the first element can be directly on or above the second element, so that the first element and the second element are in direct contact, or the first element can be indirectly on or above the second element, so that one or more elements are between the first element and the second element. Where the context permits, the words used in the singular or plural in the above specific embodiments may also include the plural or singular, respectively. The word "or" refers to a list of two or more items and covers all of the following interpretations of the word: any of the items in the list, all of the items in the list, and any combination of the items in the list.

[0104] Furthermore, unless specifically stated otherwise or otherwise understood to be used within the context, conditional language used herein (such as "can," "could," "might," "may," "eg," "for example," "such as," etc.) is generally intended to convey that certain embodiments include and other embodiments do not include certain features, elements, and / or states. Thus, such conditional language is generally not intended to imply that features, elements, and / or states are in any way required for one or more embodiments.

[0105] Although certain embodiments have been described, these embodiments are presented by way of example only and are not intended to limit the scope of the present disclosure. In fact, the novel devices, methods, and systems described herein may be implemented in a variety of other forms; in addition, various omissions, substitutions, and changes in the form of the methods and systems described herein may be made without departing from the spirit of the present disclosure. For example, when a block is presented in a given arrangement, an alternative embodiment may utilize different components and / or circuit topologies to perform similar functions, and some blocks may be deleted, moved, added, subdivided, combined, and / or modified. Each of these blocks may be implemented in a variety of different ways. Any suitable combination of the elements and actions of the various embodiments described above may be combined to provide further embodiments. The attached claims and their equivalents are intended to cover such forms or modifications that fall within the scope and spirit of the present disclosure.

Claims

1. A bonding structure, include: a first element having a first non-conductive region and a first conductive feature; as well as a second component having a second non-conductive region and a second conductive feature, the second component being bonded to the first component along a bonding interface such that the second non-conductive region is directly bonded to the first non-conductive region along the non-conductive interface and the second conductive feature is directly bonded to the first conductive feature along the conductive interface, The conductive interface between the first conductive feature and the second conductive feature has a central region and an edge region, the edge region is laterally located between the central region and the non-conductive interface, and the non-conductive interface is between the first non-conductive region and the second non-conductive region, wherein in a side cross-section of the combined structure, there are more voids at or near the edge region than at or near the central region.

2. The combined structure of claim 1 , wherein the first non-conductive region has a cavity extending at least partially through the thickness of the first non-conductive region, and the first conductive feature is formed in the cavity, the first conductive feature comprising a central portion and an edge portion, the edge portion being disposed between a sidewall of the cavity and the central portion. 3 . The bonding structure according to claim 2 , wherein the central portion has a first coefficient of thermal expansion, and the edge portion has a second coefficient of thermal expansion different from the first coefficient of thermal expansion. 4 . The bonded structure of claim 3 , wherein the central portion and the edge portion comprise the same material having different crystal orientations. The bonding structure according to claim 3 , wherein the central portion and the edge portion comprise different materials.

6. The bonded structure of claim 2, wherein the edge region comprises filaments of material of the edge portion of the first conductive feature. 7 . The bonded structure of claim 2 , wherein the center portion is partially disposed between the edge portion of the first conductive feature and the edge portion of the second conductive feature.

8. The combined structure of claim 2, wherein the second non-conductive region has a second cavity extending at least partially through the thickness of the second non-conductive region, and the second conductive feature is formed in the second cavity, the second conductive feature comprising a second center portion and a second edge portion, the second edge portion being disposed between a second sidewall of the second cavity and the second center portion. 9 . The bonding structure of claim 1 , wherein the voids at or near the central region have an average void size that is larger than an average void size of the voids at or near the edge region.

10. A component having a bonding surface, include: a non-conductive region having a cavity extending at least partially through a thickness of the non-conductive region from a contact surface of the non-conductive region, the contact surface at least partially defining the bonding surface of the element; as well as A conductive feature is formed in the cavity, the conductive feature includes a center portion and an edge portion, the edge portion is disposed between a sidewall of the cavity and the center portion, the center portion has a first thermal expansion coefficient, the edge portion has a second thermal expansion coefficient different from the first thermal expansion coefficient, the center portion is recessed to a first depth relative to the contact surface of the non-conductive region, and the edge portion is recessed to a second depth relative to the contact surface of the non-conductive region different from the first depth.

11. The element according to claim 10, wherein the contact surface has a surface structure prepared for direct bonding.

12. The element of claim 10, wherein the first coefficient of thermal expansion is greater than the second coefficient of thermal expansion.

13. The element of claim 12, wherein the central portion and the edge portion comprise the same material having different crystal orientations.

14. The element of claim 12, wherein the central portion and the edge portion comprise different materials.

15. The element of claim 10, wherein the second depth is greater than the first depth.

16. The element of claim 10, further comprising a barrier layer disposed between the edge portion and the sidewall of the cavity, the barrier layer configured to prevent or reduce diffusion of the conductive feature into the non-conductive region.

17. A component having a bonding surface, the component include: a non-conductive region having a cavity extending at least partially through a thickness of the non-conductive region from a contact surface of the non-conductive region, the contact surface at least partially defining the bonding surface of the element; as well as a conductive feature formed in the cavity, the conductive feature comprising a center portion and an edge portion, the edge portion being disposed between a sidewall of the cavity and the center portion, the center portion having a first coefficient of thermal expansion, the edge portion having a second coefficient of thermal expansion different from the first coefficient of thermal expansion, the center portion being recessed to a first depth relative to the contact surface of the non-conductive region, the edge portion being recessed to a second depth relative to the contact surface of the non-conductive region, Wherein the first coefficient of thermal expansion is at least 5% greater than the second coefficient of thermal expansion.

18. The element according to claim 17, wherein the contact surface has a surface structure prepared for direct bonding.

19. The element of claim 17, wherein the central portion and the edge portion comprise the same material having different crystal orientations.

20. The element of claim 17, wherein the central portion and the edge portion comprise different materials.

21. The element of claim 17, wherein the second depth is greater than the first depth.

22. The element of claim 17, further comprising a barrier layer disposed between the edge portion and the sidewall of the cavity.

23. A method of forming a conductive feature in a cavity in a non-conductive region of a component, the cavity extending at least partially through a thickness of the non-conductive region from a contact surface of the non-conductive region, the method include: providing a first conductive material in the cavity; removing at least a portion of the first conductive material from the cavity; providing a second conductive material in the removed portion of the first conductive material; as well as The first conductive material and the second conductive material are recessed relative to the contact surface of the non-conductive region.

24. The method of claim 23, wherein the first conductive material is recessed to a first depth relative to the contact surface of the non-conductive region, and the second conductive material is recessed to a second depth relative to the contact surface of the non-conductive region that is different from the first depth.

25. The method of claim 24, wherein the second conductive material is positioned between the first conductive material and a sidewall of the cavity.

26. The method of claim 25, wherein the first conductive material comprises copper or a cobalt alloy.

27. The method of claim 25, wherein the second depth is greater than the first depth.

28. The method of claim 23, wherein the first material has a first coefficient of thermal expansion and the second material has a second coefficient of thermal expansion, the first coefficient of thermal expansion being greater than the second coefficient of thermal expansion.

29. The method of claim 23, wherein recessing the first and second conductive materials relative to the contact surface of the non-conductive region comprises polishing the non-conductive region and the conductive features.

30. The method of claim 23, further comprising providing a barrier layer on an inner surface of the cavity.

31. A method for forming a bonding structure, the method include: A first element is provided, the first element comprising: a non-conductive region having a cavity extending at least partially through a thickness of the non-conductive region from a contact surface of the non-conductive region, the contact surface at least partially defining a bonding surface of the first element, and a conductive feature formed in the cavity and at least partially defining the bonding surface of the first element, the conductive feature comprising a center portion and an edge portion, the edge portion being disposed between a sidewall of the cavity and the center portion, the center portion having a first coefficient of thermal expansion, the edge portion having a second coefficient of thermal expansion different from the first coefficient of thermal expansion, the center portion being recessed to a first depth relative to the contact surface of the non-conductive region, and the edge portion being recessed to a second depth relative to the contact surface of the non-conductive region different from the first depth; and The bonding surface of the second element is bonded directly to the bonding surface of the first element.

32. The method of claim 31 , wherein directly bonding the bonding surfaces of the first element and the second element comprises directly bonding a non-conductive region of the second element to the non-conductive region of the first element without an intervening adhesive, and directly bonding a conductive feature of the second element to the conductive feature of the first element without an intervening adhesive.

33. The method of claim 32, wherein directly bonding the conductive feature of the second component to the conductive feature of the first component comprises annealing the conductive feature.

34. The method of claim 32, wherein the first coefficient of thermal expansion is greater than the second coefficient of thermal expansion.

35. The method of claim 34, wherein the central portion and the edge portion comprise the same material having different crystal orientations.

36. The method of claim 34, wherein the central portion and the edge portion comprise different materials.

37. The method of claim 31 , wherein the second depth is greater than the first depth.

38. The method of claim 31, wherein the conductive feature of the second element comprises a center portion and an edge portion, the center portion of the second element having a third coefficient of thermal expansion and the edge portion of the second element having a fourth coefficient of thermal expansion.

39. The method of claim 38, wherein the third coefficient of thermal expansion is greater than the fourth coefficient of thermal expansion.