Positive electrode active material for lithium secondary battery, method for producing same, and lithium secondary battery

By solidly dissolving Ti on the surface of lithium nickel manganese and cobalt composite oxide particles and processing Ti oxide, the problem of poor circulation characteristics of the positive electrode active substance of lithium nickel manganese manganese cobalt composite oxide is solved, and the excellent circulation characteristics of lithium secondary batteries are achieved. Electrochemical performance improvement.

CN119096377APending Publication Date: 2024-12-06NIPPON CHEMICAL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036468.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The poor circulation characteristics of lithium nickel manganese and cobalt composite oxide as the positive electrode active substance of lithium secondary batteries affect their performance in applications such as electric vehicles.

Method used

By solidly dissolving Ti on the surface of lithium nickel manganese cobalt composite oxide particles, a high-content and low-content areas of Ti are formed, and dry mixing and heating treatment are performed with Ti oxides to form a positive electrode active material with excellent circulation characteristics.

Benefits of technology

It significantly improves the circulation characteristics of lithium secondary batteries, enhances the circulation stability and electrochemical performance of the batteries, and is suitable for high-demand applications such as electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005102187070000201
    Figure BDA0005102187070000201
  • Figure BDA0005102187070000221
    Figure BDA0005102187070000221
  • Figure BDA0005102187070000231
    Figure BDA0005102187070000231
Patent Text Reader

Abstract

The present invention can impart excellent cycle characteristics to a lithium secondary battery using a lithium nickel manganese cobalt composite oxide as a positive electrode active material. A positive electrode active material for a lithium secondary battery according to the present invention comprises lithium nickel manganese cobalt composite oxide particles containing Ti by solid solution of Ti in lithium nickel manganese cobalt composite oxide particles represented by general formula (1), and is characterized by having a first region in which the atomic mole% of Ti is 4.0 at% or more and a second region in which the atomic mole% of Ti is less than 4.0 at%, the compound is a single phase in X-ray diffraction analysis. In the formula, M represents one or more metal elements selected from Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, Ga, Ge, Sn, Ba, W, Na and K, x is 0.98 < = x < = 1.20, y is 0.30 < = y < 1.00, z is 0 < z < = 0.50, t is 0 < t < = 0.50, p is 0 < = p < = 0.05, and y + z + t + p = 1. Li < x > Ni < y > Mn < z > Co < t > M O < 1 + x > (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the positive electrode active material, and a lithium secondary battery. Background Art

[0002] Currently, lithium cobalt oxide is used as a positive electrode active material for lithium secondary batteries. However, since cobalt is a rare metal, lithium nickel manganese cobalt composite oxides with a low cobalt content are being developed (see, for example, Patent Documents 1 and 2).

[0003] It is known that lithium secondary batteries using lithium nickel manganese cobalt composite oxide as a positive electrode active material can achieve low cost and higher capacity than lithium cobalt oxide by adjusting the atomic ratio of nickel, manganese and cobalt contained in the composite oxide (for example, see Patent Document 3).

[0004] However, in these conventional methods, lithium secondary batteries using lithium nickel manganese cobalt composite oxide as a positive electrode active material have a problem of poor cycle characteristics.

[0005] As a method for improving the cycle characteristics of lithium secondary batteries using lithium nickel manganese cobalt composite oxide as a positive electrode active material, a method of coating the surface of lithium nickel manganese cobalt composite oxide particles with a Ti-containing compound has been proposed (see, for example, Patent Document 4, Patent Document 5, etc.).

[0006] As a method for coating the particle surface of lithium nickel manganese cobalt composite oxide with a Ti-containing compound, Patent Documents 4 and 5 propose a method of mixing an alcohol salt monomer or oligomer of an organic metal compound containing Ti and an alcohol such as 2-propanol, adding a chelating agent such as acetylacetone, and then adding water to prepare a dispersion of a precursor of Ti-containing microparticles with an average particle size of 1 to 20 nm, using the dispersion to coat the particle surface of lithium nickel manganese cobalt composite oxide, and then performing a heat treatment.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2004 / 092073 Pamphlet

[0010] Patent Document 2: Japanese Patent Application Publication No. 2005-25975

[0011] Patent Document 3: Japanese Patent Application Publication No. 2011-23120

[0012] Patent Document 4: Japanese Patent Application Publication No. 2016-24968

[0013] Patent Document 5: Japanese Patent Application Publication No. 2016-72071 Summary of the invention

[0014] Technical problem to be solved by the invention

[0015] In recent years, lithium secondary batteries have been studied for use in automotive fields such as electric vehicles, hybrid vehicles, and plug-in hybrid vehicles. Therefore, in lithium secondary batteries using lithium nickel manganese cobalt composite oxide as a positive electrode active material, the cycle characteristics need to be further improved.

[0016] Therefore, an object of the present invention is to provide a positive electrode active material for a lithium secondary battery that can impart excellent cycle characteristics to a lithium secondary battery using a lithium nickel manganese cobalt composite oxide as a positive electrode active material, and a lithium secondary battery having excellent cycle characteristics.

[0017] Technical solutions for solving technical problems

[0018] In view of the above facts, the inventors of the present invention have repeatedly conducted in-depth studies and found that the cycle characteristics of a lithium secondary battery using the following lithium nickel manganese cobalt composite oxide particles as positive electrode active materials are excellent, thereby completing the present invention. The lithium nickel manganese cobalt composite oxide particles are represented by the general formula (1) in which Ti is solid-dissolved, and have, from the surface to the depth direction, a region in which Ti is solid-dissolved in an amount of more than a predetermined atomic mol % and a region in which the amount of Ti solid-dissolved is less than a predetermined atomic mol %, and are single-phase in X-ray diffraction analysis.

[0019] That is, the present invention (1) provides a positive electrode active material for a lithium secondary battery, characterized in that: it is composed of lithium nickel manganese cobalt composite oxide particles containing Ti by solid-dissolving Ti in lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1), and the lithium nickel manganese cobalt composite oxide particles have: the atomic mole % of Ti relative to the total amount of Ni, Co and Ti is 4.0 a t% or more of the first region; and Ti relative to Ni, C o The total amount of Ti is less than 4.0 atomic mol% a t% of the second region is a single-phase lithium nickel manganese cobalt composite oxide particle represented by the above general formula (1) in X-ray diffraction analysis,

[0020] LiNiyMnzCotMpO)1 +× (1)

[0021] In the formula, M represents a metal selected from the group consisting of Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, G a , G e , Sn, B a , W, N aand K. x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, y+z+t+p=1.

[0022] In addition, the present invention (2) provides the positive electrode active material for lithium secondary batteries described in (1), characterized in that the content of Ti is 100% by atomic conversion relative to Ni, Mn, C in the lithium nickel manganese cobalt composite oxide particles. o The total amount of Ti and M is 0.01 to 5.00 mol%.

[0023] In addition, the present invention (3) provides the positive electrode active material for lithium secondary batteries according to (1) or (2), characterized in that the content of residual alkali is 1.20 mass % or less.

[0024] In addition, the present invention (4) provides a positive electrode active material for a lithium secondary battery according to any one of (1) to (3), characterized in that the atomic mol % of Ti on the particle surface relative to the total amount of Ni, Co and Ti is 6.0 a t% or more.

[0025] In addition, the present invention (5) provides a positive electrode active material for a lithium secondary battery according to any one of (1) to (4), characterized in that the atomic mol % (A) of Ti at a depth of 0 nm relative to the total amount of Ni, Co and Ti is greater than that of Ti at a depth of 330 nm relative to Ni, Co and Ti. o The ratio (A / B) of the total amount of Ti to the atomic mol % (B) is 10.0 or more.

[0026] In addition, the present invention (6) provides a positive electrode active material for a lithium secondary battery as described in any one of (1) to (5), characterized in that the positive electrode active material for a lithium secondary battery is obtained by the following method, wherein the lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1) are dry-mixed with a Ti-containing oxide to allow the Ti-containing oxide to adhere to the particle surface of the lithium nickel manganese cobalt composite oxide particles to obtain composite oxide particles with the Ti-containing oxide adhered thereto, and then the composite oxide particles with the Ti-containing oxide adhered thereto are heated at a temperature of not less than 750° C. and not more than 1000° C. to obtain the positive electrode active material for a lithium secondary battery.

[0027] LixNiMnzCoMpO1 +× (1)

[0028] In the formula, M represents a metal selected from the group consisting of Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, G a , G e, Sn, B a , W, N a and K. x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, y+z+t+p=1.

[0029] In addition, the present invention (7) provides a positive electrode active material for a lithium secondary battery as described in any one of (1) to (6), characterized in that the above-mentioned positive electrode active material for a lithium secondary battery is a mixture of large particles with an average particle size of 7.5 to 30.0 μm and small particles with an average particle size of 0.50 to 7.5 μm.

[0030] In addition, the present invention (8) provides the positive electrode active material for lithium secondary batteries described in (7), characterized in that the mixing ratio of the above-mentioned large particles to the above-mentioned small particles is 7:13 to 19:1 in terms of mass ratio.

[0031] In addition, the present invention (9) provides a positive electrode active material for a lithium secondary battery as described in (7) or (8), characterized in that: the above mixture is 0.65 to nf / c m 2 The compressed density after compression treatment under the conditions of 2.7g / cm 3 above.

[0032] In addition, the present invention (10) provides a method for producing a positive electrode active material for a lithium secondary battery, characterized in that: a lithium nickel manganese cobalt composite oxide particle represented by the following general formula (1) is dry-mixed with a Ti-containing oxide to allow the Ti-containing oxide to adhere to the particle surface of the lithium nickel manganese cobalt composite oxide particle, and after obtaining the composite oxide particle with the Ti-containing oxide adhered thereto, the composite oxide particle with the Ti-containing oxide adhered thereto is heat-treated at a temperature of not less than 750° C. and not more than 1000° C.,

[0033] LiNiyMnzCotMpO1 +× (1)

[0034] In the formula, M represents a metal selected from the group consisting of Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, G a , G e , Sn, B a , W, N a and K. x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, y+z+t+p=1.

[0035] In addition, the present invention (11) provides a method for producing a positive electrode active material for a lithium secondary battery as described in (10), characterized in that: the Ti-containing oxide is TiO 2 .

[0036] Furthermore, the present invention (12) provides a lithium secondary battery characterized by using the positive electrode active material for a lithium secondary battery described in any one of (1) to (9).

[0037] Effects of the Invention

[0038] The positive electrode active material for lithium secondary batteries of the present invention can impart excellent cycle characteristics to lithium secondary batteries using lithium nickel manganese cobalt composite oxide as the positive electrode active material, and by using the positive electrode active material for lithium secondary batteries of the present invention, a lithium secondary battery with excellent cycle characteristics can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the X-ray diffraction pattern of the positive electrode active material sample obtained in Example 1.

[0040] Figure 2 This is the X-ray diffraction pattern of the positive electrode active material sample obtained in Example 2.

[0041] Figure 3 This is the X-ray diffraction pattern of the positive electrode active material sample obtained in Comparative Example 3.

[0042] Figure 4 Graph showing the change in atomic mol % of Ti in the depth direction of the positive electrode active material sample obtained in Example 1.

[0043] Figure 5 Graph showing the change in atomic mol % of Ti in the depth direction of the positive electrode active material sample obtained in Comparative Example 1.

[0044] Figure 6 These are secondary electron images and Ti element mapping images obtained by analyzing the positive electrode active material samples obtained in Example 2 and Comparative Example 3 using SEM-EDX analysis. DETAILED DESCRIPTION

[0045] The positive electrode active material for a lithium secondary battery of the present invention is characterized in that it is composed of lithium nickel manganese cobalt composite oxide particles containing Ti by solid-dissolving Ti in lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1), wherein the lithium nickel manganese cobalt composite oxide particles have, from the surface in the depth direction: a first region in which the atomic mol % of Ti relative to the total amount of Ni, Co and Ti is 4.0 at % or more; and a first region in which the atomic mol % of Ti relative to Ni, Co and Ti is 4.0 at % or more. oThe second region in which the total atomic mol % of Ti is less than 4.0 at % is a lithium nickel manganese cobalt composite oxide represented by the above general formula (1) in a single phase in X-ray diffraction analysis.

[0046] LiNiyMnzCotMpO 1+× (1)

[0047] In the formula, M represents a metal selected from the group consisting of Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, G a , G e , Sn, B a , W, N a and K. x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, y+z+t+p=1.

[0048] The positive electrode active material for lithium secondary batteries of the present invention is a lithium nickel manganese cobalt composite oxide particle containing Ti by dissolving Ti in the lithium nickel manganese cobalt composite oxide particles represented by the general formula (1). That is, the positive electrode active material for lithium secondary batteries of the present invention is a lithium nickel manganese cobalt composite oxide particle represented by the general formula (1) in which Ti is solid-dissolved. Moreover, in the positive electrode active material for lithium secondary batteries of the present invention, from the particle surface of the lithium nickel manganese cobalt composite oxide particle, there are formed in the depth direction: a first region in which the solid-dissolved amount of Ti is greater than a specified mole %; and a second region continuous with the first region in which the solid-dissolved amount of Ti is less than a specified mole %. In addition, the positive electrode active material for lithium secondary batteries of the present invention is an aggregate of lithium nickel manganese cobalt composite oxide particles that are single-phase in X-ray diffraction analysis.

[0049] As described above, the positive electrode active material for lithium secondary batteries of the present invention is different from a product in which Ti oxide is present in an adhered state on the surface of the lithium nickel manganese cobalt composite oxide particles of the core particles.

[0050] The product in which Ti oxide is attached to the surface of the lithium nickel manganese cobalt composite oxide particles of the core particles depends on the amount of Ti oxide attached, but in X-ray diffraction analysis, Ti oxide is detected as a different phase in addition to the lithium nickel manganese cobalt composite oxide of the core particles.

[0051] In contrast, the lithium nickel manganese cobalt composite oxide particles containing Ti by dissolving Ti in the lithium nickel manganese cobalt composite oxide particles represented by the general formula (1) involved in the positive electrode active material for lithium secondary batteries of the present invention do not substantially detect heterogeneous phases of Ti oxide when X-ray diffraction analysis is performed. That is, the lithium nickel manganese cobalt composite particles represented by the general formula (1) of the positive electrode active material for lithium secondary batteries of the present invention are single-phase lithium nickel manganese cobalt composite particles in X-ray diffraction analysis.

[0052] In addition, when Ti-containing oxide is attached to the particle surface of the lithium nickel manganese cobalt composite oxide particles, when the particle surface of the lithium nickel manganese cobalt composite oxide particles is analyzed by SEM-EDX at a magnification of 10,000 to 30,000 times with elemental mapping analysis of Ti, it is observed that Ti is unevenly distributed on the particle surface of the lithium nickel manganese cobalt composite oxide particles.

[0053] In contrast, in the lithium nickel manganese cobalt composite oxide particles containing Ti in which Ti is solid-dissolved in the lithium nickel manganese cobalt composite oxide particles represented by the general formula (1) involved in the positive electrode active material for the lithium secondary battery of the present invention, when the particle surface of the lithium nickel manganese cobalt composite oxide particles was analyzed by elemental mapping of Ti using SEM-EDX at a magnification of 10,000 to 30,000 times, it was observed that Ti was uniformly distributed like Co, Ni, Mn, etc.

[0054] In the positive electrode active material for lithium secondary batteries of the present invention, the lithium nickel manganese cobalt composite oxide particles to which Ti is solid-solved are composite oxides containing lithium, nickel, manganese and cobalt and are represented by the following general formula (1).

[0055] LixNiMnzCoMpO1 +× (1)

[0056] In the formula, M represents a metal selected from the group consisting of Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, G a , G e , Sn, B a , W, N a and K. x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, y+z+t+p=1.

[0057] In the general formula (1), x is 0.98≤x≤1.20. From the viewpoint of improving the initial capacity, x is preferably 1.00≤x≤1.10. In addition, y in the general formula (1) is 0.30≤y<1.00. From the viewpoint of being able to take into account both the initial capacity and the cycle characteristics, y is preferably 0.50≤y≤0.95, and particularly preferably 0.60≤y≤0.90. In addition, z in the general formula (1) is 0<z≤0.50. From the viewpoint of excellent safety, z is preferably 0.025≤z≤0.45. In addition, t is 0<t≤0.50. From the viewpoint of excellent safety, t is preferably 0.025≤t≤0.45. y+z+t+p=1. y / z is preferably (y / z)>1, particularly preferably (y / z)≥1.5, and more preferably 3≤(y / z)≤38.

[0058] In addition, M in the formula is a metal element contained in the lithium nickel manganese cobalt composite oxide represented by the general formula (1) as required for the purpose of improving battery performance such as cycle characteristics and safety, and examples of M include one or more metal elements selected from the group consisting of Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, Ga, Ge, Sn, Ba, W, Na and K. In the general formula (1), p is 0≤p≤0.050, preferably 0.0001≤p≤0.045.

[0059] In the positive electrode active material for lithium secondary batteries of the present invention, the lithium nickel manganese cobalt composite oxide particles containing Ti in a solid solution have, from the surface of the lithium nickel manganese cobalt composite oxide particles toward the depth direction: a first region containing Ti in a solid solution at a prescribed mole % or more; and a second region in which the mole % of the dissolved Ti is less than a prescribed value.

[0060] The first region is given by the following formula:

[0061] The atomic mole % of Ti relative to the total amount of Ni, Co and Ti = (Ti / (Ni+Co+Ti))×100 (wherein, Ni, Co and Ti are all atomically converted molar numbers.) The percentage (atomic mole %) of the calculated atomically converted molar number of Ti relative to the atomically converted molar number of Ni, Co and Ti is in the range of 4.0at% or above.

[0062] The first region is preferably formed to be at least 5 nm in depth from the surface of the lithium nickel manganese cobalt composite oxide particle, more preferably to be formed to be 10 nm or more, and further preferably to be formed to be 15 nm or more. In addition, the upper limit of the formation range of the first region is 100 nm or less, preferably 60 nm or less, and more preferably 50 nm or less in depth. By forming the first region in the above range, not only can the lithium ion conductivity in the second region be maintained, but also the dissolution of the transition metal from the inside of the lithium nickel manganese cobalt composite oxide particle can be suppressed, thereby improving the cycle characteristics.

[0063] The second region is given by the following formula:

[0064] The atomic mole % of Ti relative to the total amount of Ni, Co and Ti = (Ti / (Ni+Co+Ti))×100 (wherein, Ni, Co and Ti are all atomically converted molar numbers.) The area where the percentage (atomic mole %) of the calculated atomically converted molar number of Ti relative to the atomically converted molar number of Ni, Co and Ti is less than 4.0 at %.

[0065] The second region contains no Ti, or even if containing Ti, the percentage (atomic mol %) of the atomic mole number of Ti to the total mole number of atomic moles of Ni, Co, and Ti is less than 4.0 at %.

[0066] The second region is formed from the boundary with the first region to the center of the particle in the depth direction, so that the lithium ion conductivity in the second region can be maintained and the elution of transition metals from the inside of the lithium nickel manganese cobalt composite oxide particles can be suppressed, thereby improving the cycle characteristics.

[0067] In the present invention, regarding the first region and the second region, when etching is performed in the depth direction from the surface of the lithium nickel manganese cobalt composite oxide particles using argon gas by X-ray photoelectron spectroscopy (XPS), the element peaks of Ni, Co and Ti in the depth direction are measured, and the region where the atomic mole % of Ti relative to the total amount of Ni, Co and Ti is greater than 4.0 at % is judged as the first region, and the region where the atomic mole % is less than 4.0 at % is judged as the second region.

[0068] In addition, in the lithium secondary battery positive electrode active material of the present invention, the atomic mole % of Ti on the particle surface of the lithium nickel manganese cobalt composite oxide particles containing Ti in a solid solution relative to the total amount of Ni, Co and Ti is preferably 6.0 at% or more, more preferably 6.5 to 95.0 at%, further preferably 7.0 to 50.0 at%, and further preferably 10.0 to 30.0 at%. By having the atomic mole % of Ti on the surface of the lithium nickel manganese cobalt composite oxide particles within the above range, the dissolution of transition metals from the interior of the lithium nickel manganese cobalt composite oxide particles can be suppressed, the cycle characteristics can be improved, and the lithium ion conductivity can be maintained. It should be noted that the atomic mole % of Ti on the particle surface relative to the total amount of Ni, Co and Ti is based on the analysis value of 0 nm in the depth direction when the element peaks of Ni, Co and Ti in the depth direction are measured when etching is performed in the depth direction from the surface of the lithium nickel manganese cobalt composite oxide particles using argon gas by X-ray photoelectron spectroscopy (XPS) analysis, and is expressed as follows:

[0069] The value calculated as atomic mol % of Ti relative to the total amount of Ni, Co and Ti = (Ti / (Ni+Co+Ti))×100, wherein Ni, Co and Ti are all molar numbers in terms of atoms.

[0070] In the positive electrode active material for lithium secondary batteries of the present invention, the content of Ti in the lithium nickel manganese cobalt composite oxide particles containing Ti in solid solution is preferably 0.01 to 5.00 mol%, particularly preferably 0.02 to 4.50 mol%, relative to the total amount (moles) of Ni, Mn, Co and M in atomic conversion. By the amount of solid-dissolved Ti being in the above range, both the initial capacity and the cycle characteristics can be taken into account. It should be noted that the Ti content in the lithium nickel manganese cobalt composite oxide particles refers to the percentage of the total mole of atomically converted Ti contained in the lithium nickel manganese cobalt composite oxide particles as a whole relative to the total amount (moles) of atomically converted Ni, Mn, Co and M contained in the lithium nickel manganese cobalt composite oxide particles as a whole.

[0071] In the lithium secondary battery positive electrode active material of the present invention, the ratio (A / B) of "the atomic mole % (A) of Ti at a depth of 0 nm relative to the total amount of Ni, Co and Ti" to "the atomic mole % (B) of Ti at a depth of 330 nm relative to the total amount of Ni, Co and Ti" of the lithium nickel manganese cobalt composite oxide particles containing Ti in a solid solution is 10.0 or more, preferably 10.5 to 150.0, particularly preferably 11.0 to 120.0, and further preferably 15.0 to 40.0. From the viewpoint of inhibiting the dissolution of transition metals from the inside of the lithium nickel manganese cobalt composite oxide particles and improving the cycle characteristics, the above range is preferred.

[0072] The positive electrode active material for lithium secondary batteries of the present invention is a granular material of lithium nickel manganese cobalt composite oxide particles containing Ti in a solid solution. The lithium nickel manganese cobalt composite oxide particles containing Ti in a solid solution may be single particles in which primary particles are monodispersed, or may be aggregated particles in which primary particles are aggregated to form secondary particles.

[0073] The average particle size of the positive electrode active material for lithium secondary batteries of the present invention is 0.50 to 30.0 μm, preferably 1.0 to 25.0 μm, and particularly preferably 1.5 to 20.0 μm, in terms of volume conversion 50% particle size (D50) in the particle size distribution obtained by laser diffraction / scattering method. In addition, the BET specific surface area of ​​the positive electrode active material for lithium secondary batteries of the present invention is preferably 0.05 to 2.00 m 2 / g, particularly preferably 0.15 to 1.00 m 2 When the average particle size and the BET specific surface area of ​​the positive electrode active material for lithium secondary batteries of the present invention are within the above ranges, the preparation and coating properties of the positive electrode mixture can be easily achieved, and an electrode with high filling properties can be obtained.

[0074] In addition, the content of residual alkali in the positive electrode active material for lithium secondary batteries of the present invention is preferably 1.20 mass % or less, particularly preferably 1.00 mass % or less. By keeping the content of residual alkali in the positive electrode active material for lithium secondary batteries of the present invention within the above range, battery expansion and deterioration caused by gas generation caused by residual alkali can be suppressed.

[0075] It should be noted that in the present invention, the residual alkali refers to the alkaline component dissolved into water when the positive electrode active material for the lithium secondary battery of the present invention is stirred and dispersed in water at 25°C. In addition, the amount of residual alkali can be obtained by weighing 5g of the positive electrode active material for the lithium secondary battery of the present invention and 100g of pure water in a beaker, dispersing them for 5 minutes at a temperature of 25°C with a magnetic stirrer, then filtering the dispersion, and neutralizing and titrating the amount of alkali present in the obtained filtrate. It should be noted that the amount of residual alkali is a value obtained by titrating the amount of lithium and converting it into lithium carbonate.

[0076] The method for producing the positive electrode active material for lithium secondary batteries of the present invention is not particularly limited, but the positive electrode active material for lithium secondary batteries of the present invention can be suitably produced by, for example, the method for producing the positive electrode active material for lithium secondary batteries of the present invention described below.

[0077] The method for manufacturing a positive electrode active material for a lithium secondary battery of the present invention is characterized in that: lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1) are dry-mixed with a Ti-containing oxide to allow the Ti-containing oxide to adhere to the particle surface of the lithium nickel manganese cobalt composite oxide particles, and after obtaining composite oxide particles with the Ti-containing oxide adhered thereto, the composite oxide particles with the Ti-containing oxide adhered thereto are heat-treated at a temperature of not less than 750°C and not more than 1000°C.

[0078] LixNiMnzCoMpO1 +× (1)

[0079] In the formula, M represents a metal selected from Mg, Al, Ti, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, G a , G e , Sn, B a , W, N a and K. x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, y+z+t+p=1.

[0080] The lithium nickel manganese cobalt composite oxide particles represented by the general formula (1) involved in the method for producing a positive electrode active material for a lithium secondary battery of the present invention are produced, for example, by a raw material mixing step of mixing a lithium source, a nickel source, a manganese source, a cobalt source and an M source added as needed to prepare a raw material mixture and a subsequent firing step of firing the obtained raw material mixture.

[0081] As the lithium source, nickel source, manganese source, cobalt source and M source added as needed in the raw material mixing step, for example, their hydroxides, oxides, carbonates, nitrates, sulfates, organic acid salts, etc. can be used. The average particle size of the lithium source, nickel source, manganese source, cobalt source and M source is 0.50 to 30.0 μm, preferably 1.0 to 25.0 μm according to the average particle size obtained by laser diffraction / scattering method.

[0082] The nickel source, manganese source and cobalt source involved in the raw material mixing step can be compounds containing nickel atoms, manganese atoms and cobalt atoms. As compounds containing nickel atoms, manganese atoms and cobalt atoms, for example, composite oxides, composite hydroxides, composite oxyhydroxides, composite carbonates, etc. containing these atoms can be listed.

[0083] It should be noted that, as the method for preparing the compound containing nickel atoms, manganese atoms and cobalt atoms, known methods can be adopted. For example, in the case of composite hydroxides, it is possible to prepare by coprecipitation. Specifically, by mixing the aqueous solution containing the nickel atoms, cobalt atoms and manganese atoms of a prescribed amount, the aqueous solution of a complexing agent and the aqueous solution of an alkali, composite hydroxide coprecipitation can be made (with reference to Japanese Patent Laid-Open No. 10-81521 Gazette, Japanese Patent Laid-Open No. 10-81520 Gazette, Japanese Patent Laid-Open No. 10-29820 Gazette, 2002-201028 Gazette, etc.). In addition, in the case of composite carbonate, the method (Japanese Patent Laid-Open No. 2009-179545 Gazette) in which a solution (A liquid) containing nickel ion, manganese ion and cobalt ion and a solution (B liquid) containing carbonate ion or bicarbonate ion are added to a reaction vessel to react can be enumerated; or the method (Japanese Patent Laid-Open No. 2009-179544 Gazette) in which a solution (A liquid) containing nickel salt, manganese salt and cobalt salt and a solution (B liquid) containing metal carbonate or metal bicarbonate are added to a solution (C liquid) containing the same anion as the anion of the nickel salt, manganese salt and cobalt salt in the A liquid and the same anion as the anion of the metal carbonate or the metal bicarbonate in the B liquid is reacted can be enumerated. In addition, the compound containing nickel atom, manganese atom and cobalt atom can also be a commercially available product.

[0084] The average particle size of the compound containing nickel atoms, cobalt atoms, and manganese atoms is 0.50 to 100 μm, preferably 1.0 to 80.0 μm as an average particle size determined by a laser diffraction / scattering method.

[0085] In the production of lithium nickel manganese cobalt composite oxide particles represented by the general formula (1), composite hydroxides containing nickel atoms, cobalt atoms and manganese atoms are preferably used as nickel sources, manganese sources and cobalt sources from the viewpoint of good reactivity.

[0086] In the raw material mixing step, regarding the mixing ratio of the lithium source with the nickel source, manganese source, cobalt source and the M source added as needed, from the viewpoint of improving the discharge capacity, the molar ratio (Li / (Ni+Mn+Co+M)) of Li atoms to the total molar number of Ni atoms, Mn atoms, Co atoms and M atoms in the nickel source, manganese source and cobalt source (Ni+Mn+Co+M) is preferably 0.98 to 1.20, and a mixing ratio of 1.00 to 1.10 is particularly preferred.

[0087] Furthermore, in the raw material mixing step, the mixing ratio of each raw material of the nickel source, manganese source, cobalt source and M source added as required can be adjusted so that the atomic molar ratio of nickel, manganese, cobalt and M is represented by the above general formula (1).

[0088] It should be noted that, regardless of the production process of the raw material lithium source, nickel source, manganese source, cobalt source and M source, in order to produce high-purity lithium nickel manganese cobalt composite oxide particles, it is preferred to reduce the impurity content as much as possible.

[0089] In the raw material mixing step, the lithium source, nickel source, manganese source, cobalt source and the M source added as required may be mixed by either a dry process or a wet process, but dry mixing is preferred because of ease of production.

[0090] In the case of dry mixing, it is preferred to utilize a mechanical method for uniformly mixing the raw materials. As a mixing device, for example, a high-speed mixer, a super mixer, a turbo spherical mixer, an Ehrlich mixer, a Henschel mixer, a Nauta mixer, a ribbon mixer, a V-type mixer, a cone mixer, a jet mill, a micro-pulverizer (cosmomizer), a paint oscillator, a bead mill, a ball mill, etc. can be cited. It should be noted that, in a laboratory scale, a household mixer is sufficient.

[0091] In the case of wet mixing, as a mixing device, from the viewpoint of being able to prepare a slurry in which each raw material is uniformly dispersed, a medium mill is preferably used. In addition, from the viewpoint of being able to obtain a raw material mixture in which excellent reactivity and each raw material is uniformly dispersed, the slurry after the mixing process is preferably spray-dried.

[0092] The firing step is a step of obtaining a lithium nickel manganese cobalt composite oxide by firing the raw material mixture obtained in the raw material mixing step.

[0093] In the firing step, the raw material mixture is fired to react the raw materials at a firing temperature of 600 to 1000° C., preferably 700 to 950° C. The reason for this is that when the firing temperature is lower than 600° C., the reaction is insufficient and a large amount of unreacted lithium tends to remain; on the other hand, when the firing temperature exceeds 1000° C., the temporarily generated lithium nickel manganese cobalt composite oxide tends to decompose.

[0094] The firing time in the firing step is 3 hours or longer, preferably 5 to 30 hours. The firing atmosphere in the firing step is an oxidizing atmosphere of air or oxygen.

[0095] In addition, in the firing process, the firing can be performed in multiple stages. By performing the firing in multiple stages, lithium nickel manganese cobalt composite oxide particles with better cycle characteristics can be obtained. In the case of performing the firing in multiple stages, it is preferred that after firing in the range of 650 to 800° C. for 1 to 10 hours, the temperature is further raised to a temperature higher than the firing temperature, 800 to 950° C., and the firing is performed in this state for 5 to 30 hours.

[0096] The lithium nickel manganese cobalt composite oxide obtained in this way may be subjected to a plurality of firing steps as necessary.

[0097] In addition, the lithium nickel manganese composite oxide having the above-mentioned residual alkali content can be produced by the following method: in the raw material mixing step of the lithium source, the nickel source, the manganese source, the cobalt source and the M source added as required, the molar ratio (Li / (Ni+Mn+Co+M)) of Li atoms relative to the total molar number of Ni atoms, Mn atoms, Co atoms and M atoms in the nickel source, the manganese source, the cobalt source and the M source (Ni+Mn+Co+M)) is 0.98 to 1.20, and according to the mixing ratio, the calcination reaction is carried out at 700° C. or more, preferably 750 to 1000° C., for 3 hours or more, preferably 5 to 30 hours, so that the lithium source, the nickel source, the manganese source, the cobalt source and the M source added as required are fully reacted to produce the lithium nickel manganese cobalt composite oxide. In the present production method, the calcination is carried out in a multi-stage manner as described above, so that the lithium nickel manganese cobalt composite oxide having a further reduced residual alkali content can be produced.

[0098] It should be noted that the residual alkali of the positive electrode active material for lithium secondary batteries of the present invention and the determination method thereof are as described in the above-mentioned lithium nickel manganese cobalt composite oxide particles, and the residual alkali represents the alkaline component dissolved into water when the positive electrode active material for lithium secondary batteries is stirred and dispersed in water at 25°C. In addition, the amount of residual alkali can be obtained by weighing 5g of positive electrode active material for lithium secondary batteries and 100g of pure water in a beaker, dispersing them with a magnetic stirrer at a temperature of 25°C for 5 minutes, then filtering the dispersion, and neutralizing and titrating the amount of alkali present in the obtained filtrate. It should be noted that the amount of residual alkali is a value obtained by titrating the amount of lithium and converting it into lithium carbonate.

[0099] Examples of the Ti-containing oxides used in the method for producing a positive electrode active material for a lithium secondary battery of the present invention include TiO 2 、Ti 2 O 3 、Ti n O 2n-1 (n=3 to 9) and the like, and a composite oxide containing Ti and one or more selected from Mg, Li, Ni, Mn, Co and M, etc. Among them, Ti oxide is preferred from the viewpoint of improving the cycle characteristics, and TiO is particularly preferred. 2 .

[0100] From the perspective of enabling Ti to be efficiently dissolved in the shell layer on the particle surface of the lithium nickel manganese cobalt composite oxide particles, the average particle size of the Ti-containing oxide is preferably less than 100 μm, preferably 0.01 to 10.0 μm, according to the volume cumulative 50% particle size (D50) obtained by a laser diffraction / scattering method.

[0101] It should be noted that the Ti-containing oxide may be an agglomerate of primary particles to form secondary particles. In the method for manufacturing a positive electrode active material for a lithium secondary battery of the present invention, since the lithium nickel manganese cobalt composite oxide particles and the Ti-containing oxide are dry mixed, the agglomerated Ti-containing oxide is finely pulverized during the mixing, so that the micronized Ti-containing oxide can be attached to the particle surface of the lithium nickel manganese cobalt composite oxide particles.

[0102] From the viewpoint of enabling the Ti-containing oxide to efficiently adhere to the particle surface of the lithium nickel manganese cobalt composite oxide particles, when using an agglomerated Ti-containing oxide, the primary particle size of the Ti-containing oxide is preferably 2.0 μm or less, preferably 0.001 to 1.0 μm, in terms of the average particle size of the primary particles obtained by scanning electron micrographs.

[0103] From the viewpoint of being able to take both initial capacity and cycle characteristics into account within a preferred range, in the method for manufacturing a positive electrode active material for a lithium secondary battery of the present invention, the mixing amount of the Ti-containing oxide into the lithium nickel manganese cobalt composite oxide particles is preferably a mixing amount of Ti of 0.01 to 5.00 mol %, preferably 0.02 to 4.50 mol %, relative to the total amount (molar) of Ni, Mn, Co and M in the lithium nickel manganese cobalt composite oxide particles in terms of atomic conversion.

[0104] Moreover, by dry mixing the lithium nickel manganese cobalt composite oxide particles represented by the general formula (1) with the Ti-containing oxide, the Ti-containing oxide is attached to the particle surface of the lithium nickel manganese cobalt composite oxide particles represented by the general formula (1), thereby obtaining composite oxide particles with Ti-containing oxide attached, that is, lithium nickel manganese cobalt composite oxide particles represented by the general formula (1) with Ti-containing oxide attached and distributed on the particle surface.

[0105] As the device used for the mixing process, for example, there can be mentioned a high-speed mixer, a super mixer, a turbo spherical mixer, a Henschel mixer, a Nauta mixer, a ribbon mixer, a V-type mixer and the like. It should be noted that the mixing process is not limited to the mechanical method described above. Moreover, on a laboratory scale, a household mixer or a laboratory grinder is also sufficient.

[0106] In the method for producing a positive electrode active material for a lithium secondary battery of the present invention, the composite oxide particles to which the Ti-containing oxide is attached are then subjected to a heat treatment at a temperature of 750° C. to 1000° C., preferably 755 to 975° C., and particularly preferably 760 to 950° C. By performing the heat treatment, a lithium nickel manganese cobalt composite oxide particle in which the Ti-containing oxide is solid-dissolved can be obtained, wherein the lithium nickel manganese cobalt composite oxide particle has, from the surface, in the depth direction: a region containing Ti-containing solid-dissolved at a predetermined atomic mol % or more (first region); and a region (second region) in which the content of the solid-dissolved Ti is less than a predetermined atomic mol %, and is a lithium nickel manganese cobalt composite oxide represented by the above general formula (1) that is a single phase in an X-ray diffraction analysis.

[0107] In the method for producing a positive electrode active material for a lithium secondary battery of the present invention, the time of the heat treatment is not limited, and is usually more than 1 hour, preferably 2 to 10 hours, so that a positive electrode active material for a lithium secondary battery that meets the required performance can be obtained. The atmosphere for the heat treatment is preferably an oxidizing atmosphere such as air or oxygen.

[0108] Then, in the method for manufacturing a positive electrode active material for a lithium secondary battery of the present invention, as described above, the composite oxide particles to which the Ti oxide is attached are subjected to heat treatment to obtain the positive electrode active material for a lithium secondary battery of the present invention. In addition, in the method for manufacturing a positive electrode active material for a lithium secondary battery of the present invention, after the heat treatment, crushing, classification, granulation, etc. can be performed as needed.

[0109] From the viewpoint of increasing the capacity per unit volume, the positive electrode active material for the lithium secondary battery of the present invention is preferably a mixture of large particles with an average particle size of 7.5 to 30.0 μm and small particles with an average particle size of 0.50 to 7.5 μm. The average particle size of the large particles is 7.5 to 30.0 μm, preferably 8.0 to 25.0 μm, and particularly preferably 8.5 to 20.0 μm. The average particle size of the small particles is 0.5 to 7.5 μm, preferably 1.0 to 7.0 μm, and particularly preferably 1.5 to 6.5 μm. In addition, the mixing ratio of large particles to small particles is preferably 7:13 to 19:1, and particularly preferably 1:1 to 9:1 in terms of mass ratio. In addition, from the viewpoint of increasing the capacity per unit volume, it is preferred that the mixture of large particles and small particles is 0.65 tonf / cm 2 The compressed density after compression treatment under the conditions of 2.7g / cm 3 More than, preferably 2.8 to 3.3 g / cm 3 , more preferably 2.9 to 3.3 g / cm 3It should be noted that when the positive electrode active material for the lithium secondary battery of the present invention is a mixture of large particles and small particles, the mixture can be obtained by, for example, separately preparing large particles with an average particle size of 7.5 to 30.0 μm, preferably 8.0 to 25.0 μm, and particularly preferably 8.5 to 20.0 μm and small particles with an average particle size of 0.5 to 7.5 μm, preferably 1.0 to 7.0 μm, and particularly preferably 1.5 to 6.5 μm, and then mixing the obtained large particles and small particles at a specified mixing ratio.

[0110] The lithium secondary battery of the present invention uses the positive electrode active material for lithium secondary batteries of the present invention as a positive electrode active material. The lithium secondary battery of the present invention includes a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte containing a lithium salt.

[0111] The positive electrode involved in the lithium secondary battery of the present invention is formed by, for example, applying a positive electrode mixture on a positive electrode current collector and drying it. The positive electrode mixture includes a positive electrode active material, a conductive agent, a binder, and a filler added as needed. In the lithium secondary battery of the present invention, the positive electrode is uniformly coated with the positive electrode active material for the lithium secondary battery of the present invention. Therefore, the battery performance of the lithium secondary battery of the present invention is high, especially the cycle characteristics are excellent.

[0112] The content of the positive electrode active material contained in the positive electrode mixture of the lithium secondary battery of the present invention is preferably 70 to 100% by mass, particularly preferably 90 to 98% by mass.

[0113] As the positive electrode collector involved in the lithium secondary battery of the present invention, there is no particular restriction as long as it is an electronic conductor that does not cause chemical changes in the constructed battery, for example, stainless steel, nickel, aluminum, titanium, fired carbon, aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be cited. The surface of these materials can be oxidized before use, and the surface of the collector can also be made concave and convex by surface treatment. In addition, as the form of the collector, for example, foil, film, sheet, net, punching material, lath body, porous body, foam, fiber bundle, non-woven fabric molded body, etc. can be cited. The thickness of the collector is not particularly limited, preferably 1 to 500 μm.

[0114] As the conductive agent involved in the lithium secondary battery of the present invention, there is no particular restriction as long as it is an electronic conductive material that does not cause chemical changes in the constructed battery. For example, graphite such as natural graphite and artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, pyrolytic black and other carbon blacks, carbon fibers, conductive fibers such as metal fibers, metal powders such as carbon fluoride, aluminum, nickel powder, zinc oxide, potassium titanate and other conductive whiskers, conductive metal oxides such as titanium oxide, or polyphenyl derivatives, etc., as natural graphite, for example, scaly graphite, flaky graphite and earthy graphite can be cited. These can be used alone or in combination of two or more. The mixing ratio of the conductive agent is 1 to 50% by mass, preferably 2 to 30% by mass in the positive electrode mixture.

[0115] Examples of the binder for the lithium secondary battery of the present invention include starch, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, regenerated cellulose, diacetyl cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, tetrafluoroethylene-hexafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, propylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, ethylene-acrylic acid copolymer or (Na + ) ion crosslinked body, ethylene-methacrylic acid copolymer or its (Na + ) ion crosslinked body, ethylene-methyl acrylate copolymer or its (Na + ) ion crosslinked body, ethylene-methyl methacrylate copolymer or its (Na + ) ion crosslinked bodies, polysaccharides such as polyethylene oxide, thermoplastic resins, polymers with rubber elasticity, etc., these binders can be used alone or in combination of two or more. It should be noted that when using compounds such as polysaccharides containing functional groups that react with lithium, it is preferred to add compounds such as isocyanate groups to inactivate their functional groups. The mixing ratio of the binder in the positive electrode mixture is 1 to 50% by mass, preferably 5 to 15% by mass.

[0116] The filler involved in the lithium secondary battery of the present invention is a material that suppresses the volume expansion of the positive electrode in the positive electrode mixture, and can be added as needed. As a filler, any material can be used as long as it is a fibrous material that does not cause chemical changes in the constructed battery, for example, fibers of olefin polymers such as polypropylene and polyethylene, glass, carbon, etc. can be used. The amount of filler added is not particularly limited, and is preferably 0 to 30% by mass in the positive electrode mixture.

[0117] The negative electrode involved in the lithium secondary battery of the present invention is formed by coating the negative electrode material on the negative electrode collector and drying it. As the negative electrode collector involved in the lithium secondary battery of the present invention, as long as it is an electronic conductor that does not cause chemical changes in the constructed battery, it is not particularly limited, for example, stainless steel, nickel, copper, titanium, aluminum, fired carbon, copper or stainless steel The surface is treated with carbon, nickel, titanium, silver and aluminum-cadmium alloys. In addition, the surface of these materials can be oxidized before use, and the surface of the collector can also be made concave and convex by surface treatment. In addition, as the form of the collector, for example, foil, film, sheet, net, punching material, lath body, porous body, foam, fiber bundle, non-woven fabric molded body, etc. can be cited. The thickness of the collector is not particularly limited, preferably 1 to 500 μm.

[0118] The negative electrode material of the lithium secondary battery of the present invention is not particularly limited, and examples thereof include carbonaceous materials, metal composite oxides, lithium metal, lithium alloys, silicon alloys, tin alloys, metal oxides, conductive polymers, chalcogenides, Li-Co-Ni materials, Li 4 Ti 5 O 12 , lithium niobate, silicon oxide (SiO x :0.5≤x≤1.6) etc. As carbonaceous materials, for example, non-graphitizable carbon materials, graphite-based carbon materials, etc. As metal composite oxides, for example, Sn p (M 1 ) 1-p (M 2 ) q O r (Where M 1 represents one or more elements selected from the group consisting of Mn, Fe, Pb and Ge, M 2 represents one or more elements selected from Al, B, P, Si, elements of Group IA, Group IIA, Group IIIB and halogen of the periodic table, 0<p≤1, 1≤q≤3, 1≤r≤8), Li t Fe 2 O 3 (0≤t≤1), Li t WO 2(0≤t≤1) etc. Examples of metal oxides include GeO, GeO 2 、SnO、SnO 2 、PbO、PbO 2 , Pb 2 O 3 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 、Bi 2 O 3 、Bi 2 O 4 、Bi 2 O 5 Etc. Examples of the conductive polymer include polyacetylene and polyparaphenylene.

[0119] As the diaphragm involved in the lithium secondary battery of the present invention, an insulating film having a large ion permeability and a predetermined mechanical strength can be used. Because it has resistance to organic solvents and hydrophobicity, sheets and non-woven fabrics made of olefin polymers such as polypropylene or glass fibers or polyethylene are used. As the pore size of the diaphragm, it can be in a range useful for general battery use, for example, 0.01 to 10 μm. As the thickness of the diaphragm, it can be in a range of general battery use, for example, 5 to 300 μm. It should be noted that when a solid electrolyte such as a polymer is used as an electrolyte described later, the solid electrolyte can also serve as a diaphragm.

[0120] The lithium salt-containing nonaqueous electrolyte of the lithium secondary battery of the present invention is an electrolyte containing a nonaqueous electrolyte and a lithium salt. As the nonaqueous electrolyte of the lithium secondary battery of the present invention, a nonaqueous electrolyte solution, an organic solid electrolyte, or an inorganic solid electrolyte is used. Examples of the non-aqueous electrolyte include one or a mixture of two or more aprotic organic solvents such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 3-methyl-2-oxazolidinone, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, diethyl ether, 1,3-propane sultone, methyl propionate, and ethyl propionate.

[0121] As the organic solid electrolyte involved in the lithium secondary battery of the present invention, for example, there can be mentioned polyethylene derivatives, polyethylene oxide derivatives or polymers containing them, polypropylene oxide derivatives or polymers containing them, phosphate polymers, polyphosphazenes, polyaziridines, polyethylene sulfides, polyvinyl alcohols, polyvinylidene fluoride, polyhexafluoropropylene and other polymers containing ionic dissociative groups, and mixtures of polymers containing ionic dissociative groups with the above-mentioned non-aqueous electrolytes.

[0122] As the inorganic solid electrolyte involved in the lithium secondary battery of the present invention, nitrides, halides, oxoacid salts, sulfides, etc. of Li can be used, for example, Li 3 N, LiI, Li 5 NI 2 , Li 3 N-LiI-LiOH, LiSiO 4 、LiSiO 4 -LiI-LiOH、Li 2 SiS 3 , Li 4 SiO 4 , Li 4 SiO 4 -LiI-LiOH、P 2 S 5 , Li 2 S or Li 2 S-P 2 S 5 , Li 2 S-SiS 2 , Li 2 S-GeS 2 , Li 2 S-Ga 2 S 3 , Li 2 S-B 2 S 3 , Li 2 S-P 2 S 5 -X, Li 2 S-SiS 2 -X, Li 2 S-GeS 2 -X, Li 2 S-Ga 2 S 3 -X, Li 2 S-B 2 S 3 -X, etc., wherein X is selected from LiI, B 2 S 3 or Al 2 S 3At least one of the above.

[0123] In addition, when the inorganic solid electrolyte is amorphous (glass), lithium phosphate (Li 3 PO 4 ), lithium oxide (Li 2 O), lithium sulfate (Li 2 SO 4 ), phosphorus oxide (P 2 O 5 ), lithium borate (Li 3 BO 3 ) and other oxygen-containing compounds, Li 3 PO 4-u N 2u / 3 (u is 0<u<4), Li 4 SiO 4-u N 2u / 3 (u is 0<u<4), Li 4 GeO 4-u N 2u / 3 (u is 0<u<4), Li 3 BO 3-u N 2u / 3 (u is 0<u<3) etc. By adding the oxygen-containing compound or nitrogen-containing compound, the gaps in the formed amorphous skeleton can be expanded, the hindrance to the movement of lithium ions can be reduced, and the ion conductivity can be further improved.

[0124] As the lithium salt involved in the lithium secondary battery of the present invention, a lithium salt dissolved in the above-mentioned non-aqueous electrolyte is used, for example, LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 Cl 10 、LiPF 6 、LiCF 3 SO 3 、LiCF 3 CO 2 、LiAsF 6 、LiSbF 6 , LiB 10 Cl 10 、LiAlCl 4 , CH 3 SO 3 Li, CF 3 SO 3 Li, (CF 3 SO 2 ) 2A salt formed by mixing one or more of NLi, aluminum chloroborate, lithium lower aliphatic carboxylate, lithium tetraphenylborate, imide, etc.

[0125] In addition, for the purpose of improving discharge, charge characteristics and flame retardancy, the following compounds can be added to the non-aqueous electrolyte. For example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, diglyme, hexamethylphosphoramide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone and N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, polyethylene glycol, pyrrole, 2-methoxyethanol, aluminum trichloride, monomers of conductive polymer electrode active materials, triethylenephosphoramide, trialkylphosphine, morpholine, aryl compounds having a carbonyl group, hexamethylphosphoric triamide and 4-alkylmorpholine, bicyclic tertiary amines, oils, phosphonium salts and sulfonium salts, phosphazenes, carbonates, etc. can be cited. In addition, in order to make the electrolyte non-flammable, the electrolyte can contain halogen-containing solvents such as carbon tetrachloride and trifluoroethylene. In addition, in order to be suitable for high-temperature storage, carbon dioxide gas can be contained in the electrolyte.

[0126] The lithium secondary battery of the present invention is a lithium secondary battery in which even when repeated charge and discharge are performed, the deterioration of the cycle characteristics is particularly small and the energy density maintenance rate is high, and the shape of the battery can be any shape such as button-shaped, sheet-shaped, cylindrical, square, coin-shaped, etc.

[0127] The use of the lithium secondary battery of the present invention is not particularly limited, and for example, electronic devices such as notebook personal computers, laptop personal computers, pocket word processors, mobile phones, wireless handsets, portable CD players, radios, liquid crystal televisions, backup power supplies, electric shavers, memory cards, video movie cameras, etc., automobiles, electric vehicles, drones, game devices, power tools and other consumer electronic devices can be cited.

[0128] Examples

[0129] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0130] <Preparation of lithium nickel manganese cobalt composite oxide particles (LNMC) sample>

[0131] <LNMC sample 1>

[0132] Lithium carbonate (average particle size 5.7 μm) and nickel manganese cobalt composite hydroxide (Ni∶Mn∶Co = 6∶2∶2 (molar ratio), average particle size 9.8 μm) were weighed and thoroughly mixed using a household mixer to obtain a raw material mixture with a molar ratio of Li / (Ni+Mn+Co) of 1.01. It should be noted that the nickel manganese cobalt composite hydroxide used a commercially available product.

[0133] Next, the obtained raw material mixture was fired in an alumina crucible in an atmospheric atmosphere at a temperature of 700 °C for 2 hours, and then fired at a temperature of 850 °C for 10 hours. After the firing was completed, the fired product was crushed and classified. The obtained fired product was measured by XRD, and as a result, it was confirmed that it was a single-phase lithium nickel manganese cobalt composite oxide. In addition, the obtained product was spherical lithium nickel manganese cobalt composite oxide particles (LiNi 2 / g) formed by secondary aggregation with an average particle size of 10.2 μm and a BET specific surface area of 0.21 m 0.6 Mn 0.2 Co 0.2 O 2 ).

[0134] <LNMC Sample 2>

[0135] Lithium carbonate (average particle size 5.7 μm) and nickel manganese cobalt composite hydroxide (Ni∶Mn∶Co = 6∶2∶2 (molar ratio), average particle size 3.7 μm) were weighed and thoroughly mixed using a household mixer to obtain a raw material mixture with a molar ratio of Li / (Ni + Mn + Co) of 1.01. It should be noted that a commercially available product was used for the nickel manganese cobalt composite hydroxide.

[0136] Next, the obtained raw material mixture was fired in an alumina crucible in an atmospheric atmosphere at a temperature of 700 °C for 2 hours, and then fired at a temperature of 850 °C for 10 hours. After the firing was completed, the fired product was crushed and classified. The obtained fired product was measured by XRD, and as a result, it was confirmed that it was a single-phase lithium nickel manganese cobalt composite oxide. In addition, the obtained product was spherical lithium nickel manganese cobalt composite oxide particles (LiNi 2 / g) formed by secondary aggregation with an average particle size of 5.4 μm and a BET specific surface area of 0.69 m 0.6 Mn 0.2 Co 0.2 O 2 ).

[0137] The physical properties of the above-obtained lithium nickel manganese cobalt composite oxide sample (LNMC sample) are shown in Table 1.

[0138] It should be noted that the average particle size, residual alkali content, and tap density of the LMNC sample were measured as follows.

[0139] <Average particle size>

[0140] Obtained by laser diffraction / scattering method.

[0141] <Measurement of residual alkali content>

[0142] 5 g of the sample and 100 g of ultrapure water were weighed in a beaker and dispersed at 25° C. for 5 minutes using a magnetic stirrer. Next, the dispersion was filtered, and 70 ml of the filtrate was titrated using an automatic titrator (model COMTITE-2500) with 0.1N-HCl to calculate the amount of residual alkali in the sample (the value converted to lithium carbonate by measuring the amount of lithium).

[0143] <Pressed density>

[0144] Weigh 2.25g of sample and put it into a biaxial former with a diameter of 1.5cm. Then apply 0.65tonf / cm 2 The height of the compressed object was measured after 1 minute of pressure, and the pressurized density of the sample was calculated based on the apparent volume of the compressed object calculated from the height and the mass of the collected sample.

[0145] [Table 1]

[0146]

[0147] (Example 1)

[0148] 29.9 g of LNMC sample 1 was collected, and 0.0618 g of titanium oxide (TiO 2 ), and then fully mixed with a laboratory grinder to obtain the attached TiO 2 Next, the obtained attached TiO 2 The composite oxide particles were calcined at 800°C for 5 hours, heat treated, crushed and classified to obtain a positive electrode active material sample in which Ti was solid-dissolved at 0.25 mol% relative to the total amount of Ni, Mn and Co in LNMC sample 1. The average particle size (D50) of the obtained positive electrode active material was 10.2 μm, and the BET specific surface area was 0.21 m 2 / g.

[0149] In addition, the residual alkali content and press density were measured in the same manner as for the LNMC sample. The results are shown in Table 2.

[0150] Titanium oxide used was an aggregate composed of secondary particles formed by agglomeration of primary particles. The volume-converted 50% particle size (D50) determined by a laser diffraction / scattering method was 0.38 μm, and the average particle size of the primary particles determined by a SEM photograph was 0.035 μm.

[0151] The average particle size of primary particles is obtained by extracting 30 random particles under a scanning electron microscope, measuring the short axis and long axis of each particle, calculating 1 / 2 of the sum of the two, and finding the average value of the 30 particles as the average particle size.

[0152] Furthermore, the obtained positive electrode active material sample was subjected to X-ray diffraction analysis using Cu-Kα radiation as a radiation source. No TiO 2 The diffraction peaks caused by LiTiO 2 and Li 2 TiO 3 The X-ray diffraction pattern of the positive electrode active material sample is shown in Figure 1 .

[0153] In addition, using SEM-EDX (field emission scanning electron microscope SU-8220 manufactured by Hitachi High-Technologies Corporation and energy dispersive X-ray analyzer XFlash5060FlatQUAD manufactured by BRUKER), elemental mapping analysis of Ti was performed on the particle surface of the positive electrode active material sample at a magnification of 20,000 times and confirmed that Ti was evenly distributed, just like Co, Ni and Mn.

[0154] From the results of X-ray diffraction analysis, Ti element mapping analysis, and X-ray photoelectron spectroscopy (XPS) analysis described later, it was confirmed that Ti existed as a solid solution inside the particles of the positive electrode active material sample.

[0155] (Example 2)

[0156] 29.9 g of LNMC sample 2 was collected and 0.144 g of titanium oxide (TiO 2 ), and then fully mixed with a laboratory grinder to obtain the attached TiO 2 Next, the obtained attached TiO 2 The composite oxide particles were calcined at 800°C for 5 hours, heat treated, crushed and classified to obtain a positive electrode active material sample having 0.58 mol% Ti solid solution relative to the total amount of Ni, Mn and Co in LNMC sample 2. The average particle size (D50) of the obtained positive electrode active material was 4.0 μm, and the BET specific surface area was 0.69 m 2 / g.

[0157] In addition, the residual alkali content and press density were measured in the same manner as for the LNMC sample. The results are shown in Table 2.

[0158] Furthermore, the obtained positive electrode active material sample was subjected to X-ray diffraction analysis using Cu-Kα radiation as a radiation source. No TiO 2 The diffraction peaks caused by LiTiO 2 and Li 2 TiO3 The X-ray diffraction pattern of the positive electrode active material sample is shown in Figure 2 .

[0159] In addition, using SEM-EDX (field emission scanning electron microscope SU-8220 manufactured by Hitachi High-Technologies Co., Ltd. and energy dispersive X-ray analyzer XFlash5060FlatQUAD manufactured by BRUKER), the particle surface of the positive electrode active material sample was subjected to element mapping analysis of Ti at a magnification of 20,000 times and confirmed. As with Co, Ni and Mn, Ti is evenly distributed.

[0160] According to X-ray diffraction analysis, Ti element mapping analysis ( Figure 6 ) and the results of X-ray photoelectron spectroscopy (XPS) analysis described later, it can be confirmed that Ti is present as a solid solution inside the particles of the positive electrode active material sample.

[0161] [Table 2]

[0162]

[0163] 1) The Ti feed amount of Example 1 and Example 2 is as follows: 2 The percentage of the atomically converted Ti amount obtained by the feed amount relative to the total atomically converted Ni, Mn, Co and M in the LNMC sample was calculated.

[0164] (Comparative Example 1)

[0165] Weigh lithium carbonate (average particle size 5.7 μm), nickel-manganese-cobalt composite hydroxide (Ni:Mn:Co=6:2:2 (molar ratio), average particle size 9.8 μm) and titanium oxide (TiO 2 ), and fully mixed with a household mixer to obtain a raw material mixture having a molar ratio of Li / (Ni+Mn+Co) of 1.01 and 0.25 mol % of Ti attached to the total amount of Ni, Mn and Co in the nickel-manganese-cobalt composite hydroxide. It should be noted that a commercially available nickel-manganese-cobalt composite hydroxide was used.

[0166] Next, the obtained raw material mixture was fired in an alumina crucible in an air atmosphere at 700°C for 2 hours and then at 850°C for 10 hours. After the firing, the fired product was crushed and classified. The average particle size of the obtained product was 10.4 μm and the BET specific surface area was 0.31 m 2 / g.

[0167] In addition, the residual alkali content and press density were measured in the same manner as for the LNMC sample. The results are shown in Table 3.

[0168] Furthermore, the obtained positive electrode active material sample was subjected to X-ray diffraction analysis using Cu-Kα radiation as a radiation source. No TiO 2 The diffraction peaks caused by LiTiO 2 and Li 2 TiO 3 Diffraction peaks of isotropic phases.

[0169] (Comparative Example 2)

[0170] Weigh lithium carbonate (average particle size 5.7 μm), nickel-manganese-cobalt composite hydroxide (Ni:Mn:Co=6:2:2 (molar ratio), average particle size 3.7 μm) and titanium oxide (TiO 2 ), and fully mixed with a household mixer to obtain a raw material mixture having a molar ratio of Li / (Ni+Mn+Co) of 1.01 and 0.58 mol % of Ti attached to the total amount of Ni, Mn and Co in the nickel-manganese-cobalt composite hydroxide. It should be noted that a commercially available nickel-manganese-cobalt composite hydroxide was used.

[0171] Next, the obtained raw material mixture was fired in an alumina crucible in an air atmosphere at 700°C for 2 hours and then at 850°C for 10 hours. After the firing, the fired product was crushed and classified. The average particle size of the obtained product was 4.0 μm and the BET specific surface area was 0.70 m 2 / g.

[0172] In addition, the residual alkali content and press density were measured in the same manner as for the LNMC sample. The results are shown in Table 3.

[0173] Furthermore, the obtained positive electrode active material sample was subjected to X-ray diffraction analysis using Cu-Kα radiation as a radiation source. No TiO 2 The diffraction peaks caused by LiTiO 2 and Li 2 TiO 3 Diffraction peaks of isotropic phases.

[0174] [Table 3]

[0175]

[0176] 1) The Ti feed amount of Comparative Examples 1 and 2 is as follows: 2 The percentage of the atomically converted Ti amount obtained by the feed amount relative to the total atomically converted Ni, Mn, Co and M in the LNMC sample was calculated.

[0177] <Distribution state of Ti>

[0178] The positive electrode active material sample obtained in the example was etched with argon in the depth direction by X-ray photoelectron spectroscopy (XPS) analysis (apparatus name: Quantera SXM manufactured by ULVAC-PHI, Inc.). The Ti peak, Ni peak, and Co peak were measured in the depth direction, and the atomic mole % ((Ti / (Ni + Co + Ti))×100) of Ti on the particle surface and inside the particles of the positive electrode active material sample with respect to the total amount of Ni, Co, and Ti was obtained. Also, the atomic mole % of Ti on the particle surface with respect to the total amount of Ni, Co, and Ti, the formation depth of the first region, and the ratio (A / B) of "the atomic mole % of Ti with respect to the total amount of Ni, Co, and Ti at 0 nm in the depth direction (A)" to "the atomic mole % of Ti with respect to the total amount of Ni, Co, and Ti at 330 nm in the depth direction (B)" were obtained. The results are shown in Table 4. In addition, Figure 4 and Figure 5 are graphs showing the change in "atomic mole % of Ti with respect to the total amount of Ni, Co, and Ti ((Ti / (Ni + Co + Ti))×100)" in the depth direction of the positive electrode active materials obtained in Example 1 and Comparative Example 1, respectively.

[0179] It should be noted that the etching conditions are as described below.

[0180] X-ray source: (monochromatic AlKα)

[0181] Ion species: Ar +

[0182] Output power: 25 W

[0183] Acceleration voltage: 15 kV

[0184] Etching rate: 2.2 - 2.4 nm / min (in terms of SiO 2 conversion)

[0185] Orbit of the element to be measured

[0186] Co: 2p 3 / 2

[0187] Ni: 2p 3 / 2

[0188] Ti: 2p

[0189] [Table 4]

[0190]

[0191] 1) The atomic mol % of Ti on the particle surface is a value of "(Ti / (Ni+Co+Ti))×100" calculated from the measured value at a depth of 0 nm in X-ray photoelectron spectroscopy (XPS) analysis.

[0192] 2) Regarding the "first region", the sample was subjected to X-ray photoelectron analysis (XPS), and when etching was performed in the depth direction from the surface using argon gas, the element peaks of Ni, Co and Ti in the depth direction were measured, and when the atomic mole % of Ti relative to the total amount of Ni, Co and Ti ((Ti / (Ni+Co+Ti))×100) was 4.0at% or more, it was determined to be the first region, and when the atomic mole % of Ti relative to the total amount of Ni, Co and Ti ((Ti / (Ni+Co+Ti))×100) was less than 4.0at%, it was determined to be the second region.

[0193] 3) “A / B” represents the ratio (A / B) of “the atomic mole % of Ti at a depth of 0 nm relative to the total amount of Ni, Co and Ti ((Ti / (Ni+Co+Ti))×100)(A)” and “the atomic mole % of Ti at a depth of 330 nm relative to the total amount of Ni, Co and Ti ((Ti / (Ni+Co+Ti))×100)(B)”.

[0194] (Comparative Example 3)

[0195] Instead of attaching the resulting TiO 2 The composite oxide particles were calcined at 800°C for 5 hours to obtain the attached TiO 2 The composite oxide particles were calcined at 600°C for 5 hours for heat treatment. The same method as in Example 2 was used to obtain a positive electrode active material sample in which 0.58 mol% of Ti was attached relative to the total amount of Ni, Mn and Co in LNMC sample 2. The average particle size (D50) of the obtained positive electrode active material was 3.9 μm, and the BET specific surface area was 0.88 m 2 / g.

[0196] In addition, the residual alkali content and press density were measured in the same manner as for the LNMC sample. The results are shown in Table 5.

[0197] In addition, using Cu-Kα radiation as a radiation source, X-ray diffraction analysis was performed on the obtained positive electrode active material sample. No diffraction peaks other than lithium nickel manganese cobalt composite oxide were confirmed. In addition, the X-ray diffraction pattern of the positive electrode active material sample is shown in Figure 3 It should be noted that the fact that no diffraction peaks other than those of the lithium nickel manganese cobalt composite oxide were confirmed is considered to be because the amount of Ti oxide added was small.

[0198] In addition, the element mapping analysis of Ti on the particle surface of the positive electrode active material sample was performed at a magnification of 20,000 times using SEM-EDX (field emission scanning electron microscope SU-8220 manufactured by Hitachi High-Technologies Corporation and energy dispersive X-ray analyzer XFlash5060FlatQUAD manufactured by BRUKER Corporation) and confirmed that Ti was unevenly distributed.

[0199] The elemental mapping analysis results of Ti confirmed that Ti was not dissolved in the particles of the positive electrode active material sample, but existed in the form of Ti oxide on the particle surface ( Figure 6 ).

[0200] (Comparative Example 4)

[0201] Collect 29.9 g of LiCoO 2 Sample (LCO sample), to which 0.0612 g of titanium oxide (TiO 2 ), and then fully mixed with a laboratory grinder to obtain the attached TiO 2 Next, the obtained attached TiO 2 The LCO particles were calcined at 900°C for 5 hours, and after heat treatment, they were crushed and classified to obtain a positive electrode active material sample in which 0.25 mol% of Ti was solid-dissolved relative to the amount of Co in the LCO sample. The average particle size (D50) of the obtained positive electrode active material was 8.3 μm, and the BET specific surface area was 0.37 m 2 / g.

[0202] In addition, the residual alkali content and press density were measured in the same manner as for the LNMC sample. The results are shown in Table 5.

[0203] Furthermore, the obtained positive electrode active material sample was subjected to X-ray diffraction analysis using Cu-Kα radiation as a radiation source. No TiO 2 The diffraction peaks caused by LiTiO 2 and Li 2 TiO 3 The diffraction peaks of the different phases confirmed that the sample was single-phase lithium-cobalt composite oxide particles.

[0204] [Table 5]

[0205]

[0206] 1) The Ti feed amount of Comparative Example 3 is as follows: 2 The percentage of the atomically converted Ti amount obtained by the feed amount relative to the total atomically converted Ni, Mn, Co and M in the LNMC sample was calculated.

[0207] In addition, the Ti feed amount of Comparative Example 4 is as follows: 2 The percentage of the atomic-equivalent amount of Ti obtained from the feed amount relative to the atomic-equivalent amount of Co in the LCO sample was calculated.

[0208] Note: “-” in the table means not determined.

[0209] The battery performance test was carried out in the following manner.

[0210] <Preparation of lithium secondary battery 1>

[0211] 95% by mass of the positive electrode active material sample obtained in Examples 1 to 2 and Comparative Examples 1 to 4, 2.5% by mass of graphite powder, and 2.5% by mass of polyvinylidene fluoride were mixed to form a positive electrode mixture, which was dispersed in N-methyl-2-pyrrolidone to form a kneaded paste. The kneaded paste was applied on an aluminum foil, dried, pressed, and punched into a disk with a diameter of 15 mm to obtain a positive electrode plate.

[0212] The positive electrode plate is used to make a button-type lithium secondary battery using a separator, a negative electrode, a positive electrode, a current collector, a mounting metal part, an external terminal, an electrolyte, and other components. The negative electrode uses a metal lithium foil, and the electrolyte uses 1 mol LiPF 6 The product is dissolved in 1 liter of a 1:1 mixture of ethylene carbonate and ethyl methyl carbonate.

[0213] Next, the performance of the obtained lithium secondary battery was evaluated. The results are shown in Tables 6 and 7. It should be noted that LNMC sample 1 (Comparative Example 5) and LNMC sample 2 (Comparative Example 6) were used as positive electrode active materials, and lithium secondary batteries were prepared by the same method and evaluated in the same manner. The results are shown in Tables 6 and 7.

[0214] <Battery Performance Evaluation 1>

[0215] The manufactured button-type lithium secondary battery was operated at room temperature under the following test conditions, and the following battery performance was evaluated.

[0216] (1) Test conditions for cycle characteristics evaluation

[0217] First, the battery was charged at 0.5C for 2 hours to 4.3V, and then the voltage was kept at 4.3V for 3 hours, and this constant current constant voltage charging (CCCV charging) was performed. Then, the battery was discharged at 0.2C or 1.0C constant current (CC discharge) to 2.7V. These operations were considered as one cycle, and a total of 30 cycles were performed, and the discharge capacity of each cycle was measured. Among them, the first cycle, the second cycle, the 10th cycle, the 20th cycle, and the 30th cycle were CC discharged at 0.2C, and the other cycles were CC discharged at 1.0C.

[0218] (2) Initial charge capacity, initial discharge capacity (per unit active material weight)

[0219] The charge capacity and discharge capacity of the first cycle in the cycle characteristics evaluation were defined as the initial charge capacity and the initial discharge capacity.

[0220] (3) Discharge capacity at the 30th cycle (per unit active material weight)

[0221] The discharge capacity at the 30th cycle in the cycle characteristics evaluation was defined as the 30th cycle discharge capacity.

[0222] (4) Capacity maintenance rate

[0223] The capacity retention rate was calculated by the following formula based on the discharge capacities (per active material weight) at the 1st cycle and the 30th cycle in the cycle characteristics evaluation.

[0224] Capacity retention rate (%) = (discharge capacity at the 30th cycle / discharge capacity at the 1st cycle) × 100

[0225] (5) Energy density maintenance rate

[0226] The energy density maintenance rate was calculated by the following formula based on the Wh capacity (per active material weight) at each discharge in the 1st cycle and the 30th cycle in the cycle characteristic evaluation.

[0227] Energy density retention rate (%) = (discharge Wh capacity at the 30th cycle / discharge Wh capacity at the 1st cycle) × 100

[0228] [Table 6]

[0229]

[0230] [Table 7]

[0231]

[0232] <Preparation of lithium secondary battery 2>

[0233] The positive electrode active material samples and LNMC samples obtained in Examples 1 to 2 and Comparative Examples 1 to 2 were fully mixed in a household mixer to prepare a mixture of the composition shown in Table 8 to prepare a positive electrode active material sample. In addition, the press density of the positive electrode active material sample was measured in the same manner as the above-mentioned LNMC sample, and the results are shown in Table 8.

[0234] [Table 8]

[0235]

[0236] A positive electrode mixture was prepared by mixing 95% by mass of a positive electrode active material sample, 2.5% by mass of graphite powder, and 2.5% by mass of polyvinylidene fluoride, and then dispersed in N-methyl-2-pyrrolidone to prepare a kneaded paste. The kneaded paste was applied to an aluminum foil, dried, pressed, and punched into a disk with a diameter of 15 mm to obtain a positive electrode plate.

[0237] The positive electrode plate is used to make a button-type lithium secondary battery using a separator, a negative electrode, a positive electrode, a current collector, a mounting metal part, an external terminal, an electrolyte, and other components. The negative electrode uses a metal lithium foil, and the electrolyte uses 1 mol LiPF 6 The product is dissolved in 1 liter of a 1:1 mixture of ethylene carbonate and ethyl methyl carbonate.

[0238] Next, the performance of the obtained lithium secondary battery was evaluated. The results are collectively shown in Table 9.

[0239] <Battery Performance Evaluation 2>

[0240] The button-type lithium secondary battery was operated at room temperature under the following test conditions, and the cycle characteristics, initial charge capacity, initial discharge capacity (unit active material weight), charge capacity of the 30th cycle, discharge capacity of the 30th cycle (unit active material weight), capacity retention rate, and energy density retention rate were evaluated in the same manner as the performance evaluation 1 of the above-mentioned battery. In addition, the discharge capacity per unit volume was evaluated, and the results are shown in Table 9. It should be noted that the positive electrode active material samples of Example 1 and Example 2 were also evaluated using the same method. The results are shown in Table 9.

[0241] (6) Discharge capacity per unit volume

[0242] The discharge capacity per unit volume was determined from the initial discharge capacity and the electrode density based on the following calculation formula.

[0243] Discharge capacity per unit volume (mAh / cm 3 ) = discharge capacity of the first cycle (mAh / g) × electrode density (g / cm 3)×0.95(ratio of the amount of active substance in the coating agent)

[0244] The electrode density is calculated as the density of the positive electrode material by measuring the mass and thickness of an electrode prepared from a sample to be measured and subtracting the thickness and mass of the current collector therefrom.

[0245] It should be noted that the positive electrode material is a mixture of 95 mass % of a positive electrode active material sample, 2.5 mass % of graphite powder, and 2.5 mass % of polyvinylidene fluoride, and the pressing pressure during electrode preparation is 0.38 ton / cm in linear pressure.

[0246] [Table 9]

[0247]

Claims

1. A positive electrode active material for a lithium secondary battery, characterized in that: The invention is composed of lithium nickel manganese cobalt composite oxide particles containing Ti by dissolving Ti in lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1), The lithium nickel manganese cobalt composite oxide particles have, in the depth direction from the surface, a first region in which the atomic mol % of Ti relative to the total amount of Ni, Co and Ti is 4.0 at % or more; and a second region in which the atomic mol % of Ti relative to the total amount of Ni, Co and Ti is less than 4.0 at %, The positive electrode active material for lithium secondary batteries is a single-phase lithium nickel manganese cobalt composite oxide represented by the general formula (1) in X-ray diffraction analysis. LixNiMnzCoMpO01+×(1) In the formula, M represents one or more metal elements selected from Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, Ga, Ge, Sn, Ba, W, Na and K, x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, and y+z+t+p=1.

2. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The content of Ti is 0.01 to 5.00 mol % based on the total amount of Ni, Mn, Co and M in the lithium nickel manganese cobalt composite oxide particles in terms of atom.

3. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The content of residual alkali is 1.20 mass % or less.

4. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The atomic mol % of Ti in the particle surface relative to the total amount of Ni, Co and Ti is 6.0 at % or more.

5. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The ratio A / B of the atomic mol % A of Ti relative to the total amount of Ni, Co and Ti at a depth of 0 nm to the atomic mol % B of Ti relative to the total amount of Ni, Co and Ti at a depth of 330 nm is 10.0 or more.

6. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The positive electrode active material for lithium secondary battery is obtained by the following method: The method comprises dry-mixing lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1) with a Ti-containing oxide, so that the Ti-containing oxide is attached to the particle surface of the lithium nickel manganese cobalt composite oxide particles to obtain composite oxide particles with the Ti-containing oxide attached, and then heating the composite oxide particles with the Ti-containing oxide attached at a temperature of 750° C. to 1000° C. to obtain the positive electrode active material for the lithium secondary battery. LiNi,MnCotM,O1+×(1) In the formula, M represents one or more metal elements selected from Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, Ga, Ge, Sn, Ba, W, Na and K, x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, and y+z+t+p=1.

7. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The positive electrode active material for lithium secondary batteries is a mixture of large particles with an average particle size of 7.5 to 30.0 μm and small particles with an average particle size of 0.50 to 7.5 μm.

8. The positive electrode active material for lithium secondary battery according to claim 7, characterized in that: The mixing ratio of the large particles to the small particles is 7:13 to 19:1 in terms of mass ratio.

9. The positive electrode active material for lithium secondary battery according to claim 7, characterized in that: The mixture is at 0.65 tonf / cm 2 The compressed density after compression treatment under the conditions of 2.7g / cm 3 above.

10. A method for producing a positive electrode active material for a lithium secondary battery, characterized in that: The lithium nickel manganese cobalt composite oxide particles represented by the following general formula (1) are dry mixed with a Ti-containing oxide to make the Ti-containing oxide adhere to the particle surface of the lithium nickel manganese cobalt composite oxide particles to obtain composite oxide particles with the Ti-containing oxide adhered thereto, and then the composite oxide particles with the Ti-containing oxide adhered thereto are heat treated at a temperature of 750° C. to 1000° C., Li,Ni,MnCoMpO1+×(1) In the formula, M represents one or more metal elements selected from Al, Zr, Cu, Fe, Sr, Ca, V, Mo, Bi, Nb, Si, Zn, Ga, Ge, Sn, Ba, W, Na and K, x is 0.98≤x≤1.20, y is 0.30≤y<1.00, z is 0<z≤0.50, t is 0<t≤0.50, p is 0≤p≤0.05, and y+z+t+p=1.

11. The method for producing a positive electrode active material for a lithium secondary battery according to claim 10, wherein: The Ti-containing oxide is TiO2.

12. A lithium secondary battery, characterized in that: The positive electrode active material for a lithium secondary battery according to claim 1 is used.