Nonvolatile memory device

By using antiferroelectric material as the gate insulating layer in FeFET and using the positive curve of its polarization characteristic curve, the problem of insufficient deletion operation of oxide semiconductors is solved, and a stable non-volatile storage effect is achieved.

CN119096714APending Publication Date: 2024-12-06THE JAPAN SCI & TECH AGENCY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036714.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-09-20
Filing Date
2023-05-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In FeFETs using oxide semiconductors as channels, the problem of insufficient deletion operation is not sufficient, and the prior art has failed to effectively solve the problem that n-type oxide semiconductors are difficult to induce sufficient holes during the deletion operation.

Method used

The antiferroelectric material is used as the gate insulating layer, and the positive curve of the polarization characteristic curve of the antiferroelectric material is selectively used, and the load curve is shifted to the positive direction of the horizontal axis through the built-in voltage, thereby in the program and deletion state Maintain polarization state under the same condition to ensure that n-type oxide semiconductor can effectively support polarization.

Benefits of technology

The stable deletion operation of the antiferroelectric nonvolatile memory device is realized when the n-type oxide semiconductor is used as a channel, and the unique problem that the oxide semiconductor is difficult to induce holes is overcome, and the reliability of the memory device is improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096714A_ABST
    Figure CN119096714A_ABST
Patent Text Reader

Abstract

A non-volatile memory device includes a plurality of non-volatile memory elements, in which the non-volatile memory elements include a semiconductor layer including a metal oxide, a gate electrode opposing the semiconductor layer, and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode. Wherein the electron affinity of a first material forming the gate electrode is smaller than that of a second material forming the semiconductor layer, and the second material is an n-type semiconductor, or the electron affinity of the first material forming the gate electrode is larger than that of the second material forming the semiconductor layer, and the second material is an n-type semiconductor. And the second material is a p-type semiconductor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a nonvolatile memory device, and more particularly to a nonvolatile memory device having a three-dimensional stacked structure in which a plurality of nonvolatile memory elements are arranged in series. Background Art

[0002] In recent years, as the demand for nonvolatile memory devices increases, the development of nonvolatile memory devices using ferroelectrics has become increasingly active. In particular, FeFET (Ferroelectric Field Effect Transistor) using hafnium oxide-based ferroelectrics as gate insulating layers has attracted attention as a key device for realizing high-density memory devices integrated with a three-dimensional stacked structure because it can achieve low power consumption and high-speed operation compared to flash memory and has high consistency with CMOS processes.

[0003] On the other hand, with the development of ferroelectrics, attempts to use antiferroelectrics in nonvolatile memory devices are also increasing. Figure 1 The polarization characteristic curve (PV curve) of the antiferroelectric described later has a unique shape connecting two hysteresis loops, also called a butterfly curve. Figure 1 The hysteresis loop shown by the thick line in the middle can be referred to as the positive curve, and the hysteresis loop on the negative side of the vertical axis can be referred to as the negative curve. Due to the special shape of the polarization characteristic curve, the antiferroelectric has the characteristics of polarization and hysteresis when an electric field is applied, but the polarization is almost zero when the electric field is zero. Therefore, simply using the antiferroelectric as a gate insulating layer cannot achieve the effect of non-volatile storage device operation.

[0004] Non-patent documents 1 to 3 disclose a technology in which an AFeFET (Anti-Ferroelectric Field Effect Transistor) using an antiferroelectric as a gate insulating layer operates as a non-volatile storage device by using one of a negative curve and a positive curve (hereinafter also referred to as a "half hysteresis loop"). Specifically, non-patent document 1 discloses a stacked structure with an antiferroelectric as a dielectric layer. Non-patent document 2 discloses an AFeFET with an IGZO semiconductor channel using an antiferroelectric as a gate insulating layer. Non-patent document 3 discloses an AFeFET with a silicon semiconductor channel using an antiferroelectric as a gate insulating layer. In these technologies, the flat band voltage is shifted by using the work function difference between the semiconductor layer and the gate electrode, the fixed charge present in the gate insulating layer, or the dipole set at the interface of the gate insulating layer, thereby ostensibly allowing non-volatile storage operation using a half hysteresis loop of a butterfly curve. Non-patent document 4 describes the influence of the dipole set at the interface between various oxide layers and the silicon oxide layer on the flat band voltage.

[0005] Prior art literature

[0006] Non-patent literature

[0007] Non-patent literature 1: MILAN PESIC, TAIDE LI, VALERIO DI LECCE, MICHAEL HOFFMANN, MONICA MATERANO, CLAUDIA RICHTER, BENJAMIN MAX, STEFAN SLESAZECK, UWE SCHROEDER, LUCA LARCHER AND THOMAS MIKOLAJICK, "Built-In Bias Generation in Anti-Ferroelectric Stacks: Methods and Device Applications",JOURNAL OF THE ELECTRONDEVICES SOCIETY,VOLUME 6,Page(s):1019-1025, (2018)

[0008] Non-patent literature 2: Zhongxin Liang, Kechao Tang, Junchen Dong, Qijun Li, YuejiaZhou, Runteng Zhu, Yanqing Wu, Dedong Han, and Ru Huang, "A Novel High-EnduranceFeFET Memory Device Based on ZrO2 Anti Ferroelectric and IGZO Channel", 2021IEEE International Electron Devices Meeting(IEDM),Page(s):17.3.1-17.3.4,(2021)

[0009] Non-patent literature 3: Atanu K. Saha and Sumeet K. Gupta, "Modeling and Comparative Analysis of Hysteretic Ferroelectric and Anti-ferroelectric FETs", 2018 76th Device Research Conference (DRC), (2018)

[0010] Non-patent document 4: Koji Kita and Akira Toriumi, "Origin of electric dipoles formed at high-k / SiO2 interface", APPLIED PHYSICS LETTERS 94, Page(s): 132902-1-132902-3, (2009) Summary of the invention

[0011] Problem that the invention aims to solve

[0012] The inventors found in the process of studying FeFETs having an oxide semiconductor as a channel and using a ferroelectric as a gate insulating layer that FeFETs having an oxide semiconductor as a channel have a problem of insufficient deletion action. Typically, the oxide semiconductor used in FETs has n-type conductivity, so most carriers are electrons. Therefore, FeFETs using n-type oxide semiconductors as channels can induce a sufficient amount of electrons in the channel during program actions to support the polarization of the gate insulating layer. However, FeFETs using n-type oxide semiconductors as channels cannot induce a sufficient amount of holes (minority carriers) in the channel during the deletion action to support the polarization of the gate insulating layer, and there is a problem that the deletion action becomes insufficient.

[0013] The above-mentioned prior arts have not recognized the problems unique to the above-mentioned oxide semiconductors, and have not solved the problem that when an n-type oxide semiconductor is used as a channel of a non-volatile memory device, the erasing action of the AFeFET is insufficient, just like the erasing action of the above-mentioned FeFET.

[0014] In view of the above problems, one of the objects of the present invention is to realize a stable AFeFET erasing operation in a nonvolatile memory device including a plurality of AFeFETs using an n-type oxide semiconductor as a channel.

[0015] Means of solving the problem

[0016] A nonvolatile memory device in one embodiment of the present invention includes a plurality of nonvolatile memory elements, each of which has a semiconductor layer comprising a metal oxide, a gate electrode opposite to the semiconductor layer, and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, wherein the electron affinity of a first material constituting the gate electrode is less than the electron affinity of a second material constituting the semiconductor layer, and the second material is an n-type semiconductor.

[0017] A nonvolatile memory device in one embodiment of the present invention includes a plurality of nonvolatile memory elements, each of which has a semiconductor layer comprising a metal oxide, a gate electrode opposite to the semiconductor layer, and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, wherein the electron affinity of a first material constituting the gate electrode is greater than the electron affinity of a second material constituting the semiconductor layer, and the second material is a p-type semiconductor.

[0018] A nonvolatile memory device in one embodiment of the present invention includes a plurality of nonvolatile memory elements, wherein the nonvolatile memory elements have a semiconductor layer including a metal oxide, a gate electrode opposite to the semiconductor layer, a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, and an interface layer disposed between the gate insulating layer and the gate electrode, wherein the electron affinity of a first material constituting the gate electrode is less than the electron affinity of a second material constituting the gate electrode, the second material is an n-type semiconductor, and the interface layer is composed of silicon oxide.

[0019] In the above nonvolatile memory device, when the second material constituting the semiconductor layer is an n-type semiconductor, the gate insulating layer may have a resistance of -2 μC / cm 2 To -1μC / cm 2 When expressing a numerical range, the description “A to B” means “above A and below B”.

[0020] In the above nonvolatile memory device, when the second material constituting the semiconductor layer is an n-type semiconductor, the metal oxide may be Sn oxide or a composite oxide of In and Zn, and the electron affinity of the first material may also be less than 4.9 eV.

[0021] In the above nonvolatile memory device, when the second material constituting the semiconductor layer is an n-type semiconductor, the first material may also be n-type doped Si and / or Ge.

[0022] In the above nonvolatile memory device, the first material may also be a metal material.

[0023] In the above-mentioned nonvolatile storage device, when the second material constituting the semiconductor layer is an n-type semiconductor, the metal oxide may be an oxide of In or a composite oxide of In, Ga and Zn, and the electron affinity of the first material may also be below 4.3 eV.

[0024] In the above nonvolatile memory device, the first material may be n-type doped Si and / or Ge.

[0025] In the above nonvolatile memory device, the first material may also be a metal material.

[0026] A nonvolatile memory device in one embodiment of the present invention includes a plurality of nonvolatile memory elements, wherein the nonvolatile memory elements include a semiconductor layer comprising a metal oxide, a gate electrode opposite to the semiconductor layer, and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, wherein the metal oxide is Sn oxide or a composite oxide of In and Zn, and the electron affinity of the first material constituting the gate electrode may be below 4.9 eV.

[0027] A nonvolatile memory device in one embodiment of the present invention includes a plurality of nonvolatile memory elements, wherein the nonvolatile memory elements include a semiconductor layer comprising a metal oxide, a gate electrode opposite to the semiconductor layer, and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, wherein the metal oxide is an oxide of In or a composite oxide of In, Ga and Zn, and the electron affinity of the first material constituting the gate electrode is less than 4.3 eV.

[0028] In the above nonvolatile memory device, the antiferroelectric may be Hf x Zr 1-x A composite oxide represented by O2 (0≤x≤0.4).

[0029] In the above nonvolatile memory device, the gate insulating layer may have a thickness of not less than 5 nm and not more than 50 nm, preferably not less than 8 nm and not more than 30 nm, and most preferably not less than 10 nm and not more than 20 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram for explaining the polarization characteristic curve of an antiferroelectric.

[0031] Figure 2A Graphs showing the results of measuring the electrical characteristics of capacitors manufactured using antiferroelectrics.

[0032] Figure 2B Graphs showing the results of measuring the electrical characteristics of capacitors manufactured using antiferroelectrics.

[0033] Figure 3A A diagram showing a simulation model in AFeFET according to one embodiment of the present invention.

[0034] Figure 3B To show Figure 3A A diagram showing simulation results of the Id-Vg characteristics of the AFeFET model.

[0035] Figure 3C To show Figure 3A A diagram showing simulation results of an operating point analysis in the AFeFET model.

[0036] Figure 4A To show Figure 3A A diagram showing simulation results of an operating point analysis in the AFeFET model.

[0037] Figure 4B To show Figure 3A A graph showing the dependence of the Id-Vg characteristics on the fixed charge in the AFeFET model shown.

[0038] Figure 5A 1 is a cross-sectional view showing a device structure in a nonvolatile memory device according to an embodiment of the present invention.

[0039] Figure 5B A cross-sectional perspective view showing a device structure in a nonvolatile memory device according to an embodiment of the present invention.

[0040] Fig. 6A A cross-sectional view showing a device structure in a nonvolatile memory device according to an embodiment of the present invention.

[0041] Figure 6B The figure shows a cross-sectional TEM photograph of the vicinity of the trench of the prototype nonvolatile memory device.

[0042] Figure 7 FIG. 1 is a graph showing Id-Vg characteristics measured using a nonvolatile memory device according to an embodiment of the present invention.

[0043] Fig. 8A FIG. 1 is a graph showing the measurement results of the overwriting resistance of the nonvolatile memory device according to one embodiment of the present invention at room temperature.

[0044] Figure 8B FIG. 1 is a diagram showing the measurement results of the retention characteristics of the nonvolatile memory device according to one embodiment of the present invention at room temperature.

[0045] Fig. 9A To show the effect of changing the carrier concentration (N d ) is a diagram showing the simulation results of the Id-Vg characteristics under the condition of .

[0046] Fig. 9B To show the effect of changing the carrier concentration (N d ) is a diagram showing simulation results of the operating point analysis in the case of .

[0047] Fig.10 To show the carrier concentration (N) of the storage window to the oxide semiconductor layer in the AFeFET model d )’s dependency graph.

[0048] Fig.11A To show the effect of changing the film thickness (t OS ) is a diagram showing the simulation results of the Id-Vg characteristics under the condition of .

[0049] Fig. 11B To show the effect of changing the film thickness (t OS ) is a diagram showing simulation results of the operating point analysis in the case of .

[0050] Fig.12 To show the film thickness (t OS )’s dependency graph.

[0051] Fig.13A To show the effect of changing the thickness of the antiferroelectric layer (t AFe ) is a diagram showing the simulation results of the Id-Vg characteristics under the condition of .

[0052] Fig. 13B To illustrate the effect of changing the thickness of the antiferroelectric layer (t AFe ) is a diagram showing simulation results of the operating point analysis in the case of .

[0053] Fig.14 To show the storage window in the AFeFET model for the film thickness of the antiferroelectric layer (t AFe )’s dependency graph.

[0054] Fig.15A FIG. 1 is a diagram showing simulation results of Id-Vg characteristics when the composition of the antiferroelectric layer is changed in the AFeFET model.

[0055] Fig. 15B It is a diagram showing the simulation results of the operating point analysis when the composition of the antiferroelectric layer is changed in the AFeFET model.

[0056] Fig.16A FIG. 1 is a diagram showing simulation results of Id-Vg characteristics when the fixed charge of the antiferroelectric layer is changed in the AFeFET model.

[0057] Fig. 16B This is a diagram showing simulation results of an operating point analysis when the fixed charge of the antiferroelectric layer is changed in the AFeFET model. DETAILED DESCRIPTION

[0058] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings and the like. However, the present invention can be implemented in various modes without departing from the gist thereof, and should not be construed as being limited to the description of the embodiments illustrated below. For a clearer description, the accompanying drawings may schematically illustrate the width, thickness, shape, etc. of each part compared to the actual aspects, but this is merely an example and does not limit the interpretation of the present invention. In this specification and the accompanying drawings, elements having the same functions as those described with respect to the accompanying drawings are denoted by the same reference numerals, and their repeated descriptions may be omitted.

[0059] In the embodiments described below, the simulated temperature conditions are all room temperature.

[0060] [Basic idea of ​​the invention]

[0061] In realizing a nonvolatile memory device having an n-type oxide semiconductor as a channel, the inventors studied the element structure in consideration of the above-mentioned characteristics of the n-type oxide semiconductor (the characteristic that it is difficult to induce minority carriers). As a result, the inventors came up with a technical idea of ​​using the positive curve of the polarization characteristic curve (butterfly curve) of the antiferroelectric in a capacitor structure (a stack composed of a gate electrode / gate insulating layer / semiconductor layer) using an antiferroelectric as a material for the gate insulating layer. In the above-mentioned capacitor structure, the technical idea is to apply a built-in voltage to make the load curve of the FET (which will be used later) intersect with the polarization characteristic curve of the antiferroelectric. Figure 3A and Figure 3CIn addition, in the case of a nonvolatile memory device having a p-type oxide semiconductor as a channel, by applying a built-in voltage to shift the load curve in the negative direction of the horizontal axis, a negative curve of the polarization characteristic curve of the antiferroelectric can be used.

[0062] In the prior art, it has been described that a hysteresis loop on one side is used by using a model that shifts the polarization characteristic curve of an antiferroelectric by applying a built-in voltage. In contrast, in the present invention, it will be described that a hysteresis loop on the other side is used by using a model that shifts the load curve of an FET by applying a built-in voltage. However, in AFeFET, the shift of the polarization characteristic curve of the antiferroelectric and the shift of the load curve of the FET are just different models that represent the same phenomenon. That is, the shift of the polarization characteristic curve of the antiferroelectric in the negative direction of the horizontal axis and the shift of the load curve of the FET in the positive direction of the horizontal axis are both equivalent to a model that uses the positive curve of the polarization characteristic curve.

[0063] Figure 1 It is a schematic diagram used to describe the polarization characteristic curve of antiferroelectrics. Figure 1 In the figure, the horizontal axis represents the electric field and the vertical axis represents the polarization value (charge per unit area). Figure 1 As shown, a butterfly-shaped hysteresis loop consisting of two half hysteresis loops is shown. In this case, even in a polarization state (program state) with a large positive electric field applied, or a polarization state (deletion state) with a large negative electric field applied, if the electric field is zero, the polarization almost disappears and there is no residual polarization. Therefore, although the antiferroelectric cannot be used as a memory of a nonvolatile storage device as it is, a method of using it as a memory by using a half hysteresis loop is proposed.

[0064] Specifically, there is a method in which the external bias voltage V B Always apply to the gate electrode of the nonvolatile memory device to maintain an electric field corresponding to the vicinity of the center of the half hysteresis loop. In this case, if V is applied during programming B +V P voltage, when removing V B -V E If the voltage is set to , the write operation (program or delete) can be performed, but in order to maintain the storage device, an external bias voltage V must be applied even outside the write operation. B In contrast, the above-mentioned Non-Patent Document 1 proposes a method of using a half hysteresis loop by applying a built-in voltage instead of an external bias.

[0065] Non-patent document 2 discloses an antiferroelectric FET having IGZO as an n-type oxide semiconductor as a channel. Non-patent document 2 discloses a structure for applying an external bias to the AFeFET, and a structure for using a negative curve by shifting the polarization characteristic curve (butterfly curve) of the antiferroelectric in the positive direction of the horizontal axis. In non-patent document 2, as a specific method for shifting the polarization characteristic curve, a structure for applying a built-in voltage by changing the gate electrode material from TiN to Pt is proposed.

[0066] However, when a negative curve is used, the antiferroelectric layer is in a non-polarized state during programming and in a polarized state during erasure. At this time, the semiconductor layer corresponds to a depletion state during programming and a hole carrier induced state during erasure. When a negative curve is used, the action of the AFeFET matches the characteristics of silicon semiconductors, but does not match the characteristics of n-type oxide semiconductors that are difficult to generate hole carriers.

[0067] Therefore, the inventors have conceived a configuration using a positive curve opposite to the conventional technology. When the positive curve is used, the antiferroelectric layer is in a polarized state during programming and in a non-polarized state during deletion. At this time, the semiconductor layer corresponds to an electron carrier induced state during programming and corresponds to a depleted state during deletion. Therefore, when the positive curve is used, the action of the AFeFET is considered to match the characteristics of an n-type oxide semiconductor.

[0068] The inventors applied a built-in voltage to Figure 1 The polarization characteristic curve of the antiferroelectric shown crosses the load curve 10 of the FET (which will be used later). Figure 3A and Figure 3C Description) shifts to the positive direction of the horizontal axis, and the antiferroelectric maintains the polarization state when the external voltage is zero. Figure 1 As shown, the inventors set the vicinity of the center of the positive curve represented by the bold line as the FET's operating point (the intersection of the polarization characteristic curve and the load curve 10). In addition, the inventors used the above-mentioned operating point for reading the program state and the deletion state, and adopted a structure that used the antiferroelectric as a ferroelectric. Since the above-mentioned positive curve has a shape similar to the hysteresis loop of the ferroelectric, the AFeFET using the antiferroelectric as the gate insulating layer can operate similarly to the FeFET using the ferroelectric as the gate insulating layer.

[0069] exist Figure 1In the embodiment, when the polarization value in the hold state after executing the program action is Pp, and the polarization value in the hold state after executing the deletion action is Pe, the polarization value Pp represents a positive value, and the polarization value Pe represents a value close to zero. When the polarization value Pp is positive, the n-type oxide semiconductor can induce a sufficient amount of electrons (majority carriers) to support the polarization. On the other hand, when the polarization value Pe is zero (or extremely small), the n-type oxide semiconductor can fully support the polarization even if the induction of holes as minority carriers is small. That is, even if the n-type oxide semiconductor has the characteristic of not being easy to induce holes, a sufficient deletion action can be achieved.

[0070] here, Figure 2A and Figure 2B Graph showing the results of measuring the electrical characteristics of capacitors made using antiferroelectrics. Specifically, Figure 2A A PV curve is shown, in which the voltage is plotted on the horizontal axis and the polarization value (the amount of charge per unit area) is plotted on the vertical axis. Figure 2B The IV curve is shown in Figure 1, where voltage is plotted on the horizontal axis and current density is plotted on the vertical axis. The capacitor has an asymmetric structure in which zirconium oxide (Zirconia) is sandwiched between an n-type silicon layer and a titanium nitride layer. By adopting such a structure, a built-in voltage is applied to the capacitor, so that Figure 1 The load curve 10 shown is shifted in the positive direction of the horizontal axis. Since the voltage applied to the capacitor is a bias voltage of 1.5 V, the voltage sweep range is asymmetrical. The voltage is an AC voltage of 1 kHz.

[0071] like Figure 2A and Figure 2B As shown in FIG. 1 , it can be seen that as the voltage sweep range narrows, it changes from a double hysteresis loop (butterfly curve) to a single hysteresis loop. In particular, Figure 2B As shown in Figure 1, when the voltage swings with the maximum sweep width, two current peaks are observed in the positive and negative directions, while when the voltage swings with the minimum sweep width, only one current peak is observed in the positive and negative directions. Figure 2B It is shown that by reducing the voltage sweep range, only one of the two half hysteresis loops represented by the antiferroelectric can be used. Figure 2B In the figure, the negative current peak near -4.5V is caused by leakage current, and the current peak near -3.5V overlaps. In addition, the positive current peak near 6.5V is also caused by leakage current.

[0072] As described above, in the capacitor structure using the antiferroelectric, the load curve of the AFeFET is shifted in the horizontal axis direction by the asymmetric electrode structure, and then the scanning range of the voltage applied between the electrodes is appropriately adjusted. Therefore, in the capacitor structure of the present embodiment, only one of the two half hysteresis loops is used, and the polarization of the program state and the erase state can be maintained even if the voltage becomes zero. Specifically, in the present embodiment, in the case of using an n-type oxide semiconductor as a channel, the positive curve of the two half hysteresis loops represented by the antiferroelectric is used by the asymmetric electrode structure.

[0073] As described above, the inventors have found that, in the case of manufacturing a nonvolatile memory device using an n-type oxide semiconductor as a channel, it is effective to use an antiferroelectric as a gate insulating layer and selectively use a positive curve in the polarization characteristic curve of the antiferroelectric. By adopting such a structure, it is possible to overcome the problem that it is difficult for an n-type oxide semiconductor to induce hole carriers, and to realize a highly reliable nonvolatile memory device that effectively utilizes the advantages of an n-type oxide semiconductor.

[0074] [Adjustment of action points]

[0075] Based on the above basic idea, when using the positive curve of the two half hysteresis loops of the antiferroelectric, it is desirable to appropriately adjust the operating point of each storage element (AFeFET). Figure 1 As shown, the load curve 10 (i.e., the operating point) of the AFeFET is shifted so that the polarization values ​​Pp and Pe can be maintained near the center of the positive curve. In the shift of the operating point, a method of applying a built-in voltage and shifting the flat band voltage using the work function difference between the gate electrode and the oxide semiconductor, the fixed charge present in the gate insulating layer, and / or the dipole (hereinafter referred to as "interface dipole") provided at the interface between the gate insulating layers can be applied. Here, the operating point of the AFeFET will be described.

[0076] Figure 3A FIG. 1 is a diagram showing a simulation model in an AFeFET according to an embodiment of the present invention. Figure 3A As shown, the AFeFET of this embodiment can be represented by a model in which an antiferroelectric capacitor having an antiferroelectric as a dielectric and a MOS transistor having an oxide semiconductor as a channel are connected in series. Figure 3A In this paper, the antiferroelectric capacitor adopts the Preisach model and the MOS transistor adopts the disconnected FET model. In addition, it is assumed that there is a fixed charge on the node between the antiferroelectric capacitor and the MOS transistor. gis the voltage between the source and gate electrodes of the modeled AFeFET (hereinafter referred to as the “AFeFET model”) (hereinafter referred to as the “gate voltage”). The gate voltage is assigned to the first voltage (V AFe ) and a second voltage (V MOS ).

[0077] Figure 3B To show Figure 3A The graph is a simulation result of the Id-Vg characteristics in the AFeFET model shown in FIG. The horizontal axis represents the gate voltage (V g ), the vertical axis represents the drain current. The gate length (corresponding to the channel length) and gate width are set to 50μm respectively. The source-drain voltage (Vds) is set to 0.1V, and the gate voltage is swept in the range of -5V to 1V. In addition, the flat band voltage (V FB ) is set to -2.5V. Figure 3B As shown, the Id-Vg curve in the program state (dashed line) and the Id-Vg curve in the erased state (solid line) can be clearly distinguished, and it can be confirmed that it operates as an AFeFET.

[0078] then, Figure 3C To show Figure 3A The horizontal axis is the first voltage (V AFe ), the vertical axis is the polarization value (the amount of charge per unit area). Figure 3C In FIG. 3 , the polarization characteristic curve 31 of the antiferroelectric capacitor and the load curve 32 of the MOS transistor are overlapped and shown. The dotted line portion of the polarization characteristic curve 31 represents the polarization characteristic in the program state, and the solid line portion represents the polarization characteristic in the erase state.

[0079] The load curve 32 of the MOS transistor is a curve for applying a certain gate voltage V g In the case of scanning the first voltage (V AFe ) is applied with the gate voltage V g and the first voltage (V AFe ) of the corresponding second voltage (V MOS The curve plots the change in the dielectric charge (the amount of charge induced in the channel) of a MOS transistor. Figure 3C In the AFeFET model, the gate voltage V applied to the gate electrode is g The cases of -3.2 V, -1 V and 1.5 V are respectively represented as load curves 32 of the MOS transistor.

[0080] like Figure 3C As shown, when Vg When the voltage is -1V, the polarization characteristic curve 31 and the load curve 32 intersect at two points. The point where the polarization characteristic curve 31 and the load curve 32 intersect is called the operating point. The operating point 33 is the operating point when the AFeFET is in the program state, and the operating point 34 is the operating point when the AFeFET is in the delete state. The greater the distance between the operating point 33 and the operating point 34, the easier it is to distinguish between the program state and the delete state of the AFeFET.

[0081] exist Figure 3C In the load curve 32, the flat band voltage (V FB ) changes in the left-right direction. For example, the load curve 32 changes according to the work function difference between the material constituting the gate electrode of the AFeFET and the material constituting the semiconductor layer. In addition, the load curve 32 is changed by the interface dipole caused by the interface layer between the gate electrode and the gate insulating layer. That is, by adjusting the work function difference or the interface dipole, the position of the load curve 32 in the left-right direction can be changed, and the operating point can be shifted to an appropriate position. Below, a specific method for adjusting the operating point of the AFeFET will be described.

[0082] [Adjustment based on work function difference]

[0083] As mentioned above, by adjusting the flat-band voltage V of the AFeFET FB , which can make Figure 3C The load curve 32 shown is shifted in the positive or negative direction of the horizontal axis. In the case of the present embodiment, since the positive curve in the polarization characteristic curve of the antiferroelectric is selectively used, the load curve 32 is shifted to the positive side. As a method for achieving this purpose, the work function of the material constituting the gate electrode of the AFeFET can be set to be smaller than the work function of the material constituting the semiconductor layer. In addition, the work function of the semiconductor layer varies with the position of the Fermi level, that is, the carrier concentration. The work function of the metal is consistent with the electron affinity. When the carrier concentration is high, the work function of the semiconductor layer is almost equal to the electron affinity, so the electron affinity can be used as an indicator. In this case, the above method can be said to be that the electron affinity (that is, the work function) of the material constituting the gate electrode of the AFeFET is smaller than the electron affinity of the material constituting the semiconductor layer.

[0084] According to the findings of the present inventors, when driving an AFeFET having an antiferroelectric as a gate insulating layer, in order to shift the load curve 32 to a practical position, it is desirable to set a work function difference of 1 eV or more between the material constituting the gate electrode and the material constituting the semiconductor layer. In view of this, when an oxide semiconductor having a work function of about 4.4 eV, such as IGZO, is used as the semiconductor layer, a negative curve can be used by selecting a known material having a work function of 5.4 eV or more, such as Pt proposed in Non-Patent Document 2, as the material of the gate electrode.

[0085] However, in order to use a positive curve using only the work function difference as proposed in the present invention, it is necessary to select a metal having a work function of 3.4 eV or less. As metals having a low work function, metal materials containing metal oxides or alkaline earth metals (such as Cs, Ca, etc.) or lanthanide elements (such as La, Eu, etc.) are known. However, since these materials have high activity, they are subject to many restrictions when used as materials for gate electrodes in consideration of actual manufacturing processes.

[0086] Therefore, in practice, when using an oxide semiconductor with a work function of less than 4.4 eV, it is desirable to combine the later-described adjustment based on the composition of the antiferroelectric, the adjustment based on fixed charge, etc., or the adjustment based on the interface dipole with the above-mentioned adjustment based on the work function difference (i.e., the difference in electron affinity) so that a positive curve can be used.

[0087] In this embodiment, since an n-type oxide semiconductor is used as a semiconductor layer, the material of the gate electrode is a material having a work function (i.e., electron affinity) smaller than that of the n-type oxide semiconductor used as the semiconductor layer. Specifically, as the material of the gate electrode, a conductive material having a work function smaller than that of the n-type oxide semiconductor used as the semiconductor layer by 0.1 eV or more (preferably 0.4 eV or more) is used. As the conductive material, a metal material or a semiconductor material doped with impurities can be used. For example, as the material constituting the semiconductor layer, indium oxide (InO2) having a work function of about 4.4 to 4.5 eV is used. x ) or a metal oxide (IGZO) containing In, Ga, and Zn, as the material of the gate electrode, n-type doped silicon (n-type silicon) or n-type doped germanium (n-type germanium) having a work function of about 4.0 eV can be used. In addition, as the material constituting the semiconductor layer, a material with a work function larger than that of indium oxide or IGZO is used, for example, tin oxide (SnO) having a work function of about 4.8 eV is used. x) or a metal oxide containing In and Zn with a work function of about 5.0 eV (IZO), as the material of the gate electrode, titanium nitride (TiN) with a work function of about 4.4 eV or n-type silicon with a work function of about 4.0 eV can be used. In the case of using TiN as the material of the gate electrode, for example, a stacked gate structure can be adopted in which TiN is provided on a portion in contact with the gate insulating layer, and a metal layer such as tungsten (W) is provided thereon. In addition, when indium tin oxide (ITO) with a work function of about 4.7 eV or aluminum-doped zinc oxide (ZnO:Al) with a work function of about 4.6 eV is used as the material constituting the semiconductor layer, the work function difference can also be adjusted by combining with an appropriate gate electrode.

[0088] In addition, when a p-type oxide semiconductor is used as a semiconductor layer, a negative curve can be used by using a material having a work function (i.e., electron affinity) greater than that of the p-type oxide semiconductor as a material for the gate electrode. As p-type oxide semiconductors, for example, NiO, Cu2O, β-TeO2, CuCo2O4, CuAlO2, LaCuOSe, CuRhO2, SnO, Ta2SnO6, and Sn2Nb2O7 can be cited. As a material for the gate electrode, for example, RuOx or Pt having a work function of 5.3 to 5.4 eV is preferably used.

[0089] As described above, the difference in work function (or electron affinity) between the material constituting the gate electrode and the material constituting the semiconductor layer can make Figure 3C The load curve 32 shown is shifted to the positive side (positive direction). However, when the work function difference cannot be increased due to material selection limitations, sometimes the operating point cannot be shifted to an appropriate position by the work function difference alone. In this case, it is desirable to use the adjustment of fixed charges and / or interface dipoles described below in combination.

[0090] [Adjustment based on fixed charge]

[0091] Fixed charges are fixed charges existing inside or at the interface of the insulating layer. In the case of this embodiment, it is assumed that fixed charges exist inside or at the interface of the gate insulating layer composed of an antiferroelectric. Figure 3C The load curve 32 shown is shifted to the positive side, and negative fixed charges are preferably present inside or at the interface of the gate insulating layer. When zirconium oxide (ZrO2) is used as the antiferroelectric, as shown in this embodiment, oxygen defects in the film serve as positive fixed charges. Positive fixed charges make Figure 3CThe load curve 32 shown is shifted to the negative side, so it is preferred that there are fewer positive fixed charges in the gate insulating layer. However, even if there are positive fixed charges, the load curve 32 can be shifted to an appropriate position by applying negative fixed charges exceeding the amount of positive fixed charges to the gate insulating layer. According to the findings of the present inventors, the gate insulating layer composed of an antiferroelectric preferably has a -3μC / cm 2 To 2μC / cm 2 The fixed charge is preferably -2 μC / cm 2 To -1μC / cm 2 of fixed charge.

[0092] The amount of negative fixed charge present in the gate insulating layer can be adjusted by adjusting the film quality of the gate insulating layer according to the film forming conditions or intentionally adding ion species serving as negative fixed charge to the gate insulating layer after the gate insulating layer is formed. For example, the amount of negative fixed charge can be adjusted by adding ion species serving as negative fixed charge by ion implantation, plasma treatment, etc. after the gate insulating layer is formed.

[0093] Here, in Figure 3A In the AFeFET model shown, it is assumed that a fixed charge exists at the node between the antiferroelectric capacitor and the MOS transistor. The inventors have confirmed the influence of the increase and decrease of the fixed charge on the load curve 32 through simulation.

[0094] Figure 4A To show Figure 3A The figure shows the simulation results of the operating point analysis in the AFeFET model. Figure 3C Same, but in Figure 4A In FIG. 1 , the gate voltage V applied to the gate electrode of the AFeFET model is shown. g -V FB The load curve 32 is -0.5V, 1.25V and 3V. Here, the flat band voltage V FB is -1V. In addition, Figure 4A , the fixed charge of each load curve is -3μC / cm 2 To 0μC / cm 2 In the range of Figure 4A In the figure, each load curve 32 has a relative voltage to the first voltage (V AFe ) is a region where the charge density changes are constant (hereinafter referred to as a "flat region"). In the flat region 35, the MOS transistor operates in a subthreshold region.

[0095] like Figure 4A As shown, when the negative fixed charge increases, the flat area 35 of each load curve 32 shifts upward. This is considered to be because as the negative fixed charge increases, V MOSOn the other hand, when the AFeFET is in the erase state, the read current is smaller than the read current when the AFeFET is in the program state. g -V FB The load curve for 1.25V is 32( Figure 4A Take the load curve 32) in the middle as an example, at a fixed charge of -3μC / cm 2 In the case of the AFeFET in the deleted state, the operating point 34 is located near the flat region 35 of the load curve 32. That is, when the AFeFET is in the deleted state, the drain current does not flow much because the operating point is close to the subthreshold region. In contrast, the operating point 33 in the program state is located above the load curve 32, that is, away from the flat region 35. That is, when the AFeFET is in the program state, a large drain current flows.

[0096] As described above, when the negative fixed charge increases, the load curve 32 shifts upward, so that the read current in the deleted state of the AFeFET tends to decrease, while the read current in the program state tends not to change like the read current in the deleted state. That is, by increasing the negative fixed charge, the ratio of the drain current when reading in the program state of the AFeFET to the drain current when reading in the deleted state (hereinafter referred to as the "drain current ratio when reading") improves the recognizability of the information stored in the AFeFET (information of "1" or "0"). Therefore, the gate insulating layer composed of the antiferroelectric preferably has a -3μC / cm 2 To 2μC / cm 2 The fixed charge is preferably -2 μC / cm 2 To -1μC / cm 2 The fixed charge in the gate insulating layer is preferably -3 μC / cm 2 The reason for the above is that, from the viewpoint of reliability of AFeFET, if too much fixed charge exists in the gate insulating layer, degradation may be caused.

[0097] In addition, although it is described here that the load curve 32 is shifted by introducing negative fixed charges into the gate insulating layer, the present invention is not limited to this example, and the shape of the polarization characteristic curve 31 of the antiferroelectric can be changed. For example, in the case of using zirconium oxide as the antiferroelectric, by adding hafnium, the polarization characteristic curve 31 approaches the polarization characteristic curve of the ferroelectric. As a result, in this case, as in the case of adding negative fixed charges, since the operating point 34 in the erased state of the AFeFET approaches the flat region 35 of the load curve 32, the drain current ratio during reading can be increased.

[0098] By the way, in the past, in non-volatile memory elements such as FeFETs, the difference between the threshold voltage in the program state and the threshold voltage in the delete state was defined as a storage window. However, in the AFeFET of the present embodiment, as described above, it is desirable to define the ratio of the drain current during reading in the program state to the drain current during reading in the delete state (i.e., the drain current ratio during reading) as a storage window. Preferably, the gate voltage during reading is set to a voltage that turns on the AFeFET in both the program state and the delete state. This is because if the AFeFET is set to a voltage that turns on in the program state and turns off in the delete state, and the memory cells in the same block are repeatedly read, the data of adjacent memory cells may be overwritten (so-called read interference).

[0099] When the difference between the threshold voltages is defined as the memory window, the drain current when the MOS transistor operates in the subthreshold region is processed. The load curve of the MOS transistor in this case is Figure 4A Equivalent to V g -V FB Load curve 32 when -0.5V ( Figure 4A That is, the operating point exists in the region where the polarization characteristic curve 31 is almost closed. Therefore, the operating point of the program state and the operating point of the delete state are very close, and the operation of the program state cannot be effectively utilized. Figure 4A The hysteresis loop is shown.

[0100] Therefore, in order to appropriately evaluate the memory window of the AFeFET of this embodiment, the inventors define the drain current ratio during the above reading as the memory window. Figure 4A In the case of using a position where the hysteresis loop has a larger width in the vertical direction (for example, V g -V FB The position of the load curve 32 when the voltage is 1.25 V) is used to evaluate the recognizability of the stored information.

[0101] Figure 4B To show Figure 3A A graph showing the dependence of the Id-Vg characteristics on the fixed charge in the AFeFET model shown. Figure 4B In the figure, the straight line near the gate voltage of 0.16 V is the gate voltage during reading. Figure 4B In the embodiment, the drain current ratio during reading is determined by using the drain current at the intersection of the straight line and the Id-Vg characteristic curve. Specifically, in this embodiment, Figure 3A The drain current in the programmed state of the AFeFET model shown ( Figure 4B The upper curve group) and the drain current in the deleted state ( Figure 4BThe ratio between the curve group on the lower side of ) is used as the storage window evaluation.

[0102] like Figure 4B As shown in the figure, the drain current in the program state is independent of the value of the fixed charge, while the drain current in the erase state is dependent on the value of the fixed charge. The results show that the memory window (drain current ratio when reading) of the AFeFET increases as the amount of negative fixed charge inside the gate insulating layer or on the interface increases. From this point, it can also be seen that in order to ensure the memory window, the gate insulating layer composed of antiferroelectrics preferably has a -3μC / cm 2 To 2μC / cm 2 The fixed charge is preferably -2 μC / cm 2 To -1μC / cm 2 of fixed charge.

[0103] [Adjustment based on interface dipole]

[0104] Next, adjustment of the load curve 32 based on the interface dipole will be described. The interface dipole is a dipole (dipole) caused by an interface layer existing between two layers. In this embodiment, an interface layer is arranged between the gate insulating layer and the gate electrode, and the load curve 32 is shifted in the left-right direction by using the dipole caused by the interface layer. Specifically, in this embodiment, the interface dipole is introduced to make Figure 3A The flat band voltage of the AFeFET model shown is shifted, thereby shifting the load curve 32. For example, covalent silicon oxide (SiO2) or germanium oxide (GeO2) is used as an interface layer, and a dipole is formed by silicon oxide or germanium oxide and a gate insulating layer as a high dielectric constant material (High-k material).

[0105] In the case of this embodiment, since zirconium oxide is used as a gate insulating layer and silicon oxide is used as an interface layer, a dipole is formed by the stacked structure of silicon oxide and zirconium oxide. When silicon oxide and zirconium oxide come into contact, since oxide ions shift from zirconium oxide with a large spatial density of oxygen atoms to silicon oxide with a small spatial density of oxygen atoms, zirconium oxide is in an oxygen deficiency state and is positively charged, while silicon oxide is negatively charged. Therefore, a dipole is generated in which the silicon oxide side is negative and the zirconium oxide side (gate insulating layer side) is positive.

[0106] In this embodiment, since the work function of the first material constituting the gate electrode is smaller than the work function of the second material constituting the oxide semiconductor, it is preferred to form a dipole with the gate electrode side as negative and the semiconductor layer side as positive. That is, in the case of this embodiment, a structure in which a layer made of silicon oxide is provided as an interface layer between a gate insulating layer made of zirconium oxide and a gate electrode is used. That is, the AFeFET of this embodiment has a stacked structure consisting of oxide semiconductor / zirconium oxide / silicon oxide / gate electrode.

[0107] As described above, by providing silicon oxide (or germanium oxide) as an interface layer between the gate insulating layer (zirconium oxide) made of a high dielectric constant material and the gate electrode, and forming a dipole caused by the interface layer, the flat band voltage of the AFeFET can be shifted. Figure 3C The load curve 32 shown is shifted, and the position of the operating point of the AFeFET can be appropriately adjusted. The thickness of the interface layer is preferably 0.5 nm to 5 nm, and more preferably 1 nm to 2 nm. The interface layer is preferably formed by the ALD method.

[0108] [Device structure]

[0109] Hereinafter, the structure of a nonvolatile memory device 100 according to an embodiment of the present invention will be described.

[0110] Figure 5A FIG. 1 is a cross-sectional view showing the device structure of a nonvolatile memory device 100 according to an embodiment of the present invention. Figure 5A The nonvolatile memory device 100 shown in FIG. 1 includes a plurality of nonvolatile memory elements 20 (see FIG. Figure 5B ) is a three-dimensional stacked structure that is three-dimensionally integrated. A plurality of non-volatile memory elements 20 are arranged in series along the longitudinal direction of a semiconductor layer 210, wherein the cylindrical semiconductor layer 210 used as a channel is common. In this embodiment, the non-volatile memory element 20 is an AFeFET having a gate insulating layer 220 formed of an antiferroelectric.

[0111] The source electrode 120 is provided on the substrate 110. As the substrate 110, a silicon substrate or a metal substrate having an insulating surface can be used. As the source electrode 120, a metal material including titanium, aluminum, tungsten, tantalum, molybdenum, copper, etc. or a compound material including these metal materials can be used. When an n-type semiconductor substrate (for example, an n-type silicon substrate) is used as the substrate 110 to function as a source electrode, the source electrode 120 can be omitted. Figure 5A The source electrode 120 is shown.

[0112] The plurality of nonvolatile memory elements 20 are provided in series between the source electrode 120 and the drain electrode 130. The semiconductor layer 210 is electrically connected to the source electrode 120 and the drain electrode 130. That is, in the nonvolatile memory device 100, the plurality of nonvolatile memory elements 20 also share the source electrode 120 and the drain electrode 130.

[0113] The source electrode 120 is electrically connected to a source terminal 140 made of a metal material. The drain electrode 130 is electrically connected to a drain terminal 150 made of a metal material. The drain terminal 150 is connected to a bit line (not shown) of the nonvolatile memory device 100. In addition, a plurality of gate electrodes 230 are electrically connected to the gate terminal 160, respectively. The plurality of gate terminals 160 are connected to a word line (not shown) of the nonvolatile memory device 100. The source terminal 140, the drain terminal 150, and the gate terminal 160 are electrically connected to the source electrode 120, the drain electrode 130, and the gate electrode 230, respectively, through a contact hole in the passivation layer 170, an insulating layer 240 disposed between each gate electrode 230, or an insulating layer 240 disposed between the source electrode and the bottommost gate electrode 230.

[0114] Figure 5B 1 is a cross-sectional perspective view showing the element structure of a nonvolatile memory device 100 according to an embodiment of the present invention. Specifically, Figure 5B is Figure 5A The nonvolatile memory device 100 shown is an enlarged view of a portion surrounded by a frame line 200 (a portion corresponding to three nonvolatile memory elements 20 ).

[0115] like Figure 5B As shown, the nonvolatile memory element 20 of this embodiment is an AFeFET composed of a semiconductor layer 210, a gate insulating layer 220, and a gate electrode 230. In the nonvolatile memory device 100 of this embodiment, a plurality of nonvolatile memory elements 20 share the semiconductor layer 210 and the gate insulating layer 220.

[0116] The semiconductor layer 210 is a cylindrical member used as a channel of the nonvolatile memory element 20. In this embodiment, the semiconductor layer 210 includes a metal oxide. Specifically, the semiconductor layer 210 is made of indium oxide (InO x ) is formed. The film thickness of the semiconductor layer 210 is greater than 5 nm and less than 15 nm (preferably greater than 8 nm and less than 10 nm). In addition, in this embodiment, the semiconductor layer 210 is formed using an ALD (Atomic Layer Deposition) method. However, other methods may also be used as long as the semiconductor layer 210 having a uniform film thickness can be formed on the inner wall of the trench.

[0117] The semiconductor layer 210 is not limited to indium oxide, and other metal oxides may also be used. For example, a metal oxide called IGZO may be used as the semiconductor layer 210. IGZO is a metal oxide having semiconductor properties and is a compound material composed of indium, gallium, zinc, and oxygen. Specifically, IGZO is an oxide containing In, Ga, and Zn or a mixture of these oxides. The composition of IGZO is preferably In. 2-x Gax O3(ZnO) m (0 < x < 2, m is a natural number of 0 or less than 6), more preferably InGaO3(ZnO) m (m is a natural number of 0 or less than 6), most preferably InGaO3(ZnO). In addition, tin oxide (SnO2), IZO (metal oxide including In and Zn), zinc oxide (ZnO), etc. can be used.

[0118] In addition, the semiconductor layer 210 is not limited to a single-layer structure and can have a stacked structure. For example, a semiconductor layer having a stacked structure composed of a first semiconductor layer and a second semiconductor layer with a wider bandgap than the first semiconductor layer can also be used.

[0119] The gate insulating layer 220 is formed of an antiferroelectric. Specifically, in the present embodiment, zirconium oxide (ZrO2) is used as the antiferroelectric constituting the gate insulating layer 220. However, the antiferroelectric that can be used in this embodiment is not limited to zirconium oxide, and other materials having antiferroelectric characteristics can be used. In addition, as the gate insulating layer 220, a material obtained by adding hafnium to zirconium oxide can be used. By using a composite oxide in which part of the zirconium in zirconium oxide is replaced by hafnium, the shape of the polarization characteristic curve (butterfly curve) of zirconium oxide can be changed. For example, in Hf x Zr 1-x O2, 0 ≤ x < 0.5 is preferred, 0 ≤ x ≤ 0.4 is more preferred, and 0 ≤ x ≤ 0.3 is most preferred.

[0120] In the present embodiment, the gate insulating layer 220 with a film thickness of 10 nm is formed by the ALD method. However, the film thickness of the gate insulating layer 220 is not limited to this example and can be, for example, 5 nm or more and 20 nm or less (preferably 8 nm or more and 18 nm or less). The gate insulating layer 220 is provided in contact with the side surface of the semiconductor layer 210 and surrounds the semiconductor layer 210. That is, the gate insulating layer 220 can be referred to as a cylindrical member having a cylindrical semiconductor layer 210 inside. The gate insulating layer 220 of the present embodiment has -3 μC / cm 2 to 2 μC / cm 2 of fixed charge (preferably -2 μC / cm 2 to -1 μC / cm 2 of fixed charge).

[0121] The gate electrode 230 is used as a gate for controlling a program operation or an erase operation of the nonvolatile memory element 20. In this embodiment, n-type doped silicon (n-type silicon) is used as a material of the gate electrode 230. In the nonvolatile memory element 20 of this embodiment, the width of the gate electrode 230 corresponds to the channel length (L) of the nonvolatile memory element 20. The width of the gate electrode 230 is the film thickness of the n-type polysilicon layer used as the gate electrode 230. Here, in this embodiment, as a material constituting the gate electrode 230, a material having an electron affinity (i.e., a work function) smaller than the electron affinity of the material constituting the semiconductor layer 210 is used.

[0122] The gate electrode 230 is preferably formed using a gate electrode priority method. In this embodiment, a stack is formed by alternately stacking an n-type polysilicon layer used as the gate electrode 230 and an insulating layer such as silicon oxide used as the insulating layer 240 on a substrate, and then a plurality of grooves (storage holes) are formed in a vertical direction on the stack. After forming a plurality of grooves, the gate insulating layer 220 and the semiconductor layer 210 are sequentially stacked on the inner wall of the groove. Finally, the hollow portion in the semiconductor layer 210 is filled with an insulating material used as a filling member 250. Here, photolithography and reactive ion etching can be used to form the groove.

[0123] In addition, when a metal material is used as the gate electrode 230, a gate electrode last method can also be used. In the gate electrode last method, first, a stack is formed by alternately stacking virtual layers made of silicon nitride and the like and insulating layers made of silicon oxide and the like, and then a plurality of grooves (storage holes) are formed in a vertical direction on the stack. Then, the virtual layer is selectively removed, and a metal material is embedded in the space where the virtual layer is removed to form a gate electrode made of a metal material. The formation of the gate insulating layer 220 and the semiconductor layer 210 is similar to the gate electrode first method. After embedding the metal material, the above-mentioned interface layer can also be formed by embedding silicon oxide or germanium oxide to contact the metal material. However, the present invention is not limited to this method, and after forming a plurality of grooves, the interface layer, the gate insulating layer 220 and the semiconductor layer 210 can be stacked on the inner wall of the groove in sequence.

[0124] The insulating layer 240 is an insulating film for insulating and separating two adjacent gate electrodes 230. As the insulating layer 240, an insulating film such as a silicon oxide film or a silicon nitride film can be used. In the present embodiment, the film thickness of the insulating layer 240 is greater than 10nm and less than 50nm (preferably greater than 20nm and less than 40nm), but is not limited to this example. The film thickness of the insulating layer 240 can be appropriately determined based on the relationship with the channel length (i.e., the width of the gate electrode 230). However, if the film thickness of the insulating layer 240 is too thin, the adjacent non-volatile memory elements 20 may affect each other, resulting in an operational failure. In addition, if the film thickness of the insulating layer 240 is too thick, the distance between the channels of the adjacent non-volatile memory elements 20 becomes longer, which may become an obstacle to carrier displacement.

[0125] The filling member 250 is used as a filling material for filling the inside of the cylindrical semiconductor layer 210. As the filling member 250, an insulating material such as silicon oxide, silicon nitride or resin can be used. These insulating materials can be filled into the inside of the semiconductor layer 210 by a known method such as a CVD method. In addition, in the case where the diameter of the trench (storage hole) is small, the filling member 250 may not be present, in which case the semiconductor layer 210 is not in a cylindrical shape but in a cylindrical shape. In addition, the filling member 250 does not need to completely fill the inside of the cylindrical semiconductor layer 210, and a space not filled by the filling member may be left in a part of the inside of the semiconductor layer 210.

[0126] The nonvolatile memory device 100 of the present embodiment described above includes a nonvolatile memory element 20 using an oxide semiconductor as a semiconductor layer 210 and an antiferroelectric as a gate insulating layer 220. Although the nonvolatile memory element using an oxide semiconductor has the advantages of low power consumption and high reliability, as described in the prior art, the nonvolatile memory element has the disadvantage that the deletion action easily becomes insufficient. However, in the nonvolatile memory device 100 of the present embodiment, by combining an oxide semiconductor and an antiferroelectric and selectively using the hysteresis loop on the positive side of the polarization characteristic curve of the antiferroelectric, the above disadvantages are overcome and a stable deletion action is achieved.

[0127] [Example]

[0128] Hereinafter, the structure of the prototype nonvolatile memory device 300 of this embodiment and the measurement results of the electrical characteristics will be described.

[0129] Fig. 6A 1 is a cross-sectional view showing a device structure in a nonvolatile memory device 300 according to an embodiment of the present invention. Fig. 6A The nonvolatile memory device 300 shown has a structure in which two vertical type (a type in which a channel extends in a vertical direction with respect to a substrate) nonvolatile memory elements are connected in series.

[0130] exist Fig. 6A In the present invention, a bottom layer 311 made of silicon oxide is provided on a silicon substrate 310. Two gate electrodes 313 are provided on the bottom layer 311 in a manner facing each other with a groove 312 sandwiched therebetween, and an interlayer insulating layer 314 is provided on the gate electrodes 313. An opening 315 is formed in the interlayer insulating layer 314, and a gate terminal 316 electrically connected to the gate electrode 313 is provided inside the opening 315.

[0131] A gate insulating layer 317 made of zirconium oxide and a semiconductor layer 318 made of indium oxide are sequentially stacked on the inner wall of the trench 312. A source terminal 319 is electrically connected to one end of the semiconductor layer 318, and a drain terminal 320 is electrically connected to the other end of the semiconductor layer 318.

[0132] The nonvolatile memory device 300 having the above structure includes two nonvolatile memory elements, in which the gate electrode 313 and the semiconductor layer 318 face each other inside the trench 312 with the gate insulating layer 317 interposed therebetween.

[0133] Simple description Fig. 6A 1 is a method for manufacturing a nonvolatile memory device 300 shown in FIG. First, an SOI substrate is prepared, phosphorus (P) is added to the silicon layer on the box-shaped oxide film by ion implantation, and then the phosphorus is activated. Thus, an n-type silicon layer is formed on the silicon substrate (silicon substrate 310) via the box-shaped oxide film (bottom layer 311). After the n-type silicon layer is formed, the n-type silicon layer is subjected to a thermal oxidation treatment to reduce the film thickness of the n-type silicon layer. At this time, the thermal oxidation film formed by the thermal oxidation treatment is retained as it is and used as an interlayer insulating layer 314.

[0134] After the thermal oxidation treatment of the n-type silicon layer is completed, a through hole is formed that penetrates the thermal oxide film and the n-type silicon layer and reaches the box oxide film. The through hole is equivalent to Fig. 6A The trench 312 is shown. The trench 312 is formed by combining a patterning process using electron beam drawing and a RIE (Reactive Ion Etching) process.

[0135] After forming the trench 312, the n-type silicon layer and the thermal oxide film are patterned to form an island pattern. Fig. 6A The gate electrode 313 and the interlayer insulating layer 314 shown in the figure correspond to the patterned n-type silicon layer and the thermal oxide layer, respectively. The patterned n-type silicon layer and the thermal oxide film are divided into two parts by the trench 312. That is, two patterned n-type silicon layers and two patterned thermal oxide films are formed at this time.

[0136] After the patterning of the n-type silicon layer and the thermal oxide film is completed, a gate insulating layer 317 composed of an antiferroelectric is formed inside the groove 312. Here, a 10nm zirconium oxide layer is formed as the gate insulating layer 317 by the ALD method. The film formation is performed at room temperature. Next, patterning is performed by etching, and after patterning, the gate insulating layer 317 is subjected to RTA (Rapid Thermal Anneal) at 600°C. This annealing treatment is performed to crystallize the gate insulating layer 317.

[0137] After the gate insulating layer 317 was crystallized, a 10 nm indium oxide layer was formed on the gate insulating layer 317 by the ALD method as a semiconductor layer 318 composed of an oxide semiconductor. The film formation was performed at 200° C. Next, patterning was performed by etching, and after patterning, the semiconductor layer 318 was heat-treated in an ozone atmosphere at 200° C. This heat treatment was performed to reduce oxygen defects in the semiconductor layer 318 and improve the function as a semiconductor.

[0138] After forming the semiconductor layer 318, a source terminal 319 and a drain terminal 320 are formed. The source terminal 319 and the drain terminal 320 are formed by patterning the titanium nitride layer. Next, an opening 315 is formed in the interlayer insulating layer 314, and a gate terminal 316 is formed in the opening 315. The gate terminal 316 is formed by patterning the stacked structure of the titanium nitride layer and the titanium layer.

[0139] Figure 6B FIG. 2 is a diagram showing a cross-sectional TEM photograph of the vicinity of the trench of the prototype nonvolatile memory device 300. Figure 6B , a case where a hafnium oxide layer (HfO2) as a ferroelectric is used as a gate insulating layer is shown, but in the case of the above-mentioned nonvolatile memory device 300, a gate insulating layer using a zirconium oxide layer instead of the hafnium oxide layer is similarly produced. Figure 6B As shown, since the ALD method is used as the film forming method of the gate insulating layer 317 and the semiconductor layer 318, it can be understood that the film is formed with a uniform film thickness on the inner wall surface of the trench. In order to realize stable memory device operation, it is desirable to make the film thickness of the gate insulating layer 317 and the semiconductor layer 318 uniform.

[0140] Next, the electrical characteristics of the nonvolatile memory device 300 manufactured by the above-mentioned manufacturing method will be described. Fig. 6A The nonvolatile memory device 300 shown has a structure in which two nonvolatile memory elements are connected in series. Therefore, when measuring the electrical characteristics, one nonvolatile memory element is turned on and the electrical characteristics of the other nonvolatile memory element are measured.

[0141] Figure 7 1 is a graph showing Id-Vg characteristics measured using a nonvolatile memory device 300 according to an embodiment of the present invention. The channel length (Lg) of the nonvolatile memory device 300 is 50 nm, and the gate width ( Fig. 6A The length in the depth direction of the gate electrode 313) is 20μm. The voltage between the source and the drain (Vds) is 50mV. The gate voltage (Vg) is scanned within the range (-3V to 0V) where no erase / program action occurs. In addition, the program voltage (PGM) is uniformly set to +5V. Regarding the erase voltage (ERS), the Id-Vg characteristics at -5V, -5.5V, -6V, -6.5V and -7V were measured respectively. As a result, it can be confirmed that the prototype non-volatile memory device 300 performs the memory device action normally with almost no dependence on the erase voltage.

[0142] Fig. 8A This is a graph showing the results of measuring the overwrite resistance of a nonvolatile storage device 300 according to one embodiment of the present invention at room temperature. The horizontal axis represents the stress cycle, and the vertical axis represents the threshold. The square dots represent the values ​​at the write program voltage (+5V), and the round dots represent the values ​​at the write erase voltage (-7V). Fig. 8A As shown in FIG. 1 , it can be seen that the prototype nonvolatile memory device 300 has a 1×10 3 It shows stable anti-overwrite performance about times.

[0143] Figure 8B This is a diagram showing the measurement results of the retention characteristics of a nonvolatile storage device 300 according to one embodiment of the present invention at room temperature. The horizontal axis represents time, and the vertical axis represents the threshold value. The square dots represent the values ​​when the program voltage (+5V) is written, and the round dots represent the values ​​when the erase voltage (-7V) is written. Figure 8B As shown in FIG. 1 , it can be seen that the prototype nonvolatile memory device 300 has a storage capacity of up to 1×10 3 It shows stable holding characteristics for about seconds.

[0144] [Simulation results]

[0145] The inventors based on Figure 3A The AFeFET model shown simulates the dependence of electrical characteristics on various parameters. Each simulation result will be described below. In the following description, the terms "storage window" and "action point" are defined as above. That is, the storage window refers to the ratio of the drain current (read current) in the program state to the drain current in the deleted state in the AFeTFT model (that is, the drain current ratio when reading). In addition, the action point refers to the intersection of the polarization characteristic curve of the antiferroelectric capacitor and the load curve of the MOS transistor in the AFeTFT model.

[0146] First, the relationship between the electrical characteristics and the carrier concentration (N d )’s dependence on the simulation results.

[0147] Fig. 9A To illustrate the effect of changing the carrier concentration (N d ) is a diagram showing the simulation results of the Id-Vg characteristics under the condition of . Fig. 9B To illustrate the effect of changing the carrier concentration (N d ) is a diagram showing simulation results of the operating point analysis in the case of . Fig.10 To show the storage window in the AFeFET model versus the carrier concentration (N d )’s dependency graph.

[0148] The simulation conditions are basically the same as above. Figure 3A The conditions used in the simulation of the AFeFET model shown in the figure are the same. For example, the gate length and gate width are 50 μm, respectively, and the source-drain voltage (Vds) is 0.1 V. In addition, the composition of the antiferroelectric used as the gate insulating layer is Hf 0.2 Zr 0.8 That is, a composite oxide obtained by substituting a part (20 mol%) of zirconium in zirconium oxide with hafnium is used as the gate insulating layer. The film thickness (t AFe ) and the film thickness of the channel (oxide semiconductor layer) (t OS ) are 10nm respectively. In addition, the flat band voltage (V FB ) is set to -1.0 V. On the other hand, the carrier concentration (N d ) is set to be higher than the above Figure 3A The simulation conditions used in the AFeFET model shown are 1×10 19 cm -3 The low value is 1.2×10 17 cm -3 , 2.4×10 17 cm -3 , 4.8×10 17 cm -3 , 6.0×10 17 cm -3 , 7.2×10 17 cm -3 , 9.6×10 17 cm -3 , 1.2×10 18 cm -3 or 2.4×10 18 cm -3 .

[0149] like Fig. 9A as well as Fig.10 As shown in the figure, it can be seen that as the carrier concentration (N d ), the difference between the drain current in the program state and the drain current in the delete state increases slightly, and the storage window increases slightly. The reason for the increase in the storage window is that the amount of change in the drain current in the delete state is greater than the amount of change in the drain current in the program state.

[0150] like Fig. 9B As shown, as the carrier concentration (N d ) decreases, the load curve 32 shifts to the left (negative direction), so the operating point 33 in the program state and the operating point 34 in the delete state also shift to the left. At this time, in the delete state, since the operating point 34 is close to the subthreshold region (that is, close to the flat region 35 of the load curve 32), the charge balance is maintained at a low charge density, resulting in a smaller drain current. As described above, as the carrier concentration (N d ) is reduced, the drain current in the deleted state is significantly reduced compared with the drain current in the program state, so the drain current ratio during reading, that is, the storage window, is increased.

[0151] Next, the relationship between the electrical characteristics of the channel (oxide semiconductor layer) and the film thickness (t OS )’s dependence on the simulation results.

[0152] Fig.11A FIG. 1 is a diagram showing simulation results of Id-Vg characteristics when the film thickness of the oxide semiconductor layer is changed in the AFeFET model. Fig. 11B A diagram showing simulation results of an operating point analysis when the film thickness of the oxide semiconductor layer is changed in the AFeFET model. Fig.12 Graph showing the dependence of the memory window in the AFeFET model on the film thickness of the oxide semiconductor layer.

[0153] The simulation conditions are basically the same as those used Fig. 9A as well as Fig. 9B The conditions of the simulations described above are the same. However, the carrier concentration (Nd) is fixed at 1.2×10 18 cm -3 In addition, the film thickness of the oxide semiconductor layer (t OS ) is set to 3nm, 4nm, 5nm, 7nm, 10nm or 15nm.

[0154] like Fig.11A as well as Fig.12 As shown in the figure, it can be seen that as the film thickness of the oxide semiconductor layer (t OS), the difference between the drain current in the program state and the drain current in the erase state increases slightly, and the storage window increases slightly. In addition, as Fig. 11B As shown, even if the film thickness of the oxide semiconductor layer (t OS ) changes, and there is almost no shift in the position of the load curve 32, and no significant changes are seen in the positions of the operating point 33 of the program state and the operating point 34 of the delete state. Therefore, it can be seen that in the AFeFET model, the film thickness of the oxide semiconductor layer has little effect on the memory window.

[0155] Next, the effect of the electrical characteristics based on the AFeFET model on the film thickness (t AFe )’s dependence on the simulation results.

[0156] Fig.13A It is a diagram showing the simulation results of the Id-Vg characteristics when the film thickness of the antiferroelectric layer is changed in the AFeFET model. Fig. 13B This is a diagram showing simulation results of an operating point analysis when the film thickness of the antiferroelectric layer is changed in the AFeFET model. Fig.14 is a graph showing the dependence of the memory window on the film thickness of the antiferroelectric layer in the AFeFET model.

[0157] The simulation conditions are basically the same as those used Fig. 9A as well as Fig. 9B The conditions of the simulations described are the same. However, the carrier concentration (N d ) is fixed at 4.8×10 17 cm -3 The film thickness of the antiferroelectric layer (t AFe ) is set to 3nm, 4nm, 5nm, 7nm, 10nm or 15nm.

[0158] like Fig.13A and Fig.14 As shown in the figure, it can be seen that as the film thickness of the antiferroelectric layer (t AFe ) increases, the difference between the drain current in the program state and the drain current in the erase state becomes larger, and the storage window increases significantly. In particular, Fig.13A In the results shown, a significant reduction of the drain current in the erased state can be read.

[0159] like Fig. 13B As shown in the figure, it can be seen that when the film thickness of the antiferroelectric layer (t AFe) increases, the position of the load curve 32 does not change, and the polarization characteristic curve 31 shifts downward. When the film thickness of the antiferroelectric layer increases, the paraelectric dielectric composition of the antiferroelectric capacitor decreases, and the polarization characteristic curve 31 shifts downward. As a result, both the action point 33 in the program state and the action point 34 in the delete state shift downward. At this time, in the delete state, since the action point 34 is close to the subthreshold region, the charge balance is maintained at a low charge density, resulting in a smaller drain current.

[0160] As mentioned above, as the film thickness of the antiferroelectric layer (t AFe ) increases, the drain current in the erase state is significantly reduced compared to the drain current in the program state, so the storage window becomes larger. As mentioned above, the film thickness (t AFe ) is preferably greater than 5 nm and less than 50 nm, more preferably greater than 8 nm and less than 30 nm, and most preferably greater than 10 nm and less than 20 nm.

[0161] Next, the simulation results of the dependence of the electric characteristics on the composition of the antiferroelectric based on the AFeFET model will be described.

[0162] Fig.15A FIG. 1 is a diagram showing simulation results of Id-Vg characteristics when the composition of the antiferroelectric is changed in the AFeFET model. Fig. 15B This is a diagram showing the simulation results of the operating point analysis when the composition of the antiferroelectric is changed in the AFeFET model. Fig. 15B Two load curves 32 are shown, as will be described later.

[0163] The simulation conditions are basically the same as those used Fig. 9A as well as Fig. 9B The conditions of the simulations described are the same. However, the carrier concentration (N d ) is fixed at 1.2×10 18 cm -3 , the film thickness of the oxide semiconductor layer (t OS ) is fixed at 5nm. The composition of the antiferroelectric is Hf 0.1 Zr 0.9 O2、Hf 0.2 Zr 0.8 O2 or Hf 0.3 Zr 0.7 That is, the total amount of zirconium in zirconium oxide as an antiferroelectric is set to 100 mol%, and 10 mol%, 20 mol% or 30 mol% of the zirconium is replaced by a composite oxide of hafnium. In addition, the flat band voltage (V FB ) are -0.5V and -1.0V respectively.

[0164] like Fig.15AAs shown in FIG. 1 , when the composition of the antiferroelectric changes, the Id-Vg characteristic also changes. Specifically, it is found that the smaller the zirconium content in the antiferroelectric, the more the Id-Vg characteristic shifts to the right (positive direction). In addition, as Fig. 15B As shown in FIG. 3 , it can be seen that the smaller the zirconium content in the antiferroelectric, the more the polarization characteristic curve 31 shifts to the left (negative direction). Fig. 15B In, Hf 0.2 Zr 0.8 O2 and Hf 0.1 Zr 0.9 In the case of O2, the flat band voltage is -1.0V, Hf 0.3 Zr 0.7 In the case of O2, the flat band voltage is -0.5 V. The reason is that when the zirconium content is 80 mol% and 90 mol%, the flat band voltage needs to be set to -1.0 V so that V g =0 V, but when the zirconium content is 70 mol %, since the polarization characteristic curve 31 is shifted to the left as a whole, a flat band voltage of -0.5 V is sufficient.

[0165] A small absolute value of the flat band voltage means a small work function difference between the gate electrode material and the oxide semiconductor material. That is, when the zirconium content in the gate insulating layer is reduced, there is an advantage of increasing the options for the combination of the gate electrode material and the oxide semiconductor material when setting an appropriate work function difference.

[0166] like Fig. 15B As shown in the figure, when the zirconium content is 70 mol%, the operating point 33 in the program state shifts upward, so the drain current in the charge accumulation region becomes larger. On the contrary, since the operating point 34 in the erase state shifts downward, it approaches the subthreshold region and the drain current becomes smaller. Therefore, since the difference between the drain current in the program state and the drain current in the erase state becomes larger, the storage window becomes larger.

[0167] As described above, it can be seen that as the zirconium content in the gate insulating layer decreases, the memory window tends to increase. Fig.15A as well as Fig. 15B The simulation results shown in the figure show that when the zirconium content is 70 mol%, the drain current ratio during reading as the memory window is more than 10. However, it is known that as the zirconium content decreases, ferroelectric characteristics are gradually exhibited instead of antiferroelectric characteristics. Therefore, referring to the options of the combination of the gate electrode material and the oxide semiconductor material, in the case of Hf as the gate insulating layer (antiferroelectric) x Zr 1-x In O2, preferably 0.1≤x≤0.4, more preferably 0.15≤x≤0.35, and most preferably 0.2≤x≤0.3.

[0168] Next, simulation results of the dependence of electrical characteristics on fixed charges based on the AFeFET model will be described.

[0169] Fig.16A : is a diagram showing the simulation result of Id-Vg characteristics in the case where the fixed charge is changed in the AFeFET model. Fig. 16B A diagram showing simulation results of an operating point analysis when the fixed charge is changed in the AFeFET model.

[0170] The simulation conditions are basically the same as those used Fig. 9A as well as Fig. 9B The conditions of the simulations described are the same. However, the carrier concentration (N d ) is fixed at 1.2×10 18 cm -3 , the composition of the antiferroelectric is Hf 0.3 Zr 0.7 O2, film thickness (t OS ) is fixed at 5nm. In addition, the flat band voltage is -0.57V. Fixed charge (Q f ) is set to -2μC / cm 2 、-1μC / cm 2 , 0μC / cm 2 , 1μC / cm 2 or 2μC / cm 2 .

[0171] like Fig.16A As shown in , the smaller the fixed charge (the larger the absolute value of the negative fixed charge), the more the Id-Vg characteristic shifts to the right (positive direction). Fig. 16B As shown in FIG. 1 , the smaller the fixed charge, the more the flat area 35 of the load curve 32 shifts upward. Therefore, since the operating point 34 in the deleted state is close to the subthreshold region, the drain current in the deleted state becomes smaller. From the above content, it can be seen that the smaller the fixed charge, the larger the storage window. This trend is consistent with the use of Figure 4A and Figure 4B The results of the description are the same.

[0172] A person skilled in the art may appropriately add, delete, or design changes to constituent elements, or add, omit steps, or change conditions based on the nonvolatile storage device as one embodiment of the present invention, and as long as the gist of the present invention is maintained, the changes are within the scope of the present invention.

[0173] Furthermore, even if other effects are different from the effects obtained by the above-mentioned embodiments, effects that are clear from the description of this specification or that can be easily predicted by those skilled in the art can be understood as effects that can be obtained by the present invention.

[0174] Description of Reference Numerals

[0175] 31: Polarization characteristic curve, 32: Load curve, 33, 34: Operating point, 35: Flat area, 20: Non-volatile memory element, 110: Substrate, 120: Source electrode, 130: Drain electrode, 140: Source terminal, 150: Drain terminal, 160: Gate terminal, 170: Passivation layer, 210: Semiconductor layer, 220: Gate insulating layer, 230: Gate electrode, 240: Insulating layer, 250: Filling component, 310: Silicon substrate, 311: Bottom layer, 312: Channel, 313: Gate electrode, 314: Interlayer insulating layer, 315: Opening, 316: Gate terminal, 317: Gate insulating layer, 318: Semiconductor layer, 319: Source terminal, 320: Drain terminal.

Claims

1. A nonvolatile storage device comprising a plurality of nonvolatile storage elements, wherein: The non-volatile storage element comprises: a semiconductor layer comprising a metal oxide; a gate electrode opposite to the semiconductor layer; and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, The electron affinity of the first material constituting the gate electrode is lower than the electron affinity of the second material constituting the semiconductor layer, and the second material is an n-type semiconductor.

2. A nonvolatile storage device comprising a plurality of nonvolatile storage elements, wherein: The non-volatile storage element comprises: a semiconductor layer comprising a metal oxide; a gate electrode opposite to the semiconductor layer; and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, The electron affinity of the first material constituting the gate electrode is greater than the electron affinity of the second material constituting the semiconductor layer, and the second material is a p-type semiconductor.

3. A non-volatile storage device comprising a plurality of non-volatile storage elements, wherein: The non-volatile storage element comprises: a semiconductor layer comprising a metal oxide; a gate electrode, which is opposite to the semiconductor layer; a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode; and an interface layer disposed between the gate insulating layer and the gate electrode, The electron affinity of the first material constituting the gate electrode is less than the electron affinity of the second material constituting the semiconductor layer, and the second material is an n-type semiconductor, The interface layer is made of silicon oxide.

4. The nonvolatile storage device according to claim 1 or 3, wherein: The gate insulating layer has a -2μC / cm 2 To -1μC / cm 2 of fixed charge.

5. The nonvolatile storage device according to claim 1 or 3, wherein: The metal oxide is Sn oxide or a composite oxide of In and Zn, The electron affinity of the first material is 4.9 eV or less.

6. The nonvolatile memory device according to claim 5, wherein: The first material is n-type doped Si and / or Ge.

7. The nonvolatile memory device according to claim 5, wherein: The first material is a metal material.

8. The nonvolatile storage device according to claim 1 or 3, wherein: The metal oxide is an oxide of In or a composite oxide of In, Ga and Zn, The electron affinity of the first material is 4.3 eV or less.

9. The nonvolatile memory device according to claim 8, wherein: The first material is n-type doped Si and / or Ge.

10. The nonvolatile memory device according to claim 8, wherein: The first material is a metal material.

11. A non-volatile storage device comprising a plurality of non-volatile storage elements, wherein: The non-volatile storage element comprises: a semiconductor layer comprising a metal oxide; a gate electrode opposite to the semiconductor layer; and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, The metal oxide is Sn oxide or a composite oxide of In and Zn, and the electron affinity of the first material constituting the gate electrode is 4.9 eV or less.

12. A nonvolatile storage device comprising a plurality of nonvolatile storage elements, wherein: The non-volatile storage element comprises: a semiconductor layer comprising a metal oxide; a gate electrode opposite to the semiconductor layer; and a gate insulating layer composed of an antiferroelectric disposed between the semiconductor layer and the gate electrode, The metal oxide is an oxide of In or a composite oxide of In, Ga and Zn, and the electron affinity of the first material constituting the gate electrode is 4.3 eV or less.

13. The nonvolatile memory device according to claim 1, 2, 3, 11 or 12, wherein: The antiferroelectric is composed of Hf x Zr 1-x A composite oxide represented by O2 (0≤x≤0.4).

14. The nonvolatile memory device according to claim 1, 2, 3, 11 or 12, wherein: The gate insulating layer has a thickness of 5 nm to 50 nm.