AI Technical Summary

Technical Problem

Existing graphitization equipment cannot achieve continuous production, resulting in a long production cycle, and it is difficult to control the pore structure of the material to meet the market demand for low-cost, high-performance graphite materials.

Method used

The continuous graphitization process is used to accurately control the pore volume, specific surface area and true density of the negative electrode material by controlling the temperature rise and fall rate and introducing additives, forming a reasonable range to increase the lithium ion diffusion channel and electrochemical reaction area.

Benefits of technology

It improves the capacity and rate performance of the anode material, reduces production costs and energy consumption, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096378A_ABST
    Figure CN119096378A_ABST
Patent Text Reader

Abstract

The invention provides a negative electrode material and a battery, the negative electrode material comprises artificial graphite particles, the interiors and / or surfaces of the artificial graphite particles are provided with pores, the pore volume of the negative electrode material is V cm < 3 > / kg, the true density is D g / cm < 3 >, the specific surface area is S m < 2 > / g, and V * S / D is greater than or equal to 4.0 and less than or equal to 10. According to the negative electrode material and the battery provided by the invention, active sites on the surface of the negative electrode material can be effectively improved, and the rate capability of the negative electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Anode materials and batteries Technical Field

[0001] The present application relates to the technical field of negative electrode materials, and in particular, to negative electrode materials and batteries. Background Art

[0002] Graphite has become the mainstream negative electrode material for commercial lithium-ion batteries due to its advantages such as high electronic conductivity, large lithium ion diffusion coefficient, small volume change before and after lithium insertion in its layered structure, high lithium insertion capacity and low lithium insertion potential.

[0003] The graphitization equipment for traditional graphite negative electrodes mainly includes two categories: crucible furnaces and box furnaces. Both are intermittent operations. Since the graphitization process requires power outages, continuous production cannot be achieved. Moreover, due to the limited characteristics of the equipment's heating and cooling processes, the heating and cooling rates are slow, resulting in a long production cycle. Generally speaking, the graphitization cycle ranges from 15 to 50 days. During the graphitization production process, volatile matter and impurity elements in the raw materials escape under high temperature conditions, thereby forming pores inside and / or on the surface of the graphite. Generally speaking, artificial graphite has a certain number of pore structures. On the one hand, the presence of pores can increase the diffusion channels of Li+ in the graphite material and reduce the diffusion resistance of Li+, thereby effectively improving the rate performance of the material. On the other hand, excessive pore structures will lead to an increase in the specific surface area of ​​the material, which in turn leads to a deterioration in the first effect and cycle performance of the product. In fact, simply improving the pore structure does not achieve optimal rate performance, and there is still a lot of room for improvement. Most researchers only focus on exploring the impact of a single factor on the performance of graphite materials, and have not conducted in-depth research from the perspective of the synergy between multiple factors to maximize the improvement of graphite's rate performance.

[0004] Therefore, at the current stage when graphite materials have developed to a very mature stage, simply improving one parameter can no longer meet the market demand for low-cost, high-performance graphite materials. It is necessary to explore the mechanism of the coordinated action of multiple factors and develop graphite negative electrode materials that meet market demand.

[0005] Application Contents

[0006] In view of this, the present application addresses the deficiencies of the prior art and provides a new negative electrode material and battery, which achieves precise control of the internal and / or surface pore volume, specific surface area, and true density, so that they are combined and maintained within a reasonable range, thereby achieving improvements in the capacity and rate performance of the negative electrode material.

[0007] In a first aspect, the present application provides a negative electrode material, wherein the negative electrode material comprises artificial graphite, wherein the artificial graphite has pores, and the pore volume of the negative electrode material is V cm 3 / kg, true density is D g / cm 3, the specific surface area is S m 2 / g, where 4.0≤V*S / D≤10,

[0008] The pore volume was measured using ASAP2460 equipment from American company Micromeritics and the BJH Desorption cumulative volume of pores model. Calculated within the pore size range.

[0009] In some embodiments, the particle size D of the negative electrode material is 50 10μm~30μm.

[0010] In some embodiments, the particle size D of the negative electrode material is 10 ≥5μm.

[0011] In some embodiments, the particle size D of the negative electrode material is 90 ≤50μm.

[0012] In some embodiments, the pore volume of the negative electrode material is V cm 3 / kg, 5≤V≤8.

[0013] In some embodiments, the specific surface area of ​​the negative electrode material is S m 2 / g, 1.78≤S≤3.0.

[0014] In some embodiments, the true density of the negative electrode material is D g / cm 3 , 2.210≤D≤2.265.

[0015] In some embodiments, the pores include at least one of micropores and mesopores.

[0016] In some embodiments, the average pore size of the pores is

[0017] In some embodiments, the negative electrode material is measured by X-ray diffraction, and the interlayer spacing of the (002) plane is d 002 ,

[0018] In some embodiments, the peak intensity ratio of the (002) plane to the (110) plane of the artificial graphite particles is measured by X-ray diffraction. 002 / I 110 is 65.0~120.0, and the peak intensity ratio of (004) plane to (110) plane is I 004 / I 110 It is 3.0 to 6.0.

[0019] In some embodiments, the artificial graphite includes artificial graphite primary particles and / or artificial graphite secondary particles.

[0020] In some embodiments, the negative electrode material further includes amorphous carbon.

[0021] In some embodiments, the negative electrode material further includes amorphous carbon, and the mass proportion of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.

[0022] In a second aspect, the present application provides a battery, comprising the negative electrode material described in the first aspect.

[0023] The technical solution of this application has at least the following beneficial effects:

[0024] The negative electrode material provided in the application includes artificial graphite, the artificial graphite has pores inside and / or on the surface, and the pore volume of the negative electrode material is V cm 3 / kg, true density is D g / cm 3 , the specific surface area is S m 2 / g, where 4.0≤V*S / D≤10. Generally speaking, the pore volume within a certain range in artificial graphite can increase the diffusion channel of Li ions, and the specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and help improve the capacity and rate performance of the negative electrode material. On this basis, the applicant found through in-depth research that there is only enough lithium ion diffusion channel and electrochemical reaction area, and the rate performance still has a lot of room for improvement. The reason is that after lithium ions diffuse to the surface of artificial graphite, if the arrangement of carbon atoms in artificial graphite is relatively chaotic and the order is not enough, the lithium ions will enter the interior of the artificial graphite material and combine with carbon atoms to produce electrochemical reactions. The diffusion channel and electrochemical reaction area cannot be fully utilized, and the order of artificial graphite is directly related to the true density. The present application controls the V*S / D of the negative electrode material within the above range, which is conducive to the combination of lithium ions and sufficient carbon atoms under low resistance, and obtains a negative electrode material with better rate performance and capacity.

[0025] The negative electrode material provided by the present application is produced and processed by a continuous graphitization process, so that all materials are continuously fed and discharged, and the time and temperature of the high temperature zone are kept consistent, and the graphitization process controls the heating and cooling rates, so that volatiles, impurity elements and other substances in the material can escape evenly and quickly. At the same time, the pressing size is controlled and a certain amount of additives are introduced to achieve precise control of the pore volume inside and / or on the surface of the graphite. The coordinated use of the above-mentioned process methods overcomes the problems that the temperature gradient at different positions in the traditional graphitization furnace causes uneven heating of the material, and the specific surface area, pore volume, true density and other indicators of the produced products fluctuate greatly and are uncontrolled, thereby making the pore volume, specific surface area and true density of the processed materials meet the ideal control design requirements.

[0026] The negative electrode material provided in this application uses a continuous graphitization process, has low energy consumption per unit mass, has obvious advantages in cost and production cycle, and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 is a scanning electron microscope image of the negative electrode material prepared in Example 12 of the present application;

[0028] FIG2 is a pore size distribution curve of the negative electrode material prepared in Example 12 of the present application. DETAILED DESCRIPTION

[0029] To better illustrate the present application and facilitate understanding of the technical solution of the present application, the present application is further described below. However, the following embodiments are merely simplified examples of the present application and do not represent or limit the scope of protection of the present application. The scope of protection of the present application shall be subject to the claims.

[0030] In the field of negative electrode materials, the development of continuous graphitization equipment has continued for decades. As early as 1987, a patent (US06619591) disclosed equipment that can continuously graphitize carbon-containing materials. In recent years, applicants have also been continuously developing continuous graphitization equipment. For example, the patent with authorization announcement number CN211425033U applied for in 2019 discloses a vertical continuous furnace for the production of negative electrode materials for lithium batteries, which can realize continuous discharge from the discharge port and continuous feeding from the material pipeline. Compared with the traditional process, the continuous graphitization process shortens the graphitization time from several days to several hours, and the energy consumption is reduced significantly. However, the greatly shortened graphitization time leads to changes in the microstructure of artificial graphite obtained by the continuous graphitization process compared with conventional artificial graphite, especially changes in the internal pore structure of artificial graphite and changes in the crystal form. For a long time, the industry has proven that this change is difficult to meet the performance requirements of artificial graphite and is difficult to improve. Therefore, even though continuous graphitization equipment has existed for three or four decades, there has never been a precedent for the successful mass production of continuous graphitized artificial graphite negative electrode products.

[0031] In recent years, as energy has become increasingly scarce, in order to further reduce the cost of artificial graphite, the applicant has continued to develop the application of continuous graphitization equipment, with the aim of developing artificial graphite anode materials that are comparable to or even better than current conventional graphitized anode materials in terms of performance, so as to reduce the energy consumption of artificial graphite anode materials and thus reduce costs. After extensive development of preparation processes, the applicant has developed a variety of methods that can improve the adverse changes caused by rapid temperature rise and fall on artificial graphite products. After screening the products, a series of different types of artificial graphite anode materials have been obtained. Although the microstructure of these artificial graphite anode materials is different from that of conventional artificial graphite products, their electrical properties are basically comparable to those of conventional artificial graphite products, and even in some aspects, their electrical properties and processing performance are superior or stable, and they have the conditions to replace conventional artificial graphite products.

[0032] The following is a detailed description of one of the preparation processes developed by the applicant and its related products.

[0033] A method for preparing a negative electrode material comprises the following steps:

[0034] S10, pressing a mixture comprising coke powder, a binder, an additive and a solvent to obtain a first precursor, wherein the additive comprises an inorganic compound, the mass ratio of the coke powder to the additive is 100:(1-5), and the pressing size is φ(10mm-100mm)×(20mm-100mm).

[0035] S20, pre-carbonizing the first precursor to obtain a second precursor.

[0036] S30, placing the second precursor in a continuous graphitization furnace and heating it to 2800°C~3200°C at a heating rate of 13°C / min~20°C / min for graphitization treatment for 1~4 hours, and then cooling it at a cooling rate of 20°C / min~25°C / min to obtain a negative electrode material, wherein the ratio of the heating rate to the cooling rate is controlled at 0.5~1.

[0037] The method for preparing the negative electrode material provided in this application involves pressing a mixture of coke powder, a binder, an additive, and a solvent into a mold. After pre-carbonizing the first precursor, the mixture is placed in a continuous graphitization furnace. The temperature rises extremely quickly, allowing the second precursor to reach the graphitization temperature in a relatively short period of time. The additive evaporates and escapes, forming pores within and / or on the surface of the graphite particles. The pores can serve as additional lithium storage space, thereby increasing the lithium storage capacity of the graphite material. In addition, the process from entering the continuous graphitization furnace to exiting the furnace is completed in just a few hours, resulting in high thermal energy utilization and reduced production costs.

[0038] Coke powder is obtained by crushing and shaping coke raw materials, and the coke raw materials include at least one of petroleum coke, needle coke, pitch coke and isotropic coke.

[0039] In some embodiments, shaping includes at least one of pulverization, spheroidization, or classification. The median particle size of the shaped coke powder is between 15 μm and 20 μm. More specifically, it can be 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm, 18.5 μm, 19 μm, or 20 μm, etc., but these values ​​are not limited to the listed values. Other values ​​not listed within this range are also applicable. Numerous experiments have shown that controlling the median particle size of the coke powder within the above range is beneficial for achieving a balanced balance between processability, capacity, and rate capability.

[0040] In some embodiments, the mass content of carbon in the coke powder is ≥80%, specifically 80%, 81%, 82%, 85%, 90%, 95% or 96%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] In some embodiments, the solvent includes at least one of water, ethanol, acetone, benzene, toluene, quinoline, tetrahydrofuran, and carbon tetrachloride.

[0042] In some embodiments, the binder includes at least one of petroleum resin, phenolic resin, epoxy resin, coumarone resin, potato starch, wheat starch, corn starch, sweet potato starch, arrowroot starch, and tapioca starch.

[0043] In some embodiments, the additive includes one of boron oxide, boron carbide, boron nitride, silicon carbide, boron nitride, boric acid, boron chloride and sodium borate. On the one hand, the additive acts as a graphitization catalyst. On the other hand, it volatilizes and escapes through rapid temperature increase and decrease during the graphitization process, which is conducive to the formation of stable pores inside and / or on the surface of the artificial graphite.

[0044] In some embodiments, the mass ratio of coke powder, binder, solvent, and additive is 100:(3-20):(5-50):(1-5), specifically 100:3:5:1, 100:10:15:1, 100:15:20:5, 100:20:20:1, 100:20:15:3, 100:10:10:5, or 100:15:25:2, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable. Controlling the additive content within the above range is beneficial to the occurrence of the catalytic graphitization process on the one hand; on the other hand, the volatilization of the additive at high temperature can form a certain number of pores inside and / or on the surface of the graphite.

[0045] It can be understood that when the proportion of the binder in the embodiment is low (the mass ratio of the binder to the coke powder is 3-10:100), the obtained artificial graphite is mainly primary particles. When the proportion of the binder in the embodiment is high (the mass ratio of the binder to the coke powder is 10-20:100), the obtained artificial graphite is mainly secondary particles.

[0046] In some embodiments, the mixture is mixed by at least one of mechanical stirring and ultrasonic dispersion. When mechanical stirring is used, a propeller stirrer, a turbine stirrer, a flat-blade stirrer, etc. can be used, as long as the components in the mixture are fully mixed.

[0047] In some embodiments, the stirring rate is 10 r / min to 1000 r / min, and specifically can be 10 r / min, 50 r / min, 70 r / min, 100 r / min, 120 r / min, 150 r / min, 200 r / min, 300 r / min, 350 r / min, 400 r / min, 500 r / min, or 1000 r / min, etc., without limitation herein. Controlling the stirring rate within the above range is conducive to mixing the components to form a uniform mixture.

[0048] The stirring can be carried out at room temperature or in a preheated state. Preferably, the stirring temperature can be controlled at 25°C to 200°C. It can be understood that appropriate preheating is conducive to mixing the components to form a uniform mixture.

[0049] In some embodiments, the profiling method includes at least one of extrusion, molding, roller pressing, and isostatic pressing.

[0050] In some embodiments, the pressing pressure is 5 MPa to 100 MPa, specifically 5 MPa, 15 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa or 100 MPa, etc. The pressing treatment can improve the fluidity of the material during the graphitization process on the one hand, and increase the material loading and production capacity on the other hand.

[0051] During the pressing process, the pressing size is controlled to be φ(10mm~100mm)×(20mm~100mm). Controlling the pressing size within the above range is beneficial to the control of the specific surface area, and is also beneficial to the feeding and discharging of the graphitization process.

[0052] In some embodiments, the reaction temperature of the pre-carbonization treatment is 500°C to 1000°C, specifically 500°C, 550°C, 600°C, 700°C, 750°C, 800°C, 850°C, 900°C, or 1000°C, etc., but is not limited to the listed values, and other values ​​not listed within this numerical range are also applicable. It can be understood that the pre-carbonization treatment temperature within the above range is conducive to the discharge of volatile substances and other substances in the coke raw material.

[0053] In some embodiments, the holding time of the pre-carbonization treatment is 1 hour to 10 hours, specifically, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours or 10 hours, etc., but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. Preferably, the holding time of the pre-carbonization treatment is 1 hour to 4 hours,

[0054] In some embodiments, the heating rate of the pre-carbonization treatment is 5°C / min to 20°C / min, specifically 5°C / min, 6°C / min, 8°C / min, 10°C / min, 15°C / min, 15.5°C / min or 20°C / min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] In some embodiments, the cooling rate after pre-carbonization treatment is 10°C / min to 30°C / min, specifically 10°C / min, 15°C / min, 20°C / min, 25°C / min, 25.5°C / min or 30°C / min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] In some embodiments, the pre-carbonization treatment is performed under a protective atmosphere comprising at least one of nitrogen, helium, neon, argon, krypton, and xenon.

[0057] In some embodiments, the heating rate of the graphitization treatment can be 13°C / min, 15°C / min, 17°C / min, 18°C / min or 20°C / min, and the cooling rate after the graphitization treatment can be 20°C / min, 21°C / min, 22°C / min, 23°C / min, 24°C / min or 25°C / min, etc.

[0058] In some embodiments, the structure of the continuous graphitization furnace is as shown in patent CN211425033U.

[0059] In some embodiments, the graphitization process includes heating the temperature to 2800° C. to 3200° C. at a heating rate of 13° C. / min to 20° C. / min, and maintaining the temperature at 2800° C. to 3200° C. for 2 to 4 hours. It is understood that the rapid heating during the graphitization process facilitates the rapid escape of volatile matter within the coke raw material and facilitates the formation of pores in the product.

[0060] In some embodiments, the graphitization treatment temperature can be specifically 2800°C, 2850°C, 2900°C, 3000°C, 3100°C, 3150°C, 3180°C or 3200°C, etc., but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable.

[0061] In some embodiments, the holding time for the graphitization treatment is 1 hour to 4 hours, specifically, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 3.8 hours, or 4 hours, but is not limited to the listed values. Other values ​​not listed within this range are also applicable. Preferably, the holding time for the graphitization treatment is 2 hours to 3 hours.

[0062] In some embodiments, the cooling rate after graphitization is 20°C / min to 25°C / min, specifically 20°C / min, 21°C / min, 22°C / min, 23°C / min, 24°C / min, or 25°C / min, but is not limited to the listed values. Other values ​​not listed within this range are also applicable. Rapid cooling can reduce the occurrence of material oxidation reactions during the cooling process, which is beneficial for controlling the specific surface area of ​​the material. It can also greatly shorten the graphitization process cycle and reduce production costs.

[0063] In some embodiments, the ratio of the heating rate to the cooling rate during the graphitization process can be 0.5, 0.6, 0.7, 0.8, 0.9 or 1.0. Controlling the ratio of the heating rate to the cooling rate is conducive to the escape of volatile substances inside the material, thereby maintaining the product of the pore volume and specific surface area of ​​the material at a relatively constant value.

[0064] It is understandable that after the graphitization treatment, a portion of the adhesive may be difficult to convert into graphitized carbon, and the portion that cannot be converted into graphitized carbon exists on the surface of the artificial graphite particles in the form of amorphous carbon.

[0065] In some embodiments, after the graphitization treatment, at least one of pulverization, screening, and demagnetization is further performed. Preferably, after the carbonization treatment, pulverization, demagnetization, and screening are further performed in sequence.

[0066] In some embodiments, the pulverization method is any one of a mechanical pulverizer, a jet mill, and a low-temperature pulverizer.

[0067] In some embodiments, the screening method is any one of a fixed screen, a drum screen, a resonance screen, a roller screen, a vibrating screen and a chain screen, and the screening mesh number is 100 to 500 meshes. Specifically, the screening mesh number can be 100 mesh, 200 mesh, 250 mesh, 325 mesh, 400 mesh, 500 mesh, etc. The particle size of the negative electrode material is controlled within the above range, which is beneficial to improving the processing performance of the negative electrode material.

[0068] In some embodiments, the demagnetization equipment is any one of a permanent magnetic drum magnetic separator, an electromagnetic iron remover, and a pulsating high gradient magnetic separator. The purpose of demagnetization is to ultimately control the magnetic material content of the negative electrode material, avoid the discharge effect of the magnetic material on the battery, and the safety of the battery during use.

[0069] A negative electrode material comprising artificial graphite, wherein the artificial graphite has pores inside and / or on the surface, and the pore volume of the negative electrode material is V cm 3 / kg, true density is D g / cm 3 , the specific surface area is S m 2 / g, where 4.0≤V*S / D≤10, the pore volume was measured using ASAP2460 equipment from Micromeritics, USA, and the BJH Desorption cumulative volume of pores model was used. Calculated within the pore size range.

[0070] The negative electrode material provided in the present application is produced and processed by a continuous graphitization process. The time and temperature of all materials passing through the high temperature zone are kept consistent, and the heating and cooling rates are controlled so that volatiles, impurity elements and other substances in the material can escape evenly and quickly. At the same time, the introduction of a certain amount of additives can achieve precise control of the pores inside and / or on the surface of the graphite, so that the pore volume, specific surface area and true density of the material meet the ideal control design requirements. Pores are formed inside and / or on the surface of the graphite, and the pores can be used as additional lithium storage space, thereby increasing the lithium storage capacity of the negative electrode material and causing an increase in the specific surface area. When the negative electrode material is made into an electrode and applied to a battery, after the electrolyte is injected, the pores inside the artificial graphite particles are filled with the electrolyte. During charging and discharging, an electrochemical reaction occurs inside the electrode. The pores create more lithium ion diffusion channels and electrochemical reaction interfaces for the negative electrode material, which can promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and help improve the capacity and rate performance of the negative electrode material.

[0071] Generally speaking, the pore volume within a certain range in artificial graphite can increase the diffusion channel of Li ions, and the specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and help improve the capacity and rate performance of the negative electrode material. On this basis, the applicant found through in-depth research that there is only enough lithium ion diffusion channel and electrochemical reaction area, and the rate performance still has a lot of room for improvement. The reason is that after lithium ions diffuse to the surface of artificial graphite, if the carbon atoms in artificial graphite are arranged in a relatively chaotic manner and the degree of order is not enough, the lithium ions enter the interior of the artificial graphite material and combine with the carbon atoms to produce an electrochemical reaction. The hindrance is relatively large, and the diffusion channel and electrochemical reaction area cannot be fully utilized, and the degree of order of artificial graphite is directly related to the true density. The present application controls the V*S / D of the negative electrode material within the above range, which is conducive to the combination of lithium ions and sufficient carbon atoms under low resistance, and obtains a negative electrode material with better rate performance and capacity.

[0072] In some embodiments, the particle size D of the negative electrode material is 50 The median particle size of the negative electrode material is 10 μm to 30 μm. Specifically, it can be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 20 μm, 25 μm, or 30 μm, etc., without limitation. Controlling the median particle size of the negative electrode material within the above range is beneficial to improving the cycle performance of the negative electrode material.

[0073] It should be noted that D 10 Indicates the particle size corresponding to the cumulative particle size distribution percentage of the powder reaching 10%, D 50 Indicates the particle size corresponding to when the cumulative particle size distribution percentage reaches 50%, D 90 It indicates the particle size corresponding to when the cumulative particle size distribution percentage reaches 90%.

[0074] In some embodiments, the particle size D of the negative electrode material is 10 ≥5μm, specifically 5μm, 5.5μm, 6μm, 7μm, 8μm or 10μm, etc., which is not limited here.

[0075] In some embodiments, the particle size D of the negative electrode material is 90 ≤50μm, specifically 50μm, 49μm, 48μm, 47μm, 46μm, 45μm, 42μm or 40μm, etc., which is not limited here.

[0076] In some embodiments, the pore volume of the negative electrode material is V cm 3 / kg, 5≤V≤8, specifically it can be 5, 5.2, 5.5, 5.8, 6.0, 6.2, 6.5, 6.8, 7.0, 7.5 or 8.0, etc., which is not limited here.

[0077] In some embodiments, the specific surface area of ​​the negative electrode material is S m 2 / g, 1.78≤S≤3.0; specifically, it can be 1.78, 1.85, 1.95, 2.00, 2.25, 2.43, 2.57, 2.61, 2.72, 2.85, or 3.0, etc., without limitation herein. It is understandable that an excessively large specific surface area can easily lead to the formation of a solid electrolyte membrane, consuming excessive amounts of irreversible lithium salt and reducing the initial efficiency of the battery.

[0078] In some embodiments, the true density of the negative electrode material is D g / cm 3 , 2.210≤D≤2.265; specifically it can be 2.210, 2.215, 2.218, 2.220, 2.252, 2.263, 2.260 or 2.265, etc., which is not limited here.

[0079] In some embodiments, the pores include at least one of micropores and mesopores.

[0080] In some embodiments, the average pore size is Specifically, the average pore size of the pores can be or wait.

[0081] In some embodiments, the negative electrode material is measured by X-ray diffraction, and the interlayer spacing of the (002) plane is d 002 , Crystal plane interlayer spacing d 002 Within the above range, it can be seen that the graphite crystallinity of the artificial graphite particles is high, that is, the degree of graphitization is high, and the capacity of the product is high.

[0082] In some embodiments, the peak intensity ratio of the (002) plane to the (110) plane of the artificial graphite particles is measured by X-ray diffraction. 002 / I 110 is 65.0~120.0, and the peak intensity ratio of (004) plane to (110) plane is I 004 / I 110 3.0~6.0. 002 / I 110 and I 004 / I 110 In this range, the material has a high degree of orientation and low cyclic expansion. 002 / I 110 The specific ratio can be 65.0, 70.0, 75.0, 80.0, 85.3, 89.2, 90.5, 95.1, 100.0, 111.0 or 120.0, etc., which is not limited here. 004 / I 110The ratio can specifically be 3.0, 3.2, 3.5, 3.8, 4.1, 4.2, 4.5, 5.2, 5.8, 5.9 or 6.0, etc., and is not limited here.

[0083] In some embodiments, the artificial graphite includes artificial graphite primary particles and / or artificial graphite secondary particles.

[0084] In some embodiments, the negative electrode material further includes amorphous carbon, with the amorphous carbon comprising 0.1 wt% to 5 wt% of the negative electrode material. The presence of amorphous carbon provides more irregular and open diffusion pathways for lithium ions, which is beneficial for improving the material's rate performance.

[0085] In some embodiments, the specific capacity of the negative electrode material is 320 mAh / g to 370 mAh / g, and can specifically be 320 mAh / g, 340 mAh / g, 342 mAh / g, 345 mAh / g, 353 mAh / g, 355 mAh / g, 357 mAh / g, 360 mAh / g, 365 mAh / g, or 370 mAh / g, etc., without limitation herein. Preferably, the specific capacity of the negative electrode material is 340 mAh / g to 370 mAh / g.

[0086] A battery comprises the above-mentioned negative electrode material.

[0087] Those skilled in the art will appreciate that the battery preparation method described above is merely an example. Without departing from the disclosure of this application, other methods commonly used in the art may be employed, and other types of batteries may be prepared for testing, such as sodium-ion batteries, potassium-ion batteries, and the like.

[0088] The following further illustrates the embodiments of the present invention in multiple embodiments. The embodiments of the present invention are not limited to the following specific embodiments. Within the scope of protection, appropriate changes can be made to the implementation.

[0089] Example 1

[0090] The method for preparing the negative electrode material of this embodiment includes the following steps:

[0091] (1) crushing the Daqing petroleum coke raw material and shaping it with a shaping device to obtain crushed and shaped coke powder, with a median particle size controlled to be 15 μm;

[0092] (2) mixing the char powder with a phenolic resin binder, water, and boron oxide in a mass ratio of 100:6:15:2 to obtain a mixture;

[0093] (3) pressing the mixture under a pressure of 10 MPa to obtain a first precursor, wherein the size of the first precursor after pressing is φ30 mm×50 mm;

[0094] (4) pre-carbonizing the first precursor at 800° C. for 4 h, and then cooling to obtain a modified second precursor;

[0095] (5) The second precursor was graphitized at 2900°C in a continuous graphitization furnace to obtain a graphitized product. The heating curve was as follows: the temperature was increased to 2900°C at a heating rate of 15.5°C / min, kept at 2900°C for 2.5 hours, and then cooled to 30°C at a cooling rate of 22.5°C / min. The heating and cooling rate ratio during the graphitization process was controlled at 0.68;

[0096] (6) The graphitized product is processed by breaking up, demagnetizing, and 325 mesh screening to obtain the negative electrode material.

[0097] The negative electrode material comprises primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0098] Example 2

[0099] The method for preparing the negative electrode material of this embodiment includes the following steps:

[0100] (1) The raw material of Baosteel pitch coke was crushed and shaped by a shaping device to obtain crushed and shaped coke powder, with a median particle size controlled to be 16 μm;

[0101] (2) uniformly mixing coke powder with petroleum resin, benzene, and boron carbide in a mass ratio of 100:5:20:2 to obtain a mixture;

[0102] (3) pressing the mixture under a pressure of 10 MPa to obtain a first precursor, wherein the size of the first precursor after pressing is φ30 mm×50 mm;

[0103] (4) pre-carbonizing the first precursor at 800° C. for 4 h, and then cooling to obtain a modified second precursor;

[0104] (5) The second precursor was graphitized at 2900°C in a continuous graphitization furnace to obtain a graphitized product. The heating curve was as follows: the temperature was increased to 2900°C at a heating rate of 14°C / min, kept at 2900°C for 2.5 hours, and then cooled to 30°C at a cooling rate of 22.5°C / min. The heating and cooling rate ratio during the graphitization process was controlled at 0.62;

[0105] (6) The graphitized product is processed by breaking up, demagnetizing, and 250 mesh screening to obtain the negative electrode material.

[0106] The negative electrode material comprises primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0107] Example 3

[0108] The method for preparing the negative electrode material of this embodiment includes the following steps:

[0109] (1) Crushing Jinzhou needle coke raw material and shaping it through shaping equipment to obtain crushed and shaped coke powder, with a median particle size controlled to be 15 μm;

[0110] (2) mixing the char powder with a phenolic resin binder, water, and boron oxide in a mass ratio of 100:6:15:2 to obtain a mixture;

[0111] (3) Pressing the mixture under a pressure of 10 MPa to obtain a first precursor, wherein the size of the first precursor after pressing is φ30 mm×50 mm;

[0112] (4) pre-carbonizing the first precursor at 800° C. for 4 h, and then cooling to obtain a modified second precursor;

[0113] (5) The second precursor was graphitized in a continuous graphitization furnace at 2850°C to obtain a graphitized product. The heating curve was as follows: the temperature was increased to 2850°C at a heating rate of 16°C / min, kept at 2850°C for 2.5 hours, and then cooled to 30°C at a cooling rate of 22°C / min. The heating and cooling rate ratio during the graphitization process was controlled at 0.73;

[0114] (6) The graphitized product is subjected to the steps of breaking up, demagnetizing, and 250-mesh screening to obtain the negative electrode material.

[0115] The negative electrode material comprises primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0116] Example 4

[0117] The method for preparing the negative electrode material of this embodiment includes the following steps:

[0118] (1) The Jingyang needle coke raw material is crushed and shaped by a shaping device to obtain crushed and shaped coke powder, with a median particle size controlled to be 18 μm;

[0119] (2) mixing the coke powder with petroleum resin, benzene, and sodium borate in a mass ratio of 100:6:15:2 to obtain a mixture;

[0120] (3) pressing the mixture under a pressure of 10 MPa to obtain a first precursor, wherein the size of the first precursor after pressing is φ30 mm×50 mm;

[0121] (4) pre-carbonizing the precursor at 800°C for 4 hours and cooling it to obtain a modified second precursor;

[0122] (5) The second precursor was graphitized in a continuous graphitization furnace at 2850°C to obtain a graphitized product. The heating curve was as follows: the temperature was increased to 2850°C at a heating rate of 16.5°C / min, kept at 2850°C for 3 h, and then cooled to 30°C at a cooling rate of 22°C / min. The heating and cooling rate ratio during the graphitization process was controlled at 0.75;

[0123] (6) The graphitized product is subjected to the steps of breaking up, demagnetizing, and 250-mesh screening to obtain the negative electrode material.

[0124] The negative electrode material comprises primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0125] Example 5

[0126] The only difference from Example 1 is that in step (2), the coke powder is evenly mixed with the epoxy resin, water, and boron oxide in a mass ratio of 100:6:15:2 to obtain a mixture.

[0127] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0128] Example 6

[0129] The only difference from Example 1 is that in step (2), the coke powder is evenly mixed with coumarone resin, water and boron oxide in a mass ratio of 100:5:15:2 to obtain a mixture.

[0130] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0131] Example 7

[0132] The only difference from Example 1 is that in step (2), the coke powder is evenly mixed with the epoxy resin, water, and boron nitride in a mass ratio of 100:6:15:2 to obtain a mixture.

[0133] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0134] Example 8

[0135] The only difference from Example 1 is that in step (2), the coke powder is uniformly mixed with petroleum resin, toluene and boric acid in a mass ratio of 100:6:15:2 to obtain a mixture.

[0136] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0137] Example 9

[0138] The only difference from Example 1 is that in step (2), the char powder is uniformly mixed with phenolic resin, water, and boron oxide in a mass ratio of 100:3:15:2 to obtain a mixture.

[0139] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0140] Example 10

[0141] The only difference from Example 1 is that in step (2), the coke powder is evenly mixed with phenolic resin, water, and silicon carbide in a mass ratio of 100:20:15:2 to obtain a mixture.

[0142] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are secondary artificial graphite particles.

[0143] Example 11

[0144] The only difference from Example 1 is that in step (2), the char powder is evenly mixed with phenolic resin, water, and sodium borate in a mass ratio of 100:6:5:2 to obtain a mixture.

[0145] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0146] Example 12

[0147] The only difference from Example 1 is that in step (2), the char powder is uniformly mixed with phenolic resin, water, and boron oxide in a mass ratio of 100:6:50:2 to obtain a mixture.

[0148] From the scanning electron microscope image in Figure 1, it can be seen that the negative electrode material obtained in this embodiment includes primary particles and secondary particles, most of which are primary particles of artificial graphite; from the pore size distribution curve in Figure 2, it can be seen that the negative electrode material contains pores, and the pores mainly include micropores and mesopores.

[0149] Example 13

[0150] The only difference from Example 1 is that in step (2), the char powder is uniformly mixed with phenolic resin, water, and boron chloride in a mass ratio of 100:6:15:1 to obtain a mixture.

[0151] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0152] Example 14

[0153] The only difference from Example 1 is that in step (2), the char powder is evenly mixed with phenolic resin, water, and boron oxide in a mass ratio of 100:6:15:5 to obtain a mixture.

[0154] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0155] Example 15

[0156] The only difference from Example 1 is that the pressing pressure in step (3) is 5 MPa.

[0157] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0158] Example 16

[0159] The only difference from Example 1 is that the pressing pressure in step (3) is 100 MPa.

[0160] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0161] Example 17

[0162] The only difference from Example 1 is that the temperature of the pre-carbonization treatment of the precursor in step (4) is 500°C.

[0163] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0164] Example 18

[0165] The only difference from Example 1 is that the temperature of the pre-carbonization treatment of the precursor in step (4) is 1200°C.

[0166] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0167] Example 19

[0168] The only difference from Example 1 is that the temperature of the graphitization treatment in step (5) is 2800°C.

[0169] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0170] Example 20

[0171] The only difference from Example 1 is that the temperature of the graphitization treatment in step (5) is 3000°C.

[0172] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0173] Example 21

[0174] The only difference from Example 1 is that the holding time for the graphitization treatment in step (5) is 2 hours.

[0175] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0176] Example 22

[0177] The only difference from Example 1 is that the holding time for the graphitization treatment in step (5) is 4 hours.

[0178] The negative electrode material obtained in this embodiment includes primary artificial graphite particles and secondary artificial graphite particles, most of which are primary artificial graphite particles.

[0179] Comparative Example 1

[0180] The difference from Example 1 is that the second precursor obtained in step (4) is charged into a graphite crucible, and then the graphite crucible is transferred to an Acheson furnace, and the negative electrode material is obtained by high-temperature graphitization. The maximum temperature of the graphitization process is 2900°C, the maximum temperature holding time is 2.5h, the heating rate of the graphitization process is 0.7°C / min, and the cooling rate is 0.1°C / min to obtain the negative electrode material.

[0181] Comparative Example 2

[0182] The Daqing petroleum coke raw material was crushed and shaped by shaping equipment to obtain crushed and shaped coke powder. The obtained coke powder with a median particle size of 15 μm was directly loaded into a graphite crucible, and then the graphite crucible was transferred to an Acheson furnace for high-temperature graphitization to obtain a negative electrode material. The maximum temperature of the graphitization process was 2900°C, the maximum temperature holding time was 8h, the heating rate of the graphitization process was 0.7°C / min, and the cooling rate was 0.1°C / min to obtain a negative electrode material.

[0183] Comparative Example 3

[0184] The Daqing petroleum coke raw material was pre-carbonized at 800°C for 4 hours and then put into a continuous graphitization furnace. The heating curve was as follows: the temperature was increased to 2800°C at a heating rate of 15°C / min, kept at 2800°C for 2.5 hours, and then cooled to 30°C at a cooling rate of 10°C / min. The heating and cooling rate ratio during the graphitization process was controlled at 1.5. The graphitized product was crushed and shaped to obtain the negative electrode material, and the median particle size of the crushed negative electrode material was controlled at 15μm.

[0185] Test Method

[0186] (1) Test method for median particle size of negative electrode materials:

[0187] The particle size distribution range of the negative electrode material was tested by Malvern laser particle size analyzer.

[0188] (2) Testing method for pore volume and average pore diameter of negative electrode materials:

[0189] The test was carried out using the ASAP2460 equipment of American Micromeritics. The pore volume V and average pore diameter were calculated using the BJH Desorption cumulative volume of pores model. Calculated within the pore size range.

[0190] (3) Testing method for specific surface area of ​​negative electrode material:

[0191] The dynamic specific surface area rapid tester JW-DX of Beijing Jingwei Gaobo Science and Technology Co., Ltd. was used for testing. The unit is m 2 / g.

[0192] (4) Test method for true density of negative electrode material:

[0193] The Anton Paconta PENTAPYC 5200e true density meter is used for testing. The Archimedean principle of gas displacement (density = mass / volume) and the Bohr law (PV = nRT) of inert gases with small molecular diameters under certain conditions are used to accurately measure the true volume of the material being tested, thereby obtaining its true specific gravity in g / cm 3 ;

[0194] (5) Testing method of surface morphology of negative electrode materials:

[0195] The surface morphology of the negative electrode material particles was observed using a Hitachi S4800 scanning electron microscope.

[0196] (6) X-ray diffraction characterization of the interlayer spacing d of the (002) plane of the material 002 , the unit is ; The peak intensity ratios of the (002) plane and the (110) plane and the peak intensity ratios of the (004) plane and the (110) plane.

[0197] (7) Battery performance test method:

[0198] The negative electrode materials, carboxymethyl cellulose (abbreviated as CMC), conductive carbon black (abbreviated as SP), and styrene-butadiene rubber (abbreviated as SBR) prepared in Examples 1 to 22 and Comparative Examples 1 to 3 were magnetically stirred in deionized water for 8 hours in a mass ratio of 95:1.5:1.5:2 to mix them evenly. The mixed slurry was coated on copper foil and vacuum-dried at 60°C as a working electrode. Metallic lithium was used as the counter electrode and reference electrode, the diaphragm was Celgard2325, and the electrolyte was 1 mol·L-1LiPF6-EC (ethylene carbonate) / DMC (dimethyl carbonate) / EMC (ethyl methyl carbonate) (volume ratio of 1:1:1). The CR2016 button cell assembly was completed in a glove box filled with high-purity argon.

[0199] The first discharge capacity / first discharge efficiency test was performed on a LAND battery tester with the following charge and discharge conditions: 2 h rest; discharge: 0.1C to 0.005V, 0.09C, 0.08C…0.02C to 0.001V; 15 min rest; charge: 0.1C to 1.5V; 15 min rest.

[0200] The button half-cell was subjected to rate performance testing at 25±2°C, and the charge-discharge specific capacity and coulombic efficiency at 0.2C, 1C and 2C were obtained.

[0201] The test method for cyclic expansion is to prepare the electrode sheet from the negative electrode material and assemble it into a mold battery. The expansion rate of the mold battery after 20 cycles is recorded by a sensor. The expansion rate = the change in electrode thickness d / the original thickness of the electrode sheet * 100%.

[0202] The results of the performance tests of the negative electrode materials obtained in the above examples and comparative examples are shown in Table 1 below, and the results of the performance tests of batteries made of the negative electrode materials are shown in Table 2 below:

[0203] Table 1. Comparison of negative electrode material performance

[0204]

[0205]

[0206] Table 2. Battery performance comparison results

[0207]

[0208]

[0209] According to the test data of Examples 1 to 22, it can be seen that pores are formed inside and / or on the surface of the graphite prepared in the examples of the present application, which improves the high-rate charging performance of the material. This is because when the negative electrode material is made into an electrode and applied to a lithium-ion battery, the lithium ions can fully combine with the carbon atoms in the artificial graphite under relatively low resistance, diffuse rapidly at the solid-liquid interface and in the solid phase, reduce concentration polarization, and help improve the rate performance of the negative electrode material. Among them, in Examples 3 and 4, because needle coke is used as the coke raw material, the rate performance of the tested battery is worse than that of other examples. This is due to the properties of the needle coke itself, and it cannot be concluded that the solution of the present application cannot solve the technical problem of poor rate performance.

[0210] In addition, when V*S / D is controlled in the range of 4.0 to 10, the more effective active sites on the surface of artificial graphite as a negative electrode material for lithium insertion and deintercalation reactions, the higher the specific capacity of the negative electrode material tends to be.

[0211] The negative electrode materials prepared in the Acheson furnace graphitization furnace in Comparative Examples 1 and 2 can be seen to have a certain pore structure, but the V*S / D is out of the above range, and the rate performance of artificial graphite as a negative electrode material is significantly reduced. In addition, the production process consumes a lot of energy, has a high thermal energy utilization rate, and significantly increases production time and cost.

[0212] Although Comparative Example 3 adopts a continuous graphitization process to prepare the negative electrode material, the coke raw material particles are directly put into the continuous graphitization furnace without using additives, controlling the ratio of the heating and cooling rates, and other process improvements. As a result, V*S / D deviates from the above range, and the capacity and rate performance are worse than those of Example 1 produced under the same process conditions.

[0213] Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the claims. Any person skilled in the art may make several possible changes and modifications without departing from the concept of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.

Claims

1. A negative electrode material, characterized in that The negative electrode material comprises artificial graphite, the artificial graphite has pores inside and / or on the surface, and the pore volume of the negative electrode material is V cm 3 / kg, true density is D g / cm 3 , the specific surface area is S m 2 / g, where 4.0≤V*S / D≤10, The pore volume was measured using ASAP2460 equipment from American company Micromeritics and the BJH Desorption cumulative volume of pores model. Calculated within the pore size range.

2. The negative electrode material according to claim 1, characterized in that The negative electrode material satisfies at least one of the following characteristics: (1) Particle size D of the negative electrode material 50 10μm~30μm; (2) The particle size D of the negative electrode material 10 ≥5μm; (3) The particle size D of the negative electrode material 90 ≤50μm.

3. The negative electrode material according to claim 1 or 2, characterized in that The negative electrode material satisfies at least one of the following characteristics: (1) The pore volume of the negative electrode material is V cm 3 / kg, 5≤V≤8; (2) The specific surface area of ​​the negative electrode material is S m 2 / g, 1.78≤S≤3.0; (3) The true density of the negative electrode material is D g / cm 3 , 2.210≤D≤2.

265.

4. The negative electrode material according to claim 1 or 2, characterized in that The pores include at least one of micropores and mesopores.

5. The negative electrode material according to claim 4, characterized in that The average pore size of the pores is 6. The negative electrode material according to claim 1 or 2, characterized in that The negative electrode material is measured by X-ray diffraction, and the interlayer spacing of the (002) plane is d 002 , 7. The negative electrode material according to claim 1 or 2, characterized in that The X-ray diffraction test shows that the peak intensity ratio of the (002) plane to the (110) plane of the artificial graphite is I 002 / I 110 is 65.0~120.0, and the peak intensity ratio of (004) plane to (110) plane is I 004 / I 110 It is 3.0 to 6.

0.

8. The negative electrode material according to claim 1 or 2, characterized in that The artificial graphite includes artificial graphite primary particles and / or artificial graphite secondary particles.

9. The negative electrode material according to claim 1 or 2, characterized in that The negative electrode material satisfies at least one of the following characteristics: (1) The negative electrode material further comprises amorphous carbon; (2) The negative electrode material further includes amorphous carbon, and the mass proportion of the amorphous carbon in the negative electrode material is 0.1 wt% to 5 wt%.

10. A battery, characterized in that: The battery comprises the negative electrode material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Lithium ion battery negative electrode active material, lithium ion battery negative electrode, lithium ion battery, battery pack and battery power vehicle

    CN109553085A

  • Carbon material, method for producing carbon material, and non-aqueous secondary battery using carbon material

    CN110451499A

  • Starting material of negative electrode material for nonaqueous secondary batteries, negative electrode material for nonaqueous secondary batteries, negative electrode for nonaqueous secondary batteries, and nonaqueous secondary battery

    CN113646920A

  • Graphite negative electrode material and lithium ion secondary battery

    JP2015207408A

  • Method of manufacturing negative electrode material for nonaqueous secondary battery

    JP2016184581A